Preparation method of Bi3O4Br catalyst for degrading tetracycline

By adjusting the Bi/Br ratio and synthesizing Bi3O4Br nanosheet catalysts, the problems of low conversion rate and narrow spectral response range of traditional catalysts were solved, and a highly efficient photocatalytic degradation effect of tetracycline was achieved.

CN122352294APending Publication Date: 2026-07-10WUHAN UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510042768.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-01-10
Publication Date
2026-07-10

AI Technical Summary

Technical Problem

Existing semiconductor catalysts suffer from low conversion rates and high electron-hole recombination rates due to band structure limitations, making it difficult to achieve efficient solar energy utilization. Furthermore, BiOBr nanosheets have narrow spectral response ranges, low carrier separation, small specific surface areas, and poor pollutant adsorption capabilities.

Method used

By using NaOH as a structure control agent and adjusting the Bi/Br ratio, a Bi3O4Br nanosheet catalyst with abundant oxygen vacancies was synthesized via a hydrothermal method, thereby increasing the specific surface area and photocatalytic active sites and improving the oxygen vacancy concentration.

Benefits of technology

The prepared Bi3O4Br catalyst exhibits high catalytic activity in the photocatalytic degradation of tetracycline, with a larger specific surface area and more photocatalytic reaction active sites, high oxygen vacancy concentration, high photogenerated carrier generation rate and migration efficiency, and low electron-hole recombination efficiency, which significantly improves the photocatalytic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005237441560000011
    Figure HDA0005237441560000011
  • Figure HDA0005237441560000012
    Figure HDA0005237441560000012
  • Figure HDA0005237441560000021
    Figure HDA0005237441560000021
Patent Text Reader

Abstract

This invention discloses a method for preparing a Bi3O4Br catalyst for the efficient degradation of tetracycline, comprising the following steps: S1, mixing bismuth nitrate and potassium bromide in an aqueous solution at room temperature, stirring, and filtering after the reaction to obtain a precipitate; S2, washing and drying the obtained precipitate to obtain a BiOBr precursor; S3, placing the obtained BiOBr precursor in a sodium hydroxide solution of a certain concentration and reacting at a certain temperature to obtain the Bi3O4Br catalyst. Experimental results show that the Bi3O4Br catalyst has a larger specific surface area and more photocatalytic active sites than pure Bi3O4Br, and has a higher oxygen vacancy (OV) concentration, exhibiting high catalytic activity in the photocatalytic degradation of tetracycline. This photocatalyst has broad practical value and application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of photocatalytic material synthesis technology, and specifically relates to a method for preparing a Bi3O4Br catalyst for the degradation of tetracycline. Background Technology

[0002] Semiconductor photocatalytic degradation technology offers a green, low-cost, and highly efficient way to convert solar energy into chemical energy, thus addressing the energy and environmental crisis. The core challenge of this advanced technology is designing highly efficient catalysts to maximize the absorption of sunlight and generate a large number of photogenerated carriers to drive redox reactions. However, most traditional semiconductor catalysts suffer from low conversion rates due to band structure limitations, and high electron-hole recombination rates also hinder the achievement of ideal solar energy utilization. Constructing defects (primarily oxygen vacancies) is one effective method to improve the photocatalytic performance of metal oxides. Increasing the oxygen vacancy content effectively promotes charge transfer and accelerates the activation of molecular oxygen, resulting in more active substances participating in the reaction. Ultimately, by adjusting the crystal structure, band gap energy, and carrier mobility, the photocatalytic activity of the catalyst can be improved.

[0003] Defect construction is a common strategy to improve electron-hole separation efficiency, and the band structure, especially the conduction band position, is also crucial to the activity of photocatalytic reactions. Electron reactivity and the reactive radicals generated by the reaction with water both influence the conduction band minimum. Pure two-dimensional BiOBr nanosheets suffer from drawbacks such as narrow spectral response range, low carrier separation, small specific surface area, and poor pollutant adsorption capacity. The Bi and Br contents in BiOBr crystals dominate the conduction band minimum and valence band maximum of BiOBr. Therefore, we used NaOH as a structure control agent to adjust the Bi / Br ratio. A two-dimensional Bi3O4Br nanosheet photocatalyst with a bismuth-rich structure and abundant oxygen vacancy concentration was designed and synthesized using a simple hydrothermal method, and its application in the photocatalytic degradation of tetracycline hydrochloride was investigated. Summary of the Invention

[0004] To address the problems existing in the prior art, the present invention aims to provide a method for preparing a Bi3O4Br catalyst for the degradation of tetracycline. The Bi3O4Br prepared by this method has a larger specific surface area and more active sites for photocatalytic reactions than pure Bi3O4Br, and has a higher oxygen vacancy (OV) concentration, exhibiting high catalytic activity in the photocatalytic degradation of tetracycline.

[0005] To achieve the above objectives, the present invention adopts the following technical solution:

[0006] The first aspect of the present invention provides a method for preparing a Bi3O4Br catalyst for degrading tetracycline, comprising the following steps:

[0007] S1. Bismuth nitrate and potassium bromide are mixed in an aqueous solution at room temperature and stirred. After the reaction, a precipitate is formed and filtered to obtain the precipitate.

[0008] S2. Wash and dry the obtained precipitate to obtain the BiOBr precursor;

[0009] S3. The obtained BiOBr precursor is placed in a sodium hydroxide solution of a certain concentration and reacted at a certain temperature to obtain the Bi3O4Br catalyst.

[0010] Preferably, in step S1, the molar ratio of bismuth nitrate to potassium bromide is 1:1, the hydrothermal reaction temperature is 120°C, and the reaction time is 12 hours.

[0011] Preferably, in step S2, the washing solvent is water and ethanol, and the drying temperature is 60°C.

[0012] Preferably, in step S3, the concentration of the sodium hydroxide aqueous solution is 0.1 mol / L and the solution volume is 20 ml.

[0013] Preferably, in step S3, the alkalization temperature is 120°C and the time is 9 hours.

[0014] A second aspect of the present invention provides a Bi3O4Br catalyst with high photocatalytic activity prepared by the above preparation method.

[0015] A third aspect of the present invention provides the application of the above-mentioned Bi3O4Br catalyst in the catalytic degradation of tetracycline.

[0016] The present invention has the following beneficial effects:

[0017] This invention utilizes NaOH aqueous solution as a structure control agent to replace bromide ions in the BiOBr precursor, adjusting the Bi / Br ratio to achieve the prerequisites for synthesizing Bi3O4Br, ultimately enabling BiOBr to recombine and generate the Bi3O4Br catalyst. Experimental results show that this Bi3O4Br catalyst has a larger specific surface area and more photocatalytic active sites than pure Bi3O4Br, and exhibits a higher oxygen vacancy (OV) concentration, demonstrating high catalytic activity in the photocatalytic degradation of tetracycline. Attached Figure Description

[0018] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0019] Figure 1XRD patterns of Bi3O4Br (Bi3O4Br-W), BiOBr-W, and Bi3O4Br-650 prepared in Example 1 and Comparative Examples 1-2;

[0020] Figure 2 SEM images of Bi3O4Br (Bi3O4Br-W), BiOBr-W, and Bi3O4Br-650 prepared in Example 1 and Comparative Examples 1-2;

[0021] Figure 3 Solid-state UV absorption spectra of Bi3O4Br (Bi3O4Br-W), BiOBr-W, and Bi3O4Br-650 prepared in Examples 1 and Comparative Examples 1-2;

[0022] Figure 4 Photocurrent response diagrams of Bi3O4Br (Bi3O4Br-W), BiOBr-W, and Bi3O4Br-650 prepared in Example 1 and Comparative Examples 1-2;

[0023] Figure 5 Photoluminescence spectra of Bi3O4Br (Bi3O4Br-W) and Bi3O4Br-650 prepared in Example 1 and Comparative Examples 1-2;

[0024] Figure 6 The graph shows the performance of Bi3O4Br (Bi3O4Br-W), BiOBr-W, and Bi3O4Br-650 prepared for Example 1 and Comparative Examples 1-2 as catalysts for the degradation of tetracycline.

[0025] Figure 7 The first-order reaction rate constants of tetracycline degradation by Bi3O4Br (Bi3O4Br-W), BiOBr-W, and Bi3O4Br-650 prepared for Examples 1 and Comparative Examples 1-2 are shown in the figure.

[0026] Figure 8 XPS O1s spectra of Bi3O4Br (Bi3O4Br-W), BiOBr-W, and Bi3O4Br-650 prepared in Examples 1 and Comparative Examples 1-2. Detailed Implementation

[0027] In the following description, specific details such as particular system structures and techniques are set forth for illustrative purposes and not for limitation, in order to provide a thorough understanding of the embodiments of the present invention. However, those skilled in the art will understand that the present invention may also be implemented in other embodiments without these specific details. The present invention will now be described in detail with reference to embodiments.

[0028] Example 1

[0029] (1) Weigh 0.97g of bismuth nitrate pentahydrate and add it to 30ml of distilled water. Dissolve it at room temperature to obtain a bismuth nitrate solution. Weigh 0.24g of potassium bromide and add it to the bismuth nitrate solution. Stir magnetically for 0.5h at room temperature. Transfer the solution to a 100ml Teflon reactor and hydrothermally react at 120℃ for 12h.

[0030] (2) The obtained precipitate was filtered, and the filter cake was washed several times with deionized water and ethanol. It was then dried in an oven at 60°C to obtain a white precipitate BiOBr precursor.

[0031] (3) The dried sample was placed in 20 ml of 0.1 mol / L sodium hydroxide aqueous solution and stirred for 0.5 h until homogeneous. The solution was transferred to 100 ml of Teflon reaction vessel and hydrothermally heated at 120 °C for 9 h to obtain a white precipitate. The precipitate was filtered, and the cake was washed several times with deionized water and ethanol. It was then dried in an oven at 60 °C to obtain Bi3O4Br, denoted as Bi3O4Br-W.

[0032] Comparative Example 1

[0033] (1) Weigh 0.97g of bismuth nitrate pentahydrate and add it to 30ml of distilled water. Dissolve it at room temperature to obtain a bismuth nitrate solution. Weigh 0.24g of potassium bromide and add it to the bismuth nitrate solution. Stir magnetically for 0.5h at room temperature. Transfer the solution to a 100ml Teflon reactor and hydrothermally react at 120℃ for 12h to obtain a white precipitate.

[0034] (2) The obtained precipitate was filtered, and the filter cake was washed several times with deionized water and ethanol. It was then dried in an oven at 60°C to obtain a white precipitate, BiOBr precursor, denoted as BiOBr-W.

[0035] Comparative Example 2

[0036] 0.61 g BiOBr-W and 0.93 g Bi2O3 were dispersed in 20 ml of ethanol solution and stirred for 0.5 h. The mixture was dried at 80 °C. The resulting powder was placed in a tube furnace and treated at 650 °C for 10 h (5 °C / min) in air atmosphere to obtain Bi3O4Br, denoted as Bi3O4Br-650.

[0037] Characterization and performance testing

[0038] (a) The Bi3O4Br (Bi3O4Br-W), BiOBr-W, and Bi3O4Br-650 prepared in Example 1 and Comparative Examples 1-2 were characterized, and the results are shown in the figure. Figure 1-2 .

[0039] Depend on Figure 1XRD results showed that the prepared Bi3O4Br-W and Bi3O4Br-650 matched the diffraction peaks in standard card PDF#00-037-0700; the prepared BiOBr matched the diffraction peaks in standard card PDF#01-085-0862. After NaOH modification, the characteristic diffraction peaks remained strong and sharp, without any correlation shift. This indicates the successful preparation of the three catalyst samples.

[0040] Depend on Figure 2 The SEM images show the morphological differences among the three samples. BiOBr-W is a relatively regular nanosheet. The SEM image of Bi3O4Br-W also shows a nanosheet shape, but the nanosheets are thinner and lighter than those of BiOBr-W. After NaOH modification, it breaks into even thinner and more fragmented nanosheets, and the number of nanosheets increases significantly. However, the overall morphology of Bi3O4Br-650 does not change significantly compared to BiOBr-W and Bi3O4Br-W; Bi3O4Br-650 has a blocky morphology.

[0041] Analysis of the XRD and SEM test results above shows that this invention utilizes NaOH aqueous solution as a structure control agent to adjust the Bi / Br ratio, achieving the prerequisite conditions for synthesizing Bi3O4Br-W. By controlling the NaOH concentration, the prepared Bi3O4Br-W catalyst has a nanosheet morphology. On the other hand, the Bi3O4Br-W catalyst breaks down into thinner and more fragmented nanosheets than BiOBr-W, and the number of nanosheets is significantly increased. This will endow the catalyst with a larger specific surface area and more active sites for photocatalytic reactions, which is beneficial to improving the performance of photocatalytic degradation of tetracycline hydrochloride.

[0042] (b) UV testing was performed on Bi3O4Br (Bi3O4Br-W), BiOBr-W, and Bi3O4Br-650 prepared in Examples 1 and Comparative Examples 1-2. The results are shown in […]. Figure 3 .

[0043] Depend on Figure 3 The UV test results show that, in the range of 200–450 nm, the Bi3O4Br-W catalyst sample prepared in Example 1 has stronger light absorption characteristics compared to BiOBr-W and Bi3O4Br-650.

[0044] (c) Photocurrent tests were performed on the Bi3O4Br (Bi3O4Br-W), BiOBr-W, and Bi3O4Br-650 prepared in Examples 1 and Comparative Examples 1-2. The specific steps were as follows: 2 mg of each of the Bi3O4Br-W, BiOBr-W, and Bi3O4Br-650 prepared in Examples 1 and 1-2 were added to 500 μL of ethanol to form a suspension. Then, 20 μL of Nafion was added and the suspension was ultrasonically dispersed. 520 μL of each suspension was coated onto the surface of an FTO glass, with a coating area of ​​1 cm². 2 The electrode was dried to obtain the working electrode. Photocurrent measurements were performed on a CHI660E electrochemical workstation using a three-electrode system: an Ag / AgCl electrode as the reference electrode, a platinum sheet as the counter electrode, and a 0.5M sodium sulfate aqueous solution as the electrolyte. Photocurrent measurements were conducted under an argon atmosphere at room temperature using a xenon lamp (420nm filter) as the light source. The photocurrent measurement results are shown below. Figure 4 .

[0045] Depend on Figure 4 Photocurrent testing results show that, compared to BiOBr-W and Bi3O4Br-650, the Bi3O4Br-W sample prepared in Example 1 exhibits the strongest photocurrent response. This indicates that the Bi3O4Br-W sample possesses a higher photogenerated carrier generation rate and migration efficiency. These highly active photogenerated carriers can promote redox reactions in the photocatalytic process, resulting in higher photocatalytic performance of the photocatalyst.

[0046] (d) The PL tests were performed on Bi3O4Br (Bi3O4Br-W) and Bi3O4Br-650 prepared in Example 1 and Comparative Example 2, and the results are shown in the figure. Figure 5 .

[0047] Depend on Figure 5 The PL spectroscopy results show that, compared with Bi3O4Br-650, the Bi3O4Br-W sample prepared in Example 1 has the lowest photoluminescence intensity, indicating that the recombination efficiency of photogenerated electrons and holes in this catalyst is the lowest, and the lifetime of photogenerated electrons and holes is significantly extended.

[0048] In summary, the Bi3O4Br-W sample prepared by the method of this invention has a nanosheet-like structure and a large specific surface area, and the photogenerated electron-hole recombination efficiency is reduced.

[0049] (e) Catalyst activity

[0050] Evaluation of the photocatalytic degradation performance of tetracycline by the catalyst

[0051] Specific steps: First, weigh 30 mg of Bi3O4Br (Bi3O4Br-W), BiOBr-W, and Bi3O4Br-650 prepared in Example 1 and Comparative Examples 1-2, and place them separately in a 50 mL photocatalytic reactor containing 20 mg / L freshly prepared TC solution (pH=7). After stirring evenly, allow it to stand in the dark for 30 min to reach adsorption-desorption equilibrium. Then, conduct photocatalytic degradation experiments under 300W xenon lamp illumination. During the experiment, maintain the reactor temperature at approximately 20℃ to eliminate the influence of temperature on the experimental results. Every 10 min, 3 mL of solution is drawn from the reactor, filtered, and the absorbance at 360 nm is measured using a 722s visible spectrophotometer to evaluate the degradation performance of each photocatalyst. Results are shown below. Figure 6 and Figure 7 .

[0052] Depend on Figure 6 The results show that the tetracycline degradation rate of the Bi3O4Br-W sample reached 83.6% within 90 minutes, which is about 4 times that of the tetracycline degradation rate catalyzed by the control sample Bi3O4Br-650 under the same experimental conditions.

[0053] Depend on Figure 7 The results show that the tetracycline degradation reaction catalyzed by Bi3O4Br-W is a first-order reaction with a rate constant of 4.1 × 10⁻⁶. -2 The rate constant of the catalytic reaction of tetracycline degradation was significantly higher than that of the other two catalyst samples, and was about 6 times that of the Bi3O4Br-650 sample.

[0054] Depend on Figure 8 The results show that the peak positions at 529.75 eV, 529.73 eV, and 530.11 eV are characteristic of Bi-O bonds, while the peaks at 530.89 eV, 530.92 eV, and 531.79 eV are attributed to surface oxygen. The peak intensity of surface oxygen is related to the concentration of oxygen vacancies (OV). Therefore, in the comparison figure, the peak intensity of surface oxygen in Bi3O4Br-W is significantly higher than that in BiOBr-W and Bi3O4Br-650. This result fully demonstrates that oxygen vacancies (OV) exist in the three photocatalysts BiOBr-W, Bi3O4Br-W, and Bi3O4Br-650, and that the oxygen vacancy concentration in Bi3O4Br-W is much higher than that in BiOBr-W and Bi3O4Br-650.

[0055] This invention is not limited to the specific embodiments described above. Any modifications made by those skilled in the art based on the above concept without creative effort are within the scope of protection of this invention.

Claims

1. A method for preparing a Bi3O4Br catalyst for the degradation of tetracycline, characterized in that, Includes the following steps: S1. Bismuth nitrate and potassium bromide are mixed in an aqueous solution at room temperature and stirred. After the reaction, a precipitate is formed and filtered to obtain the precipitate. S2. Wash and dry the obtained precipitate to obtain the BiOBr precursor; S3. The obtained BiOBr precursor is placed in a sodium hydroxide solution of a certain concentration and reacted at a certain temperature to obtain the Bi3O4Br catalyst.

2. The method for preparing the Bi3O4Br catalyst for degrading tetracycline according to claim 1, characterized in that, In step S1, the molar ratio of bismuth nitrate to potassium bromide is 1:1, the hydrothermal reaction temperature is 120°C, and the reaction time is 12 hours.

3. The method for preparing the Bi3O4Br catalyst for degrading tetracycline according to claim 1, characterized in that, In step S2, the washing solvent is water and ethanol, and the drying temperature is 60°C.

4. The method for preparing the Bi3O4Br catalyst for degrading tetracycline according to claim 1, characterized in that, In step S3, the concentration of the sodium hydroxide aqueous solution is 0.1 mol / L, and the solution volume is 20 ml.

5. The method for preparing the Bi3O4Br catalyst for degrading tetracycline according to claim 1, characterized in that, In step S3, the alkalization temperature is 120°C and the time is 9 hours.

6. A Bi3O4Br catalyst prepared by the preparation method according to any one of claims 1-5.