Modified melamine sponge as well as preparation method and application thereof
By loading carbon black, polydopamine and octadecamine on melamine sponge, the photothermal conversion ability is improved, and the problem of poor absorption effect of existing sponges is solved, achieving efficient absorption and recycling of heavy oil.
Patent Information
- Application Number
- CN202411406331.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-10
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-10-10
AI Technical Summary
The existing superhydrophobic and super-lipophilic sponges have poor absorption effects in oil-water separation and water surface oil pollution adsorption. They can only absorb oil or organic solvents with about 50 times their own weight, making it difficult to effectively deal with marine pollution caused by offshore crude oil leakage and industrial emissions.
Modified by loading the melamine sponge with carbon black, polydopamine and octadecamine, using carbon black as the photothermal conversion material, polydopamine as the binder and solar absorber, and octadecamine as the superhydrophobic modification reagent, the modified product was prepared by using carbon black as the photothermal conversion material, polydopamine as the binder and solar absorber, and octadecamine as the superhydrophobic modification reagent. Metamine sponge improves its adsorption performance and photothermal conversion capability.
The surface temperature of the modified melamine sponge can quickly increase under simulated sunlight irradiation, increasing the oil absorption rate and capacity. It can maintain the absorption capacity by more than 100 times its own weight after 10 cycles of oil absorption, significantly improving the heavy oil and extra thickening. Oil absorption properties.
Smart Images

Figure CN119081226A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of petroleum resource cleaning and recovery, and specifically relates to a modified melamine sponge and a preparation method and application thereof. Background Art
[0002] With the development of the chemical industry, the demand for offshore crude oil extraction and the transportation of petroleum and chemical solvents has increased. The leakage of crude oil and chemicals during storage and transportation and the illegal discharge of industries have caused great harm to marine and freshwater resources. Therefore, efficient crude oil spill treatment and recovery technology is urgently needed. The average global seawater temperature is about 20°C. At this temperature, it is very difficult to separate water and crude oil for reabsorption and recovery. Superhydrophobic and superoleophilic sponges with selective absorption have great application prospects in oil-water separation and oil adsorption on water surfaces. However, the absorption effect of this super hydrophobic and super oleophilic sponge is still poor, and it can only absorb oil or organic solvent about 50 times its own weight. For example, CN110003519A records a method for preparing a super hydrophobic sponge with photothermal effect and magnetic drive flame retardancy, comprising the following steps: step (1) pretreating the melamine sponge: immersing the melamine sponge in deionized water, ultrasonically cleaning it, taking it out and drying it, then immersing it in an organic solvent for ultrasonic cleaning, and drying it to obtain the pretreated melamine sponge; step (2) preparing nano magnetic particles and PDMS treatment solution: adding PDMS prepolymer to an organic solvent, and magnetically stirring it, then adding a curing agent, and stirring it to disperse it evenly; then, under mechanical stirring and ultrasonic dispersion, adding the nano magnetic particles to the PDMS resin solution, stirring it ultrasonically, and obtaining the nano magnetic particles and PDMS treatment solution; step (3) immersing the pretreated melamine sponge in the nano magnetic particles and PDMS treatment solution, squeezing out the excess treatment solution in the melamine sponge after ultrasonic treatment, and then vacuum drying the soaked melamine sponge to obtain the super hydrophobic sponge.
[0003] Therefore, how to improve the adsorption performance of sponges has become a technical problem that needs to be solved urgently in this field. Summary of the invention
[0004] The purpose of the present invention is to provide a modified melamine sponge and a preparation method and application thereof. The modified melamine sponge provided by the present invention has excellent selective absorption and large-capacity absorption performance for heavy oil.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions: The invention provides a modified melamine sponge, comprising a melamine sponge and carbon black, polydopamine and octadecylamine loaded on the melamine sponge.
[0006] The present invention also provides a method for preparing the modified melamine sponge described in the above technical solution, comprising the following steps: (1) immersing the melamine sponge in a carbon black dispersion to load the melamine sponge once, thereby obtaining a melamine sponge loaded with carbon black; (2) immersing the carbon black loaded melamine sponge obtained in step (1) in a tris(hydroxymethyl)aminomethane (Tris) buffer solution containing dopamine hydrochloride to perform in-situ polymerization to obtain a melamine sponge loaded with carbon black and polydopamine; (3) Immersing the melamine sponge loaded with carbon black and polydopamine obtained in step (2) in an organic solution of octadecylamine for secondary loading to obtain a modified melamine sponge.
[0007] Preferably, in step (1), the particle size of the carbon black is 20-30 nm, and the specific surface area of the carbon black is 150-190 m 2 / g, the volatile content of carbon black is 7~8%.
[0008] Preferably, the concentration of the carbon black dispersion in step (1) is 1.5-2.5 g / L.
[0009] Preferably, the time for one loading in step (1) is 15 to 30 minutes.
[0010] Preferably, the concentration of dopamine hydrochloride in the tris(hydroxymethylaminomethane) buffer solution containing dopamine hydrochloride in step (2) is 1.5-2.5 g / L.
[0011] Preferably, the time of the in-situ polymerization in step (2) is 16 to 24 hours.
[0012] Preferably, the concentration of the organic solution of octadecylamine in step (3) is 3.0-4.5 wt %.
[0013] Preferably, the secondary loading time in step (3) is 25 to 40 minutes.
[0014] The present invention also provides the use of the modified melamine sponge described in the above technical solution or the modified melamine sponge prepared by the preparation method described in the above technical solution in absorbing heavy oil.
[0015] The present invention provides a modified melamine sponge, comprising a melamine sponge and carbon black, polydopamine and octadecylamine loaded on the melamine sponge. The present invention uses carbon black as a photothermal conversion material loaded on the melamine sponge, so that the melamine sponge has photothermal conversion performance; using polydopamine as a binder can not only effectively strengthen the adhesion between the carbon black and the melamine sponge skeleton, but also introduce roughness due to its own deposition, thereby improving hydrophobicity; at the same time, polydopamine also has broadband solar energy absorption characteristics, and has a synergistic effect with carbon black in photothermal conversion; in addition, polydopamine contains amine functional groups and more cyclized indole structures, which increases the types and quantities of groups on the melamine sponge and increases the loading amount of octadecylamine; using octadecylamine as a superhydrophobic modification agent to obtain a modified melamine sponge; this modified melamine sponge has superhydrophobicity, can prevent water from being absorbed while absorbing oil, and also has excellent photothermal conversion ability, can quickly convert the absorbed sunlight into its own heat, and then in-situ heat the contacted heavy oil, so that the viscosity of the heavy oil is reduced, the fluidity is increased, thereby improving the oil absorption rate and increasing the oil absorption capacity. The experimental results show that the water contact angle of the modified melamine sponge provided by the present invention is 153.2±0.6°, and the water contact angle of the modified melamine sponge provided by the present invention is 153.2±0.6° at 1.0 kW / m 2 Under simulated sunlight, the surface temperature of the modified melamine sponge can reach 76.2°C within 1 minute, showing efficient photothermal conversion performance; the oil absorption capacity of heavy oil and extra heavy oil of 3671~44204mPa·s can reach 114~126 times of its own weight. After 10 cycles of oil absorption, the absorption capacity still remains at more than 100 times of its own weight. The modified melamine sponge shows excellent absorption and cycle performance in absorbing heavy oil and extra heavy oil. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 The present invention is a process flow chart for preparing modified melamine sponge; Figure 2 is the water contact angle of the clean melamine sponge in Example 1; Figure 3 The water contact angle of the modified melamine sponge prepared in Example 1; Figure 4 The water contact angle of the modified melamine sponge prepared in Example 2; Figure 5 The water contact angle of the modified melamine sponge prepared in Example 3; Figure 6 The water contact angle of the modified melamine sponge prepared in Comparative Example 4; Figure 7 The water contact angle of the modified melamine sponge prepared in Example 4; Figure 8 The water contact angle of the modified melamine sponge prepared in Comparative Example 5; Fig. 9The temperature of the upper and lower surfaces of the modified melamine sponge prepared in Example 1 varies with different light intensities; Fig.10 The temperature of the upper surface of the modified melamine sponge irradiated with different light intensities changes with time; Fig.11 The oil absorption capacity of the modified melamine sponge prepared in Example 1 when adsorbing crude oil A for ten cycles; Fig.12 The oil absorption capacity of the modified melamine sponge prepared in Example 1 when adsorbing crude oil B for ten cycles; Fig.13 The oil absorption capacity of the modified melamine sponge prepared in Example 1 when adsorbing crude oil C for ten cycles; Fig.14 The modified melamine sponge prepared in Example 1 is a photograph of the modified melamine sponge after ten cycles of adsorbing crude oil A and then washed and dried, and the water contact angle thereof; Fig.15 The modified melamine sponge prepared in Example 1 is a photograph of the modified melamine sponge after ten cycles of adsorption of crude oil B and washing and drying, as well as the water contact angle; Fig.16 The modified melamine sponge prepared in Example 1 is a photograph of the modified melamine sponge after ten cycles of adsorption of crude oil C and then washed and dried, as well as the water contact angle; Fig.17 This is the process of the modified melamine sponge prepared in Example 1 absorbing heavy oil on water. DETAILED DESCRIPTION
[0017] The invention provides a modified melamine sponge, comprising a melamine sponge and carbon black, polydopamine and octadecylamine loaded on the melamine sponge.
[0018] In the present invention, the water contact angle of the modified melamine sponge is preferably ≥150°; the modified melamine sponge is preferably ≥150°; 2 The surface temperature preferably rises to above 76°C within 1 minute under sunlight irradiation; for a viscosity of 3×10 3 ~4.5×10 4 mPa·s heavy oil and extra heavy oil, the absorption capacity of the modified melamine sponge is preferably 114 to 126 times the weight of the modified melamine sponge itself.
[0019] The present invention uses carbon black as a photothermal conversion material loaded on a melamine sponge, so that the melamine sponge has photothermal conversion performance; using polydopamine as a binder can not only effectively strengthen the adhesion between the carbon black and the melamine sponge skeleton, but also introduce roughness due to its own deposition, thereby improving hydrophobicity; at the same time, polydopamine also has the characteristics of broadband solar energy absorption, and has a synergistic effect with carbon black in photothermal conversion; in addition, polydopamine contains amine functional groups and more cyclized indole structures, which increases the types and quantities of groups on the melamine sponge and increases the loading amount of octadecylamine; using octadecylamine as a superhydrophobic modification agent to obtain a modified melamine sponge; the modified melamine sponge has superhydrophobicity, can prevent water from being absorbed while absorbing oil, and also has excellent photothermal conversion ability, can quickly convert absorbed sunlight into its own heat, and then in-situ heat the contacted heavy oil, so that the viscosity of the heavy oil is reduced, the fluidity is increased, and thus the oil absorption rate and oil absorption capacity are improved.
[0020] The modified melamine sponge provided by the present invention can quickly heat itself up through solar heat, thereby heating crude oil in situ, absorbing crude oil quickly and with high capacity, and after absorbing the oil, the absorbed oil can be squeezed out and recycled.
[0021] The present invention also provides a method for preparing the modified melamine sponge described in the above technical solution, comprising the following steps: (1) immersing the melamine sponge in a carbon black dispersion to load the melamine sponge once, thereby obtaining a melamine sponge loaded with carbon black; (2) immersing the carbon black loaded melamine sponge obtained in step (1) in a tris(hydroxymethyl)aminomethane buffer solution containing dopamine hydrochloride to perform in-situ polymerization to obtain a melamine sponge loaded with carbon black and polydopamine; (3) Immersing the melamine sponge loaded with carbon black and polydopamine obtained in step (2) in an organic solution of octadecylamine for secondary loading to obtain a modified melamine sponge.
[0022] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known in the art.
[0023] The present invention immerses the melamine sponge in a carbon black dispersion liquid and performs a loading operation to obtain the carbon black loaded melamine sponge.
[0024] In the present invention, the porosity of the melamine sponge is preferably 95-99%, more preferably 99%; the density of the melamine sponge is preferably 9.0-9.8 kg / m 3 , more preferably 9.5 kg / m 3 .
[0025] In the present invention, the melamine sponge is preferably cut, cleaned and dried in sequence before use.
[0026] The present invention has no special limitation on the cutting operation, and the cutting operation can be performed by those skilled in the art to the desired size.
[0027] In the present invention, the cleaning preferably comprises: ultrasonically cleaning the melamine sponge with anhydrous ethanol and ultrapure water in sequence; the ultrasonic cleaning time is independently preferably 15 to 30 minutes, more preferably 20 minutes. The present invention can remove dirt on the melamine sponge by cleaning the melamine sponge.
[0028] In the present invention, the drying temperature is preferably 50-80° C., more preferably 60° C.; the drying time is preferably 8-24 h, more preferably 8 h.
[0029] In the present invention, the carbon black dispersion is preferably obtained by ultrasonically treating carbon black and ultrapure water. The present invention has no particular limitation on the operation of ultrasonically treating carbon black and ultrapure water to prepare the carbon black dispersion, as long as the carbon black dispersion is obtained.
[0030] In the present invention, the particle size of the carbon black is preferably 20-30 nm; the specific surface area of the carbon black is preferably 150-190 m 2 / g; the volatile matter of the carbon black is preferably 7~8%.
[0031] In the present invention, the concentration of the carbon black dispersion is preferably 1.5-2.5 g / L, more preferably 2.0 g / L. In the present invention, limiting the concentration of the carbon black dispersion to the above range can improve the modification effect on the melamine sponge.
[0032] The present invention has no special requirement on the usage of the melamine sponge and the carbon black dispersion, as long as the melamine sponge can be completely immersed.
[0033] The present invention has no particular limitation on the operation of immersing the melamine sponge in the carbon black dispersion, and the operation well known to those skilled in the art can be adopted.
[0034] In the present invention, the primary loading is preferably carried out under ultrasonic conditions. The present invention has no special requirements on the power of the ultrasound, and the ultrasound power well known in the art can be used. The present invention utilizes ultrasound to fully disperse the carbon black and load it onto the melamine sponge; during the ultrasonic immersion of the melamine sponge in the carbon black dispersion, a large amount of carbon black nanoparticles are loaded on the surface of the melamine sponge to improve the light-to-heat conversion performance of the melamine sponge.
[0035] In the present invention, the time of the primary loading is preferably 15 to 30 minutes, more preferably 20 minutes. The present invention has no particular limitation on the temperature of the primary loading, and it can be carried out at room temperature.
[0036] After the first loading is completed, the present invention preferably takes out the product obtained from the first loading from the carbon black dispersion and then dries it to obtain a melamine sponge loaded with carbon black.
[0037] The present invention has no particular limitation on the operation of taking out the carbon black dispersion, and the operation well known to those skilled in the art may be adopted.
[0038] In the present invention, the drying temperature is preferably 50-80° C., more preferably 60° C.; the drying time is preferably 8-24 h, more preferably 8 h.
[0039] After obtaining the melamine sponge loaded with carbon black, the present invention immerses the melamine sponge loaded with carbon black in a tris(hydroxymethyl)aminomethane) buffer solution containing dopamine hydrochloride to perform in-situ polymerization to obtain a melamine sponge loaded with carbon black and polydopamine. The present invention uses polydopamine formed by self-polymerization of dopamine as a binder, which can not only effectively strengthen the adhesion between carbon black and the sponge skeleton, but also introduce roughness due to its own deposition and improve hydrophobicity; polydopamine also has broadband solar energy absorption characteristics and has a synergistic effect with carbon black in terms of photothermal conversion; at the same time, polydopamine contains amine functional groups and more cyclized indole structures, which increases the types and quantities of groups on the melamine sponge, making it easier to subsequently graft octadecylamine.
[0040] In the present invention, the Tris buffer solution containing dopamine hydrochloride is preferably obtained by mixing dopamine hydrochloride, Tris and ultrapure water.
[0041] In the present invention, the concentration of dopamine hydrochloride in the Tris buffer solution containing dopamine hydrochloride is preferably 1.5-2.5 g / L, more preferably 2.0 g / L; the pH of the Tris buffer solution containing dopamine hydrochloride is preferably 8.3-8.7, more preferably 8.5; the concentration of Tris in the Tris buffer solution containing dopamine hydrochloride is preferably 50 mM.
[0042] In the present invention, the pH value of the Tris buffer solution containing dopamine hydrochloride is preferably adjusted using dilute hydrochloric acid.
[0043] In the present invention, the volume ratio of the Tris buffer solution containing dopamine hydrochloride to the melamine sponge loaded with carbon black is preferably ≥ 5. By limiting the above volume ratio, the present invention can ensure that dopamine can fully wrap the surface of the melamine sponge skeleton after self-polymerization into polydopamine.
[0044] The present invention has no particular limitation on the operation of immersing the carbon black-loaded melamine sponge in a tris(hydroxymethyl)aminomethane buffer solution containing dopamine hydrochloride, and the operation well known to those skilled in the art can be adopted.
[0045] In the present invention, the time of the in-situ polymerization is preferably 16 to 24 hours, more preferably 18 to 20 hours; the in-situ polymerization is preferably carried out under stirring conditions; and the stirring rate is preferably 400 to 500 rpm.
[0046] After the in-situ polymerization is completed, the present invention preferably removes the product obtained by the in-situ polymerization from the Tris buffer solution containing dopamine hydrochloride, and then washes and dries it in sequence to obtain a melamine sponge loaded with carbon black and polydopamine.
[0047] The present invention has no particular limitation on the operation of taking out from the Tris buffer solution containing dopamine hydrochloride, and the operation well known to those skilled in the art can be adopted.
[0048] In the present invention, the washing liquid used in the washing is preferably ultrapure water. The present invention has no special limitation on other operations of the washing, as long as the ultrapure water becomes clear.
[0049] In the present invention, the drying temperature is preferably 50-80° C., more preferably 60° C.; the drying time is preferably 8-24 h, more preferably 8 h.
[0050] After obtaining the melamine sponge loaded with carbon black and polydopamine, the present invention immerses the melamine sponge loaded with carbon black and polydopamine in an organic solution of octadecylamine for secondary loading to obtain a modified melamine sponge. The present invention uses octadecylamine as a super-hydrophobic modification agent to be grafted on the melamine sponge, so that the melamine sponge has super-hydrophobicity, can prevent water from being absorbed while absorbing oil, thereby improving the oil absorption rate and oil absorption capacity.
[0051] In the present invention, the solvent of the organic solution of octadecylamine is preferably anhydrous ethanol; the concentration of the organic solution of octadecylamine is preferably 3.0-4.5wt%, more preferably 3.5wt%. In the present invention, anhydrous ethanol is cheap and has a low pollution degree, and will not inhibit the reaction process in the subsequent modification process of melamine sponge.
[0052] The present invention has no particular limitation on the method for preparing the organic solution of octadecylamine, and operations familiar to those skilled in the art may be used.
[0053] In an embodiment of the present invention, the preparation method of the organic solution of octadecylamine is to mix anhydrous ethanol and octadecylamine, heat to 60° C. in a water bath, and then cool to room temperature.
[0054] The present invention has no particular limitation on the operation of immersing the melamine sponge loaded with carbon black and polydopamine into the organic solution of octadecylamine, and the operation well known to those skilled in the art can be adopted.
[0055] In the present invention, the time of the secondary loading is preferably 25 to 40 minutes, more preferably 30 minutes. The present invention has no particular limitation on the temperature of the secondary loading, and it can be carried out at room temperature.
[0056] After the secondary loading is completed, the present invention preferably takes out the product obtained by the secondary loading from the solution, and then sequentially performs primary drying, washing and secondary drying to obtain a modified melamine sponge.
[0057] The present invention has no particular limitation on the operation of taking out the substance from the solution, and any operation well known to those skilled in the art may be used.
[0058] In the present invention, the primary drying temperature is preferably 25-60° C., more preferably 60° C.; the primary drying time is preferably 8-24 hours, more preferably 8 hours. The primary drying of the present invention can make the octadecylamine loaded on the sponge more uniformly and firmly.
[0059] In the present invention, the washing agent used in the washing is preferably anhydrous ethanol. The present invention has no special limitation on the washing operation, and the operation well known to those skilled in the art can be used.
[0060] In the present invention, the secondary drying temperature is preferably 25-60° C., more preferably 60° C.; the secondary drying time is preferably 8-24 h, more preferably 8 h.
[0061] The preparation method provided by the invention is simple to operate.
[0062] The process flow chart of the present invention for preparing modified melamine sponge is as follows Figure 1 shown.
[0063] from Figure 1 It can be seen that the melamine sponge is first immersed in a carbon black dispersion for ultrasonic treatment, taken out and dried to obtain a melamine sponge loaded with carbon black; then the melamine sponge loaded with carbon black is immersed in a Tris buffer solution containing dopamine hydrochloride, stirred, taken out and dried to obtain a melamine sponge loaded with carbon black and polydopamine; finally, the melamine sponge loaded with carbon black and polydopamine is immersed in an anhydrous ethanol solution of octadecylamine for modification, taken out and dried to obtain a modified melamine sponge.
[0064] The present invention also provides the use of the modified melamine sponge described in the above technical solution or the modified melamine sponge prepared by the preparation method described in the above technical solution in absorbing heavy oil.
[0065] The present invention has no special limitation on the application operation of the modified melamine sponge in absorbing heavy oil, and the application operation well known to those skilled in the art can be adopted.
[0066] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0067] Example 1 The modified melamine sponge consists of a melamine sponge and carbon black, polydopamine and octadecylamine loaded on the melamine sponge; The preparation method of the modified melamine sponge consists of the following steps: (1) The melamine sponge was cut into cubes of 2 cm × 2 cm × 2 cm, and then ultrasonically cleaned with anhydrous ethanol and ultrapure water for 20 min respectively, and then dried in an oven at 60 ° C for 8 h to obtain a clean melamine sponge; the porosity of the melamine sponge was 99% and the density was 9.5 kg / m 3 ; (2) 0.2 g of carbon black was added to 100 mL of ultrapure water, and ultrasonicated for 20 min to obtain a carbon black dispersion with a concentration of 2.0 g / L. The clean melamine sponge obtained in step (1) was immersed in the carbon black dispersion, and loaded once by ultrasonicating for 20 min. After being taken out, the sponge was directly placed in a 60° C. oven for drying for 8 h to obtain a melamine sponge loaded with carbon black; wherein the particle size of the carbon black was 20-30 nm, and the specific surface area was 150-190 m 2 / g, volatile matter is 7~8%; (3) diluting concentrated hydrochloric acid to 1 M, then dissolving 1 g of dopamine hydrochloride in 500 mL of ultrapure water, adding 50 mM Tris thereto, stirring to dissolve, measuring the pH of the prepared solution using a pH meter, and adding 1 M hydrochloric acid dropwise to the prepared solution until the pH of the solution is 8.5, thereby obtaining a Tris buffer solution containing dopamine hydrochloride; wherein the concentration of dopamine hydrochloride in the Tris buffer solution containing dopamine hydrochloride is 2.0 g / L; (4) immersing the carbon black loaded melamine sponge obtained in step (2) into the Tris buffer solution containing dopamine hydrochloride obtained in step (3), stirring at 500 rpm for 24 hours for in-situ polymerization, then taking out, washing with ultrapure water until the water is clear, and then drying in an oven at 60° C. for 8 hours to obtain a melamine sponge loaded with carbon black and polydopamine; wherein the volume ratio of the Tris buffer solution containing dopamine hydrochloride to the carbon black loaded melamine sponge is 5; (5) Add 96.5 g of anhydrous ethanol to a beaker, add 3.5 g of octadecylamine to the beaker, heat in a water bath to 60° C., and then cool the solution to room temperature to obtain an anhydrous ethanol solution of octadecylamine with a concentration of 3.5 wt %. Then immerse the melamine sponge loaded with carbon black and polydopamine obtained in step (4) in the anhydrous ethanol solution of octadecylamine, let it stand for 30 minutes for secondary loading, then take it out and place it in an oven at 60° C. for 8 hours to obtain a sponge wrapped by a white shell of octadecylamine. Then place the sponge in anhydrous ethanol until the white shell is completely dissolved, and finally place it in an oven at 60° C. for 8 hours to obtain a modified melamine sponge, which is recorded as OPCM.
[0068] Example 2 On the basis of Example 1, the concentration of the anhydrous ethanol solution of octadecylamine was changed to 3.0 wt %, and other conditions remained unchanged.
[0069] Example 3 On the basis of Example 1, the concentration of the anhydrous ethanol solution of octadecylamine was changed to 4.0 wt %, and other conditions remained unchanged.
[0070] Example 4 On the basis of Example 1, the secondary load time was changed to 40 min, and other conditions remained unchanged.
[0071] Comparative Example 1 The preparation method of the carbon black loaded melamine sponge is as follows: based on Example 1, the concentration of the carbon black dispersion is changed to 1.5 g / L, and other conditions remain unchanged.
[0072] Comparative Example 2 The preparation method of the carbon black loaded melamine sponge is as follows: based on Example 1, the concentration of the carbon black dispersion is changed to 2.5 g / L, and other conditions remain unchanged.
[0073] Comparative Example 3 The preparation method of the carbon black loaded melamine sponge is as follows: based on Example 1, the concentration of the carbon black dispersion is changed to 1.0 g / L, and other conditions remain unchanged.
[0074] Comparative Example 4 On the basis of Example 1, the concentration of the anhydrous ethanol solution of octadecylamine was changed to 2.5 wt %, and other conditions remained unchanged.
[0075] Comparative Example 5 On the basis of Example 1, the secondary load time was changed to 20 min, and other conditions remained unchanged.
[0076] Structure and performance characterization: 1. The photothermal temperature of the melamine sponge loaded with carbon black in Example 1 and Comparative Examples 1 to 3 was measured. The photothermal temperature was measured by simulating a xenon lamp with a 1 kW / m2 The surface temperature of the carbon black loaded melamine sponge (CM) was measured by infrared thermal imager under sunlight irradiation. The results are shown in Table 1.
[0077] Table 1 Surface temperature of melamine sponge loaded with carbon black in Example 1 and Comparative Examples 1 to 3
[0078] It can be seen from Table 1 that the photothermal temperature of CM increases with the increase of carbon black dispersion concentration; when the carbon black dispersion concentration is 1.0 g / L, the surface temperature of CM only reaches 66.7 °C; when the carbon black dispersion concentration is 2.0 g / L and 2.5 g / L, the surface temperature of CM can reach about 75 °C.
[0079] 2. The clean melamine sponge in Example 1, and the modified melamine sponge prepared in Examples 1 to 3 and Comparative Example 4 were tested for water contact angle: the melamine sponge and the modified melamine sponge were placed flat on the instrument platform using a Teclis Tracker interfacial tension meter produced by a French company. The syringe provided by the instrument was used to adopt the hanging drop method. 5 μL of deionized water was dripped on the surface of the sponge each time. The water contact angle was calculated using the sessile drop young-Laplace software. Five different locations were selected on each sample for repeated measurement, and the average value and standard deviation were calculated. The results are shown in FIG. Figures 2 to 6 As shown in Table 2, Figure 2 is the water contact angle of the clean melamine sponge in Example 1; Figure 3 The water contact angle of the modified melamine sponge prepared in Example 1; Figure 4 The water contact angle of the modified melamine sponge prepared in Example 2; Figure 5 The water contact angle of the modified melamine sponge prepared in Example 3; Figure 6 This is the water contact angle of the modified melamine sponge prepared in Comparative Example 4.
[0080] Table 2 Water contact angles of the clean melamine sponge in Example 1, and the modified melamine sponges prepared in Examples 1 to 3 and Comparative Example 4
[0081] Depend on Figures 2 to 6 It can be seen from Table 2 that the hydrophobicity of the modified melamine sponge increases with the increasing concentration of the anhydrous ethanol solution of octadecylamine; when the concentration of the anhydrous ethanol solution of octadecylamine is 2.5wt%, the water contact angle of the modified melamine sponge is <150°, and when the concentration of octadecylamine is 3.5wt% and 4.0wt%, the water contact angle of the modified melamine sponge is >153°, which is superhydrophobic. The stronger the hydrophobicity, the higher the oil-water separation efficiency.
[0082] 3. The water contact angle test was performed on the modified melamine sponge prepared in Example 4 and Comparative Example 5 according to the above method. The results are as follows: Figure 7-8 As shown in Table 3, Figure 7 The water contact angle of the modified melamine sponge prepared in Example 4; Figure 8 This is the water contact angle of the modified melamine sponge prepared in Comparative Example 5.
[0083] Table 3 Water contact angles of the clean melamine sponge in Example 1, and the modified melamine sponges prepared in Examples 1, 4, and Comparative Example 5
[0084] Depend on Figure 2 , 3 , 7~8 and Table 3, it can be seen that when the secondary loading time is 30 min, the water contact angle of the modified melamine sponge reaches the maximum.
[0085] 4. The photothermal conversion temperature of the modified melamine sponge OPCM prepared in Example 1 was tested: a xenon lamp was used as a light source to simulate sunlight, and the light intensity of the xenon lamp was set to 0.5 kW / m 2 , 1.0kW / m 2 , 1.5kW / m 2 , 2.0kW / m 2 , 2.5kW / m 2 , respectively irradiated for 6 minutes, and one cycle process was 10 minutes, that is, the process from turning on the light source OPCM to starting to heat up to turning off the light source OPCM temperature down to room temperature was 10 minutes. The change of the surface temperature of the modified melamine sponge with time was recorded using an infrared thermal imager. The results are as follows Fig. 9 and 10 As shown, Fig. 9 The temperature of the upper and lower surfaces of the modified melamine sponge prepared in Example 1 varies with different light intensities; Fig.10 This is a graph showing the change in surface temperature over time of modified melamine sponge irradiated with different light intensities.
[0086] Depend on Fig. 9 and 10 It can be seen that as the light intensity increases from 0.5kW / m 2 Up to 2.5kW / m 2 , the upper surface temperature of the modified melamine sponge increased from 46.5℃ to 117.2℃; when the light intensity was 1.0 kW / m 2When the light power is 0.5, the surface temperature of the modified melamine sponge can reach 76.2℃. Obviously, the steady-state temperature at the top of the modified melamine sponge is positively correlated with the light power, and the steady-state temperature at the bottom is also similar. Under different light intensities, the surface temperature of the modified melamine sponge rises rapidly and reaches stability within 1 minute, indicating that the modified melamine sponge can quickly convert the absorbed light into heat and transfer it to the bottom of the sponge. Therefore, the rapid temperature rise and thermal conductivity of the surface of the modified melamine sponge can reduce the viscosity of heavy oil, increase the fluidity of heavy oil, and thus improve the oil absorption efficiency.
[0087] 5. The heavy oil absorption performance of the modified melamine sponge prepared in Examples 1 to 4 was tested: three heavy oils and extra heavy oils with different viscosities (at room temperature of 20°C, the viscosities were crude oil A: 44204 mPa·s, crude oil B: 9373 mPa·s and crude oil C: 3671 mPa·s), the dry weight of the modified melamine sponge that did not absorb the heavy oil was first weighed and recorded, and then the dry weight of the modified melamine sponge was measured at 1 kW / m 2 Under simulated sunlight, the modified melamine sponge was immersed in heavy oil for 40 minutes, and was gently picked up with tweezers. When no excess oil drops were left, the mass of the modified melamine sponge that had absorbed the heavy oil was weighed. The absorption capacity of the modified melamine sponge for heavy oil (Q W , g / g) is calculated by the following formula:
[0088] Wherein, m0 is the dry weight of the modified melamine sponge without absorbing heavy oil, and m1 is the mass of the modified melamine sponge that has absorbed heavy oil.
[0089] According to the formula, we can calculate: The maximum saturated absorption capacity of the modified melamine sponge prepared in Example 1 for crude oil A is 126 g / g, crude oil B is 117 g / g, and crude oil C is 114 g / g. In the absence of light, the modified melamine sponge is difficult to be immersed in the heavy oil. After 43 minutes, the modified melamine sponge was immersed in crude oil C; after 1 hour, the modified melamine sponge was immersed in crude oil B for about 1 cm. The modified melamine sponge remained on the surface of crude oil A. At 1 kW / m 2 Under the irradiation of simulated sunlight, the modified melamine sponge is completely immersed in the surfaces of crude oil A, B, and C for approximately 33 minutes, 10 minutes, and 6.5 minutes, respectively, and the immersion speed is greatly improved. This shows that the photothermal conversion of solar energy plays a key role in the oil absorption of the modified sponge. The good photothermal conversion performance of the modified melamine sponge heats the heavy oil after heating, reduces the viscosity of the heavy oil, and increases its fluidity; in addition, the hydrophobic effect and capillary force of the modified melamine sponge accelerate its absorption rate of crude oil; the oil absorption capacity increases, which can reach more than 114 times the weight of the sponge itself.
[0090] The maximum saturated absorption capacity of the modified melamine sponge prepared in Example 2 for crude oil A is 124 g / g, that for crude oil B is 116 g / g, and that for crude oil C is 114 g / g.
[0091] The maximum saturated absorption capacity of the modified melamine sponge prepared in Example 3 for crude oil A is 127 g / g, that for crude oil B is 117 g / g, and that for crude oil C is 114 g / g.
[0092] The maximum saturated absorption capacity of the modified melamine sponge prepared in Example 4 for crude oil A is 125 g / g, that for crude oil B is 117 g / g, and that for crude oil C is 113 g / g.
[0093] 6. Test the cyclic oil absorption performance of the modified melamine sponge prepared in Example 1: The oil absorption method in 5 above enables the modified melamine sponge to absorb heavy oil. After each oil absorption is completed, the absorbed oil is released by squeezing. The heavy oil absorption capacity of the modified melamine sponge is calculated according to the formula in 5. After each oil absorption is completed, it is recorded as a completed oil absorption cycle. Then, the squeezed sponge is placed in 40 mL of cyclohexane and soaked for 3 times in sequence, each time for 5 minutes, taken out, squeezed to release the absorbed cyclohexane, and then placed in a 60°C oven to dry for 3.5 hours, and then it can be used to absorb heavy oil again. The results are as follows. Figures 11 to 16 As shown, Fig.11 The oil absorption capacity of the modified melamine sponge prepared in Example 1 when adsorbing crude oil A for ten cycles; Fig.12 The oil absorption capacity of the modified melamine sponge prepared in Example 1 when adsorbing crude oil B for ten cycles; Fig.13 The oil absorption capacity of the modified melamine sponge prepared in Example 1 when adsorbing crude oil C for ten cycles; Fig.14 The modified melamine sponge prepared in Example 1 is a photograph of the modified melamine sponge after ten cycles of adsorbing crude oil A and then washed and dried, and the water contact angle; Fig.15 The modified melamine sponge prepared in Example 1 is a photograph of the modified melamine sponge after ten cycles of adsorption of crude oil B and then washed and dried, as well as the water contact angle; Fig.16 The modified melamine sponge prepared in Example 1 absorbs crude oil C for ten cycles and then is washed and dried, as well as the water contact angle.
[0094] Depend on Figures 11 to 16 It can be seen that after 10 cycles, the absorption capacity of the modified melamine sponge is still maintained at more than 100 times of its own weight, showing a relatively outstanding high absorption capacity; and the modified melamine sponge is not damaged, showing good rigidity and toughness; at the same time, the modified melamine sponge still has an excellent hydrophobic state, and the water contact angles are 142.2°, 147.5° and 144.7°, all above 140°. Its excellent performance in cyclic oil absorption is due to its solid hydrophobic modification, stable mechanical properties and excellent photothermal properties.
[0095] 7. The modified melamine sponge prepared in Example 1 was subjected to a water surface oil absorption experiment: 1 g of thick oil was dropped on a petri dish filled with tap water at 20°C, and a magnetic stirrer was used to gently stir the oil droplets to disperse, simulating the dispersion and floating of thick oil spilled at sea. A xenon lamp was used as a light source to simulate sunlight, and the light intensity of the xenon lamp was set to 1.0 kW / m 2 The modified melamine sponge is placed on the water surface to simulate sunlight. The modified melamine sponge floats on the water surface and quickly absorbs the heavy oil on the water surface. This is because the super hydrophobicity of the modified melamine sponge enables it to float on the water surface, and it does not absorb water while absorbing oil. Under simulated sunlight, the modified melamine sponge transfers the absorbed heat to the bottom, heats the heavy oil on the water surface, reduces the viscosity of the heavy oil, and accelerates the absorption rate of the heavy oil.
[0096] Fig.17 This is the process of absorbing heavy oil on water by the modified melamine sponge prepared in Example 1. In the absence of light, the modified melamine sponge can hardly absorb the heavy oil on water. Regardless of light or not, the unmodified original melamine sponge cannot absorb the heavy oil quickly, and sinks to the bottom of the water quickly due to its lack of super hydrophobicity and becomes saturated with water.
[0097] In summary, using the method provided by the present invention, the water contact angle of the modified melamine sponge prepared in Example 1 is 153.2±0.6°, which is a superhydrophobic state; at 1.0 kW / m 2 Under simulated sunlight, the surface temperature of the modified melamine sponge can reach 76.2℃ within 1 minute, showing efficient photothermal conversion performance. Therefore, the modified melamine sponge can quickly heat up the heavy oil under light, increase the fluidity of the heavy oil, and thus improve the oil absorption efficiency; the oil absorption capacity of the modified melamine sponge for heavy oil and extra heavy oil with a viscosity of 3671~44204mPa·s can reach 114~126 times of its own weight. After 10 cycles of oil absorption, the absorption capacity still remains at more than 100 times of its own weight. The modified melamine sponge shows excellent absorption performance and cycle performance in absorbing heavy oil and extra heavy oil.
[0098] It can be seen from the above examples and comparative examples that the modified melamine sponge provided by the present invention has excellent performance in selectively absorbing heavy oil.
[0099] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A modified melamine sponge, characterized in that: The invention comprises a melamine sponge and carbon black, polydopamine and octadecylamine loaded on the melamine sponge.
2. The method for preparing the modified melamine sponge according to claim 1, characterized in that: The following steps are involved: (1) immersing the melamine sponge in a carbon black dispersion to load the melamine sponge once, thereby obtaining a melamine sponge loaded with carbon black; (2) immersing the carbon black loaded melamine sponge obtained in step (1) in a tris(hydroxymethyl)aminomethane buffer solution containing dopamine hydrochloride to perform in-situ polymerization to obtain a melamine sponge loaded with carbon black and polydopamine; (3) Immersing the melamine sponge loaded with carbon black and polydopamine obtained in step (2) in an organic solution of octadecylamine for secondary loading to obtain a modified melamine sponge.
3. The preparation method according to claim 2, characterized in that: In the step (1), the particle size of the carbon black is 20-30 nm, and the specific surface area of the carbon black is 150-190 m 2 / g, the volatile content of carbon black is 7~8%.
4. The preparation method according to claim 2, characterized in that: The concentration of the carbon black dispersion in step (1) is 1.5-2.5 g / L.
5. The preparation method according to claim 2, characterized in that: The time for one load in step (1) is 15 to 30 minutes.
6. The preparation method according to claim 2, characterized in that: The concentration of dopamine hydrochloride in the tris(hydroxymethylaminomethane) buffer solution containing dopamine hydrochloride in step (2) is 1.5-2.5 g / L.
7. The preparation method according to claim 2, characterized in that: The time of the in-situ polymerization in step (2) is 16 to 24 hours.
8. The preparation method according to claim 2, characterized in that: The concentration of the organic solution of octadecylamine in step (3) is 3.0-4.5 wt %.
9. The preparation method according to claim 2, characterized in that: The time of the secondary load in step (3) is 25 to 40 minutes.
10. Use of the modified melamine sponge according to claim 1 or the modified melamine sponge prepared by the preparation method according to any one of claims 2 to 9 in absorbing heavy oil.
Citation Information
Patent Citations
Polydopamine modified melamine sponge oil-water separation material and preparation method and application thereof
CN108940231A
Hydrophilic modified melamine sponge as well as preparation method and application thereof
CN115584053A
Preparation method and application of charcoal-loaded melamine sponge
CN118387961A
Equipment for Manufacturing Reagent Containers of Various Sizes
KR102148700B1
Carbon black dispersion and use thereof
WO2014132809A1