Preparation method and application of Au-ITO composite SERS substrate

The Au-ITO composite SERS substrate addresses the limitations of gold nanoparticle-based substrates by enhancing Raman signal and catalyzing the oxidation of PATP molecules to DMAB molecules through improved electric field intensity and electron propagation.

CN119080404AInactive Publication Date: 2024-12-06LIAONING UNIVERSITY

Patent Information

Application Number
CN202411161871.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing SERS substrates, particularly those using gold nanoparticles, have limited ability to enhance the Raman signal and catalyze the oxidation of PATP molecules to DMAB molecules due to weak electromagnetic enhancement and chemical interaction.

Method used

A composite SERS substrate is formed by combining Au nanoparticles with ITO glass sheets, enhancing the electric field intensity at their interface to improve Raman signal detection and catalyze the oxidation of PATP molecules to DMAB molecules.

Benefits of technology

The Au-ITO composite substrate increases the Raman signal intensity and accelerates the oxidation reaction of PATP molecules, providing a stronger electric field and improved catalytic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080404A_ABST
    Figure CN119080404A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of SERS detection, and particularly relates to a preparation method and application of an Au-ITO composite SERS substrate. The preparation method comprises the following steps: firstly, preparing gold nanoparticles which are uniformly distributed and have the same size through a sodium citrate reduction method, and then loading the gold nanoparticles on an ITO (Indium Tin Oxide) glass sheet to prepare a novel SERS (Surface Enhanced Raman Scattering) substrate. The novel SERS substrate formed by combining the ITO glass sheet and the gold nanoparticles is different from a conventional SERS substrate with independent Au nanoparticles, and a stronger intrinsic Raman signal of a probe molecule can be detected by the novel SERS substrate. As the SERS substrate needs to be compounded with an ITO glass sheet during preparation, higher electric field intensity can be obtained at a compound interface, so that an intrinsic Raman signal of a probe molecule can be enhanced, and the SERS substrate can be better used for detecting and analyzing chemical substances.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of SERS detection, and particularly relates to a preparation method and application of an Au-ITO composite SERS substrate. Background Art

[0002] Surface enhanced Raman scattering (SERS) technology has the characteristics of fast response, simple operation, high sensitivity, non-destructive testing, and no interference with aqueous solutions. It has great development potential in the fields of medical diagnosis, catalytic reaction, biological analysis and environmental testing. There are generally two theories about the SERS enhancement mechanism. One is physical enhancement, which is considered to be dominant in the SERS enhancement mechanism, also known as electromagnetic enhancement. It is related to the metal surface plasmon resonance (SPR). Therefore, metal nanoparticles with regular size, uniform arrangement and aggregation state have stronger SERS enhancement performance. The other is chemical enhancement, which is related to charge transfer (CT). The CT phenomenon occurs between the SERS substrate and the probe molecule through valence bond binding or chemical adsorption. The sensitivity of SERS spectroscopy often depends on an efficient and stable SERS substrate. Since the discovery of SERS technology, gold and silver nanoparticles have been widely used as SERS substrates because of their good SPR effect, conductivity and easy preparation.

[0003] The PATP molecule is an organic compound with a chemical formula of C6H7NS. It is composed of three groups: thiol, benzene ring and amine. It is widely used in the fields of synthetic dyes and pesticides. Because it contains thiol, it is easy to adsorb on the surface of SERS substrate and is widely used in SERS detection. Gold, silver and other precious metal nanoparticles will generate electrons and holes due to the SPR effect, among which holes can oxidize PATP molecules to generate DMAB molecules. PATP molecules can easily undergo oxidation reaction on silver nanoparticles to produce DMAB molecules. However, because the enhancement effect of gold nanoparticles is weak, it is difficult to oxidize PATP molecules to generate DMAB molecules. Indium tin oxide (ITO) is one of the most widely used transparent conductive oxide films. Due to its good conductivity and optical transparency, it is an ideal material for the development of various technologies such as biosensors, flat panels, photovoltaics, etc. ITO is composed of indium oxide (In2O3) and tin oxide (SnO2) in a ratio of 9:1. It is a transparent and colorless conductive film. ITO thin films can be produced using many techniques such as ion beam sputtering, electron beam evaporation, chemical vapor deposition, magnetron sputtering and chemical solution deposition, and are widely used in electrochemistry, solar cells and biosensors.

[0004] Based on the excellent performance of Au nanoparticles and ITO glass sheets, if the two are combined to form a unique composite SERS substrate, it can physically enhance the PATP molecules and catalyze the oxidation reaction of PATP molecules to generate DMAB molecules, which will be of great significance. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention designs and synthesizes an Au-ITO composite SERS substrate, which can generate a stronger electric field intensity at the interface between Au nanoparticles and ITO glass sheets, thereby enhancing the intrinsic Raman signal of the probe molecule, and can be better used for detecting and analyzing chemical substances.

[0006] The technical solution adopted by the present invention is:

[0007] An Au-ITO composite SERS substrate, the preparation method of which comprises the following steps:

[0008] 1) dissolving sodium citrate powder in water, adding chloroauric acid solution, and obtaining gold nanoparticles by chemical reduction method;

[0009] 2) After ultrasonication and centrifugation, the gold nanoparticles are loaded on a clean ITO glass sheet;

[0010] 3) Drying the composite substrate obtained in step 2) in an oven to obtain an Au-ITO composite SERS substrate.

[0011] Preferably, in the above-mentioned Au-ITO composite SERS substrate, in step 1), the amount of sodium citrate powder used is 1 g, the amount of water used is 100 mL, and the amount of chloroauric acid used is 0.024 mol.

[0012] Preferably, in the above-mentioned Au-ITO composite SERS substrate, in step 1), the temperature at which the sodium citrate powder is dissolved in water is 5-25°C.

[0013] Preferably, in the above-mentioned Au-ITO composite SERS substrate, in step 1), the temperature of the chemical reduction method is 90-100° C., and the heating time is 1-1.5 h.

[0014] Preferably, in the above-mentioned Au-ITO composite SERS substrate, in step 2), the ultrasonic conditions are: temperature of 5-25° C., and time of 5-10 min.

[0015] Preferably, in the above-mentioned Au-ITO composite SERS substrate, in step 2), the pretreatment method of the ITO glass sheet is: first rinse the ITO glass sheet with a large amount of water, then gently wipe the ITO conductive surface with alcohol cotton, and finally blow dry with N2 for standby use.

[0016] Preferably, in the above-mentioned Au-ITO composite SERS substrate, in step 3), the drying temperature is 50-60° C., and the drying time is 2-4 h.

[0017] Application of any of the above-mentioned Au-ITO composite SERS substrates in catalyzing the oxidation reaction of PATP molecules to generate DMAB molecules.

[0018] Furthermore, the above application method is as follows: under 633nm laser irradiation, the Au-ITO composite SERS substrate is immersed in a PATP solution to enhance the Raman signal of the PATP molecules, and the Au-ITO composite SERS substrate catalyzes the oxidation reaction of the PATP molecules to generate DMAB molecules.

[0019] Preferably, in the above application, the pH of the PATP solution is 5.

[0020] The present invention utilizes the construction of Au-ITO composite SERS substrate to enhance the Raman spectrum of PATP molecules and catalyze the oxidation reaction of PATP molecules. The beneficial effects of this method can be attributed to three aspects:

[0021] 1. The construction of Au-ITO composite SERS substrate can increase the specific surface area of ​​the material and provide more "hot spots";

[0022] 2. The introduction of ITO accelerates the propagation rate of electrons and holes, thereby enhancing the Raman spectrum of PATP molecules;

[0023] 3. The Au-ITO composite SERS substrate forms an electric field at the interface between Au nanoparticles and ITO glass, physically enhancing the Raman spectrum of PATP molecules and then catalyzing the oxidation reaction of PATP molecules to generate DMAN molecules. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a TEM image of Au nanoparticles in Example 1 at a scale of 50 nm.

[0025] Figure 2 This is a TEM image of Au nanoparticles in Example 1 at a scale of 20 nm.

[0026] Figure 3 This is the UV-visible absorption graph of the Au nanoparticles in Example 1.

[0027] Figure 4 It is the Raman spectrum of the PATP molecule under 633nm laser in Example 1 and the SERS spectrum of the PATP molecule adsorbed on the Au nanoparticles and the Au-ITO composite substrate respectively.

[0028] Figure 5 In Example 1, the PATP molecules adsorbed on the Au nanoparticles and the DMAB molecules on the Au-ITO composite substrate under 633 nm laser light were detected at 1140 cm -1 、1390cm-1 and 1439cm -1 , and the characteristic peak of PATP molecule at 1080 cm -1 Intensity ratio diagram.

[0029] Figure 6 The PATP molecules in Example 1 are adsorbed on the Au-ITO composite substrate with the characteristic peak of DMAB molecules at 1140 cm -1 A plot of the area of ​​the scan selected for intensity.

[0030] Figure 7 This is the SERS spectrum graph collected after randomly performing 10 Raman detections on the PATP molecule on the Au-ITO composite substrate using 633 nm laser irradiation in Example 1.

[0031] Figure 8 This is the electric field enhancement diagram of the Au-ITO composite substrate calculated using FDTD simulation in Example 1.

[0032] Fig. 9 This is the electric field enhancement diagram of Au nanoparticles calculated using FDTD simulation in Example 1.

[0033] Fig.10 It is the SERS spectrum diagram of PATP molecules adsorbed on the Au-ITO composite substrate under 633nm laser at different pH values ​​in Example 2. DETAILED DESCRIPTION

[0034] In order to better understand the technical solution of the present invention, a specific embodiment is further described in detail, but the solution is not limited thereto.

[0035] Example 1: Au-ITO composite SERS substrate

[0036] The preparation method is as follows:

[0037] 1) Dissolve 1 g of sodium citrate powder in a clean beaker containing 100 mL of deionized water. After standing for a while, put the solution into a 100 mL volumetric flask to obtain a 1% sodium citrate solution.

[0038] 2) Add 1 mL of sodium citrate solution and 1 mL of 0.024 mol chloroauric acid into a round-bottom flask containing 100 mL of deionized water, and heat and stir at 1000 rpm for 1 hour at 100°C. After the solution is cooled to room temperature, ultrasonicate for 5-10 minutes, centrifuge, and collect the solution in a volumetric flask.

[0039] 3) First rinse the ITO glass sheet with plenty of water, then use alcohol cotton to gently wipe the ITO conductive surface, and finally blow it dry with N2 and set it aside.

[0040] 4) dripping the solution collected in step 2) onto an ITO glass sheet, placing the sheet in an oven, and drying the sheet at a temperature of 50-60° C. for 2-4 hours to obtain an Au-ITO composite SERS substrate.

[0041] 5) The prepared Au-ITO composite SERS substrate was immersed in a PATP solution for 2 h, and naturally air-dried at room temperature for later use.

[0042] The Au nanoparticles prepared in step 2) and collected in the volumetric flask were subjected to TEM test. The test results are as follows: Figure 1 and Figure 2 As shown in the figure, it can be seen that the Au nanoparticles are spherical, with a diameter of about 20nm and are evenly distributed, indicating that the Au nanoparticles are successfully prepared. The Au nanoparticles prepared in step 2) are subjected to ultraviolet absorption spectrum test, and the test results are as follows Figure 3 As shown, it can be seen from the figure that the ultraviolet absorption peak of Au nanoparticles is located at 521nm, indicating the successful preparation of Au nanoparticles.

[0043] The Au-ITO composite SERS substrate prepared in Example 1 was used to conduct experiments based on the SERS technology using PATP as a probe molecule. The test process was as follows: a laser with a wavelength of 633 nm was used as an excitation light source, and PATP was used as a probe molecule on the Au-ITO composite SERS substrate based on the SERS technology. Figure 4 , Figure 5 , Figure 6 and Figure 7 As shown, it can be seen that the Au-ITO composite SERS substrate prepared in Example 1 can enhance the Raman signal of PATP molecules, and then catalyze the oxidation reaction of PATP molecules to generate DMAB molecules. And the PATP molecules were randomly detected 10 times on the Au-ITO composite substrate, and it was found that the Raman signal peaks were neat and the Raman intensity did not change significantly, indicating that the Au-ITO composite SERS substrate has good uniformity and reproducibility. The electric field enhancement diagrams of the Au-ITO composite substrate and Au nanoparticles were simulated and calculated using FDTD, as shown in Figure 1. Figure 8 and Fig. 9 As shown, it is further proved from theoretical calculation that the Au-ITO composite substrate has excellent enhancement effect, can enhance the Raman spectrum of PATP molecules, and catalyze the oxidation reaction of PATP molecules to generate DMAB molecules.

[0044] Example 2: An Au-ITO composite SERS substrate (PATP molecules under different pH environments)

[0045] The preparation method is as follows:

[0046] 1) Dissolve 1 g of sodium citrate powder in a clean beaker containing 100 mL of deionized water. After standing for a while, put the solution into a 100 mL volumetric flask to obtain a 1% sodium citrate solution.

[0047] 2) Add 1 mL of sodium citrate solution and 1 mL of 0.024 mol chloroauric acid into a round-bottom flask containing 100 mL of deionized water, and heat and stir at 1000 rpm for 1 hour at 100°C. After the solution is cooled to room temperature, ultrasonicate for 5-10 minutes, centrifuge, and collect the solution in a volumetric flask.

[0048] 3) First rinse the ITO glass sheet with plenty of water, then use alcohol cotton to gently wipe the ITO conductive surface, and finally blow it dry with N2 and set it aside.

[0049] 4) dripping the solution collected in step 2) onto an ITO glass sheet, placing the sheet in an oven, and drying the sheet at a temperature of 50-60° C. for 2-4 hours to obtain an Au-ITO composite SERS substrate.

[0050] 5) The prepared Au-ITO composite SERS substrate was immersed in PATP solutions under different pH environments for 2 h, and naturally air-dried at room temperature for later use.

[0051] The Au-ITO composite SERS substrate prepared in Example 2 was used to conduct experiments based on the SERS technology using PATP as a probe molecule. The test process was as follows: a laser with a wavelength of 633 nm was used as an excitation light source, and PATP was used as a probe molecule on the Au-ITO composite SERS substrate based on the SERS technology. Fig.10 As shown, it can be seen that the Au-ITO composite SERS substrate prepared in Example 2 can enhance the Raman signal of the PATP molecule under different pH conditions; under the condition of pH = 5, the Raman signal peak intensity of the PATP molecule is the strongest, and the Au-ITO composite SERS substrate can catalyze the oxidation reaction of the PATP molecule to generate DMAB molecules.

Claims

1. An Au-ITO composite SERS substrate, characterized in that: The preparation method comprises the following steps: 1) dissolving sodium citrate powder in water, adding chloroauric acid solution, and obtaining gold nanoparticles by chemical reduction method; 2) After ultrasonication and centrifugation, the gold nanoparticles are loaded on a clean ITO glass sheet; 3) Drying the composite substrate obtained in step 2) in an oven to obtain an Au-ITO composite SERS substrate.

2. The Au-ITO composite SERS substrate according to claim 1, characterized in that: In step 1), the amount of sodium citrate powder used is 1 g, the amount of water used is 100 mL, and the amount of chloroauric acid used is 0.024 mol.

3. The Au-ITO composite SERS substrate according to claim 1, characterized in that: In step 1), the temperature at which the sodium citrate powder is dissolved in water is 5-25°C.

4. The Au-ITO composite SERS substrate according to claim 1, characterized in that: In step 1), the temperature of the chemical reduction method is 90-100° C. and the heating time is 1-1.5 h.

5. The Au-ITO composite SERS substrate according to claim 1, characterized in that: In step 2), the ultrasonic conditions are: temperature 5-25° C., time 5-10 min.

6. The Au-ITO composite SERS substrate according to claim 1, characterized in that: In step 2), the pretreatment method of the ITO glass sheet is: first rinse the ITO glass sheet with a large amount of water, then gently wipe the ITO conductive surface with alcohol cotton, and finally blow dry with N2 for standby use.

7. The Au-ITO composite SERS substrate according to claim 1, characterized in that: In step 3), the drying temperature is 50-60° C. and the drying time is 2-4 hours.

8. Use of the Au-ITO composite SERS substrate according to any one of claims 1 to 7 in catalyzing the oxidation reaction of PATP molecules to generate DMAB molecules.

9. The use according to claim 8, characterized in that: The method is as follows: Under 633nm laser irradiation, the Au-ITO composite SERS substrate is immersed in a PATP solution, the Raman signal of the PATP molecule is enhanced, and the Au-ITO composite SERS substrate catalyzes the oxidation reaction of the PATP molecule to generate DMAB molecules.

10. The use according to claim 9, characterized in that: The pH of the PATP solution is 5.

Citation Information

Patent Citations

  • Two-dimensional gold membrane self-assembly preparation method with surface enhanced Raman scattering effect

    CN101961791A

  • Tyrosinase activity detection method based on recyclable SERS sensor

    CN109342391A

  • Surface plasma resonance immunoassay method for embedded Au nano-film electrode

    CN110579612A

  • Preparation method of Raman substrate based on three-dimensional dendritic gold nanomaterial

    CN111766227A

  • Process for preparing film electrode of gold-monocrystal nano island array

    CN1356543A

Cited By

  • Ag-MoO2 composite SERS (Surface Enhanced Raman Scattering) substrate as well as preparation method and application thereof

    CN120369620A