Determination method of phosphorus pentoxide and special equipment thereof

The dedicated device for determining phosphorus pentoxide automates solvent addition and stirring, addressing the complexity of existing methods and enabling efficient simultaneous measurement of different sample types.

CN119086806APending Publication Date: 2024-12-06CENT LAB OF YUNNAN GEOLOGICAL & MINERAL EXPLORATION & DEV BUREAU (KUNMING MINERAL RESOURCES SUPERVISION & TESTING CENT MINISTRY OF LAND & RESOURCES)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411270424.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing methods for determining phosphorus pentoxide in phosphate rock samples are cumbersome and complicated, and cannot measure soluble ore and manganese-containing samples simultaneously.

Method used

A method involving the use of a dedicated device with a sample carrier and piston extrusion system to automate the addition of solvents and stirring, allowing for simultaneous measurement of different types of samples by sliding and rotating the carrier to the appropriate beaker, and synchronously injecting solvents and stirring the samples.

Benefits of technology

Accelerates the measurement process by automating solvent addition and stirring, enabling efficient and simultaneous determination of phosphorus pentoxide in various types of samples.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119086806A_ABST
    Figure CN119086806A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of phosphorus pentoxide determination, and discloses a phosphorus pentoxide determination method and special equipment thereof. Comprising a soluble ore sample beaker, a connecting plate is fixedly connected to the soluble ore sample beaker, a manganese-containing sample beaker is fixedly connected to the side, away from the soluble ore sample beaker, of the connecting plate, a beaker cover is installed on the manganese-containing sample beaker, and a low-temperature electric heating plate is installed on the lower side of the soluble ore sample beaker; through cooperation of structures such as the sample carrying disc and the piston extrusion plates, the sample carrying disc drives a sample to slide downwards and then rotate, the sample is conveyed into a corresponding easily-soluble ore sample beaker or a manganese-containing sample beaker along the feeding sliding frame, and meanwhile, a cam extrusion block is driven to extrude the corresponding piston extrusion plate; solvent in the first solvent piston or the second solvent piston is injected into the corresponding easily-soluble ore sample beaker or the manganese-containing sample beaker, the effect of accelerating the measuring process is achieved, and the solvent and water are quantitatively injected through the design of the pistons.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of determination of phosphorus pentoxide, in particular to a determination method of phosphorus pentoxide and special equipment thereof. Background Art

[0002] The method for determining phosphorus pentoxide in phosphate rock samples is to first prepare the corresponding chemical solvent and crush the phosphate rock sample into specified particles. Then, double blank tests are performed throughout the analysis process. One to three samples of primary standard phosphate rock are selected and analyzed simultaneously. The determination steps are divided into acid-soluble decomposition samples and alkali-soluble decomposition samples. The acid-soluble decomposition samples are different for different types of phosphate rock samples. The determination steps for soluble ore samples and manganese-containing samples are also different.

[0003] Existing measuring devices are mostly manual, weighing the sample, adding it to a beaker, then adding the corresponding amount of solvent, heating it, and evaporating it. The steps are cumbersome and the operation is complicated. At the same time, soluble ore samples and manganese-containing samples cannot be measured at the same time. Summary of the invention

[0004] In order to solve the problem that the determination method of phosphorus pentoxide in phosphate ore proposed in the above background technology has cumbersome steps and complicated operations, the present invention provides a determination method of phosphorus pentoxide and a dedicated device thereof.

[0005] To achieve the above object, the present invention provides the following technical solution: a method for determining phosphorus pentoxide, comprising the following steps: S1. Use nitric acid to dissolve the soluble ore sample. Weigh 0.1-0.2g of phosphate rock sample and add it to the sample carrier. Then slide the sample carrier downward, rotate the sample carrier to place the sample in the manganese sample beaker through the feed slide, and at the same time, the cam extrusion block squeezes the piston extrusion plate so that the 20ml water in the first solvent piston wets the sample. At the same time, add 15-20ml nitric acid to the sample in the first solvent piston, cover the beaker, place it on the hot plate and heat it to 600℃, dissolve the phosphate rock sample by rotating the stirring block, remove the beaker cover, evaporate for 15 minutes until it is almost dry, add 2ml nitric acid and 20ml water to the soluble ore sample beaker or the manganese sample beaker, heat to 620℃ to dissolve the soluble salt, and make up to volume; S2. The manganese-containing sample is dissolved by hydrochloric acid and nitric acid. 0.1-0.2g of phosphate rock sample is weighed and placed in the sample carrier. Then the sample carrier is slid downward, and the sample carrier is rotated to place the sample in the soluble ore sample beaker through the feed slide. While rotating the sample carrier in the opposite direction, the piston extrusion plate in the second solvent piston is squeezed to make the water in the second solvent piston wet the sample. At the same time, the second solvent piston adds 10mL of hydrochloric acid to the soluble ore sample beaker, and heats to 600℃ on a low-temperature electric hot plate. Evaporate for 15 minutes until it is nearly dry. Slide the sample carrier downward again, rotate the sample carrier to squeeze the piston extrusion plate on the third solvent piston, add 5mL of nitric acid along the cup wall, and blow the cup wall with 10ml of water. Evaporate for 5 minutes until it is nearly dry. Add 2mL of nitric acid and 20mL of water to the soluble ore sample beaker or the manganese-containing sample beaker, heat to 620℃ to dissolve the soluble salt, and fix the volume. S3. Weigh 0.2~0.5g of a sample with high iron content, place it in a porcelain crucible with 8g of mixed flux added in advance, stir well, cover it with a layer of flux, place it in a high-temperature furnace and heat it to 750℃ and keep it for 45min, take it out, cool it, transfer the semi-melted material into a 150mL beaker, wash the crucible with water and dilute it to 50mL, boil it for several minutes, crush the frit, if there is high-valent manganese color, add a little sodium peroxide and boil it to reduce, after cooling, dilute it to a 100mL volumetric flask with water, take 25mL of the clear solution and place it in a 100mL volumetric flask, add a drop of phenolphthalein indicator, neutralize it with nitric acid until the red color disappears and the excess is 3.0mL; S4. Weigh 0.2~0.5g of semi-melted and incompletely decomposed high-iron sample or some silicate stone sample, place it in a corundum crucible, add 5g of sodium peroxide, stir well, cover with another layer, place it in a 700℃ high-temperature furnace to melt for 10min, take out the crucible, cool it, place it in a 250mL beaker, add 50~60mL of hot water to soak it, wash out the crucible with water, boil it on a hot plate for several minutes, transfer it to a 100mL volumetric flask after cooling, dilute it to the scale with water, shake well, take 25mL of the clear liquid and place it in a 100mL volumetric flask, add a drop of phenolphthalein indicator, neutralize it with nitric acid until the red color disappears and the excess is 3.0mL; S5. Take 0, 0.5, 1, 2, 4, 7, and 10 mL of phosphorus pentoxide standard solution and put them into 100 mL volumetric flasks respectively, add 2.5 mL of nitric acid, dilute to about 30 mL with water, add 10 mL of ammonium vanadium molybdate color developer, shake well, make up to volume with water, let it stand for 30 minutes, and measure the absorbance at a wavelength of 420-470 nm on a spectrophotometer with the reagent blank as a reference. Draw a calibration curve, select 1-3 phosphate rock standard substances, and prepare the corresponding solutions according to steps S1 to S4, and measure the absorbance at a wavelength of 420 nm with the reagent blank as a reference.

[0006] Special equipment for determining phosphorus pentoxide, comprising a soluble ore sample beaker, a connecting plate fixedly connected to the soluble ore sample beaker, a manganese-containing sample beaker fixedly connected to the side of the connecting plate away from the soluble ore sample beaker, a beaker cover installed on the manganese-containing sample beaker, a low-temperature electric heating plate installed on the lower side of the soluble ore sample beaker, and an electric heating plate installed on the lower side of the manganese-containing sample beaker; Among them, a symmetrically distributed sliding bracket is fixedly connected to the connecting plate, a sample carrier is slidably connected to the sliding bracket, a feed slide is fixedly connected to the sliding bracket at the lower side of the sample carrier, a spring extrusion block is slidably connected inside the sliding bracket, a first return spring is arranged between the spring extrusion block and the sliding bracket, and a rotating slider is fixedly connected to the end of the sample carrier away from the cam extrusion block.

[0007] Preferably, the sliding bracket is provided with a sliding groove for the sample carrier and the spring extrusion block to slide, and a through hole for the sample carrier to rotate is provided under the sliding groove of the sliding bracket, and the sliding portion of the sample carrier in the sliding bracket is rectangular.

[0008] Preferably, the size of the sample carrier's loading tray is the same as the spacing of the sliding bracket, the slide size of the feed slide is the same as the size of the sample carrier's loading tray, and the inclination angle of the sample carrier's slide is the same as the inclination angle after the sample carrier's loading tray is rotated ninety degrees.

[0009] Preferably, a first solvent bracket is fixedly connected to the connecting plate, a first solvent piston is mounted on the first solvent bracket, and a piston extrusion plate is slidably connected inside the first solvent piston.

[0010] Preferably, a second solvent bracket is fixedly connected to the connecting plate, a second solvent piston and a third solvent piston are mounted on the second solvent bracket, and a piston extrusion plate is slidably connected to the second solvent piston and the third solvent piston.

[0011] Preferably, the upper piston tube of the second solvent piston is filled with hydrochloric acid, the lower piston tube of the second solvent piston is filled with water, the upper piston tube of the third solvent piston is filled with nitric acid, the lower piston tube of the third solvent piston is filled with water, the upper piston tube of the first solvent piston is filled with nitric acid, and the lower piston tube of the first solvent piston is filled with water.

[0012] Preferably, a sliding piston is slidably connected in the water-filled piston tubes of the first solvent piston, the second solvent piston and the third solvent piston, an extrusion spring is arranged between the sliding piston and the piston extrusion plate, a limiting spring is arranged between the sliding piston and the first solvent piston, the second solvent piston or the third solvent piston respectively, a connecting tube is arranged between the first solvent piston and the manganese-containing sample beaker, and a connecting tube is arranged between the second solvent piston and the third solvent piston and the soluble ore sample beaker.

[0013] Preferably, the sliding bracket is rotatably connected to a rotating block on one side away from the first solvent bracket, the rotating block is provided with a slide groove adapted to the rotating slider, the beaker cover is rotatably connected to a rotating cover plate, and a transmission belt is wound between the rotating cover plate and the rotating block.

[0014] Preferably, a threaded shaft is fixedly connected inside the manganese-containing sample beaker, an upper threaded extrusion piece is threadedly connected to the threaded shaft, a lower sliding piece is slidably connected to the upper threaded extrusion piece, a stirring block is fixedly connected to the lower side of the lower sliding piece, a second return spring is arranged between the upper threaded extrusion piece and the lower sliding piece, an extrusion protrusion is fixedly connected to the rotating cover plate, and the extrusion protrusion is extruded and matched with the upper threaded extrusion piece.

[0015] Compared with the prior art, the present invention has the following beneficial effects: The present invention cooperates with structures such as a sample carrier and a piston extrusion plate, and slides the sample downward with the sample carrier, and then rotates to transport the sample along the feed slide to the corresponding soluble ore sample beaker or manganese-containing sample beaker, and at the same time drives the cam extrusion block to squeeze the corresponding piston extrusion plate, and injects the solvent in the first solvent piston or the second solvent piston into the corresponding soluble ore sample beaker or manganese-containing sample beaker, so as to achieve the effect of accelerating the measurement process, and quantitatively inject the solvent and water through the piston design; The present invention arranges the cooperation of structures such as a sample carrier and a rotating cover plate, and the rotation of the sample carrier drives the rotating slider to rotate, which in turn drives the rotating block to rotate synchronously, and then drives the rotating cover plate to rotate through a transmission belt, so that the rotating cover plate and the beaker cover are in an open state, and at the same time, the upper threaded extrusion sheet is squeezed to make the stirring block rotate and stir, so that the sample carrier rotates to add materials and stirs at the same time, and the sample carrier rotates and stirs at the same time, so as to achieve the effect of synchronous stirring, thereby accelerating the measurement process. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a schematic diagram of the structure of the present invention; Figure 2 This is a schematic diagram of the feeding structure of the present invention; Figure 3 This is an exploded view of the charging structure of the present invention; Figure 4 This is a schematic diagram of solvent addition in the present invention; Figure 5 A half-section schematic diagram of a solvent piston of the present invention; Figure 6 This is a schematic diagram of the stirring connection structure of the present invention; Figure 7 This is a schematic diagram of the stirring structure of the present invention; Figure 8 This is an exploded view of the stirring structure of the present invention.

[0017] In the figure: 100, soluble ore sample beaker; 101, manganese sample beaker; 102, connecting plate; 103, beaker cover; 200, electric heating plate; 201, low temperature electric heating plate; 300, sliding bracket; 301, sample carrier; 302, feed slide; 303, cam extrusion block; 304, spring extrusion block; 305, first return spring; 306, rotating slide; 400, first solvent bracket; 401, second solvent bracket; 40 2. First solvent piston; 403. Second solvent piston; 404. Third solvent piston; 405. Piston extrusion plate; 406. Extrusion spring; 407. Sliding piston; 408. Limiting spring; 500. Rotating block; 501. Rotating cover plate; 502. Driving belt; 503. Extrusion convex block; 504. Threaded shaft; 505. Upper threaded extrusion sheet; 506. Lower sliding sheet; 507. Second return spring; 508. Stirring block. DETAILED DESCRIPTION

[0018] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] like Figures 1 to 8 As shown, the present invention provides a method for determining phosphorus pentoxide, comprising the following steps: S1. The soluble ore sample is dissolved by nitric acid. 0.1-0.2 g of phosphate rock sample is weighed and added to the sample carrier 301. Then the sample carrier 301 is slid downward, and the sample carrier 301 is rotated to place the sample in the manganese sample beaker 101 through the feed slide 302. At the same time, the cam extrusion block 303 squeezes the piston extrusion plate 405 so that the 20 ml water in the first solvent piston 402 wets the sample. At the same time, 15-20 ml of nitric acid is added to the sample in the first solvent piston 402. The beaker cover 103 is covered, and the sample is placed on the electric heating plate 200 and heated to 600° C. The phosphate rock sample is dissolved by rotating the stirring block 508. The beaker cover 103 is removed, and the sample is evaporated for 15 minutes until it is nearly dry. 2 ml of nitric acid and 20 ml of water are added to the soluble ore sample beaker 100 or the manganese sample beaker 101, and the sample is heated to 620° C. to dissolve the soluble salt, and the volume is constant. S2. The manganese-containing sample is dissolved by using hydrochloric acid and nitric acid. 0.1-0.2 g of phosphate rock sample is weighed and placed in the sample carrier 301. Then, the sample carrier 301 is slid downward, and the sample carrier 301 is rotated to place the sample in the easily soluble ore sample beaker 100 through the feed slide 302. While rotating the sample carrier 301 in the opposite direction, the piston squeezing plate 405 in the second solvent piston 403 is squeezed to make the water in the second solvent piston 403 wet the sample. At the same time, the second solvent piston 403 is pushed into the easily soluble ore sample beaker 100. Add 10mL of hydrochloric acid, heat to 600°C on a low-temperature electric hot plate 201, evaporate for 15 minutes until nearly dry, slide the sample carrier 301 downward again, rotate the sample carrier 301 to squeeze the piston squeezing plate 405 on the third solvent piston 404, add 5mL of nitric acid along the cup wall, and purge the cup wall with 10ml of water, evaporate for 5 minutes until nearly dry, add 2mL of nitric acid and 20mL of water to the soluble ore sample beaker 100 or the manganese-containing sample beaker 101, heat to 620°C to dissolve the soluble salt, and fix the volume; S3. Weigh 0.2~0.5g of a sample with high iron content, place it in a porcelain crucible with 8g of mixed flux added in advance, stir well, cover it with a layer of flux, place it in a high-temperature furnace and heat it to 750℃ and keep it for 45min, take it out, cool it, transfer the semi-melted material into a 150mL beaker, wash the crucible with water and dilute it to 50mL, boil it for several minutes, crush the frit, if there is high-valent manganese color, add a little sodium peroxide and boil it to reduce, after cooling, dilute it to a 100mL volumetric flask with water, take 25mL of the clear solution and place it in a 100mL volumetric flask, add a drop of phenolphthalein indicator, neutralize it with nitric acid until the red color disappears and the excess is 3.0mL; S4. Weigh 0.2~0.5g of semi-melted and incompletely decomposed high-iron sample or some silicate stone sample, place it in a corundum crucible, add 5g of sodium peroxide, stir well, cover with another layer, place it in a 700℃ high-temperature furnace to melt for 10min, take out the crucible, cool it, place it in a 250mL beaker, add 50~60mL of hot water to soak it, wash out the crucible with water, boil it on a hot plate for several minutes, transfer it to a 100mL volumetric flask after cooling, dilute it to the scale with water, shake well, take 25mL of the clear liquid and place it in a 100mL volumetric flask, add a drop of phenolphthalein indicator, neutralize it with nitric acid until the red color disappears and the excess is 3.0mL; S5. Take 0, 0.5, 1, 2, 4, 7, and 10 mL of phosphorus pentoxide standard solution and put them into 100 mL volumetric flasks respectively, add 2.5 mL of nitric acid, dilute to about 30 mL with water, add 10 mL of ammonium vanadium molybdate color developer, shake well, make up to volume with water, let it stand for 30 minutes, and measure the absorbance at a wavelength of 420-470 nm on a spectrophotometer with the reagent blank as a reference. Draw a calibration curve, select 1-3 phosphate rock standard substances, and prepare the corresponding solutions according to steps S1 to S4, and measure the absorbance at a wavelength of 420 nm with the reagent blank as a reference.

[0020] like Figures 1 to 5 As shown, a special device for determining phosphorus pentoxide includes a soluble ore sample beaker, a connecting plate 102 is fixedly connected to the soluble ore sample beaker 100, a manganese-containing sample beaker 101 is fixedly connected to the side of the connecting plate 102 away from the soluble ore sample beaker 100, a beaker cover 103 is installed on the manganese-containing sample beaker 101, a low-temperature electric heating plate 201 is installed on the lower side of the soluble ore sample beaker 100, and an electric heating plate 200 is installed on the lower side of the manganese-containing sample beaker 101; Among them, a symmetrically distributed sliding bracket 300 is fixedly connected to the connecting plate 102, a sample carrier 301 is slidably connected to the sliding bracket 300, a feed slide 302 is fixedly connected to the sliding bracket 300 at the lower side of the sample carrier 301, a spring extrusion block 304 is slidably connected inside the sliding bracket 300, a first reset spring 305 is arranged between the spring extrusion block 304 and the sliding bracket 300, and a rotating slider 306 is fixedly connected to the end of the sample carrier 301 away from the cam extrusion block 303.

[0021] The sliding bracket 300 is provided with a slide groove for the sample carrier 301 and the spring extrusion block 304 to slide. The lower side of the slide groove of the sliding bracket 300 is provided with a through hole for the sample carrier 301 to rotate. The sliding part of the sample carrier 301 in the sliding bracket 300 is rectangular.

[0022] The size of the sample carrier 301 is the same as the spacing of the sliding bracket 300, the slide size of the feed slide 302 is the same as the size of the sample carrier 301, and the inclination angle of the slide of the sample carrier 301 is the same as the inclination angle of the sample carrier 301 after the sample carrier 301 is rotated ninety degrees.

[0023] The connecting plate 102 is fixedly connected with a first solvent support 400 , on which a first solvent piston 402 is mounted, and inside of the first solvent piston 402 a piston extrusion plate 405 is slidably connected.

[0024] The connecting plate 102 is fixedly connected with a second solvent support 401 , and a second solvent piston 403 and a third solvent piston 404 are mounted on the second solvent support 401 . The second solvent piston 403 and the third solvent piston 404 are both slidably connected with a piston squeezing plate 405 .

[0025] The upper piston tube of the second solvent piston 403 is filled with hydrochloric acid, the lower piston tube of the second solvent piston 403 is filled with water, the upper piston tube of the third solvent piston 404 is filled with nitric acid, the lower piston tube of the third solvent piston 404 is filled with water, the upper piston tube of the first solvent piston 402 is filled with nitric acid, and the lower piston tube of the first solvent piston 402 is filled with water.

[0026] A sliding piston 407 is slidably connected in the water-filled piston tubes of the first solvent piston 402, the second solvent piston 403 and the third solvent piston 404, an extrusion spring 406 is arranged between the sliding piston 407 and the piston extrusion plate 405, a limiting spring 408 is arranged between the sliding piston 407 and the first solvent piston 402, the second solvent piston 403 or the third solvent piston 404 respectively, a connecting pipe is arranged between the first solvent piston 402 and the manganese-containing sample beaker 101, and connecting pipes are arranged between the second solvent piston 403 and the third solvent piston 404 and the soluble ore sample beaker 100.

[0027] The above scheme is adopted: by placing the sample in the sample carrier 301, controlling the sample carrier 301 to slide downward, and then rotating clockwise or counterclockwise according to the type of the sample, the sample is respectively transported to the soluble ore sample beaker 100 or the manganese-containing sample beaker 101 through the feeding slide 302. Since the size of the sample carrier 301 is the same as the slideway size of the feeding slide 302, the sample in the sample carrier 301 can be completely slid into the soluble ore sample beaker 100 or the manganese-containing sample beaker 101, and the sample carrier 301 is rotated to feed the sample. At the same time, the cam extrusion block 303 is driven to rotate, thereby squeezing the corresponding piston extrusion plate 405, and the solvents required for different types of samples are added into the easily soluble ore sample beaker 100 or the manganese-containing sample beaker 101. The extrusion spring 406 and the limit spring 408 arranged in the piston cavity filled with water in the first solvent piston 402, the second solvent piston 403 and the third solvent piston 404 are used to control the sliding of the sliding piston 407, thereby controlling the amount of water injected, and controlling the entry amount of the piston extrusion plate 405 to control the entry amount of different solvents.

[0028] like Figures 6 to 8 As shown, the sliding bracket 300 is rotatably connected to a rotating block 500 on one side away from the first solvent bracket 400. The rotating block 500 is provided with a slide groove adapted to the rotating slider 306. A rotating cover plate 501 is rotatably connected inside the beaker cover 103. A transmission belt 502 is wound between the rotating cover plate 501 and the rotating block 500.

[0029] A threaded shaft 504 is fixedly connected inside the manganese-containing sample beaker 101, an upper threaded extrusion piece 505 is threadedly connected to the threaded shaft 504, a lower sliding piece 506 is slidably connected to the upper threaded extrusion piece 505, a stirring block 508 is fixedly connected to the lower side of the lower sliding piece 506, a second return spring 507 is arranged between the upper threaded extrusion piece 505 and the lower sliding piece 506, and an extrusion protrusion 503 is fixedly connected to the rotating cover plate 501, and the extrusion protrusion 503 is extruded and matched with the upper threaded extrusion piece 505.

[0030] The above scheme is adopted: the rotation of the sample carrier 301 drives the rotating cover plate 501 to rotate synchronously, so that the sample slides into the manganese-containing sample beaker 101, and at the same time, the upper threaded extrusion sheet 505 is squeezed by the extrusion protrusion 503 to slide downward, so that the upper threaded extrusion sheet 505 drives the lower sliding sheet 506 and the stirring block 508 to rotate synchronously, and the upper threaded extrusion sheet 505 and the lower sliding sheet 506 are connected through the sliding connection, so that the upper threaded extrusion sheet 505 slides downward without being affected by the lower sliding sheet 506 and the stirring block 508 not sliding downward, and then the same amount of nitric acid and water are added to the soluble ore sample beaker 100 and the manganese-containing sample beaker 101, and the soluble ore sample beaker 100 or the manganese-containing sample beaker 101 is heated by the electric heating plate 200 or the low-temperature electric heating plate 201 respectively, so as to carry out subsequent measurements.

[0031] The working principle and use process of the present invention: When measuring phosphorus pentoxide, the sample is decomposed by acid dissolution. For easily soluble ore samples, a proper amount of sample is first weighed and placed in the loading tray of the sample carrier 301. Then, the operator controls the sample carrier 301 to slide downward along the sliding bracket 300, driving the spring extrusion block 304 to slide synchronously and squeeze the first reset spring 305. When the sample carrier 301 slides to the through hole position of the sliding bracket 300, the operator then controls the sample carrier 301 to rotate counterclockwise, and slides the sample in the sample carrier 301 through the feed slide 302 into the manganese-containing sample beaker 101. During the rotation of the sample carrier 301, the cam extrusion block 303 on the sample carrier 301 is driven to rotate synchronously, and then the cam extrusion block 304 is driven to rotate synchronously. The wheel extrusion block 303 squeezes the piston extrusion plate 405, causing the piston extrusion plate 405 to slide into the first solvent piston 402, and then squeezes the sliding piston 407 to slide in the same direction through the extrusion spring 406, and squeezes the limit spring 408, thereby limiting the sliding distance of the sliding piston 407, and the water in the piston tube filled with water in the first solvent piston 402 is squeezed into the manganese-containing sample beaker 101 through the connecting tube between the water and the manganese-containing sample beaker 101. At the same time, the piston extrusion plate 405 squeezes the nitric acid piston tube of the first solvent piston 402, and squeezes 15~20mL of nitric acid into the manganese-containing sample beaker 101 through the connecting tube, and then starts the electric heating plate 200 to heat the manganese-containing sample beaker 101 to 600℃.

[0032] For the manganese-containing sample, similarly, the sample is weighed and quantitatively placed in the sample carrier 301, and then the operator controls the sample carrier 301 to slide downward to the through-hole position of the sliding bracket 300, and then controls the sample carrier 301 to rotate clockwise, and then the sample in the sample carrier 301 is transported to the soluble ore sample beaker 100 through the feeding slide 302, and at the same time, the cam extrusion block 303 is driven to rotate synchronously through the sample carrier 301, thereby squeezing the piston extrusion plate 405 on the second solvent piston 403. Then, the water and hydrochloric acid in the second solvent piston 403 are injected into the soluble ore sample beaker 100 through the connecting pipe, and then the low-temperature electric heating plate 201 is started to heat the soluble ore sample beaker 100. When the water evaporates and is close to a dry state, the sample carrier 301 is controlled to continue to slide downward, and then rotated clockwise again to squeeze the piston squeezing plate 405, and the nitric acid and water in the third solvent piston 404 are added into the soluble ore sample beaker 100 along the inner wall of the soluble ore sample beaker 100.

[0033] When the sample carrier 301 slides to the through hole position of the sliding bracket 300 and rotates, the rotating slider 306 is driven to slide synchronously, and then the rotating slider 306 slides into the slide groove of the rotating block 500. When the sample carrier 301 rotates counterclockwise, the rotating block 500 is driven to rotate synchronously, and then the rotating cover plate 501 is driven to rotate synchronously through the transmission belt 502, so that the sample in the sample carrier 301 slides to the opening of the rotating cover plate 501 and the beaker cover 103 through the feeding slide 302, and then enters the manganese-containing sample beaker 101. When the rotating cover plate 501 rotates, the extrusion protrusion 503 is driven by the rotating cover plate 501 to extrude the upper threaded extrusion piece 5 05, and then through the threaded connection between the upper threaded extrusion sheet 505 and the threaded shaft 504, the upper threaded extrusion sheet 505 rotates in the process of sliding downward under extrusion, thereby driving the lower sliding sheet 506 and the stirring block 508 to rotate synchronously, stirring the mixture of the sample and the solvent in the manganese-containing sample beaker 101 to dissolve the sample. When the sample carrier 301 rotates in the reverse direction and resets, the extrusion protrusion 503 no longer squeezes the upper threaded extrusion sheet 505. Under the elastic force of the second reset spring 507, the upper threaded extrusion sheet 505 slides upward and resets, and at the same time drives the lower sliding sheet 506 and the stirring block 508 to rotate in the reverse direction, further stirring the mixture of the sample and the solvent.

[0034] Subsequently, the operator adds 2 mL of nitric acid and 20 mL of water into the soluble ore sample beaker 100 and the manganese-containing sample beaker 101, respectively, and heats the soluble ore sample beaker 100 or the manganese-containing sample beaker 101 by the electric heating plate 200 or the low-temperature electric heating plate 201 to dissolve the soluble salt, make up the volume, take the test solution, operate according to the calibration curve analysis steps, use the blank solution as a reference, and measure the absorbance.

[0035] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0036] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. The method for determining phosphorus pentoxide is characterized in that: The following steps are involved: S1. The soluble ore sample is dissolved in nitric acid. 0.1-0.2 g of phosphate rock sample is weighed and added to the sample carrier (301). Then the sample carrier (301) is slid downward and rotated to place the sample in the manganese sample beaker (101) through the feed slide (302). At the same time, the cam extrusion block (303) squeezes the piston extrusion plate (405) so that the 20 ml water in the first solvent piston (402) wets the sample. Add 15-20 mL of nitric acid to the sample through the solvent piston (402), cover the beaker with a lid (103), place on a hot plate (200) and heat to 600°C, dissolve the phosphate rock sample by rotating the stirring block (508), remove the lid (103), evaporate for 15 minutes until nearly dry, add 2 mL of nitric acid and 20 mL of water to a soluble ore sample beaker (100) or a manganese-containing sample beaker (101), heat to 620°C to dissolve the soluble salt, and fix the volume; S2. The manganese-containing sample is dissolved by using hydrochloric acid and nitric acid. 0.1-0.2 g of the phosphate rock sample is weighed and placed in the sample carrier (301). The sample carrier (301) is then slid downward. The sample carrier (301) is rotated to place the sample in the easily soluble ore sample beaker (100) through the feed slide (302). The sample carrier (301) is rotated in the opposite direction while squeezing the piston squeezing plate (405) in the second solvent piston (403) so that the water in the second solvent piston (403) wets the sample. At the same time, the second solvent piston (403) is pushed toward the easily soluble ore sample beaker (100). 10 mL of hydrochloric acid is added to the beaker (100), heated to 600°C on a low-temperature electric hot plate (201), evaporated for 15 minutes until nearly dry, the sample carrier (301) is slid downward again, the sample carrier (301) is rotated to squeeze the piston squeezing plate (405) on the third solvent piston (404), 5 mL of nitric acid is added along the wall of the cup, and the wall of the cup is washed with 10 ml of water, evaporated for 5 minutes until nearly dry, 2 mL of nitric acid and 20 mL of water are added to the soluble ore sample beaker (100) or the manganese-containing sample beaker (101), heated to 620°C to dissolve the soluble salt, and the volume is fixed; S3. Weigh 0.2~0.5g of a sample with high iron content, place it in a porcelain crucible with 8g of mixed flux added in advance, stir well, cover it with a layer of flux, place it in a high-temperature furnace and heat it to 750℃ and keep it for 45min, take it out, cool it, transfer the semi-melted material into a 150mL beaker, wash the crucible with water and dilute it to 50mL, boil it for several minutes, crush the frit, if there is high-valent manganese color, add a little sodium peroxide and boil it to reduce, after cooling, dilute it to a 100mL volumetric flask with water, take 25mL of the clear solution and place it in a 100mL volumetric flask, add a drop of phenolphthalein indicator, neutralize it with nitric acid until the red color disappears and the excess is 3.0mL; S4. Weigh 0.2~0.5g of semi-melted and incompletely decomposed high-iron sample or some silicate stone sample, place it in a corundum crucible, add 5g of sodium peroxide, stir well, cover with another layer, place it in a 700℃ high-temperature furnace to melt for 10min, take out the crucible, cool it, place it in a 250mL beaker, add 50~60mL of hot water to soak it, wash out the crucible with water, boil it on a hot plate for several minutes, transfer it to a 100mL volumetric flask after cooling, dilute it to the scale with water, shake well, take 25mL of the clear liquid and place it in a 100mL volumetric flask, add a drop of phenolphthalein indicator, neutralize it with nitric acid until the red color disappears and the excess is 3.0mL; S5. Take 0, 0.5, 1, 2, 4, 7, and 10 mL of phosphorus pentoxide standard solution and put them into 100 mL volumetric flasks respectively, add 2.5 mL of nitric acid, dilute to about 30 mL with water, add 10 mL of ammonium vanadium molybdate color developer, shake well, make up to volume with water, let it stand for 30 minutes, and measure the absorbance at a wavelength of 420-470 nm on a spectrophotometer with the reagent blank as a reference. Draw a calibration curve, select 1-3 phosphate rock standard substances, and prepare the corresponding solutions according to steps S1 to S4, and measure the absorbance at a wavelength of 420 nm with the reagent blank as a reference.

2. A dedicated device for determining phosphorus pentoxide, applied to the method for determining phosphorus pentoxide as claimed in claim 1, comprising a soluble ore sample beaker (100), characterized in that: The soluble ore sample beaker (100) is fixedly connected to a connecting plate (102), a manganese-containing sample beaker (101) is fixedly connected to the connecting plate (102) on a side away from the soluble ore sample beaker (100), a beaker cover (103) is installed on the manganese-containing sample beaker (101), a low-temperature electric heating plate (201) is installed on the lower side of the soluble ore sample beaker (100), and an electric heating plate (200) is installed on the lower side of the manganese-containing sample beaker (101); The connecting plate (102) is fixedly connected to a symmetrically distributed sliding bracket (300), the sliding bracket (300) is slidably connected to a sample carrier (301), the sliding bracket (300) is fixedly connected to a feed slide (302) at the lower side of the sample carrier (301), the sliding bracket (300) is slidably connected to a spring extrusion block (304), a first return spring (305) is provided between the spring extrusion block (304) and the sliding bracket (300), and a rotating slider (306) is fixedly connected to one end of the sample carrier (301) away from the cam extrusion block (303).

3. The special equipment for measuring phosphorus pentoxide according to claim 2, characterized in that: The sliding bracket (300) is provided with a sliding groove for the sample carrier (301) and the spring extrusion block (304) to slide, and a through hole for the sample carrier (301) to rotate is provided on the lower side of the sliding groove of the sliding bracket (300), and the sliding portion of the sample carrier (301) in the sliding bracket (300) is rectangular.

4. The special equipment for measuring phosphorus pentoxide according to claim 2, characterized in that: The size of the loading tray of the sample tray (301) is the same as the spacing between the sliding bracket (300), the size of the slideway of the feed slide (302) is the same as the size of the loading tray of the sample tray (301), and the inclination angle of the slideway of the sample tray (301) is the same as the inclination angle of the loading tray of the sample tray (301) after rotating ninety degrees.

5. The special equipment for measuring phosphorus pentoxide according to claim 2, characterized in that: A first solvent support (400) is fixedly connected to the connecting plate (102), a first solvent piston (402) is mounted on the first solvent support (400), and a piston extrusion plate (405) is slidably connected inside the first solvent piston (402).

6. The special equipment for determination of phosphorus pentoxide according to claim 5, characterized in that: The connecting plate (102) is fixedly connected to a second solvent support (401), a second solvent piston (403) and a third solvent piston (404) are mounted on the second solvent support (401), and a piston extrusion plate (405) is slidably connected to the second solvent piston (403) and the third solvent piston (404).

7. The special equipment for determination of phosphorus pentoxide according to claim 6, characterized in that: The upper piston tube of the second solvent piston (403) is filled with hydrochloric acid, the lower piston tube of the second solvent piston (403) is filled with water, the upper piston tube of the third solvent piston (404) is filled with nitric acid, the lower piston tube of the third solvent piston (404) is filled with water, the upper piston tube of the first solvent piston (402) is filled with nitric acid, and the lower piston tube of the first solvent piston (402) is filled with water.

8. The special equipment for determination of phosphorus pentoxide according to claim 7, characterized in that: The water-filled piston tubes of the first solvent piston (402), the second solvent piston (403) and the third solvent piston (404) are all slidably connected with sliding pistons (407); an extrusion spring (406) is arranged between the sliding piston (407) and the piston extrusion plate (405); a limit spring (408) is arranged between the sliding piston (407) and the first solvent piston (402), the second solvent piston (403) or the third solvent piston (404), respectively; a connecting pipe is arranged between the first solvent piston (402) and the manganese-containing sample beaker (101); and connecting pipes are arranged between the second solvent piston (403) and the third solvent piston (404) and the soluble ore sample beaker (100).

9. The special equipment for measuring phosphorus pentoxide according to claim 2, characterized in that: A rotating block (500) is rotatably connected to a side of the sliding bracket (300) away from the first solvent bracket (400); the rotating block (500) is provided with a sliding groove adapted to fit the rotating slider (306); a rotating cover plate (501) is rotatably connected inside the beaker cover (103); a transmission belt (502) is wound between the rotating cover plate (501) and the rotating block (500).

10. The special equipment for determination of phosphorus pentoxide according to claim 9, characterized in that: A threaded shaft (504) is fixedly connected inside the manganese-containing sample beaker (101), an upper threaded extrusion sheet (505) is threadedly connected to the threaded shaft (504), a lower sliding sheet (506) is slidably connected to the upper threaded extrusion sheet (505), a stirring block (508) is fixedly connected to the lower side of the lower sliding sheet (506), a second return spring (507) is arranged between the upper threaded extrusion sheet (505) and the lower sliding sheet (506), and an extrusion protrusion (503) is fixedly connected to the rotating cover plate (501), and the extrusion protrusion (503) is extruded and matched with the upper threaded extrusion sheet (505).