Method for precisely controlling surface roughness of polyimide film

By performing incomplete thermal imidation and dilute solution treatment in the polyimide film forming process, the surface roughness of the polyimide film is controlled by two coating processes, and the high surface density of the polyimide film is solved The problem of composite bonding performance has achieved precision control of film surface roughness and improved bonding performance.

CN119081196APending Publication Date: 2024-12-06FIBERRAY PHOTONICS (SUZHOU) HIGH-TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411320915.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The high surface density caused by the existing polyimide film forming process makes it difficult to bond with other materials, and it is difficult to precisely control the surface roughness, affecting the bonding performance.

Method used

The primary film was obtained by synthesizing polyamic acid in aprotic polar solvent, incomplete thermal imidation was performed, and the film surface roughness was controlled by two coating processes. A dense and controllable polyimide film is formed.

Benefits of technology

It realizes precise control of the surface roughness of polyimide film, improves the composite bonding performance with other materials, and is suitable for different application needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081196A_ABST
    Figure CN119081196A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of polyimide film preparation, and particularly relates to a method for precisely controlling the surface roughness of a polyimide film. The preparation method comprises the following steps: synthesizing a precursor polyamide acid required by the polyimide film by commercialized equal equivalent dianhydride monomer and diamine monomer in an aprotic polar solvent, completing the synthesis of the polyamide acid under the protection of dry nitrogen, and taking out a small part of the polyamide acid for diluting into a polyamide acid solution with the solid content of less than 10%; the preparation method comprises the following steps: coating a carrier with polyamide acid with the solid content of 20% according to actual requirements to form a polyamide acid film, and carrying out incomplete thermal imidization to obtain a primary polyimide film; and taking down the primary film from the carrier, immersing the primary film in the dilute solution, scraping the redundant solution through two glass rods to form a uniform film, and putting the uniform film into a vacuum oven to finish hot imidization, thereby obtaining the finished polyimide film. The film is coated twice and subjected to thermal imidization, so that a film surface with precise and controllable roughness is formed, and later application is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polyimide film preparation, and in particular relates to a method for precisely controlling the surface roughness of a polyimide film. Background Art

[0002] Polyimide film has been widely used in various harsh environments since its introduction in the 1960s due to its excellent properties such as high heat resistance, strong insulation, and radiation resistance. In practical applications, it is often involved in compounding and bonding with other materials to meet various different needs. For example, polyimide is not resistant to hydrolysis and atomic oxygen attack, so it is often compounded with fluorocarbon materials. Due to the needs of electronic circuits, it is often involved in compounding with copper foil.

[0003] The existing film-forming process of polyimide is generally to form a film from its precursor polyamic acid, and then obtain a commercial polyimide film through thermal imidization. The thermal imidization process is often accompanied by unidirectional or bidirectional stretching. Such a polyimide film has very excellent mechanical properties, but it also has a very high surface density and is difficult to composite (bond) with other materials.

[0004] Usually, different materials are composited or bonded by pressing them together physically, or by penetrating or bonding the surfaces of the two objects with an intermediate adhesive, or by directly bonding the two materials. The bonding of polymer materials often involves the mutual penetration and entanglement of polymer materials at the interface, so the morphology and roughness of the surface are directly related to the improvement of its bonding performance, so it is extremely necessary to precisely control the surface morphology and roughness of the material. Summary of the invention

[0005] In order to solve the above-mentioned technical problems, this application provides the following technical solutions:

[0006] The present invention provides a method for precisely controlling the surface roughness of a polyimide film, comprising the following steps:

[0007] S1: adding equivalent amounts of dianhydride monomer and diamine monomer into a non-protonic polar solvent, completing the reaction under the protection of ice bath and dry nitrogen to obtain polyamic acid (PAA) with a solid content of 20%;

[0008] S2: adding the polyamic acid to the same aprotic polar solvent as in step S1, and stirring under the protection of dry nitrogen to obtain a dilute polyamic acid solution;

[0009] S3: coating the polyamic acid solution obtained in step S1 on a carrier to form a film, and after the solvent is volatilized, vacuum heating is performed once to thermally imidize the polyamic acid (incomplete imidization) to obtain a primary polyimide film;

[0010] S4: soaking the primary polyimide film of step S3 in the diluted polyamic acid solution of step S2, adding the diluted polyamic acid solution, scraping off the polyamic acid solution after soaking, and performing secondary vacuum heating to completely thermally imidize the polyamic acid to obtain a finished polyimide film.

[0011] Preferably, in step S1, the solid content after adding the aprotic polar solvent is 19.5-20.5 wt%.

[0012] Preferably, in step S1, the aprotic polar solvent is selected from N,N-dimethylacetamide (DMAC); the dianhydride monomer is selected from pyromellitic dianhydride (PMDA); and the diamine monomer is selected from diphenyl ether diamine (ODA).

[0013] Preferably, in step S1, the reaction time is 10-14 hours.

[0014] Preferably, in step S2, the stirring time is 1-3 hours and the speed is 200-400 rpm.

[0015] Preferably, in step S2, the solid content of the polyamic acid solution is 20 wt%.

[0016] Preferably, in step S3, the solvent is volatilized at 75-85° C. and 1 atmosphere for 10-14 hours.

[0017] Preferably, in step S3, the vacuum heating condition is 240-260° C. for 3-5 hours.

[0018] Preferably, in step S3, the degree of initial thermal imidization is 40-80%.

[0019] Preferably, in step S4, the dilution concentration is 0.5-10wt%.

[0020] Preferably, in step S4, the secondary vacuum heating is performed at 340-360° C. for 3-5 hours.

[0021] Preferably, in step S4, the method of scraping off the polyamic acid solution is to remove excess solution through a slit mold.

[0022] Preferably, the thickness of the polyimide finished film is 15-55 μm, and the surface root mean square roughness (RMS) is 10 nm to 0.1 μm.

[0023] Specifically, the method for precisely controlling the surface roughness of a polyimide film comprises the following steps:

[0024] The precursor polyamic acid required for the polyimide membrane is synthesized from commercial equivalents of dianhydride monomers and diamine monomers in a non-protonic polar solvent (see the schematic diagram of the synthesis route). Figure 1 ), the solid content is generally designed to be 20% (the weight percentage of dianhydride monomer and diamine monomer in the solution), the synthesis of polyamic acid is completed under the protection of dry nitrogen, a small part of which is taken out for dilution into a dilute polyamic acid solution with a solid content of less than 10%; the polyamic acid with a solid content of 20% is coated on the carrier as required to form a polyamic acid film, and incomplete thermal imidization is performed to obtain a primary polyimide film; after the primary film is removed from the carrier, it is immersed in the aforementioned dilute solution, and then the excess solution is scraped off by two glass rods (used in the laboratory to simulate the gap mold in the actual production process) to form a uniform film and then placed in a vacuum oven to complete thermal imidization to obtain a finished polyimide film. See the process Figure 2 .

[0025] The technical solution of the present invention has the following advantages over the prior art:

[0026] The principle of the present invention is that the incompletely imidized polyimide primary film is self-sustaining and has a relatively dense surface density, but the polyamic acid therein is still soluble in the non-protonic polar solvent used in the reaction. At this time, a dilute polyamic acid solution is coated on the surface of the primary film and then a complete thermal imidization process is carried out. The polyamic acid in the dilute solution will produce molecular-level entanglement with the incompletely imidized polyamic acid in the initial film at the interface, and more polyamic acid in the dilute solution will complete the final thermal imidization on the surface of the initial film, and form different roughness of the membrane surface according to the solid content of the dilute solution.

[0027] The membrane adopts a double coating process and completes thermal imidization to form a membrane surface with precisely controllable roughness to facilitate subsequent applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic diagram of the synthesis route of polyimide;

[0029] Figure 2 It is a schematic diagram of the process route for laboratory preparation and precise control of the surface roughness of the polyimide film provided in Example 1;

[0030] Figure 3 This is a measured image (atomic force microscope) of the surface roughness of a polyimide film that has not been coated with a dilute polyamic acid solution for the second time.

[0031] Figure 4 This is a measured image (atomic force microscope) of the surface roughness of a polyimide film that was coated twice with a dilute polyamic acid solution having a solid content of 1.25 wt%.

[0032] Figure 5The figure is a measured image (atomic force microscope) of the surface roughness of a polyimide film after secondary coating with a dilute polyamic acid solution with a solid content of 1.25 wt%. DETAILED DESCRIPTION

[0033] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0034] Example 1

[0035] This embodiment provides a polyimide film with precisely controlled surface roughness, and the specific steps are as follows:

[0036] 1. Raw materials: Weigh equivalent ratios of pyromellitic anhydride (PMDA: actual 5.0066 g) and diphenyl ether diamine (ODA: actual 4.5925 g) in N'N-dimethylacetamide (DMAC: actual 38.85 g) as solvent (actual solid content: 19.8%)

[0037] 2. Synthesis of polyamic acid: At room temperature (23°C + / - 3°C), first dissolve ODA in DMAC, then add PMDA, and react in an ice bath with a magnetic stirrer (speed 300 rpm) for 12 hours under the protection of dry nitrogen to complete the synthesis of polyamic acid (PAA);

[0038] 3. Dilution of polyamic acid: Take the PAA described in 2 and add DMAC, stir for 2 hours on a magnetic stirrer (300 rpm) under dry nitrogen protection at room temperature to dilute to a PAA solution with a solid content of 1.25%;

[0039] 4. Preparation of polyimide primary membrane: Take the PAA mentioned above and, at room temperature, Figure 2 Schematic process for coating a polyamic acid film; volatilizing the solvent at 80°C and 1 atmosphere (1atm) for 12 hours; heating at 250°C and vacuum conditions (-0.01MPa) for 4 hours to obtain a primary polyimide film;

[0040] 5. Preparation of finished polyimide membrane: After immersing the primary membrane in the PAA solution with a solid content of 1.25% described in 3, a glass rod such as Figure 2 The excess PAA solution was scraped off; the polyimide finished film was obtained by heating at 350°C under vacuum conditions (-0.01 MPa) for 4 hours. The thickness of the polyimide in this embodiment was 25 μm.

[0041] Example 2

[0042] This embodiment provides a polyimide film with precisely controlled surface roughness, and the specific steps are as follows:

[0043] 1. Raw materials: Weigh equivalent ratios of pyromellitic anhydride (PMDA: actual 5.0066 g) and diphenyl ether diamine (ODA: actual 4.5925 g) in N'N-dimethylacetamide (DMAC: actual 38.85 g) as solvent (actual solid content: 19.8%)

[0044] 2. Synthesis of polyamic acid: At room temperature (23°C + / - 3°C), first dissolve ODA in DMAC, then add PMDA, and react in an ice bath with a magnetic stirrer (speed 300 rpm) for 12 hours under the protection of dry nitrogen to complete the synthesis of polyamic acid (PAA);

[0045] 3. Dilution of polyamic acid: Take the PAA described in 2 and add DMAC, stir for 2 hours on a magnetic stirrer (300 rpm) under dry nitrogen protection at room temperature to dilute to a PAA solution with a solid content of 2.5%;

[0046] 4. Preparation of polyimide primary membrane: Take the PAA mentioned above and, at room temperature, Figure 2 Schematic process for coating a polyamic acid film; volatilizing the solvent at 80°C and 1 atmosphere (1atm) for 12 hours; heating at 250°C and vacuum conditions (-0.01MPa) for 4 hours to obtain a primary polyimide film;

[0047] 5. Preparation of finished polyimide membrane: After immersing the primary membrane in the PAA solution with a solid content of 2.5% described in 3, a glass rod such as Figure 2 The excess PAA solution was scraped off; the polyimide finished film was obtained by heating at 350°C under vacuum conditions (-0.01 MPa) for 4 hours. The thickness of the polyimide in this embodiment was 25 μm.

[0048] Example 3

[0049] This embodiment provides a polyimide film with precisely controlled surface roughness, and the specific steps are as follows:

[0050] 1. Raw materials: Weigh equivalent ratios of pyromellitic anhydride (PMDA: actual 5.0066 g) and diphenyl ether diamine (ODA: actual 4.5925 g) in N'N-dimethylacetamide (DMAC: actual 38.85 g) as solvent (actual solid content: 19.8%)

[0051] 2. Synthesis of polyamic acid: At room temperature (23°C + / - 3°C), first dissolve ODA in DMAC, then add PMDA, and react in an ice bath with a magnetic stirrer (speed 200 rpm) for 10 hours under the protection of dry nitrogen to complete the synthesis of polyamic acid (PAA);

[0052] 3. Dilution of polyamic acid: Take the PAA described in 2 and add DMAC, stir for 1 hour on a magnetic stirrer (speed 200 rpm) under dry nitrogen protection at room temperature to dilute to a PAA solution with a solid content of 0.5 wt%;

[0053] 4. Preparation of polyimide primary membrane: Take the PAA mentioned above and, at room temperature, Figure 2 Schematic process for coating a polyamic acid film; volatilizing the solvent at 80°C and 1 atmosphere (1atm) for 12 hours; heating at 250°C and vacuum conditions (-0.01MPa) for 4 hours to obtain a primary polyimide film;

[0054] 5. Preparation of finished polyimide membrane: After immersing the primary membrane in the PAA solution with a solid content of 0.5 wt % described in 3, a glass rod such as Figure 2 The excess PAA solution was scraped off; the polyimide finished film was obtained by heating at 340° C. under vacuum conditions (-0.01 MPa) for 3 hours. The thickness of the polyimide in this embodiment was 15 μm.

[0055] Example 4

[0056] This embodiment provides a polyimide film with precisely controlled surface roughness, and the specific steps are as follows:

[0057] 1. Raw materials: Weigh equivalent ratios of pyromellitic anhydride (PMDA: actual 5.0066 g) and diphenyl ether diamine (ODA: actual 4.5925 g) in N'N-dimethylacetamide (DMAC: actual 38.85 g) as solvent (actual solid content: 19.8%)

[0058] 2. Synthesis of polyamic acid: At room temperature (23°C + / - 3°C), first dissolve ODA in DMAC, then add PMDA, and react in an ice bath with a magnetic stirrer (speed 400 rpm) for 14 hours under the protection of dry nitrogen to complete the synthesis of polyamic acid (PAA);

[0059] 3. Dilution of polyamic acid: Take the PAA described in 2 and add DMAC, stir for 3 hours on a magnetic stirrer (speed 400 rpm) under dry nitrogen protection at room temperature to dilute to a PAA solution with a solid content of 10 wt%;

[0060] 4. Preparation of polyimide primary membrane: Take the PAA mentioned above and, at room temperature, Figure 2 Schematic process for coating a polyamic acid film; volatilizing the solvent at 80°C and 1 atmosphere (1atm) for 12 hours; heating at 250°C and vacuum conditions (-0.01MPa) for 4 hours to obtain a primary polyimide film;

[0061] 5. Preparation of polyimide finished film: After immersing the primary film 4 in the PAA solution with a solid content of 10 wt % 3, a glass rod such as Figure 2 The excess PAA solution was scraped off; the polyimide finished film was obtained by heating at 360° C. under vacuum conditions (-0.01 MPa) for 5 hours. The thickness of the polyimide in this embodiment is 55 μm.

[0062] Effect evaluation 1

[0063] Figure 1 The synthesis reaction of the polyamic acid is shown. Figure 2 The polyamic acid film, polyimide film, and the laboratory preparation process for precisely controlling the surface roughness of the polyimide film are shown. Figures 3 to 5 The surface roughness of the polyimide film in various states in Example 1 was tested using an atomic force microscope.

[0064] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.

Claims

1. A method for precisely controlling the surface roughness of a polyimide film, characterized in that: The steps include: S1: adding equivalent amounts of dianhydride monomer and diamine monomer into a non-protonic polar solvent, completing the reaction under the protection of ice bath and dry nitrogen to obtain a polyamic acid solution with a solid content of 20%; S2: adding the polyamic acid to the aprotic polar solvent used in step S1, and stirring under dry nitrogen protection to obtain a polyamic acid dilute solution with a solid content of less than 10%; S3: coating the polyamic acid solution with a solid content of 20% obtained in step S1 on a carrier to form a film, and after the solvent is volatilized, vacuum heating is performed once to complete the initial thermal imidization of the polyamic acid to obtain a primary polyimide film; S4: soaking the primary polyimide film in step S3 in the dilute polyamic acid solution in step S2, scraping off the polyamic acid solution after soaking, and performing secondary vacuum heating to completely thermally imidize the polyamic acid to obtain a finished polyimide film.

2. The method for precisely controlling the surface roughness of a polyimide film according to claim 1, characterized in that: In the step S1, the solid content after adding the solvent is 19.5-20.5 wt%.

3. The method for precisely controlling the surface roughness of a polyimide film according to claim 1, characterized in that: In the step S1, the aprotic polar solvent is selected from N,N-dimethylacetamide; the dianhydride monomer is selected from pyromellitic dianhydride; and the diamine monomer is selected from diphenyl ether diamine.

4. The method for precisely controlling the surface roughness of a polyimide film according to claim 1, characterized in that: In step S1, the reaction time is 10-14 hours.

5. The method for precisely controlling the surface roughness of a polyimide film according to claim 1, characterized in that: In the step S3, the solvent is volatilized at 75-85° C. and 1 atmosphere for 10-14 hours.

6. The method for precisely controlling the surface roughness of a polyimide film according to claim 1, characterized in that: In step S3, the vacuum heating condition is 240-260° C. for 3-5 hours.

7. The method for precisely controlling the surface roughness of a polyimide film according to claim 1, characterized in that: In the step S3, the degree of initial thermal imidization is 40-80%.

8. The method for precisely controlling the surface roughness of a polyimide film according to claim 1, characterized in that: In the step S4, the dilution concentration is 0.5-10 wt %.

9. The method for precisely controlling the surface roughness of a polyimide film according to claim 1, characterized in that: In step S4, the secondary vacuum heating is performed at 340-360° C. for 3-5 hours.

10. The method for precisely controlling the surface roughness of a polyimide film according to claim 1, characterized in that: The thickness of the polyimide finished film is 15-55 μm, and the root mean square roughness of the surface is 10 nm to 0.1 μm.