Asphalt-based hard carbon material as well as preparation method and application thereof

The use of peroxynitric acid treatment and subsequent pre-carbonization and carbonization processes on asphalt to create pitch-based hard carbon materials addresses the low capacity and rate performance issues, resulting in improved electrochemical properties and higher charge and discharge efficiencies for sodium-ion batteries.

CN119079973APending Publication Date: 2024-12-06WUHAN BISIDI BATTERY MATERIAL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411195511.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing asphalt-based hard carbon materials for sodium-ion batteries suffer from low capacity and poor rate performance due to uncontrollable liquid phase carbonization, leading to small interlayer spacing and orientation, and existing modifications do not effectively improve electrochemical performance.

Method used

A method involving the use of peroxynitric acid to treat asphalt, followed by pre-carbonization and carbonization, which introduces nitrogen doping and pore formation through deep oxidation and cross-linking, enhancing electrical conductivity and electrochemical properties.

Benefits of technology

The resulting pitch-based hard carbon material exhibits improved rate performance and capacity, with enhanced electrical conductivity and electrochemical properties, as demonstrated by higher charge and discharge efficiencies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005016262390000011
    Figure HDA0005016262390000011
  • Figure HDA0005016262390000012
    Figure HDA0005016262390000012
Patent Text Reader

Abstract

The invention belongs to the technical field of battery materials, and particularly relates to an asphalt-based hard carbon material as well as a preparation method and application thereof. The preparation method comprises the following steps: mixing asphalt and peroxynitric acid substances for reaction to obtain a mixed material, and then performing pre-carbonization and carbonization treatment on the mixed material to prepare the asphalt-based hard carbon material. According to the present invention, the peroxy-nitric acid substance is used to treat the asphalt, such that the strong oxidizing property of the peroxy-nitric acid substance enables the asphalt to be deeply oxidized, such as the hydroxyl group is oxidized into the aldehyde group, and the cross-linking and carbon layer rearrangement effects can be provided; in addition, the peroxy-nitric acid substance also has a nitrogen doping effect, and nitrogen is introduced in the reaction process of the asphalt and the peroxy-nitric acid substance, so that the electrical conductivity of the finally obtained asphalt-based hard carbon material is improved, and the electrochemical performance of the asphalt-based hard carbon material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of battery materials, and in particular relates to a pitch-based hard carbon material and a preparation method and application thereof. Background Art

[0002] Since sodium resources are relatively abundant compared to lithium resources, sodium-ion batteries have gradually received attention and importance. The performance of sodium-ion batteries depends to a large extent on the electrode materials. As a key component of the battery, the negative electrode has an important impact on the practicality and cost of the battery. In the field of sodium-ion batteries, carbon-based materials, titanium-based materials, alloys, organic compounds, etc. are often used for the negative electrode. Among them, carbon-based materials have the advantages of high cost-effectiveness, high abundance, and adjustable structure. They are very promising negative electrode materials for sodium-ion batteries. Hard carbon is a highly amorphous structure with short-range graphitization. Compared with the graphite structure, the interlayer distance (0.37-0.42nm) of hard carbon is larger, with abundant voids or pores and abundant defects.

[0003] The precursor materials of hard carbon negative electrode materials for sodium ion batteries are mainly divided into four types: biomass precursors, sugar precursors, synthetic resin precursors, and asphalt precursors. Asphalt-based precursors have the advantages of low cost, high carbon content, and high carbon yield, and are considered to be potential carbon sources for synthetic carbon negative electrodes. Asphalt is a by-product of the coal or petroleum industry, mainly composed of a large number of polycyclic aromatic hydrocarbons (PAHs) and structurally related heterocyclic compounds. It has a low price and low ash content, and can be used to form nearly parallel carbon layers during heating to ensure high carbon yield and conductivity. However, direct pyrolysis of asphalt forms a microstructure with small interlayer spacing and high orientation during the uncontrollable liquid phase carbonization process, resulting in poor rate performance of sodium ion batteries. The hard carbon negative electrode materials obtained using asphalt in the prior art also have the problem of low capacity.

[0004] The prior art also attempts to modify asphalt to obtain porous carbon to improve the electrochemical performance of the battery. However, the porous carbon obtained by the existing modification method is not effective in improving battery performance and needs further improvement. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a pitch-based hard carbon material and a preparation method and application thereof. The pitch-based hard carbon material prepared by the preparation method of the present invention has high rate performance and capacity.

[0006] A first aspect of the present invention provides a method for preparing a pitch-based hard carbon material.

[0007] Specifically, a method for preparing a pitch-based hard carbon material comprises the following steps:

[0008] The asphalt is mixed with a peroxynitric acid substance to obtain a mixture, and then the mixture is subjected to pre-carbonization and carbonization treatment to obtain the asphalt-based hard carbon material.

[0009] The second aspect of the present invention provides a pitch-based hard carbon material prepared by the above-mentioned preparation method.

[0010] The third aspect of the present invention provides an application of a pitch-based hard carbon material, and specifically relates to a sodium ion battery, comprising the pitch-based hard carbon material.

[0011] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0012] The present invention provides a method for preparing an asphalt-based hard carbon material, including treatment of asphalt with peroxynitric acid, pre-carbonization and carbonization. The present invention uses peroxynitric acid to treat asphalt. First, the strong oxidizing property of peroxynitric acid causes deep oxidation of asphalt, such as oxidation of hydroxyl groups to aldehyde groups, and can also play a role in cross-linking and rearrangement of carbon layers; secondly, the peroxynitric acid mixes with asphalt to react, and the generated nitro and other groups will penetrate into the asphalt molecules. In the subsequent high-temperature treatment process such as carbonization, the nitro and other groups will react and escape, which can play a role in pore formation; in addition, the nitro and other groups may cause the escape of carbon atoms around them or carbon atoms connected to them, which will also play a role in pore formation.

[0013] In addition, pernitric acid substances also have the function of nitrogen doping. During the reaction of asphalt with pernitric acid substances, nitrogen element will be introduced, so that the electrical conductivity of the final asphalt-based hard carbon material is improved, thereby improving the electrochemical properties of the asphalt-based hard carbon material such as capacity and rate performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 The charge and discharge curves of button batteries assembled from asphalt-based hard carbon materials of Example 1 and Comparative Example 1;

[0015] Figure 2 This is a rate performance diagram of the button cell assembled from the asphalt-based hard carbon material of Example 1. DETAILED DESCRIPTION

[0016] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present application, and are not used to limit the present application.

[0017] In the description of the present application, the term "including" means "including but not limited to". Various embodiments of the present invention may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present invention; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0018] In this application, "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.

[0019] In the present application, "at least one", "at least one" and other similar descriptions specifically refer to one or more, one or more; "multiple", "multiple" and other similar descriptions specifically refer to two or more, two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all represent: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or plural, respectively.

[0020] A first aspect of the present invention provides a method for preparing a pitch-based hard carbon material, comprising: mixing asphalt with a peroxynitric acid-like substance to obtain a mixture, and then pre-carbonizing and carbonizing the mixture to obtain the pitch-based hard carbon material.

[0021] Specifically, the present invention provides a method for preparing a pitch-based hard carbon material, comprising the following steps:

[0022] Step S11: mixing asphalt with peroxynitric acid to obtain a mixture;

[0023] Step S12: subjecting the mixed material to the pre-carbonization treatment under a protective gas atmosphere to obtain a pre-carbonized material;

[0024] Step S13: subjecting the pre-carbonized material to the carbonization treatment under a protective gas atmosphere to obtain the pitch-based hard carbon material.

[0025] The present invention uses pernitric acid substances to treat asphalt. First, the strong oxidizing property of pernitric acid substances causes deep oxidation of asphalt, such as oxidation of hydroxyl groups to aldehyde groups, and can also play a role in cross-linking and rearrangement of carbon layers; secondly, pernitric acid substances react with asphalt to generate nitro groups and other groups that penetrate into the asphalt molecules. In subsequent high-temperature treatment processes such as carbonization, nitro groups and other groups will react and escape, which can play a role in pore formation; in addition, nitro groups and other groups may cause the escape of carbon atoms around them or carbon atoms connected to them when they escape, which can also play a role in pore formation. In addition, pernitric acid substances also have the effect of nitrogen doping. Nitrogen elements will be introduced into asphalt during the reaction with pernitric acid substances, so that the conductivity of the final asphalt-based hard carbon material is improved. The electrochemical properties such as capacity and rate of the final prepared asphalt-based hard carbon material can be improved by pore formation and nitrogen doping.

[0026] In step S11:

[0027] In some embodiments of the present invention, the peroxynitric acid substance may include at least one of peroxynitric acid, peroxynitrous acid or peroxynitrite. The peroxynitrite may specifically include one or more of sodium peroxynitrite and / or potassium peroxynitrite. The mass ratio of the asphalt to the peroxynitric acid substance is 2-5:1, specifically, 2:1, 3:1, 4:1, 5:1, etc.

[0028] In some embodiments, the peroxynitric acid substance is mixed with asphalt in the form of an aqueous solution, that is, the peroxynitric acid substance aqueous solution is mixed with asphalt. Specifically, the concentration of the peroxynitric acid substance aqueous solution can be 1-2 mol / L, for example, 1.5-2 mol / L.

[0029] In some embodiments of the present invention, the asphalt includes coal tar or petroleum tar. The use of coal tar helps to reduce production costs. Further, the softening point of the asphalt is not less than 150°C, for example, the softening point is 200-300°C, more specifically, for example, 150°C, 200°C, 280°C, 300°C. The sulfur content of the asphalt is less than 0.1wt% (wt% means weight percentage), for example, 0.01wt%-0.08wt%. Low sulfur content is conducive to reducing the adverse effects of impurities on the electrochemical properties of asphalt-based hard carbon materials.

[0030] In some embodiments of the present invention, the D of the asphalt 50 Less than or equal to 10 μm. For example, less than or equal to 6 μm, specifically 1 μm, 5 μm, 6 μm, 9 μm. Smaller particle size helps to increase the contact area between asphalt and peroxynitric acid substances, making the reaction more complete.

[0031] In some embodiments of the present invention, the temperature of the mixed reaction is 30-50°C, and the time is 1-12h. For example, the temperature of the mixed reaction can be 30°C, 40°C, or 50°C; the time of the mixed reaction can be 2-12h, 4-6h, and more specifically 1h, 2h, 4h, 6h, or 12h. In this embodiment, on the one hand, the mixed reaction at a relatively low temperature (30-50°C) can achieve oxidative crosslinking; on the other hand, within this temperature range, peroxide nitric acid substances can exist stably, and the mixed reaction has good safety.

[0032] It is understandable that the mixing reaction method may include known mixing methods such as stirring or ultrasound. In a specific embodiment, asphalt is stirred and mixed with peroxynitric acid substances, and heated to react under stirring to obtain a mixture.

[0033] It is understandable that the mixing reaction can be carried out in an air atmosphere, or in a protective atmosphere such as nitrogen, argon, etc.

[0034] In some embodiments, after step S11 and before step S12, that is, before the mixture is pre-carbonized, the process further includes: nitrifying the mixture. Specifically, the nitrification process includes: adding water to the mixture, heating, and obtaining a nitrified mixture.

[0035] Specifically, the heating temperature during the nitration treatment may be 70-90°C, for example 75-80°C, specifically 75°C, 80°C, 85°C, 90°C, etc.

[0036] The water may include at least one of distilled water, ultrapure water or deionized water, and specifically, the distilled water may be double distilled water. The mass of the added water may be more than twice the mass of the mixture, for example, 3-10 times, specifically 3 times, 5 times, 8 times, 10 times, etc., so as to fully dilute the nitrate ions and increase further contact with the asphalt.

[0037] In this embodiment, after the peroxide nitric acid substance is consumed in step S11, more than 2 times of water is added to the mixture in this step to dilute the nitrate ions and the like generated by the reaction of the peroxide nitric acid substance, and the mixture is heated to 70-90°C for reaction, which can promote further contact between the nitric acid substance and the asphalt and the nitration reaction, thereby deepening the degree of asphalt nitration. Nitration is accompanied by oxidation side reactions, leading to the formation of nitrate ions, phenolic groups, carbonyl groups and sulfoxide groups, which is conducive to the increase of disorder and electronic conductivity of the final asphalt-based hard carbon material.

[0038] In step S12:

[0039] The protective gas includes nitrogen or a rare gas. The rare gas is, for example, one of argon, helium, and krypton. It is understood that the present invention may refer to the description herein for any use of a protective gas.

[0040] In some embodiments of the present invention, the temperature of the pre-carbonization treatment is 400-900° C., for example, 400-750° C., 400-900° C. The time of the pre-carbonization treatment can be 1-5 hours, for example, 2-4 hours.

[0041] In some embodiments of the present invention, after the pre-carbonization treatment is completed, the pre-carbonized material is crushed. For example, crushed to D 50 To 1-10μm, more specific D 50 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, and 10μm.

[0042] In step S13:

[0043] In some embodiments of the present invention, the carbonization temperature is 1200-1700° C., and the time is 0.5-4 hours. Specifically, the carbonization temperature can be 1200-1300° C., 1300-1500° C., 1500-1700° C., etc. The carbonization time can be 0.5-1 hour, 1-2 hours, 2-3 hours, 3-4 hours, etc.

[0044] In some embodiments of the present invention, after step S13, that is, after the carbonization treatment is completed, a coating treatment is further included, and the coating treatment process includes: mixing the material after the carbonization treatment with the coating asphalt, and then heating and coating the material under a protective gas atmosphere to obtain an asphalt-based hard carbon material. The coating treatment can reduce the surface defects of the material obtained after the carbonization, thereby improving the electrochemical performance of the hard carbon negative electrode material (for example, improving the charge specific capacity).

[0045] Specifically, the coating asphalt can be selected from petroleum asphalt with a softening point of 220-280° C. The weight of the coating asphalt used is 5%-12% of the weight of the material after carbonization treatment. For example, 5%-10%. Specifically, for example, 5%, 10%, 12%.

[0046] In some embodiments of the present invention, the temperature of the heat coating treatment is 1200-1700° C., and the time is 1-3 hours. Further, the temperature of the heat coating treatment is 1300-1500° C., and the time is 0.5-1.5 hours.

[0047] In some embodiments of the present invention, the heating and coating process further includes a crushing process, wherein the material after the carbonization process and the coated asphalt are mixed and crushed to D50 The thickness is 2-8 μm, for example, 3-8 μm, more specifically, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, and 8 μm.

[0048] A second aspect of the present invention provides a pitch-based hard carbon material, which is prepared by the method for preparing a pitch-based hard carbon material provided by the present invention.

[0049] The third aspect of the present invention provides an application of a pitch-based hard carbon material, which can be specifically applied to sodium ion batteries, for example, it can be used as a negative electrode material of a sodium ion battery.

[0050] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0051] Example 1

[0052] A method for preparing a pitch-based hard carbon material, comprising the following steps:

[0053] Step (1): Treatment of peroxynitric acid

[0054] Coal tar pitch (softening point 200°C) containing less than 0.1 wt% sulfur was mixed with a 2 mol / L aqueous solution of peroxynitric acid in a mass ratio of 3:1. 50 ≤6μm, the mixing process is to mix at 50°C with a magnetic stirrer at 100 rpm for 4h to obtain a mixture;

[0055] Step (2): Nitrification

[0056] Adding double distilled water to the mixture of step (1), and placing it in a hot oven at 80° C. overnight to obtain a nitrated mixture;

[0057] Step (3): Pre-carbonization

[0058] The nitrated mixed material obtained in step (2) is added into a tubular furnace, and heated to 750° C. for pre-carbonization for 2 h under the protection of an inert gas (argon), and the cooled block is crushed to obtain a pre-carbonized material powder;

[0059] Step (4): Carbonization

[0060] The pre-carbonized material powder obtained in step (3) is placed in a tubular furnace, and heated to 1300° C. for high-temperature carbonization treatment for 2 h under the protection of an inert gas (argon) to obtain a powdered carbon material;

[0061] Step (5): Coating

[0062] The carbon material obtained in step (4) is mixed with coated asphalt (the coated asphalt is petroleum asphalt with a softening point of 220°C, and the weight of the coated asphalt is 10% of the carbon material), and the mixture is fully crushed and mixed by a powder grinder to control the particle size D 50 The mixture is then placed in a tubular furnace and heated to 1300°C under the protection of an inert gas (argon) for coating treatment for 1 hour to obtain a pitch-based hard carbon material.

[0063] Example 2

[0064] A method for preparing a pitch-based hard carbon material, comprising the following steps:

[0065] Step (1): Treatment of peroxynitric acid

[0066] Coal tar pitch (softening point 200°C) containing less than 0.1 wt% sulfur was mixed with a 2 mol / L aqueous solution of peroxynitric acid in a mass ratio of 3:1. 50 ≤6μm, the mixing process is to mix at 50°C with a magnetic stirrer at 100 rpm for 4h to obtain a mixture;

[0067] Step (2): Pre-carbonization

[0068] The mixed material obtained in step (1) is added into a tubular furnace, and heated to 750° C. for pre-carbonization treatment for 2 h under the protection of an inert gas (argon), and the cooled block is crushed to obtain a pre-carbonized material powder;

[0069] Step (3): Carbonization

[0070] The pre-carbonized material powder obtained in step (2) is placed in a tubular furnace, and heated to 1300° C. for high-temperature carbonization treatment for 2 h under the protection of an inert gas (argon) to obtain a powdered carbon material;

[0071] Step (4): Coating

[0072] The carbon material obtained in step (3) is mixed with coated asphalt (the coated asphalt is petroleum asphalt with a softening point of 220°C, and the weight of the coated asphalt is 10% of the carbon material), and the mixture is fully crushed and mixed by a powder grinder to control the particle size D 50 The mixture is then placed in a tubular furnace and heated to 1300°C under the protection of an inert gas (argon) for coating treatment for 1 hour to obtain a pitch-based hard carbon material.

[0073] Example 3

[0074] A method for preparing a pitch-based hard carbon material, comprising the following steps:

[0075] Step (1): Treatment of peroxynitric acid

[0076] Coal tar pitch (softening point 200°C) containing less than 0.1 wt% sulfur was mixed with a 2 mol / L aqueous solution of peroxynitric acid in a mass ratio of 3:1. 50 ≤6μm, the mixing process is to mix at 50°C with a magnetic stirrer at 100 rpm for 4h to obtain a mixture;

[0077] Step (2): Nitrification

[0078] Adding double distilled water to the mixture of step (1), and placing it in a hot oven at 80° C. overnight to obtain a nitrated mixture;

[0079] Step (3): Pre-carbonization

[0080] The nitrated mixed material obtained in step (2) is added into a tubular furnace, and heated to 750° C. for pre-carbonization for 2 h under the protection of an inert gas (argon), and the cooled block is crushed to obtain a pre-carbonized material powder;

[0081] Step (4): Carbonization

[0082] The pre-carbonized material powder obtained in step (3) is placed in a tubular furnace, and heated to 1300° C. for high-temperature carbonization treatment for 2 hours under the protection of an inert gas (argon) to obtain a pitch-based hard carbon material.

[0083] Example 4

[0084] Compared with Example 1, the only difference of Example 4 is that the stirring time of step (1) of Example 4 is 1 hour, and the rest of the process is the same as that of Example 1.

[0085] Example 5

[0086] Compared with Example 1, the only difference of Example 5 is that the stirring time of step (1) of Example 5 is 12 hours, and the rest of the process is the same as Example 1.

[0087] Example 6

[0088] Compared with Example 1, the only difference of Example 6 is that in step (1) of Example 6, coal tar and a 2 mol / L aqueous solution of pernitric acid are mixed in a mass ratio of 2:1, and the rest of the process is the same as that of Example 1.

[0089] Example 7

[0090] Compared with Example 1, the only difference of Example 7 is that in step (1) of Example 7, coal tar and a 2 mol / L aqueous solution of pernitric acid are mixed in a mass ratio of 4:1, and the rest of the process is the same as that of Example 1.

[0091] Example 8

[0092] Compared with Example 1, the only difference of Example 8 is that in step (1) of Example 8, coal tar and a 2 mol / L aqueous solution of pernitric acid are mixed in a mass ratio of 5:1, and the rest of the process is the same as that of Example 1.

[0093] Comparative Example 1

[0094] A method for preparing a pitch-based hard carbon material, comprising the following steps:

[0095] Step (1): Oxygen pre-oxidation treatment

[0096] Coal tar pitch (softening point of 200° C.) containing less than 0.1 wt% sulfur is placed in a muffle furnace and oxidized at 180° C. for 2 h to obtain a mixed material;

[0097] Step (2): Pre-carbonization

[0098] The mixed material obtained in step (1) is added into a tubular furnace, and heated to 750° C. for pre-carbonization treatment for 2 h under the protection of an inert gas (argon), and the cooled block is crushed to obtain a pre-carbonized material powder;

[0099] Step (3): Carbonization

[0100] The pre-carbonized material powder obtained in step (2) is placed in a tubular furnace, and heated to 1300° C. for high-temperature carbonization treatment for 2 h under the protection of an inert gas (argon) to obtain a powdered carbon material;

[0101] Step (4): Coating

[0102] The carbon material obtained in step (3) is mixed with coated asphalt (the coated asphalt is petroleum asphalt with a softening point of 220°C, and the weight of the coated asphalt is 10% of the carbon material), and the mixture is fully crushed and mixed by a powder grinder to control the particle size D 50 The mixture is then placed in a tubular furnace and heated to 1300°C under the protection of an inert gas (argon) for coating treatment for 1 hour to obtain a pitch-based hard carbon material.

[0103] Comparative Example 2

[0104] A method for preparing a pitch-based hard carbon material, comprising the following steps:

[0105] Step (1): Treatment with concentrated nitric acid

[0106] Coal tar pitch (softening point 200°C) containing less than 0.1 wt% sulfur was mixed with concentrated nitric acid (8 mol / L) in a mass ratio of 3:1. 50 ≤6μm, the mixing process is to mix at 160°C with a magnetic stirrer at 100 rpm for 2h to obtain a mixed material;

[0107] Step (2): Clean and dry

[0108] The mixture obtained in step (1) was washed with deionized water until it was neutral, and then dried in an oven at 80° C. for 12 h to obtain a dry mixture;

[0109] Step (3): Pre-carbonization

[0110] The dried mixed material obtained in step (2) is added into a tube furnace, and heated to 750° C. for pre-carbonization for 2 h under the protection of an inert gas (argon), and the cooled block is crushed to obtain a pre-carbonized material powder;

[0111] Step (4): Carbonization

[0112] The pre-carbonized material powder obtained in step (3) is placed in a tubular furnace, and heated to 1300° C. for high-temperature carbonization treatment for 2 h under the protection of an inert gas (argon) to obtain a powdered carbon material;

[0113] Step (5): Coating

[0114] The carbon material obtained in step (4) is mixed with coated asphalt (the coated asphalt is petroleum asphalt with a softening point of 220°C, and the weight of the coated asphalt is 10% of the carbon material), and the mixture is fully crushed and mixed by a powder grinder to control the particle size D 50 The mixture is then placed in a tubular furnace and heated to 1300°C under the protection of an inert gas (argon) for coating treatment for 1 hour to obtain a pitch-based hard carbon material.

[0115] Comparative Example 3

[0116] Compared with Example 1, the difference of Comparative Example 3 is that, in step (1) of Comparative Example 3, a mixture of equal masses of concentrated sulfuric acid and concentrated nitric acid (the concentration of the concentrated sulfuric acid is 18.4 mol / L, the concentration of the concentrated nitric acid is 8 mol / L, and the concentrated sulfuric acid and the concentrated nitric acid are mixed in a volume ratio of 1:1 to obtain a mixture) is used to replace the aqueous peroxynitric acid solution in Example 1, and the rest of the process is the same as Example 1.

[0117] Product effect testing

[0118] The asphalt-based hard carbon materials obtained in the above Examples 1-8 and Comparative Examples 1-3 were respectively prepared into button-type batteries.

[0119] The specific steps for preparing button batteries are as follows: asphalt-based hard carbon material is mixed with conductive carbon Super-P and PVDF (polyvinylidene fluoride) in a mass ratio of 92:3:3, and then N-methylpyrrolidone (NMP) is used as solvent. After mixing evenly, it is coated on aluminum foil and dried in a vacuum oven at 102°C. After rolling, it is cut into circular electrode sheets with a diameter of 8mm, with sodium sheets as the negative electrode, the electrolyte is a NaPF6 lipid electrolyte of model NP-001, and the diaphragm is a glass fiber diaphragm. The button batteries are assembled in a glove box filled with argon.

[0120] The charge and discharge performance of the prepared button battery was tested. The battery test adopted the Xinwei battery test system. The test method adopted constant current and constant voltage discharge and constant current charging. The charge and discharge test was carried out at a current density of 0.1C. The discharge cut-off voltage was 0V and the charge cut-off voltage was 2.5V. The results are shown in Table 1.

[0121] The rate performance of the button cell prepared in Example 1 was tested. The battery test was conducted using a Xinwei battery test system. The test method used constant current charge and discharge. The charge and discharge tests were conducted at current densities of 0.1C, 0.5C, 1C, and 5C, respectively. The discharge cut-off voltage was 0V, and the charge cut-off voltage was 2.5V. The results are as follows: Figure 2 As shown, from Figure 2 It can be seen that the button cell corresponding to Example 1 still maintains a high specific capacity even at 1C and 5C rates, indicating that the asphalt-based hard carbon material corresponding to Example 1 has good rate performance.

[0122] Table 1

[0123] Charge capacity (mAh / g) Charge and discharge efficiency (%) Example 1 313.95 86.19 Example 2 293.56 86.05 Example 3 308.59 83.52 Example 4 286.52 81.79 Example 5 314.81 86.08 Example 6 310.52 87.29 Example 7 299.59 86.22 Example 8 292.11 86.35 Comparative Example 1 226.03 79.91 Comparative Example 2 276.59 84.99 Comparative Example 3 281.52 85.59

[0124] It can be seen from Table 1 that the charging specific capacities corresponding to Examples 1-8 of the present invention are significantly higher than those of Comparative Examples 1-3.

[0125] Compared with Example 1, step (1) of comparative example 1 adopts oxygen pre-oxidation treatment, which results in a significant decrease in the charge capacity and charge-discharge efficiency of the asphalt-based hard carbon material prepared in comparative example 1. This indicates that the treatment with peroxynitric acid-like substances in step (1) of the present invention and the nitration treatment in step (2) can enhance the charge capacity and charge-discharge efficiency of the asphalt-based hard carbon material. Figure 1 The charge and discharge curves of button batteries assembled from asphalt-based hard carbon materials in Example 1 and Comparative Example 1 are shown in Table 1. Figure 1 It can also be seen that the charge and discharge specific capacity corresponding to Example 1 is significantly higher than that of Comparative Example 1.

[0126] Compared with Example 1, the step (1) of Comparative Example 2 uses concentrated nitric acid treatment instead of the steps (1) and (2) of the present invention, resulting in a significant decrease in the charge capacity and charge-discharge efficiency of the pitch-based hard carbon material prepared in Comparative Example 2. This shows that the treatment with peroxynitric acid in step (1) of the present invention and the nitration treatment in step (2) can enhance the charge capacity and charge-discharge efficiency of the pitch-based hard carbon material.

[0127] Compared with Example 1, the step (1) of Comparative Example 3 uses a mixture of concentrated sulfuric acid and concentrated nitric acid of equal mass to replace the aqueous peroxynitric acid solution in Example 1, resulting in a significant decrease in the charge specific capacity and charge-discharge efficiency of the pitch-based hard carbon material prepared in Comparative Example 3. This shows that the treatment with peroxynitric acid in step (1) of the present invention and the nitration treatment in step (2) can enhance the charge specific capacity and charge-discharge efficiency of the pitch-based hard carbon material.

[0128] Compared with Example 1, Example 2 does not have the nitration treatment of step (2), resulting in a decrease in the charging capacity and charge-discharge efficiency of the asphalt-based hard carbon material of Example 2, indicating that the nitration treatment of step (2) helps to improve the charging capacity and charge-discharge efficiency of the asphalt-based hard carbon material.

[0129] Compared with Example 1, Example 3 did not undergo coating treatment, resulting in a decrease in the charging capacity and charge-discharge efficiency of the asphalt-based hard carbon material of Example 3, indicating that coating treatment helps to improve the charging capacity and charge-discharge efficiency of the asphalt-based hard carbon material.

Claims

1. A method for preparing a pitch-based hard carbon material, characterized in that: The following steps are involved: The asphalt is mixed with a peroxynitric acid substance to react to obtain a mixture, and then the mixture is pre-carbonized and carbonized to obtain the asphalt-based hard carbon material.

2. The preparation method according to claim 1, characterized in that: The peroxynitric acid substance includes at least one of peroxynitric acid, peroxynitrous acid or peroxynitrite, wherein the peroxynitrite includes sodium peroxynitrite and / or potassium peroxynitrite; And / or, the mass ratio of the asphalt to the peroxynitric acid substance is 2-5:1; And / or, the peroxynitric acid substance is mixed with asphalt in the form of an aqueous solution, and the concentration of the peroxynitric acid substance aqueous solution is 1-2 mol / L.

3. The preparation method according to claim 1, characterized in that: The pre-carbonization and carbonization treatment of the mixed material comprises: The mixed material is subjected to the pre-carbonization treatment under a protective gas atmosphere to obtain a pre-carbonized material; The pre-carbonized material is subjected to the carbonization treatment under a protective gas atmosphere to obtain the pitch-based hard carbon material.

4. The preparation method according to claim 3, characterized in that: The asphalt includes coal asphalt or petroleum asphalt; and / or, the softening point of the asphalt is not less than 150°C; and / or, the sulfur content of the asphalt is less than 0.1 wt%; and / or, the D of the asphalt 50 Less than or equal to 10μm; And / or, the temperature of the mixed reaction is 30-50° C., and the time of the mixed reaction is 1-12 h; And / or, the protective gas includes nitrogen or a rare gas; And / or, the temperature of the pre-carbonization treatment is 400-900°C; And / or, the pre-carbonization treatment time is 1-5h; and / or, after the pre-carbonization treatment is completed, the pre-carbonized material is crushed; And / or, the carbonization temperature is 1200-1700° C., and the time is 0.5-4 hours.

5. The preparation method according to claim 1 or 3, characterized in that: Before the mixed material is subjected to the pre-carbonization treatment, the mixed material is subjected to the nitrification treatment, and the nitrification treatment process includes: adding water to the mixed material, heating, and obtaining the nitrified mixed material.

6. The preparation method according to claim 5, characterized in that: The heating temperature during the nitration treatment is 70-90°C; And / or, during the nitrification treatment, the water includes at least one of distilled water, ultrapure water or deionized water; And / or, during the nitrification process, the mass of the water is twice or more than the mass of the mixture.

7. The preparation method according to claim 3, characterized in that: After the carbonization treatment is completed, a coating treatment is also included. The coating treatment process includes: mixing the material after the carbonization treatment with coating asphalt, and then heating and coating under a protective gas atmosphere to obtain an asphalt-based hard carbon material.

8. The preparation method according to claim 7, characterized in that: The softening point of the coated asphalt is petroleum asphalt of 220-280°C; and / or, the weight of the coated asphalt is 5%-12% of the weight of the material after the carbonization treatment; And / or, the heating and coating treatment further includes a crushing treatment before the carbonization treatment, wherein the material mixed with the coated asphalt is crushed to D 50 2-8μm; And / or, the temperature of the heating coating treatment is 1200-1700° C., and the time is 1-3 hours.

9. A pitch-based hard carbon material, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 8.

10. A sodium ion battery, characterized in that: Includes the pitch-based hard carbon material as described in claim 9.

Citation Information

Patent Citations

  • Nitric acid and / or nitrate modified carbon-based negative electrode material and preparation method and application thereof

    CN111987293A

  • Asphalt-based hard carbon negative electrode material, preparation method and sodium ion battery

    CN115611264A

  • Asphalt-based hard carbon, preparation method and application of asphalt-based hard carbon in sodium-ion battery

    CN116573632A

  • Asphalt-based carbon material as well as preparation method and application thereof

    CN117945391A

  • Carbon powder having enhanced electrical characteristics and use of same

    CN1318209A