Antistatic plastic master batch and preparation method thereof
By using quaternary ammonium structure additives to form chemical bonds with polyethylene and fillers in antistatic plastic masterbatches, a hybrid crosslinking network structure is constructed, and the existing antistatic instability problem is solved and the plastic masterbatches are realized. Stable and improved antistatic, antibacterial and weathering properties.
Patent Information
- Application Number
- CN202411245053.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The antistatic properties of existing internally added antistatic plastic masterbatches are unstable and gradually decrease with the use time, and the plastic is prone to static hazards.
Using additives containing quaternary ammonium salt structures, a hybrid crosslinking network structure is constructed by forming chemical bonds with polyethylene and fillers, which improves the dispersion and stability of fillers, and adsorbs the positive ions of quaternary ammonium salts to bacterial cell walls. and neutralize the charge on the plastic surface to achieve antibacterial and antistatic effects.
It improves the antistatic, antibacterial, wear resistance and weather resistance of plastic masterbatches, and has more stable and excellent performance, avoiding static hazards and bacterial contamination.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to an antistatic plastic masterbatch and a preparation method thereof. Background Art
[0002] Plastics have excellent performance, but they do not have mildew-proof and antibacterial properties, so their application areas are limited. In addition, plastics themselves have large volume resistance and are very likely to produce static electricity hazards, such as distortion of precision instruments, scrapping of electronic components, fires and explosions, etc.
[0003] At present, in order to prepare antistatic plastics, antistatic agents are added to plastic masterbatches. Antistatic agents can be divided into anionic, cationic, nonionic, zwitterionic and polymer types according to their structure. According to the method of use, there are two major categories: external coating type and internal addition type. External coating antistatic agents use solvents and require additional external coating processes, which not only makes the process complicated, but also has a short service life. Therefore, more and more people tend to use internal addition antistatic agents. However, the antistatic properties of internal addition antistatic plastic masterbatches in the prior art are unstable and will gradually decrease with the extension of service time. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the prior art and provide an antistatic plastic masterbatch and a preparation method thereof.
[0005] The purpose of the present invention can be achieved through the following technical solutions: An antistatic plastic masterbatch comprises the following raw materials in parts by weight: 100 parts of polyethylene, 20-30 parts of fillers, 4-9 parts of additives, 0.8-1.5 parts of light stabilizers, 0.8-1.5 parts of antioxidants, 0.5-1 parts of lubricants, and 0.02-0.05 parts of initiators.
[0006] Furthermore, the filler is one or more of acetylene black, carbon nanotubes, graphene, nano calcium carbonate, silicon powder, silicon dioxide, nano titanium dioxide, aluminum hydroxide, and magnesium hydroxide.
[0007] Furthermore, the filler is a mixture of acetylene black, silicon powder, nano titanium dioxide and magnesium hydroxide in a mass ratio of (0.3-0.5):2:2:(1-3).
[0008] Furthermore, the auxiliary agent is prepared by the following steps: S1. Replace the air in a dry three-necked flask with nitrogen, then add N,N-dimethyl-1,3-diaminopropane, epoxybutene and benzene in sequence, stir thoroughly, heat to 65°C, keep warm for 6 hours, perform vacuum distillation after the reaction, purify by column chromatography (a mixed solvent of benzene and methanol is selected as the eluent, and the volume ratio of benzene to methanol is 9:1), and perform vacuum distillation to obtain intermediate 1; the dosage ratio of N,N-dimethyl-1,3-diaminopropane, epoxybutene and benzene is 14.5mL:8.1mL:100mL; The molar ratio of N,N-dimethyl-1,3-diaminopropane to epoxybutene is controlled to be 1.1-1.2:1. 2 The epoxy group of epoxybutene undergoes an addition reaction under heating conditions. The reaction process is as follows:
[0009] S2. Under nitrogen protection, add intermediate 1, 4-chloro-1-butene and chloroform into a dry three-necked flask, mix well, then slowly add triethylamine, then stir and heat to 75°C for 2h, distill under reduced pressure after the reaction, purify by column chromatography (a mixed solvent of chloroform and methanol is selected as the eluent, and the volume ratio of chloroform to methanol is 99:1), and distill under reduced pressure to obtain intermediate 2; the amount ratio of intermediate 1, 4-chloro-1-butene, triethylamine and chloroform is 13.8g:8.7mL:16.7mL:100mL; The molar ratio of intermediate 1 and 4-chloro-1-butene is controlled to be 1:1.05-1.1. Under heating, -NH- of intermediate 1 and -Cl of 4-chloro-1-butene undergo substitution reaction. Triethylamine is used as an acid binding agent. The reaction process is as follows:
[0010] S3, nitrogen was blown into a dry three-necked flask for 30 minutes to remove the air and moisture in the flask, and then intermediate 2, tetradecane chloride and DMSO (dimethyl sulfoxide) were added, and pyridine was slowly added after stirring to dissolve, and then the temperature was raised to 80°C, and the reaction was kept warm for 3 hours. After the reaction was completed, vacuum distillation was performed, column chromatography was used for purification (a mixed solvent of benzene and ether was selected as the eluent, and the volume ratio of benzene and ether was 6:4), and vacuum distillation was performed to obtain intermediate 3; the usage ratio of intermediate 2, tetradecane chloride, pyridine and DMSO was 17.2g:44.2mL:15.4mL:120mL; The molar ratio of intermediate 2 to tetradecane chloride is controlled to be 1:2.1-2.2. Under heating, the tertiary amine group of intermediate 2 and the -Cl of tetradecane chloride undergo substitution reaction. Pyridine is used as an acid binding agent. The reaction process is as follows:
[0011] S4. Blow nitrogen gas into a dry three-necked flask for 30 minutes to exclude air and moisture, then add intermediate 3, bis[3-(triethoxysilyl)propyl]amine, DMSO and tetraisopropyl titanate in sequence, stir thoroughly, heat to 90°C and react for 24 hours. After the reaction, cool to room temperature, distill under reduced pressure, wash with anhydrous ethanol three times, and dry at 80°C for 12 hours. The whole process is carried out under nitrogen protection to obtain an auxiliary agent; the dosage ratio of intermediate 3, bis[3-(triethoxysilyl)propyl]amine, tetraisopropyl titanate and DMSO is 41.5g:28.6mL:0.056g:180mL.
[0012] The molar ratio of intermediate 3 and bis[3-(triethoxysilyl)propyl]amine is controlled to be 1:1.05-1.1, and the hydroxyl group of intermediate 3 and the silaneoxy group of bis[3-(triethoxysilyl)propyl]amine undergo the following chemical reaction under the catalysis of tetraisopropyl titanate. The reaction process is shown below:
[0013] The additive contains multiple quaternary ammonium salt structures, and the alkyl chain of the quaternary ammonium salt contains 14 carbon atoms. The quaternary ammonium salt structure dissociates into a positively charged quaternary ammonium salt cation—N + Ions can be adsorbed onto the cell wall of negatively charged bacteria, thereby destroying the bacterial cell membrane and denaturing its protein, hindering the replication and reproduction of DNA, etc., thereby achieving an antibacterial effect. At the same time, when the carbon number of the alkyl chain of the quaternary ammonium salt structure is 12 to 16, the antibacterial effect is better, especially when it is 14, the antibacterial effect is the best; in addition, the quaternary ammonium salt structure has positive ions, which can neutralize the charge on the surface of the plastic masterbatch to form a thin charge layer to play a role, so that the charge can be easily removed, thereby giving the plastic masterbatch antistatic properties; in addition, the quaternary ammonium salt structure can not only reduce the surface charge, but also prevent dust and oil stains. Therefore, the auxiliary agent of the present invention not only has excellent antibacterial effect, but also has good antistatic effect and antifouling properties.
[0014] The additive contains abundant silaneoxy groups, which can form chemical bonds with the hydroxyl groups on the surface of the filler, thereby greatly reducing the surface energy of the filler and increasing the interface compatibility between the filler and polyethylene. The oil-soluble long carbon chain in the additive can further promote the interface compatibility between the filler and other organic raw materials, so that the filler of the present invention can be highly dispersed in the plastic masterbatch, fully exert its effect, and give the plastic masterbatch excellent antistatic properties, wear resistance and weather resistance. This chemical bonding can also promote the dispersion and stability of the additive, and the carbon-carbon double bond at the end of the additive can produce a chemical reaction with the unreacted carbon-carbon double bond at the end of the polyethylene under the action of the initiator. Therefore, the additive of the present invention can be highly dispersed and stabilized in the plastic masterbatch, and a cross-linked hybrid network structure is also formed between the polyethylene, the additive and the filler. This network structure enables each raw material to exert a long-term effect, and the antistatic properties, antibacterial properties, wear resistance and weather resistance of the plastic masterbatch are also more stable and more excellent.
[0015] Furthermore, the light stabilizer is one or more of the light stabilizer AM-101, the light stabilizer GW-622, the ultraviolet absorber UV-531, and the ultraviolet absorber UV-9.
[0016] Furthermore, the antioxidant is one or more of antioxidant 1010, antioxidant 168, antioxidant 1035, antioxidant DLTP, and antioxidant 1076.
[0017] Furthermore, the lubricant is one or more of stearic acid, zinc stearate, calcium stearate, and magnesium stearate.
[0018] Furthermore, the initiator is one or more of dicumyl peroxide, dibenzoyl peroxide, and azobisisobutyronitrile.
[0019] A method for preparing an antistatic plastic masterbatch comprises the following steps: The raw materials are weighed by weight and mixed evenly, then added to a high-speed kneader for kneading and crushing, and then extruded and granulated by a twin-screw extruder to prepare an antistatic plastic masterbatch.
[0020] The beneficial effects of the present invention are as follows: the additive of the present invention contains a quaternary ammonium salt structure with a long carbon chain (14 carbons), and there are chemical reactions between polyethylene and the additive, and between the additive and the filler. Therefore, a hybrid cross-linked network structure is formed between polyethylene, the additive and the filler. Therefore, the filler and the additive can be highly dispersed and stably present in the plastic masterbatch, and can fully play their roles. In addition, due to the synergistic effect of other raw materials, the plastic masterbatch of the present invention has excellent and stable antistatic, antibacterial, weather resistance, wear resistance and other properties. DETAILED DESCRIPTION
[0021] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example
[0022] Preparation of auxiliary agent, the specific steps are as follows: S1. Replace the air in a 250 mL dry three-necked flask with nitrogen, then add 14.5 mL of N,N-dimethyl-1,3-diaminopropane, 8.1 mL of epoxybutene and 100 mL of benzene in sequence, stir thoroughly, heat to 65°C, and keep warm for 6 hours. After the reaction is completed, perform vacuum distillation, column chromatography purification (a mixed solvent of benzene and methanol is selected as the eluent, and the volume ratio of benzene and methanol is 9:1), and vacuum distillation to obtain intermediate 1; S2, under nitrogen protection, add 13.8 g of intermediate 1, 8.7 mL of 4-chloro-1-butene and 100 mL of chloroform into a 250 mL dry three-necked flask, mix well, then slowly add 16.7 mL of triethylamine, then stir and heat to 75 ° C for 2 h, after the reaction is completed, distill under reduced pressure, purify by column chromatography (the eluent is a mixed solvent of chloroform and methanol, the volume ratio of chloroform to methanol is 99:1), and distill under reduced pressure to obtain intermediate 2; S3, nitrogen was blown into a 500 mL dry three-necked flask for 30 min to remove air and moisture in the flask, then 17.2 g of intermediate 2, 44.2 mL of tetradecane chloride and 120 mL of DMSO were added, and 15.4 mL of pyridine was slowly added after stirring to dissolve, and then the temperature was raised to 80°C, and the reaction was kept warm for 3 h. After the reaction was completed, vacuum distillation was performed, column chromatography was performed for purification (a mixed solvent of benzene and ether was selected as the eluent, and the volume ratio of benzene and ether was 6:4), and vacuum distillation was performed to obtain intermediate 3; S4. Blow nitrogen gas into a 500mL dry three-necked flask for 30 minutes to exclude air and moisture, and then add 41.5g of intermediate 3, 28.6mL of bis[3-(triethoxysilyl)propyl]amine, 180mL of DMSO and 0.056g of tetraisopropyl titanate in sequence. After sufficient stirring, heat to 90°C and keep warm for reaction for 24 hours. After the reaction is completed, cool to room temperature, distill under reduced pressure, wash with anhydrous ethanol for 3 times, and dry at 80°C for 12 hours. The whole process is carried out under nitrogen protection to obtain an auxiliary agent. Example
[0023] Preparation of auxiliary agent, the specific steps are as follows: The remaining steps remain unchanged, and only step S4 of Example 1 is removed to prepare the auxiliary agent. Example
[0024] To prepare antistatic plastic masterbatch, the specific steps are as follows: 100 parts of polyethylene, 3 parts of carbon nanotubes, 7.5 parts of nano-calcium carbonate, 2 parts of silicon dioxide, 7.5 parts of aluminum hydroxide, 4 parts of the additive prepared in Example 1, 0.8 parts of ultraviolet absorber UV-531, 0.5 parts of antioxidant 1076, 0.3 parts of antioxidant DLTP, 0.5 parts of stearic acid, and 0.02 parts of azobisisobutyronitrile were weighed by weight and mixed evenly, then added to a high-speed kneader, kneaded and crushed, and then extruded and granulated through a twin-screw extruder to prepare an antistatic plastic masterbatch. Example
[0025] To prepare antistatic plastic masterbatch, the specific steps are as follows: 100 parts of polyethylene, 1.2 parts of acetylene black, 7.5 parts of silicon powder, 7.5 parts of nano titanium dioxide, 3.8 parts of magnesium hydroxide, 4 parts of the additive prepared in Example 1, 0.8 parts of ultraviolet absorber UV-531, 0.5 parts of antioxidant 1076, 0.3 parts of antioxidant DLTP, 0.5 parts of stearic acid, and 0.02 parts of azobisisobutyronitrile were weighed by weight and mixed evenly, then added to a high-speed kneader, kneaded and crushed, and then extruded and granulated through a twin-screw extruder to prepare an antistatic plastic masterbatch. Example
[0026] To prepare antistatic plastic masterbatch, the specific steps are as follows: 100 parts of polyethylene, 1.5 parts of acetylene black, 7.5 parts of silicon powder, 7.5 parts of nano titanium dioxide, 7.5 parts of magnesium hydroxide, 8 parts of the additive prepared in Example 1, 0.4 parts of light stabilizer GW-622, 0.8 parts of ultraviolet absorber UV-9, 1.2 parts of antioxidant 1035, 0.9 parts of zinc stearate, and 0.04 parts of diisopropylbenzene peroxide were weighed and mixed uniformly, then added to a high-speed kneader, kneaded and crushed, and then extruded and granulated through a twin-screw extruder to prepare an antistatic plastic masterbatch. Example
[0027] To prepare antistatic plastic masterbatch, the specific steps are as follows: 100 parts of polyethylene, 2 parts of acetylene black, 8 parts of silicon powder, 8 parts of nano titanium dioxide, 12 parts of magnesium hydroxide, 9 parts of the additive prepared in Example 1, 0.5 parts of light stabilizer AM-101, 1 part of ultraviolet absorber UV-531, 1 part of antioxidant 1010, 0.5 parts of antioxidant 168, 1 part of magnesium stearate, and 0.05 parts of dibenzoyl peroxide were weighed by weight and mixed evenly, then added to a high-speed kneader, kneaded and crushed, and then extruded and granulated through a twin-screw extruder to prepare an antistatic plastic masterbatch.
[0028] Comparative Example 1 To prepare plastic masterbatch, the specific steps are as follows: The remaining steps remain unchanged, only the auxiliary agent in Example 6 is replaced by the auxiliary agent prepared in Example 2 to prepare the plastic masterbatch.
[0029] Comparative Example 2 To prepare plastic masterbatch, the specific steps are as follows: The remaining steps remain unchanged, only the auxiliary agent in Example 6 is replaced by 6 parts of the auxiliary agent prepared in Example 2 and 3 parts of 3-aminopropyltrimethoxysilane to prepare a plastic masterbatch.
[0030] Comparative Example 3 To prepare plastic masterbatch, the specific steps are as follows: The remaining steps remain unchanged, only the additives in Example 6 are removed to prepare the plastic masterbatch.
[0031] Performance Testing The plastic masterbatches of Examples 3-6 and Comparative Examples 1-3 were made into films, and corresponding samples were prepared according to different standards. The antibacterial and antistatic properties were tested. The test results are shown in Table 1 below: Table 1
[0032] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0033] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. An antistatic plastic masterbatch, characterized in that: The invention comprises the following raw materials in parts by weight: 100 parts of polyethylene, 20-30 parts of fillers, 4-9 parts of additives, 0.8-1.5 parts of light stabilizers, 0.8-1.5 parts of antioxidants, 0.5-1 parts of lubricants, and 0.02-0.05 parts of initiators; Wherein, the auxiliary agent is prepared by the following steps: S1. Replace the air in the flask with nitrogen, add N,N-dimethyl-1,3-diaminopropane, epoxybutene and benzene, stir, react at 65°C for 6h, distill under reduced pressure, purify by column chromatography, and distill under reduced pressure to obtain intermediate 1; S2, under nitrogen protection, add intermediate 1, 4-chloro-1-butene and chloroform into a flask, add triethylamine after mixing, react at 75°C for 2h, distill under reduced pressure, purify by column chromatography, and distill under reduced pressure to obtain intermediate 2; S3, after nitrogen blowing into the flask, add intermediate 2, tetradecane chloride and DMSO, stir, add pyridine, react at 80°C for 3h, distill under reduced pressure, purify by column chromatography, and distill under reduced pressure to obtain intermediate 3; S4. Purge the flask with nitrogen, add intermediate 3, bis[3-(triethoxysilyl)propyl]amine, DMSO and tetraisopropyl titanate, stir, react at 90°C for 24h, cool, distill under reduced pressure, wash and dry to obtain an auxiliary agent.
2. The antistatic plastic masterbatch according to claim 1, characterized in that: The amount ratio of N,N-dimethyl-1,3-diaminopropane, epoxybutene and benzene in step S1 is 14.5mL:8.1mL:100mL; the amount ratio of intermediate 1, 4-chloro-1-butene, triethylamine and chloroform in step S2 is 13.8g:8.7mL:16.7mL:100mL; the amount ratio of intermediate 2, tetradecane chloride, pyridine and DMSO in step S3 is 17.2g:44.2mL:15.4mL:120mL; the amount ratio of intermediate 3, bis[3-(triethoxysilyl)propyl]amine, tetraisopropyl titanate and DMSO in step S4 is 41.5g:28.6mL:0.056g:180mL.
3. The antistatic plastic masterbatch according to claim 1, characterized in that: The filler is one or more of acetylene black, carbon nanotubes, graphene, nano calcium carbonate, silicon powder, silicon dioxide, nano titanium dioxide, aluminum hydroxide, and magnesium hydroxide.
4. The antistatic plastic masterbatch according to claim 3, characterized in that: The filler is a mixture of acetylene black, silicon powder, nano titanium dioxide and magnesium hydroxide in a mass ratio of (0.3-0.5):2:2:(1-3).
5. The antistatic plastic masterbatch according to claim 1, characterized in that: The light stabilizer is one or more of the light stabilizer AM-101, the light stabilizer GW-622, the ultraviolet absorber UV-531, and the ultraviolet absorber UV-9.
6. The antistatic plastic masterbatch according to claim 1, characterized in that: The antioxidant is one or more of antioxidant 1010, antioxidant 168, antioxidant 1035, antioxidant DLTP, and antioxidant 1076.
7. The antistatic plastic masterbatch according to claim 1, characterized in that: The lubricant is one or more of stearic acid, zinc stearate, calcium stearate and magnesium stearate.
8. The antistatic plastic masterbatch according to claim 1, characterized in that: The initiator is one or more of dicumyl peroxide, dibenzoyl peroxide and azobisisobutyronitrile.
9. The method for preparing an antistatic plastic masterbatch according to claim 1, characterized in that: The following steps are involved: The raw materials are weighed by weight and mixed evenly, then added to a high-speed kneader for kneading and crushing, and then extruded and granulated by a twin-screw extruder to prepare an antistatic plastic masterbatch.
Citation Information
Cited By
Anti-fog head-up display film for automobile and preparation method of anti-fog head-up display film