Aluminum oxide sheet with high radius-thickness ratio and preparation method

By using aluminum source slurry of aluminum hydroxide and sodium oxide in the preparation of alumina sheets, combined with crystal growth regulators and molten salts, the diameter-thickness ratio of the alumina sheets was successfully improved, and the oxidation in the prior art was solved The problem of limited application of aluminum sheets improves grinding efficiency and the pass rate of polishing products.

CN119080042APending Publication Date: 2024-12-06CHALCO SHANDONG CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411267840.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art is difficult to prepare alumina sheets with a diameter-thickness ratio of more than 40, which limits its application range.

Method used

The aluminum source slurry includes aluminum hydroxide and sodium oxide, and then hydrothermal reaction, drying, calcining and purification are carried out after stirring and mixing. The thickness and twinning degree of the aluminum source slurry are adjusted by using crystal growth regulators and molten salts to improve the thickness and twinning degree of the aluminum source slurry. The diameter-thickness ratio of the aluminum oxide flakes.

Benefits of technology

The alumina sheet has a diameter-thickness ratio of more than 40, which improves its application flexibility and grinding efficiency, and improves the pass rate of polished products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080042A_ABST
    Figure CN119080042A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of aluminum oxide products, in particular to an aluminum oxide sheet with a high radius-thickness ratio and a preparation method. The preparation method comprises the following steps: stirring and mixing an auxiliary agent and aluminum source slurry to obtain a dispersion system; performing hydrothermal reaction on the dispersion system to obtain precursor slurry; drying the precursor slurry to obtain flaky precursor powder; roasting the fused salt and the flaky precursor powder to obtain a roasted material; and carrying out purification treatment on the roasted material to obtain an aluminum oxide sheet, wherein the auxiliary agent comprises a crystal growth regulator, and the weight m1 of the crystal growth regulator and the weight m2 of the aluminum hydroxide meet the relational expression: m1: m2 = (0.2-15): 100; the mass m3 of the fused salt and the weight m4 of the flaky precursor powder meet the relational expression: m3: m4 = (1: 4)-(1: 6). The preparation method can improve the radius-thickness ratio of the aluminum oxide sheet to be greater than 40.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of preparation of aluminum oxide products, and in particular to an aluminum oxide sheet with a high aspect ratio and a preparation method thereof. Background Art

[0002] Flake aluminum oxide is a functional powder material with excellent performance. It has obvious scaly structural characteristics and a large diameter-to-thickness ratio, and belongs to α-Al2O3. Flake aluminum oxide has the advantages of high hardness, high melting point, excellent corrosion resistance, high temperature resistance and high thermal conductivity. It can be widely used in fine abrasive polishing, thermal conductive fillers, pearlescent pigments, microelectronics processing, functional coatings and other fields. Among them, the flake aluminum oxide used for abrasive polishing has a hard crystal structure and a flat plate structure, and the particles of the flake aluminum oxide powder are arranged neatly, which can increase the friction between the flake aluminum oxide abrasive and the product, which undoubtedly speeds up the grinding speed of the flake aluminum oxide abrasive. In addition, compared with conventional nano-alumina, flake aluminum oxide with a flat and smooth flake surface is not easy to scratch the object being ground (such as semiconductor silicon wafers, smart phone housings, etc.), and the qualified product rate of the product can be increased by 10% to 15%.

[0003] At present, the main preparation methods of flaky aluminum oxide include solid phase sintering method, hydrothermal method, molten salt method, sol-gel method, etc. However, the diameter-to-thickness ratio of flaky aluminum oxide obtained by these methods is difficult to reach more than 40, which makes the current application of flaky aluminum oxide very limited. Summary of the invention

[0004] The present application provides an aluminum oxide sheet with a high aspect ratio and a preparation method thereof, so as to solve the following technical problem: how to improve the aspect ratio of the aluminum oxide sheet.

[0005] In a first aspect, the present application provides a method for preparing an aluminum oxide sheet with a high aspect ratio, wherein the raw material of the preparation method comprises an aluminum source slurry, the chemical composition of the aluminum source slurry comprises aluminum hydroxide and sodium oxide, the mass concentration of the aluminum hydroxide is 100 g / L to 200 g / L, and the mass concentration of the sodium oxide is 10 g / L to 5 g / L; the preparation method comprises:

[0006] The auxiliary agent and the aluminum source slurry are stirred and mixed to obtain a dispersed system;

[0007] subjecting the dispersed system to a hydrothermal reaction to obtain a precursor slurry;

[0008] Drying the precursor slurry to obtain a flake precursor powder;

[0009] calcining the molten salt and the flake precursor powder to obtain a calcined material; and

[0010] Purifying the calcined material to obtain aluminum oxide flakes;

[0011] Wherein, the auxiliary agent includes a crystal growth regulator, and the weight m1 of the crystal growth regulator and the weight m2 of the aluminum hydroxide satisfy the relationship: m1:m2=(0.2-15):100;

[0012] The mass m3 of the molten salt and the weight m4 of the flaky precursor powder satisfy the relationship: m3:m4=(1:4)~(1:6).

[0013] Optionally, the crystal growth regulator includes phosphate and / or titanium salt; when the crystal growth regulator includes phosphate, the weight m5 of the phosphate and the weight m2 of the aluminum hydroxide satisfy the relationship: m5:m2=(0.1-5):100;

[0014] In the case where the crystal growth regulator includes a titanium salt, the weight m6 of the titanium salt and the weight m2 of the aluminum hydroxide satisfy the relationship: m6:m2=(0.1-1):100.

[0015] Optionally, in the case where the crystal growth regulator includes a phosphate, the phosphate includes phosphorus pentoxide and / or sodium phosphate dodecahydrate;

[0016] In the case where the crystal growth regulator comprises a titanium salt, the titanium salt comprises titanium dioxide and / or titanyl sulfate.

[0017] Optionally, the auxiliary agent further includes a dispersant, and the weight m7 of the dispersant and the weight m2 of the aluminum hydroxide satisfy the relationship: m7:m2=(0.01-0.5):100;

[0018] The type of the dispersant includes at least one of the following:

[0019] Polyethylene glycol, sodium carboxymethylcellulose, polyacrylate and sodium maleate.

[0020] Optionally, the auxiliary agent further includes a guiding agent, and the weight m8 of the guiding agent and the weight m2 of the aluminum hydroxide satisfy the relationship: m8:m2=(0.5-10):100;

[0021] The types of directing agents include pseudo-boehmite and / or boehmite.

[0022] Optionally, the type of the molten salt includes at least one of the following:

[0023] Sodium sulfate, potassium sulfate, sodium chloride, potassium chloride, sodium fluoride and potassium fluoride.

[0024] Optionally, the hydrothermal reaction includes a hydrothermal heating section and a hydrothermal insulation section, the terminal temperature of the hydrothermal heating section is 170°C to 230°C, the heating rate of the hydrothermal heating section is 1°C / min to 3°C / min, and the time of the hydrothermal insulation section is 0h to 4h.

[0025] Optionally, the calcination temperature is 1100° C. to 1350° C., and the calcination time is 2 h to 5 h.

[0026] Optionally, the drying temperature is less than 230°C.

[0027] In a second aspect, the present application provides an aluminum oxide flake with a high aspect ratio, wherein the aluminum oxide flake is obtained by the preparation method described in the first aspect, and the aspect ratio of the aluminum oxide flake is greater than 40.

[0028] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0029] The present invention provides a method for preparing an aluminum oxide sheet with a high aspect ratio. The raw materials of the preparation method include an aluminum source slurry. The chemical composition of the aluminum source slurry includes aluminum hydroxide and sodium oxide. The mass concentration of the aluminum hydroxide is 100 g / L to 200 g / L, and the mass concentration of the sodium oxide is 10 g / L to 5 g / L. The preparation method comprises: stirring and mixing an auxiliary agent and the aluminum source slurry to obtain a dispersed system; subjecting the dispersed system to a hydrothermal reaction to obtain a precursor slurry; and The material is dried to obtain a flaky precursor powder; the molten salt and the flaky precursor powder are calcined to obtain a calcined material; the calcined material is purified to obtain an aluminum oxide flake; wherein the auxiliary agent includes a crystal growth regulator, and the weight m1 of the crystal growth regulator and the weight m2 of the aluminum hydroxide satisfy the relationship: m1:m2=(0.2-15):100; the mass m3 of the molten salt and the weight m4 of the flaky precursor powder satisfy the relationship: m3:m4=(1:4)-(1:6). The aluminum source slurry used in the preparation method satisfies: the chemical composition of the aluminum source slurry may include aluminum hydroxide and sodium oxide, and the mass concentration of aluminum hydroxide may be 100g / L to 200g / L, and the mass concentration of sodium oxide may be 10g / L to 5g / L, which can promote the aluminum source slurry to have sufficient aluminum hydroxide and sodium oxide, so as to facilitate the subsequent auxiliary agent to fully combine with the aluminum source slurry to obtain a dispersed system; in addition, the auxiliary agent may include a crystal growth regulator, and the weight m1 of the crystal growth regulator and the total weight m2 of the aluminum hydroxide in the aluminum source slurry may satisfy the relationship: m1:m2=(0.2-15):100, in the subsequent hydrothermal reaction During the process, the crystal growth regulator of the auxiliary agent in the dispersion system can be used to adjust the thickness of the flat surface of aluminum hydroxide in the aluminum source slurry, and induce the crystal growth of the flat surface of aluminum hydroxide to increase the aspect ratio of the flat surface of alumina, thereby increasing the aspect ratio of the alumina flakes; in addition, the mass m3 of the molten salt and the weight m4 of the flaky precursor powder can satisfy the relationship: m3:m4=(1:4)~(1:6), and sufficient molten salt can be provided in the roasting stage. Sufficient molten salt can control the twinning and agglomeration degree of the flaky precursor powder in the roasting stage, thereby increasing the aspect ratio of the flat surface of the flaky precursor powder, and further increasing the aspect ratio of the alumina flakes. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0031] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0032] Figure 1 A schematic flow chart of a method for preparing an aluminum oxide sheet with a high aspect ratio provided in an embodiment of the present application;

[0033] Figure 2 This is a scanning electron microscope image of a flake precursor powder in a method for preparing an aluminum oxide flake with a high aspect ratio provided in Example 1 of the present application;

[0034] Figure 3 A scanning electron microscope image of an aluminum oxide sheet with a high aspect ratio provided in Example 1 of the present application in one direction;

[0035] Figure 4 A scanning electron microscope image of another direction of an aluminum oxide sheet with a high aspect ratio provided in Example 1 of the present application;

[0036] Figure 5 An X-ray diffraction pattern of an aluminum oxide flake with a high aspect ratio provided in Example 1 of the present application. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0038] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity and should not be understood as a rigid limitation on the scope of the present application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values ​​within the range; for example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which applies regardless of the range; in addition, whenever a numerical range is indicated in this document, it is meant to include any cited numbers (fractions or integers) within the indicated range.

[0039] In this document, the terms including "including" and "including" mean "including but not limited to". Relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. "And / or" describes the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone; where A and B can be singular or plural. "At least one" means one or more, and "plurality" means two or more; "at least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single or plural items; for example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple. Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0040] Figure 1 The schematic diagram of the process of preparing an aluminum oxide sheet with a high aspect ratio provided in an embodiment of the present application is exemplarily shown;

[0041] like Figure 1 As shown, the embodiment of the present application provides a method for preparing an aluminum oxide sheet with a high aspect ratio, wherein the raw material of the preparation method includes an aluminum source slurry, the chemical composition of the aluminum source slurry includes aluminum hydroxide and sodium oxide, the mass concentration of the aluminum hydroxide is 100g / L to 200g / L, and the mass concentration of the sodium oxide is 10g / L to 5g / L; the preparation method comprises:

[0042] S1. stirring and mixing the additive and the aluminum source slurry to obtain a dispersed system;

[0043] S2. subjecting the dispersed system to a hydrothermal reaction to obtain a precursor slurry;

[0044] S3. Drying the precursor slurry to obtain a flaky precursor powder;

[0045] S4. calcining the molten salt and the flaky precursor powder to obtain a calcined material; and

[0046] S5. The calcined material is purified to obtain an alumina sheet;

[0047] Wherein, the auxiliary agent includes a crystal growth regulator, and the weight m1 of the crystal growth regulator and the weight m2 of the aluminum hydroxide satisfy the relationship: m1:m2=(0.2-15):100;

[0048] The mass m3 of the molten salt and the weight m4 of the flaky precursor powder satisfy the relationship: m3:m4=(1:4)~(1:6).

[0049] The weight m1 of the crystal growth regulator and the weight m2 of aluminum hydroxide can satisfy the relationship: m1:m2=0.2:100, 0.5:100, 1.0:100, 1.5:100, 2.0:100, 2.5:100, 3.0:100, 3.5:100, 4.0:100, 4.5:100, 5.0:100, 5.5:100, 6.0:100, 6.5:100, 7.0:100 , 7.5:100, 7.0:100, 7.5:100, 8.0:100, 8.5:100, 9.0:100, 9.5:100, 10.0:100, 10.5:100, 11.0:100, 11.5:100, 12.0:100, 12.5:100, 13.0:100, 13.5:100, 14.0:100, 14.5:100, or 15.0:100.

[0050] The mass m3 of the molten salt and the weight m4 of the flaky precursor powder may satisfy the relationship: m3:m4=1:4, 1:5 or 1:6.

[0051] It should be noted that the preparation method of the aluminum source slurry can be first using sodium aluminate solution as raw material, and adding aluminum hydroxide seeds to the sodium aluminate solution to promote the decomposition of the sodium aluminate solution to generate a micro-powder aluminum hydroxide slurry, and then removing the adsorbed alkaline substances in the micro-powder aluminum hydroxide slurry, and finally adding water to the micro-powder aluminum hydroxide slurry from which the adsorbed alkaline substances have been removed to obtain an aluminum source slurry.

[0052] It should be noted that the aluminum hydroxide seed crystals can be prepared by a seed separation method or a carbon separation method, the particle size of the aluminum hydroxide seed crystals satisfies D50<4.5μm, and the weight m9 of the aluminum hydroxide seed crystals and the weight m10 of the sodium aluminate solution satisfy the relationship: m9:m10=(0.5~5):100.

[0053] It should be noted that the sodium aluminate solution can be prepared by sintering, Bayer process or aluminum hydroxide re-dissolution method to obtain a crude sodium aluminate solution, and then finely filtered to obtain the α K It is 1.4 to 1.7.

[0054] It should be noted that the hydrothermal reaction can be carried out in a reactor, and during the hydrothermal reaction, the volume V1 of the dispersed system and the total volume V2 of the reactor satisfy the relationship: V1:V2≤70:100.

[0055] It should be noted that the purification treatment includes cooling, washing, refining treatment, drying, crushing and grading in sequence. The cooling method can be natural cooling or slow cooling controlled by a cooling program. The washing water used for the washing can be reverse osmosis water, deionized water or distilled water. The refining treatment can use a dispersant solution such as sodium hexametaphosphate to depolymerize and grade the washed roasted material, and then wash and separate the depolymerized and graded roasted material. The dispersant solution can be the same as or different from the composition of the aforementioned dispersant. When the dispersant solution is sodium hexametaphosphate, the weight of the sodium hexametaphosphate can be 0.1% to 0.3% of the weight of the dispersant solution.

[0056] In some optional embodiments, the crystal growth regulator includes phosphate and / or titanium salt; when the crystal growth regulator includes phosphate, the weight m5 of the phosphate and the weight m2 of the aluminum hydroxide satisfy the relationship: m5:m2=(0.1-5):100;

[0057] In the case where the crystal growth regulator includes a titanium salt, the weight m6 of the titanium salt and the weight m2 of the aluminum hydroxide satisfy the relationship: m6:m2=(0.1-1):100;

[0058] In these embodiments, the crystal growth regulator may include phosphate and / or titanium salt, and in the case where the crystal growth regulator includes phosphate, the weight m5 of the phosphate and the weight m2 of the aluminum hydroxide may satisfy the relationship: m5:m2=(0.1~5):100, which can encourage the dispersed system to have a sufficient amount of phosphate, and a sufficient amount of phosphate can control the morphology and thickness of the aluminum hydroxide to reduce the risk of twinning and agglomeration of aluminum hydroxide, thereby adjusting the thickness of the flat surface of aluminum hydroxide in the aluminum source slurry and inducing the crystal growth of the flat surface of aluminum hydroxide to increase the aspect ratio of the flat surface of aluminum oxide; in addition, in the case where the crystal growth regulator includes titanium salt, the weight m6 of the titanium salt and the weight m2 of the aluminum hydroxide may satisfy the relationship: m6:m2=(0.1~1):100, which can encourage the dispersed system to have a sufficient amount of titanium salt, and a sufficient amount of titanium salt can effectively reduce the thickness of the flat surface of aluminum hydroxide to increase the aspect ratio of the flat surface of aluminum hydroxide.

[0059] The weight m5 of the phosphate and the weight m2 of the aluminum hydroxide can satisfy the relationship: m5:m2=0.1:100, 0.2:100, 0.5:100, 1.0:100, 1.5:100, 2.0:100, 2.5:100, 3.0:100, 3.5:100, 4.0:100, 4.5:100 or 5.0:100.

[0060] The weight m6 of the titanium salt and the weight m2 of the aluminum hydroxide can satisfy the relationship: m6:m2=0.1:100, 0.2:100, 0.3:100, 0.4:100, 0.5:100, 0.6:100, 0.7:100, 0.8:100, 0.9:100 or 1.0:100.

[0061] In some optional embodiments, when the crystal growth regulator includes a phosphate, the phosphate includes phosphorus pentoxide and / or sodium phosphate dodecahydrate;

[0062] In the case where the crystal growth regulator comprises a titanium salt, the titanium salt comprises titanium dioxide and / or titanyl sulfate;

[0063] In these embodiments, when the crystal growth regulator includes a phosphate, the phosphate includes phosphorus pentoxide and / or sodium phosphate dodecahydrate. Additionally, when the crystal growth regulator includes a titanium salt, the titanium salt may include titanium dioxide and / or titanium oxysulfate. The thickness of the flat surface of aluminum hydroxide in the aluminum source slurry can be further adjusted by using phosphates and iron salts, thereby improving the aspect ratio of the flat surface of aluminum hydroxide.

[0064] In some optional embodiments, the auxiliary agent further includes a dispersant, and the weight m7 of the dispersant and the weight m2 of the aluminum hydroxide satisfy the relationship: m7:m2=(0.01-0.5):100;

[0065] The type of the dispersant includes at least one of the following:

[0066] polyethylene glycol, sodium carboxymethylcellulose, polyacrylate, and sodium maleate;

[0067] In these embodiments, the auxiliary agent may also include a dispersant, and the weight m7 of the dispersant and the weight m2 of the aluminum hydroxide may satisfy the relationship: m7:m2=(0.01-0.5):100. In addition, the types of dispersants may include: at least one of polyethylene glycol, sodium carboxymethyl cellulose, polyacrylate and sodium maleate, which may promote the presence of a sufficient amount of dispersant in the aluminum source slurry. A sufficient amount of dispersant may promote sufficient and uniform dispersion between the aluminum source slurry and the seed growth regulator to obtain a dispersed system with a better degree of dispersion, thereby effectively adjusting the aspect ratio of the flat surface of aluminum hydroxide to improve the aspect ratio of the flat surface of aluminum hydroxide.

[0068] The weight m7 of the dispersant and the weight m2 of aluminum hydroxide may satisfy the relationship: m7:m2=0.01:100, 0.02:100, 0.05:100, 0.1:100, 0.2:100, 0.3:100, 0.4:100 or 0.5:100.

[0069] In some optional embodiments, the auxiliary agent further includes a directing agent, and the weight m8 of the directing agent and the weight m2 of the aluminum hydroxide satisfy the relationship: m8:m2=(0.5-10):100;

[0070] The types of the directing agent include pseudo-boehmite and / or boehmite;

[0071] In these embodiments, the auxiliary agent may also include a directing agent, and the weight m8 of the directing agent and the weight m2 of the aluminum hydroxide may satisfy the relationship: m8:m2=(0.5-10):100. In addition, the type of the directing agent may include pseudo-boehmite and / or boehmite, which may enable the aluminum source slurry to have a sufficient amount of the directing agent. A sufficient amount of the directing agent may further enable the seed growth regulator and the dispersant to effectively adjust the aspect ratio of the flat surface of the aluminum hydroxide, thereby improving the aspect ratio of the flat surface of the aluminum hydroxide.

[0072] The weight m8 of the directing agent and the weight m2 of aluminum hydroxide can satisfy the relationship: m8:m2=0.5:100, 1.5:100, 2.0:100, 2.5:100, 3.0:100, 3.5:100, 4.0:100, 4.5:100, 5.0:100, 5.5:100, 6.0:100, 6.5:100, 7.0:100, 7.5:100, 8.0:100, 8.5:100, 9.0:100, 9.5:100 or 10.0:100.

[0073] In some optional embodiments, the type of the molten salt includes at least one of the following:

[0074] Sodium sulfate, potassium sulfate, sodium chloride, potassium chloride, sodium fluoride and potassium fluoride;

[0075] In these embodiments, the types of molten salts may include: at least one of sodium sulfate, potassium sulfate, sodium chloride, potassium chloride, sodium fluoride and potassium fluoride. The molten salts may be used during the calcination stage to control the twinning and agglomeration degree of the flaky precursor powder, thereby improving the aspect ratio of the flat surface of the flaky precursor powder.

[0076] It should be noted that the molten salt may use a molten salt product with an industrial purity of more than 98%.

[0077] In some optional embodiments, the hydrothermal reaction includes a hydrothermal heating section and a hydrothermal insulation section, the terminal temperature of the hydrothermal heating section is 170°C to 230°C, the heating rate of the hydrothermal heating section is 1°C / min to 3°C / min, and the time of the hydrothermal insulation section is 0h to 4h;

[0078] In these embodiments, the hydrothermal reaction may include a hydrothermal heating section and a hydrothermal insulation section, and the terminal temperature of the hydrothermal heating section may be 170°C to 230°C, and the heating rate of the hydrothermal heating section may be 1°C / min to 3°C / min, and the time of the hydrothermal insulation section is 0h to 4h, which can prompt the additive in the dispersed system to adjust the thickness of the flat surface of aluminum hydroxide in the aluminum source slurry to induce the crystal growth of the flat surface of aluminum hydroxide, thereby improving the diameter-to-thickness ratio of the flat surface of aluminum oxide.

[0079] The terminal temperature of the hydrothermal heating stage can be 170°C, 180°C, 190°C, 200°C, 210°C, 220°C or 230°C.

[0080] The heating rate of the hydrothermal heating stage can be 1°C / min, 1.5°C / min, 2.0°C / min, 2.5°C / min or 3.0°C / min.

[0081] In some optional embodiments, the calcination temperature is 1100° C. to 1350° C., and the calcination time is 2 h to 5 h;

[0082] In these embodiments, the calcination temperature can be 1100°C to 1350°C, and the calcination time can be 2h to 5h. The flaky precursor powder with a high aspect ratio can be converted into alumina flakes with a high aspect ratio by calcination to increase the aspect ratio of the flat surface of the alumina.

[0083] The calcination temperature may be 1100°C, 1150°C, 1200°C, 1250°C, 1300°C or 1350°C.

[0084] The calcination time may be 2 h, 2.5 h, 3.0 h, 3.5 h, 4.0 h, 4.5 h or 5.0 h.

[0085] It should be noted that the roasting can be carried out in equipment such as a muffle furnace, a tunnel kiln, a push plate kiln, a roller kiln, and a microwave heating kiln.

[0086] In some optional embodiments, the drying temperature is less than 230°C;

[0087] In these embodiments, the drying temperature may be less than 230° C., so as to avoid the excessively high drying temperature from prematurely converting the precursor slurry into alumina flakes, thereby affecting the calcination effect.

[0088] It should be noted that the drying method may be flash drying, spray drying, oven drying, drying chamber drying, etc.

[0089] Based on a general inventive concept, the present application provides an aluminum oxide sheet with a high aspect ratio, wherein the aluminum oxide sheet is obtained by the preparation method, and the aspect ratio of the aluminum oxide sheet is greater than 40.

[0090] The aluminum oxide flakes are realized based on the above-mentioned preparation method. The specific steps of the preparation method can refer to the above-mentioned embodiments. Since the aluminum oxide flakes adopt part or all of the technical solutions of the above-mentioned embodiments, they at least have all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be described one by one here.

[0091] The present application is further described below in conjunction with specific examples. The experimental methods in the following examples that do not specify specific conditions are usually measured according to industry standards; if there are no corresponding industry standards, they are carried out according to common international standards, conventional conditions, or conditions recommended by the manufacturer.

[0092] Example 1

[0093] A method for preparing an aluminum oxide sheet with a high aspect ratio, wherein the raw materials of the preparation method include an aluminum source slurry, the chemical composition of the aluminum source slurry includes aluminum hydroxide and sodium oxide, the mass concentration of the aluminum hydroxide is 150 g / L, and the mass concentration of the sodium oxide is 8 g / L; the method comprises:

[0094] S1. stirring and mixing the additive and the aluminum source slurry to obtain a dispersed system;

[0095] S2. subjecting the dispersed system to a hydrothermal reaction in a reactor to obtain a precursor slurry;

[0096] S3. Drying the precursor slurry to obtain a flaky precursor powder;

[0097] S4. calcining the molten salt and the flaky precursor powder to obtain a calcined material; and

[0098] S5. The calcined material is purified to obtain an alumina sheet;

[0099] The preparation process of the aluminum source slurry includes: adding aluminum hydroxide seeds with a particle size of 3.9 μm to a sintered sodium aluminate solution for seed separation to obtain an aluminum hydroxide filter cake, and adding distilled water to prepare a 150 g / L slurry; the aluminum hydroxide seeds are prepared by a carbon separation method;

[0100] The auxiliary agent includes a crystal growth regulator, and the weight m1 of the crystal growth regulator and the weight m2 of the aluminum hydroxide satisfy the relationship: m1:m2=3:100;

[0101] The mass m3 of the molten salt and the weight m4 of the flaky precursor powder satisfy the relationship: m3:m4=1:4.

[0102] The crystal growth regulator is phosphate, and the weight m5 of the phosphate and the weight m2 of the aluminum hydroxide satisfy the relationship:

[0103] m5:m2=3:100.

[0104] The phosphate is sodium phosphate dodecahydrate.

[0105] The additive also includes a dispersant, and the weight of the dispersant m7 and the weight of the aluminum hydroxide m2 satisfy the relationship: m7:m2=0.5:100;

[0106] The type of dispersant is sodium polyacrylate.

[0107] The auxiliary agent also includes a guiding agent, and the weight of the guiding agent m8 and the weight of the aluminum hydroxide m2 satisfy the relationship: m8:m2=0.5:100;

[0108] The type of directing agent is boehmite.

[0109] The type of molten salt is a mixture of sodium sulfate and potassium sulfate, and the weight m11 of the sodium sulfate and the weight m12 of the potassium sulfate satisfy the relationship: m11:m12=1:2.

[0110] The volume V1 of the dispersed system and the total volume V2 of the reactor satisfy the relationship: V1:V2=70:100.

[0111] The hydrothermal reaction includes a hydrothermal heating section and a hydrothermal insulation section. The terminal temperature of the hydrothermal heating section is 200°C, the heating rate of the hydrothermal heating section is 2°C / min, and the time of the hydrothermal insulation section is 2h.

[0112] The calcination temperature is 1200°C, the calcination heating rate is 2°C / min, and the calcination time is 5h.

[0113] The drying temperature was 150°C.

[0114] Example 2

[0115] Based on the contents disclosed in Example 1, the following modifications are further made:

[0116] The auxiliary agent includes a crystal growth regulator, and the weight m1 of the crystal growth regulator and the weight m2 of the aluminum hydroxide satisfy the relationship: m1:m2=1:100;

[0117] The mass m3 of the molten salt and the weight m4 of the flaky precursor powder satisfy the relationship: m3:m4=1:4.

[0118] The crystal growth regulator is titanium salt, and the weight m6 of the titanium salt and the weight m2 of aluminum hydroxide satisfy the relationship: m6:m2=1:100.

[0119] The titanium salt is titanyl sulfate.

[0120] The additive also includes a dispersant, and the weight of the dispersant m7 and the weight of the aluminum hydroxide m2 satisfy the relationship: m7:m2=0.5:100;

[0121] The type of dispersant is polyethylene glycol.

[0122] The auxiliary agent also includes a guiding agent, and the weight m8 of the guiding agent and the weight m2 of the aluminum hydroxide satisfy the relationship: m8:m2=1:100;

[0123] The type of directing agent is boehmite.

[0124] The type of molten salt is a mixture of sodium sulfate and potassium sulfate, and the weight m11 of the sodium sulfate and the weight m12 of the potassium sulfate satisfy the relationship: m11:m12=1:2.

[0125] The hydrothermal reaction includes a hydrothermal heating section and a hydrothermal insulation section. The terminal temperature of the hydrothermal heating section is 180°C, the heating rate of the hydrothermal heating section is 2°C / min, and the time of the hydrothermal insulation section is 2h.

[0126] The calcination temperature is 1200°C, the calcination heating rate is 2°C / min, and the calcination time is 5h.

[0127] The drying temperature was 150°C.

[0128] Example 3

[0129] Based on the contents disclosed in Example 1, the following modifications are further made:

[0130] Use remelting sodium aluminate solution to replace sintering sodium aluminate solution.

[0131] The auxiliary agent includes a crystal growth regulator, and the weight m1 of the crystal growth regulator and the weight m2 of the aluminum hydroxide satisfy the relationship: m1:m2=3:100;

[0132] The mass m3 of the molten salt and the weight m4 of the flaky precursor powder satisfy the relationship: m3:m4=1:4.

[0133] The crystal growth regulator is phosphate, and the weight m5 of the phosphate and the weight m2 of the aluminum hydroxide satisfy the relationship:

[0134] m5:m2=3:100.

[0135] The phosphate is sodium phosphate dodecahydrate.

[0136] The additive also includes a dispersant, and the weight of the dispersant m7 and the weight of the aluminum hydroxide m2 satisfy the relationship: m7:m2=0.5:100;

[0137] The type of dispersant is sodium polyacrylate.

[0138] The auxiliary agent also includes a guiding agent, and the weight of the guiding agent m8 and the weight of the aluminum hydroxide m2 satisfy the relationship: m8:m2=2:100;

[0139] The type of directing agent is pseudo-boehmite.

[0140] The type of molten salt is a mixture of sodium sulfate and potassium sulfate, and the weight m11 of the sodium sulfate and the weight m12 of the potassium sulfate satisfy the relationship: m11:m12=1:2.

[0141] The hydrothermal reaction includes a hydrothermal heating section and a hydrothermal insulation section. The terminal temperature of the hydrothermal heating section is 200°C, the heating rate of the hydrothermal heating section is 2°C / min, and the time of the hydrothermal insulation section is 2h.

[0142] The calcination temperature is 1200°C, the calcination heating rate is 2°C / min, and the calcination time is 5h.

[0143] The drying temperature was 100°C.

[0144] Example 4

[0145] Based on the contents disclosed in Example 1, the following modifications are further made:

[0146] The particle size of the aluminum hydroxide seed crystals satisfies D50 of 4.5 μm.

[0147] The auxiliary agent includes a crystal growth regulator, and the weight m1 of the crystal growth regulator and the weight m2 of the aluminum hydroxide satisfy the relationship: m1:m2=1:100;

[0148] The mass m3 of the molten salt and the weight m4 of the flaky precursor powder satisfy the relationship: m3:m4=1:4.

[0149] The crystal growth regulator is titanium salt, and the weight m6 of the titanium salt and the weight m2 of aluminum hydroxide satisfy the relationship: m6:m2=1:100.

[0150] The titanium salt is titanyl sulfate.

[0151] The additive also includes a dispersant, and the weight of the dispersant m7 and the weight of the aluminum hydroxide m2 satisfy the relationship: m7:m2=0.5:100;

[0152] The type of dispersant is polyethylene glycol.

[0153] The auxiliary agent also includes a guiding agent, and the weight m8 of the guiding agent and the weight m2 of the aluminum hydroxide satisfy the relationship: m8:m2=1:100;

[0154] The type of directing agent is boehmite.

[0155] The type of molten salt is a mixture of sodium sulfate and potassium sulfate, and the weight m11 of the sodium sulfate and the weight m12 of the potassium sulfate satisfy the relationship: m11:m12=1:2.

[0156] The hydrothermal reaction includes a hydrothermal heating section and a hydrothermal insulation section. The terminal temperature of the hydrothermal heating section is 200°C, the heating rate of the hydrothermal heating section is 2°C / min, and the time of the hydrothermal insulation section is 2h.

[0157] The calcination temperature is 1300°C, the calcination heating rate is 2°C / min, and the calcination time is 2.5h.

[0158] The drying temperature was 150°C.

[0159] Example 5

[0160] Based on the contents disclosed in Example 1, the following modifications are further made:

[0161] Bayer process sodium aluminate solution is used to sinter the sodium aluminate solution instead of the sintering process. The chemical composition of the aluminum source slurry includes aluminum hydroxide and sodium oxide. The mass concentration of aluminum hydroxide is 130g / L, and the mass concentration of sodium oxide is 10g / L.

[0162] The auxiliary agent includes a crystal growth regulator, and the weight m1 of the crystal growth regulator and the weight m2 of the aluminum hydroxide satisfy the relationship: m1:m2=3:100;

[0163] The mass m3 of the molten salt and the weight m4 of the flaky precursor powder satisfy the relationship: m3:m4=1:4.

[0164] The crystal growth regulator is phosphate, and the weight m5 of the phosphate and the weight m2 of the aluminum hydroxide satisfy the relationship:

[0165] m5:m2=3:100.

[0166] The phosphate is sodium phosphate dodecahydrate.

[0167] The additive also includes a dispersant, and the weight of the dispersant m7 and the weight of the aluminum hydroxide m2 satisfy the relationship: m7:m2=0.5:100;

[0168] The type of dispersant is sodium polyacrylate.

[0169] The auxiliary agent also includes a guiding agent, and the weight m8 of the guiding agent and the weight m2 of the aluminum hydroxide satisfy the relationship: m8:m2=1:100;

[0170] The type of directing agent is pseudo-boehmite.

[0171] The type of molten salt is a mixture of sodium sulfate and potassium sulfate, and the weight m11 of the sodium sulfate and the weight m12 of the potassium sulfate satisfy the relationship: m11:m12=1:2.

[0172] The hydrothermal reaction includes a hydrothermal heating section and a hydrothermal insulation section. The terminal temperature of the hydrothermal heating section is 230°C, the heating rate of the hydrothermal heating section is 2°C / min, and the time of the hydrothermal insulation section is 2h.

[0173] The calcination temperature is 1100°C, the calcination heating rate is 2°C / min, and the calcination time is 5h.

[0174] The drying temperature was 100°C.

[0175] Example 6

[0176] Based on the contents disclosed in Example 1, the following modifications are further made:

[0177] The auxiliary agent includes a crystal growth regulator, and the weight m1 of the crystal growth regulator and the weight m2 of the aluminum hydroxide satisfy the relationship: m1:m2=1:100;

[0178] The mass m3 of the molten salt and the weight m4 of the flaky precursor powder satisfy the relationship: m3:m4=1:6.

[0179] The crystal growth regulator is a titanium salt, and the weight m6 of the titanium salt and the weight m2 of the aluminum hydroxide satisfy the relationship:

[0180] m6:m2=0.5:100.

[0181] The titanium salt is titanium dioxide.

[0182] The additive also includes a dispersant, and the weight of the dispersant m7 and the weight of the aluminum hydroxide m2 satisfy the relationship: m7:m2=0.5:100;

[0183] The type of dispersant is polyethylene glycol.

[0184] The auxiliary agent also includes a guiding agent, and the weight m8 of the guiding agent and the weight m2 of the aluminum hydroxide satisfy the relationship: m8:m2=1:100;

[0185] The type of directing agent is pseudo-boehmite.

[0186] The type of molten salt is a mixture of sodium sulfate and potassium sulfate, and the weight m11 of the sodium sulfate and the weight m12 of the potassium sulfate satisfy the relationship: m11:m12=1:2.

[0187] The hydrothermal reaction includes a hydrothermal heating section and a hydrothermal insulation section. The terminal temperature of the hydrothermal heating section is 180°C, the heating rate of the hydrothermal heating section is 2°C / min, and the time of the hydrothermal insulation section is 2h.

[0188] The calcination temperature is 1200°C, the calcination heating rate is 2°C / min, and the calcination time is 5h.

[0189] The drying temperature was 100°C.

[0190] Example 7

[0191] Based on the contents disclosed in Example 1, the following modifications are further made:

[0192] The auxiliary agent includes a crystal growth regulator, and the weight m1 of the crystal growth regulator and the weight m2 of the aluminum hydroxide satisfy the relationship: m1:m2=5:100;

[0193] The mass m3 of the molten salt and the weight m4 of the flaky precursor powder satisfy the relationship: m3:m4=1:5.

[0194] The crystal growth regulator is a phosphate salt, and the weight m5 of the phosphate salt and the weight m2 of aluminum hydroxide satisfy the relationship: m5:m2=2:100.

[0195] The phosphate salt is phosphorus pentoxide.

[0196] The additive also includes a dispersant, and the weight of the dispersant m7 and the weight of the aluminum hydroxide m2 satisfy the relationship: m7:m2=0.5:100;

[0197] The type of dispersant is polyethylene glycol.

[0198] The auxiliary agent also includes a guiding agent, and the weight m8 of the guiding agent and the weight m2 of the aluminum hydroxide satisfy the relationship: m8:m2=1:100;

[0199] The type of directing agent is boehmite.

[0200] The type of molten salt is a mixture of sodium sulfate and potassium sulfate, and the weight m11 of the sodium sulfate and the weight m12 of the potassium sulfate satisfy the relationship: m11:m12=1:2.

[0201] The hydrothermal reaction includes a hydrothermal heating section and a hydrothermal insulation section. The terminal temperature of the hydrothermal heating section is 180°C, the heating rate of the hydrothermal heating section is 2°C / min, and the time of the hydrothermal insulation section is 2h.

[0202] The calcination temperature is 1200°C, the calcination heating rate is 2°C / min, and the calcination time is 5h.

[0203] The drying temperature was 100°C.

[0204] Comparative Example 1

[0205] Based on the contents disclosed in Example 1, the following modifications are further made:

[0206] The mass m3 of the molten salt and the weight m4 of the flaky precursor powder satisfy the relationship: m3:m4=1:4.

[0207] The type of molten salt is a mixture of sodium sulfate and potassium sulfate, and the weight m11 of the sodium sulfate and the weight m12 of the potassium sulfate satisfy the relationship: m11:m12=1:2.

[0208] The hydrothermal reaction includes a hydrothermal heating section and a hydrothermal insulation section. The terminal temperature of the hydrothermal heating section is 200°C, the heating rate of the hydrothermal heating section is 2°C / min, and the time of the hydrothermal insulation section is 2h.

[0209] The calcination temperature is 1200°C, the calcination heating rate is 2°C / min, and the calcination time is 5h.

[0210] The drying temperature was 150°C.

[0211] Comparative Example 2

[0212] Based on the contents disclosed in Example 1, the following modifications are further made:

[0213] The mass m3 of the molten salt and the weight m4 of the flaky precursor powder satisfy the relationship: m3:m4=1:4.

[0214] The additive also includes a dispersant, and the weight of the dispersant m7 and the weight of the aluminum hydroxide m2 satisfy the relationship: m7:m2=0.5:100;

[0215] The type of dispersant is sodium polyacrylate.

[0216] The auxiliary agent also includes a guiding agent, and the weight of the guiding agent m8 and the weight of the aluminum hydroxide m2 satisfy the relationship: m8:m2=0.5:100;

[0217] The type of directing agent is pseudo-boehmite.

[0218] The type of molten salt is a mixture of sodium sulfate and potassium sulfate, and the weight m11 of the sodium sulfate and the weight m12 of the potassium sulfate satisfy the relationship: m11:m12=1:2.

[0219] The hydrothermal reaction includes a hydrothermal heating section and a hydrothermal insulation section. The terminal temperature of the hydrothermal heating section is 200°C, the heating rate of the hydrothermal heating section is 2°C / min, and the time of the hydrothermal insulation section is 2h.

[0220] The calcination temperature is 1200°C, the calcination heating rate is 2°C / min, and the calcination time is 5h.

[0221] The drying temperature was 100°C.

[0222] Comparative Example 3

[0223] Based on the contents disclosed in Example 1, the following modifications are further made:

[0224] The weight m1 of the crystal growth regulator and the weight m2 of the aluminum hydroxide satisfy the relationship: m1:m2=30:100.

[0225] The mass m3 of the molten salt and the weight m4 of the flaky precursor powder satisfy the relationship: m3:m4=1:4.

[0226] The crystal growth regulator is phosphate, and the weight m5 of the phosphate and the weight m2 of the aluminum hydroxide satisfy the relationship:

[0227] m5:m2=3:100.

[0228] The phosphate is sodium phosphate dodecahydrate.

[0229] The additive also includes a dispersant, and the weight of the dispersant m7 and the weight of the aluminum hydroxide m2 satisfy the relationship: m7:m2=0.5:100;

[0230] The type of dispersant is sodium polyacrylate.

[0231] The auxiliary agent also includes a guiding agent, and the weight of the guiding agent m8 and the weight of the aluminum hydroxide m2 satisfy the relationship: m8:m2=0.5:100;

[0232] The type of directing agent is pseudo-boehmite.

[0233] The type of molten salt is a mixture of sodium sulfate and potassium sulfate, and the weight m11 of the sodium sulfate and the weight m12 of the potassium sulfate satisfy the relationship: m11:m12=1:2.

[0234] The hydrothermal reaction includes a hydrothermal heating section and a hydrothermal insulation section. The terminal temperature of the hydrothermal heating section is 200°C, the heating rate of the hydrothermal heating section is 2°C / min, and the time of the hydrothermal insulation section is 2h.

[0235] The calcination temperature is 1200°C, the calcination heating rate is 2°C / min, and the calcination time is 5h.

[0236] The drying temperature was 100°C.

[0237] Comparative Example 4

[0238] Based on the contents disclosed in Example 1, the following modifications are further made:

[0239] The auxiliary agent includes a crystal growth regulator, and the weight m1 of the crystal growth regulator and the weight m2 of the aluminum hydroxide satisfy the relationship: m1:m2=3:100;

[0240] The mass m3 of the molten salt and the weight m4 of the flaky precursor powder satisfy the relationship: m3:m4=1:4.

[0241] The crystal growth regulator is phosphate, and the weight m5 of the phosphate and the weight m2 of the aluminum hydroxide satisfy the relationship:

[0242] m5:m2=3:100.

[0243] The phosphate is sodium phosphate dodecahydrate.

[0244] The auxiliary agent also includes a guiding agent, and the weight of the guiding agent m8 and the weight of the aluminum hydroxide m2 satisfy the relationship: m8:m2=0.5:100;

[0245] The type of directing agent is boehmite.

[0246] The type of molten salt is a mixture of sodium sulfate and potassium sulfate, and the weight m11 of the sodium sulfate and the weight m12 of the potassium sulfate satisfy the relationship: m11:m12=1:2.

[0247] The hydrothermal reaction includes a hydrothermal heating section and a hydrothermal insulation section. The terminal temperature of the hydrothermal heating section is 200°C, the heating rate of the hydrothermal heating section is 2°C / min, and the time of the hydrothermal insulation section is 2h.

[0248] The calcination temperature is 1200°C, the calcination heating rate is 2°C / min, and the calcination time is 5h.

[0249] The drying temperature was 150°C.

[0250] Comparative Example 5

[0251] Based on the contents disclosed in Example 1, the following modifications are further made:

[0252] The auxiliary agent includes a crystal growth regulator, and the weight m1 of the crystal growth regulator and the weight m2 of the aluminum hydroxide satisfy the relationship: m1:m2=3:100;

[0253] The mass m3 of the molten salt and the weight m4 of the flaky precursor powder satisfy the relationship: m3:m4=1:4.

[0254] The crystal growth regulator is phosphate, and the weight m5 of the phosphate and the weight m2 of the aluminum hydroxide satisfy the relationship:

[0255] m5:m2=3:100.

[0256] The phosphate is sodium phosphate dodecahydrate.

[0257] The weight of the dispersant m7 and the weight of the aluminum hydroxide m2 satisfy the relationship: m7:m2=10:100:

[0258] The type of dispersant is sodium polyacrylate.

[0259] The auxiliary agent also includes a guiding agent, and the weight of the guiding agent m8 and the weight of the aluminum hydroxide m2 satisfy the relationship: m8:m2=0.5:100;

[0260] The type of directing agent is boehmite.

[0261] The type of molten salt is a mixture of sodium sulfate and potassium sulfate, and the weight m11 of the sodium sulfate and the weight m12 of the potassium sulfate satisfy the relationship: m11:m12=1:2.

[0262] The hydrothermal reaction includes a hydrothermal heating section and a hydrothermal insulation section. The terminal temperature of the hydrothermal heating section is 200°C, the heating rate of the hydrothermal heating section is 2°C / min, and the time of the hydrothermal insulation section is 2h.

[0263] The calcination temperature is 1200°C, the calcination heating rate is 2°C / min, and the calcination time is 5h.

[0264] The drying temperature was 150°C.

[0265] Comparative Example 6

[0266] Based on the contents disclosed in Example 1, the following modifications are further made:

[0267] No directing agent was added.

[0268] The auxiliary agent includes a crystal growth regulator, and the weight m1 of the crystal growth regulator and the weight m2 of the aluminum hydroxide satisfy the relationship: m1:m2=3:100;

[0269] The mass m3 of the molten salt and the weight m4 of the flaky precursor powder satisfy the relationship: m3:m4=1:4.

[0270] The crystal growth regulator is phosphate, and the weight m5 of the phosphate and the weight m2 of the aluminum hydroxide satisfy the relationship:

[0271] m5:m2=3:100.

[0272] The phosphate is sodium phosphate dodecahydrate.

[0273] The additive also includes a dispersant, and the weight of the dispersant m7 and the weight of the aluminum hydroxide m2 satisfy the relationship: m7:m2=0.5:100;

[0274] The type of dispersant is sodium polyacrylate.

[0275] The type of molten salt is a mixture of sodium sulfate and potassium sulfate, and the weight m11 of the sodium sulfate and the weight m12 of the potassium sulfate satisfy the relationship: m11:m12=1:2.

[0276] The hydrothermal reaction includes a hydrothermal heating section and a hydrothermal insulation section. The terminal temperature of the hydrothermal heating section is 200°C, the heating rate of the hydrothermal heating section is 2°C / min, and the time of the hydrothermal insulation section is 2h.

[0277] The calcination temperature is 1200°C, the calcination heating rate is 2°C / min, and the calcination time is 5h.

[0278] The drying temperature was 150°C.

[0279] Comparative Example 7

[0280] Based on the contents disclosed in Example 1, the following modifications are further made:

[0281] The auxiliary agent includes a crystal growth regulator, and the weight m1 of the crystal growth regulator and the weight m2 of the aluminum hydroxide satisfy the relationship: m1:m2=3:100;

[0282] The mass m3 of the molten salt and the weight m4 of the flaky precursor powder satisfy the relationship: m3:m4=1:4.

[0283] The crystal growth regulator is phosphate, and the weight m5 of the phosphate and the weight m2 of the aluminum hydroxide satisfy the relationship:

[0284] m5:m2=3:100.

[0285] The phosphate is sodium phosphate dodecahydrate.

[0286] The additive also includes a dispersant, and the weight of the dispersant m7 and the weight of the aluminum hydroxide m2 satisfy the relationship: m7:m2=0.5:100;

[0287] The type of dispersant is sodium polyacrylate.

[0288] The auxiliary agent also includes a guiding agent, and the weight m8 of the guiding agent and the weight m2 of the aluminum hydroxide satisfy the relationship: m8:m2=20:100;

[0289] The type of directing agent is boehmite.

[0290] The type of molten salt is a mixture of sodium sulfate and potassium sulfate, and the weight m11 of the sodium sulfate and the weight m12 of the potassium sulfate satisfy the relationship: m11:m12=1:2.

[0291] The volume V1 of the dispersed system and the total volume V2 of the reactor satisfy the relationship: V1:V2=70:100.

[0292] The hydrothermal reaction includes a hydrothermal heating section and a hydrothermal insulation section. The terminal temperature of the hydrothermal heating section is 200°C, the heating rate of the hydrothermal heating section is 2°C / min, and the time of the hydrothermal insulation section is 2h.

[0293] The calcination temperature is 1200°C, the calcination heating rate is 2°C / min, and the calcination time is 5h.

[0294] The drying temperature was 150°C.

[0295] Related experiments and effect data:

[0296] Figure 2 The scanning electron microscope image of the flake precursor powder in the method for preparing an aluminum oxide flake with a high aspect ratio provided in Example 1 of the present application is exemplarily shown;

[0297] Figure 3 The scanning electron microscope image of one direction of an aluminum oxide sheet with a high aspect ratio provided in Example 1 of the present application is exemplarily shown;

[0298] Figure 4 The scanning electron microscope image of another direction of an aluminum oxide sheet with a high aspect ratio provided in Example 1 of the present application is exemplarily shown;

[0299] Figure 5 The X-ray diffraction pattern of an aluminum oxide sheet with a high aspect ratio provided in Example 1 of the present application is exemplarily shown;

[0300] 1. The particle size distribution of the flake precursor powder obtained in each example is tested, wherein the scanning electron microscope image of the flake precursor powder obtained in Example 1 is as follows: Figure 2 The measured particle size distribution is shown in Table 1.

[0301] Table 1 Particle size distribution test results of the flake precursor powder obtained in each embodiment

[0302]

[0303] 2. The aluminum oxide flake products obtained in each embodiment and comparative example were characterized and tested, and the results are shown in Table 2. Among them, the scanning electron microscope images of the aluminum oxide flakes obtained in Example 1 in different directions are shown in Table 2. Figure 3 and Figure 4As shown, the X-ray diffraction pattern of the aluminum oxide flakes obtained in Example 1 is as shown Figure 5 shown.

[0304]

[0305] As can be seen from Table 2, the embodiment of the present application provides a method for preparing alumina flakes with a high aspect ratio. The preparation method can use additives including seed crystal growth regulators and molten salts to control the hydration reaction and roasting of the aluminum source slurry, respectively, thereby controlling the twinning and agglomeration degree of the aluminum source slurry to improve the thickness of the flat surface of aluminum hydroxide at each stage, thereby increasing the aspect ratio of the alumina flakes to >40.

[0306] In summary, the embodiments of the present application provide a method for preparing alumina flakes with a high aspect ratio. The preparation method can use additives including seed crystal growth regulators and molten salts, and respectively control the process parameters of the hydration reaction and roasting of the aluminum source slurry to control the twinning and agglomeration degree of the aluminum source slurry, thereby improving the thickness of the flat surface of aluminum hydroxide at each stage, and thereby improving the aspect ratio of the alumina flakes.

[0307] In addition, an embodiment of the present application provides a method for preparing aluminum oxide flakes with a high aspect ratio. The aluminum oxide flakes prepared thereby not only have a high aspect ratio, but also have high self-sharpening properties, which can effectively improve the grinding efficiency of the aluminum oxide flakes used as a grinding aid in the actual application stage.

[0308] In addition, an embodiment of the present application provides an aluminum oxide sheet with a high aspect ratio. The overall surface of the aluminum oxide sheet is flat and smooth, and can be used as an abrasive for precision polishing, and the qualified rate of the product after precision polishing can be increased from 10% to 15%.

[0309] The above is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. It will be apparent to those skilled in the art that various modifications to these embodiments are possible, and the general principles defined in the present application can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to these embodiments shown in the present application, but will conform to the widest scope consistent with the principles and novel features applied for by the present application.

Claims

1. A method for preparing an aluminum oxide sheet with a high aspect ratio, characterized in that: The raw materials of the preparation method include aluminum source slurry, the chemical composition of the aluminum source slurry includes aluminum hydroxide and sodium oxide, the mass concentration of the aluminum hydroxide is 100g / L to 200g / L, and the mass concentration of the sodium oxide is 10g / L to 5g / L; the preparation method comprises: The auxiliary agent and the aluminum source slurry are stirred and mixed to obtain a dispersed system; subjecting the dispersed system to a hydrothermal reaction to obtain a precursor slurry; Drying the precursor slurry to obtain a flake precursor powder; calcining the molten salt and the flake precursor powder to obtain a calcined material; and Purifying the calcined material to obtain aluminum oxide flakes; Wherein, the auxiliary agent includes a crystal growth regulator, and the weight m1 of the crystal growth regulator and the weight m2 of the aluminum hydroxide satisfy the relationship: m1:m2=(0.2-15):100; The mass m3 of the molten salt and the weight m4 of the flaky precursor powder satisfy the relationship: m3:m4=(1:4)~(1:6).

2. The preparation method according to claim 1, characterized in that: The crystal growth regulator includes phosphate and / or titanium salt; when the crystal growth regulator includes phosphate, the weight m5 of the phosphate and the weight m2 of the aluminum hydroxide satisfy the relationship: m5:m2=(0.1-5):100; In the case where the crystal growth regulator includes a titanium salt, the weight m6 of the titanium salt and the weight m2 of the aluminum hydroxide satisfy the relationship: m6:m2=(0.1-1):

100.

3. The preparation method according to claim 2, characterized in that: In the case where the crystal growth regulator comprises a phosphate, the phosphate comprises phosphorus pentoxide and / or sodium phosphate dodecahydrate; In the case where the crystal growth regulator comprises a titanium salt, the titanium salt comprises titanium dioxide and / or titanyl sulfate.

4. The preparation method according to claim 1, characterized in that: The auxiliary agent also includes a dispersant, and the weight m7 of the dispersant and the weight m2 of the aluminum hydroxide satisfy the relationship: m7:m2=(0.01-0.5):100; The type of the dispersant includes at least one of the following: Polyethylene glycol, sodium carboxymethylcellulose, polyacrylate and sodium maleate.

5. The preparation method according to claim 1, characterized in that: The auxiliary agent also includes a guiding agent, and the weight m8 of the guiding agent and the weight m2 of the aluminum hydroxide satisfy the relationship: m8:m2=(0.5-10):100; The types of directing agents include pseudo-boehmite and / or boehmite.

6. The preparation method according to claim 1, characterized in that: The type of the molten salt includes at least one of the following: Sodium sulfate, potassium sulfate, sodium chloride, potassium chloride, sodium fluoride and potassium fluoride.

7. The preparation method according to claim 1, characterized in that: The hydrothermal reaction includes a hydrothermal heating section and a hydrothermal insulation section. The terminal temperature of the hydrothermal heating section is 170°C to 230°C, the heating rate of the hydrothermal heating section is 1°C / min to 3°C / min, and the time of the hydrothermal insulation section is 0h to 4h.

8. The preparation method according to claim 1, characterized in that: The calcination temperature is 1100° C. to 1350° C., and the calcination time is 2 h to 5 h.

9. The preparation method according to claim 1, characterized in that: The drying temperature is less than 230°C.

10. An aluminum oxide sheet with a high aspect ratio, characterized in that: The aluminum oxide flakes are obtained by the preparation method according to any one of claims 1 to 9, and the diameter-to-thickness ratio of the aluminum oxide flakes is greater than 40.

Citation Information

Cited By

  • Preparation method of ultralow-sodium flake alumina

    CN121470523A