Composite material, powder material, abrasive material and method for producing composite material

A composite material with thin, dense oxide ceramic coatings on non-oxide ceramics or diamonds addresses the challenge of unstable interfaces by enhancing surface functional groups and wettability, improving abrasive material performance and resin composites.

JP2024143454APending Publication Date: 2024-10-11NORITAKE MACHINE TECHNO CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023056146
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing methods for surface modification of non-oxide ceramics and diamonds using oxide ceramics result in thick films, leading to unstable interfaces and limited applicability, as they are difficult to deposit thinly and are limited to materials that directly bond with nitride ceramics.

Method used

A composite material is developed with non-oxide ceramics or diamonds coated by a thin, dense film of metal or metalloid oxide ceramics, characterized by pores with a maximum peak diameter of 5 nm or less, enhancing surface functional groups and wettability.

Benefits of technology

The composite material exhibits improved surface modification, increased functional groups, and enhanced dispersibility and wettability with resins, leading to better performance in abrasive materials and resin composites.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143454000001_ABST
    Figure 2024143454000001_ABST
Patent Text Reader

Abstract

To provide a composite material, powder material containing the composite material and an abrasive containing the composite material, which have obtained a surface modification effect by thinly covering oxide ceramic, and a method for producing the composite material.SOLUTION: The composite material disclosed herein is a composite material comprising a non-oxide ceramic or diamond, and a metal or semi-metal oxide ceramic adhered to a surface of the non-oxide ceramic or diamond, wherein the oxide ceramic is an aggregate of a plurality of particles, has pores between the particles of the oxide ceramic, and has a maximum peak pore diameter of 5 nm or less in a differential pore volume distribution of the oxide ceramic determined by a non-localized density functional (NLDFT) method.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to composite materials, powder materials, abrasive materials, and methods for making composite materials. [Background technology]

[0002] Non-oxide ceramics and diamond are used in various applications, such as abrasives and heat dissipation members (heat dissipation sheets, etc.), because of their high hardness and excellent thermal conductivity. On the other hand, non-oxide ceramics and diamond have few surface functional groups and low affinity (wettability) with other materials (for example, resins, etc.). In order to improve such affinity, composite materials are used in which the surface is coated with oxide ceramics having many hydroxyl groups, as in Patent Documents 1 and 2. For example, Patent Document 1 discloses abrasives for vitrified bond grinding wheels, in which the surface of cubic boron nitride is coated with an aluminum oxide layer or a silicon oxide layer with an average thickness of 0.1 to 10 μm. Patent Document 2 discloses silica-coated metal nitride particles, which are coated with sintered silica particles (oxide ceramic particles) directly bonded to the surface of metal nitride particles (non-oxide ceramic particles) and covered with almost no gaps. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 7-108461 [Patent Document 2] JP 2015-101510 A Summary of the Invention [Problem to be solved by the invention]

[0004] In surface modification using oxide ceramics, it is preferable to apply the oxide ceramics as thinly as possible in order to utilize the inherent physical properties of non-oxide ceramics and diamond. In Patent Document 1, the oxide ceramics are applied as a thick film. It is difficult to apply the oxide ceramics thinly because the ratio of the unstable oxide ceramic-non-oxide ceramic interface to the amount of oxide ceramics is high. In Patent Document 2, silica particles are directly bonded to the nitride ceramics to coat them. For this reason, the oxide ceramics that can be used in the technology disclosed in Patent Document 2 are limited to materials that directly bond to nitride ceramics.

[0005] The technology disclosed herein has been created in view of the above, and aims to provide a composite material that has a surface modification effect achieved by being thinly coated with an oxide ceramic. Another aim is to provide a powder material containing the composite material, an abrasive material containing the composite material, and a method for producing the composite material. [Means for solving the problem]

[0006] The composite material disclosed herein is a composite material comprising a non-oxide ceramic or diamond, and a metal or semi-metal oxide ceramic adhered to a surface of the non-oxide ceramic or diamond, wherein the oxide ceramic is an aggregate of a plurality of particles, has pores between the particles of the oxide ceramic, and has a maximum peak pore diameter of 5 nm or less in a differential pore volume distribution of the oxide ceramic determined by a non-localized density functional (NLDFT) method.

[0007] In the above composite material, the oxide ceramics attached to the surface of the non-oxide ceramic or diamond exist as an aggregate of multiple particles. The maximum peak pore size of the oxide ceramics is 5 nm or less. That is, the above composite material is composed of mostly small oxide ceramic particles. In other words, the majority of the oxide ceramic particles have small particle sizes and are relatively densely assembled. This allows the formation of a thin and dense oxide ceramic film on the surface of the non-oxide ceramic or diamond, achieving efficient surface modification.

[0008] In a preferred embodiment of the composite material disclosed herein, the pore surface area per unit mass of the oxide ceramics when the pore diameter of the oxide ceramics is 5 nm or less is 10 m 2 / g or more. According to this configuration, the oxide ceramic is suitably present as an aggregate of a plurality of particles in the composite material.

[0009] In a preferred embodiment of the composite material disclosed herein, the ratio of the surface area of ​​pores having a pore diameter of 2 nm or less to the surface area of ​​pores having a pore diameter of 10 nm or less in the oxide ceramic is 30% or more. By attaching the oxide ceramic to the surface of the non-oxide ceramic or diamond in the above-mentioned configuration, it is possible to increase the number of functional groups on the surface of the non-oxide ceramic or diamond.

[0010] In a preferred embodiment of the composite material disclosed herein, the oxide ceramic contains at least one compound selected from the group consisting of alumina, silica, zirconia, titania, ceria, yttria, iron oxide, zinc oxide, and zeolite. In a preferred embodiment of the composite material disclosed herein, the oxide ceramic contains a mixture or composite oxide selected from the group consisting of amorphous alumina, γ-alumina, amorphous silica, and amorphous zirconia. According to this configuration, it is possible to provide a composite material in which the oxide ceramic is attached in the form of an aggregate of a plurality of particles.

[0011] In a preferred embodiment of the composite material disclosed herein, the non-oxide ceramic is a nitride ceramic. In a preferred embodiment of the composite material disclosed herein, the nitride ceramic contains at least one compound selected from the group consisting of aluminum nitride and boron nitride. With this configuration, the oxide ceramic is preferably attached, so that a composite material can be provided in which the effect of increasing surface functional groups is preferably exhibited.

[0012] In a preferred embodiment of the composite material disclosed herein, when the composite material is mixed with a separate phase of water and a non-polar solvent, 70% or more of the composite material is present in the aqueous phase, which allows the surface modification effect of the ceramic oxide to be favorably obtained.

[0013] As another aspect of the technology disclosed herein, there is provided a powder material containing the composite material in powder form. According to this configuration, since the composite material having the above configuration is in powder form, it is possible to provide a powder material that can be suitably composited with other materials.

[0014] The composite material disclosed herein has a large number of functional groups on the surface of the composite material, and therefore has good dispersibility in resins, and can therefore be suitably used as a filler for resin materials that have good dispersibility in resins.

[0015] As another aspect of the technology disclosed herein, an abrasive material containing the above composite material is provided. Such an abrasive material is suitably provided with a surface functional group. Therefore, the wettability between the abrasive material and a binder (typically, vitrified bond, resin bond, etc.) is good, and by using the abrasive material disclosed herein, it is possible to provide a grinding wheel with suitably improved grinding wheel strength.

[0016] As another aspect of the technology disclosed herein, a method for producing a composite material is provided. The method for producing a composite material disclosed herein is a method for producing a composite material including a non-oxide ceramic or diamond and an oxide ceramic of a metal or metalloid attached to the surface of the non-oxide ceramic or diamond, and includes a step of attaching a resinate containing a metal or metalloid, which is a raw material of the oxide ceramic, to the non-oxide ceramic or diamond, and a step of decomposing the resinate, in which the oxide ceramic is an aggregate of a plurality of particles in the composite material, pores are present between the particles of the oxide ceramic, and the maximum peak pore size in the differential pore volume distribution of the oxide ceramic obtained by the non-localized density functional (NLDFT) method is 5 nm or less. According to this method, a thin and dense oxide ceramic film can be formed on the surface of the non-oxide ceramic or diamond, and a composite material with an efficient surface modification effect can be produced.

[0017] In a preferred embodiment of the manufacturing method disclosed herein, the decomposition step is heat-treated at 800° C. or less. This effectively prevents the oxide ceramic from sintering, and the oxide ceramic is formed as an aggregate of multiple particles. This allows thin, dense oxide ceramic particles to be more effectively attached to the non-oxide ceramic or diamond. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is a partially enlarged view that illustrates a composite material according to one embodiment. [Diagram 2] FIG. 2 is an FE-SEM image (magnification: 50,000) relating to Example 1. [Diagram 3] FIG. 3 is an FE-SEM image (magnification: 50,000) relating to Example 2. [Figure 4] FIG. 4 is an FE-SEM image (magnification: 50,000) relating to Example 3. [Diagram 5] FIG. 5 is an FE-SEM image (100,000x) of Example 8. [Figure 6] FIG. 6 is an FE-SEM image (100,000x) of Example 9. [Figure 7] FIG. 7 is an FE-SEM image (magnification: 50,000) relating to Example 12. [Figure 8] FIG. 8 is an FE-SEM image (magnification: 50,000) relating to Example 13. [Figure 9] FIG. 9 is an FE-SEM image (100,000x) of Example 14. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] An embodiment of the present technology will be described below. Matters other than those specifically mentioned in this specification and necessary for implementing the present technology can be understood as design matters for a person skilled in the art based on the conventional technology in the relevant field. The present technology can be implemented based on the contents disclosed in this specification and the technical common sense in the relevant field. In this specification, when a numerical range is described as "A to B (where A and B are arbitrary numerical values)", it means "A or more and B or less", and also includes the meanings of "more than A and less than B", "more than A and B or less", and "more than A and less than B".

[0020] Fig. 1 is a schematic partially enlarged view showing a composite material 100 according to one embodiment. As shown in Fig. 1, the composite material 100 disclosed herein includes a non-oxide ceramic or diamond (substrate portion 10) and an oxide ceramic 20. The composite material 100 may also include other components not shown. Hereinafter, in this specification, the "non-oxide ceramic or diamond" is also referred to as the "substrate portion".

[0021] The substrate 10 is a core made of non-oxide ceramics or diamond. Examples of non-oxide ceramics used in the substrate 10 include ceramics made of non-oxides such as nitrides, carbides, borides, and apatite, among which nitride ceramics are preferred. Examples of nitride ceramics used in the substrate 10 include aluminum nitride (AlN), boron nitride (BN), silicon nitride (Si3N4), and gallium nitride (GaN), among which aluminum nitride or boron nitride, or a mixture thereof, are preferred. From the viewpoint of favorably exerting the effect of increasing the functional groups on the substrate 10 surface by the oxide ceramics, it is particularly preferred to use boron nitride as the substrate 10. Examples of boron nitride used in the substrate 10 include cubic boron nitride (cBN), hexagonal boron nitride (hBN), among which hexagonal boron nitride is preferably used. In addition, the substrate 10 is preferably diamond. The substrate 10 may be made of any one material alone or in combination of two or more materials depending on the required properties and applications of the composite material 100 .

[0022] The oxide ceramic 20 is attached to the surface of the substrate 10. As shown in FIG. 1, the oxide ceramic 20 is attached as an aggregate of multiple particles. Here, the oxide ceramic 20 is a porous body (porous structure) having many pores 11 between the particles of the oxide ceramic 20. With this structure, the functional group concentration is high in the portion where the oxide ceramic 20 is attached. Note that the "aggregate of multiple particles" in the specification refers to, for example, an agglomerate of particles or an incomplete sintered body (a body in which multiple particles are necked together).

[0023] The oxide ceramics 20 typically include metal or metalloid oxide ceramics. The oxide ceramics 20 preferably include at least one compound selected from the group consisting of alumina, silica, zirconia, titania, ceria, yttria, iron oxide, zinc oxide, and zeolite. The oxide ceramics 20 also preferably include a mixture or composite oxide selected from the group consisting of amorphous alumina, γ-alumina, amorphous silica, and amorphous zirconia. According to this configuration, a high concentration of functional groups (mainly hydroxyl groups) is introduced to the surface of the oxide ceramics 20, making the surface easily hydrophilic and easily microparticulating. For this reason, it is suitable for use in that the oxide ceramics 20, which has a porous structure, can be easily formed. In addition, the term "metalloid" in the specification refers to a "metalloid element," typically referring to Si, B, Sb, and Te.

[0024] The oxide ceramics 20 are attached generally uniformly. It is preferable that the oxide ceramics 20 are attached (present widely) over a wide area of ​​the surface of the substrate 10. This allows the effect of modifying the surface of the substrate 10 by the oxide ceramics 20, typically the effect of increasing functional groups, to be favorably exhibited.

[0025] It is preferable that at least a part of the composite material 100 has a surface exposed portion 12 where the surface of the substrate portion 10 is exposed. In other words, the surface exposed portion 12 indicates a portion where the oxide ceramics 20 is not attached to the surface of the substrate portion 10. This reduces the inhibition of the characteristics of the substrate portion 10.

[0026] The surface exposure rate (%) of the substrate 10 in the composite material 100 is preferably 2% or more, 5% or more, 10% or more, 20% or more, 30% or more, or 40% or more. On the other hand, the surface exposure rate (%) of the substrate 10 in the composite material 100 is preferably 90% or less, 80% or less, 70% or less, 60% or less, or 50% or less. If the surface exposure rate is too low, it is not preferable because the expression of the characteristics of the substrate 10 is suppressed. On the other hand, if the surface exposure rate is too high, it is not preferable because the surface modification effect of the substrate 10 by the oxide ceramic is reduced. Note that the "surface exposure rate of the substrate" in this specification can be measured, for example, based on the following procedure. First, a composite material having a planar area of ​​100 μm2 on an image is measured. 2 An SEM image including the above is obtained. By analyzing the obtained SEM image, the total area of ​​the composite material and the area of ​​the exposed base material 10 (non-oxide ceramic or diamond) are calculated, and can be calculated using the following formula (I). Surface exposure rate (%) = (area of ​​exposed non-oxide ceramic or diamond surface) / (total area of ​​composite) × 100 (I).

[0027] The composite material 100 disclosed herein is characterized in that the oxide ceramic 20 is an aggregate of a plurality of particles, and the maximum peak pore diameter in the differential pore volume distribution of the oxide ceramic 20 obtained by the non-localized density functional theory (NLDFT) method is 5 nm or less. The pores 11 of the oxide ceramic 20 having the maximum peak pore diameter of 5 nm or less are generally composed of small particles of the oxide ceramic 20. In other words, the majority of the particles of the oxide ceramic 20 have small diameters, and these particles are relatively densely assembled. This forms a thin and dense oxide ceramic film on the surface of the substrate 10, and the surface is efficiently modified. The "maximum peak pore diameter in the differential pore volume distribution of the oxide ceramic obtained by the non-localized density functional theory (NLDFT) method" can be obtained by acquiring a nitrogen adsorption isotherm at -196°C and analyzing it by the NLDFT method. For example, the particle surface of the non-oxide ceramic or diamond is observed in advance with a scanning electron microscope or a transmission electron microscope, and the absence of pores in the required analysis range (for example, 200 nm or less, 100 nm or less, 50 nm or less, 20 nm or less, 10 nm or less, 5 nm or less, 1 nm or less) is confirmed, and then the above measurement is performed on the entire composite material to measure the pore size and pore volume between the particles of the oxide ceramic. In addition, after obtaining a nitrogen adsorption isotherm for the entire composite material, the composite material is subjected to ultrasonic dispersion to remove the oxide ceramic, and then the nitrogen adsorption isotherm of the non-oxide ceramic or diamond is obtained again and excluded for measurement. In addition, after obtaining a nitrogen adsorption isotherm for the entire composite material, either the substrate part (non-oxide ceramic or diamond) of the composite material or the oxide ceramic is dissolved and removed, and either the nitrogen adsorption isotherm is obtained again and excluded for measurement.

[0028] The peak pore diameter in the pore diameter distribution of the oxide ceramic 20 by the NLDFT method is preferably 5 nm or less, more preferably 3 nm or less, 2.5 nm or less, 2.2 nm or less, or 2 nm or less, in the differential pore volume distribution. The lower limit of the peak pore diameter in the pore diameter distribution of the oxide ceramic 20 is not particularly limited, but is preferably 0.35 nm or more, for example. The lower limit of the pore diameter analysis by the nitrogen gas adsorption method is 0.35 nm.

[0029] The pore surface area (m2) per unit mass of the oxide ceramic 20 when the pore diameter of the oxide ceramic 20 is 5 nm or less 2 / g) is 10m 2 / g or more is preferable, and 20m 2 / g or more, 50m 2 / g or more, 90m 2 / g or more, 100m 2 / g or more, 200m 2 / g or more is more preferable. When the pore surface area is within the above-mentioned numerical range, it indicates that the oxide ceramic 20 has a certain amount of pores, that is, the oxide ceramic 20 is not highly densified and preferably exists as an aggregate of a plurality of particles. Similarly, the pore surface area (m 2 / g) is 10m 2 / g or more is preferable, and 20m 2 / g or more, 30m 2 / g or more, 50m 2 / g or more, 100m 2 / g or more. In addition, the pore surface area per unit mass of the oxide ceramic 20 when the pore diameter of the oxide ceramic 20 is 1 nm or less is preferably 10 m 2 / g or more, 20m 2 / g or more, 30m 2 / g or more, 40m 2 / g or more, 80m 2 It is preferable that the molecular weight is 1 / g or more.

[0030] The pore surface area (m2) per unit mass of the oxide ceramic 20 when the pore diameter of the oxide ceramic 20 is 2 nm or less 2 Although there is no particular upper limit for the mass ratio of the oxide ceramic 20 adhered to the substrate 10, from the viewpoint of maintaining the strength of the oxide ceramic 20 adhered to the substrate 10 and suppressing the falling off, it is preferable that the upper limit is 10,000 m 2 / g or less is preferable, and 5000m 2 / g or less, 3000m 2 / g or less, 2000m 2 / g or less, 1000m 2 / g or less is more preferable.

[0031] The ratio of the surface area of ​​the pores of the composite material 100 having a diameter of 2 nm or less to the surface area of ​​the pores of the composite material 100 having a diameter of 10 nm or less is 30% or more, and preferably 40% or more, 50% or more, or 60% or more. This value means that the ratio of the pores 11 (micropores) having a diameter of 2 nm or less among the fine pores having a diameter of 10 nm or less in the pores 11 in the composite material 100 is large. This indicates that the particle diameter of the oxide ceramics 20 constituting these pores 11 is small and relatively densely assembled. When the pores 11 of the composite material 100 have a diameter of 2 nm or less, they are filled with water vapor in the air in a normal atmosphere. The surface properties are similar to those of non-porous oxide ceramics (Reference: M. Fuji, J.Soc.Powder Technol., Japan, 40, 355-363 (2003)). Therefore, this configuration allows the surface of the base material 10 to be efficiently modified.

[0032] In the composite material 100, the pore volume (cm) per unit mass of the oxide ceramic 20 when the pore diameter of the oxide ceramic 20 is 5 nm or less 3 / g) is 0.01 cm 3 / g or more, preferably 0.02 cm 3 / g or more, 0.03cm 3 / g or more, 0.05cm 3 / g or more, 0.09cm 3 / g or more. With such a pore volume, the surface modification effect of the oxide ceramic 20 is preferably exhibited. In addition, in the composite material 100, the pore volume (cm) per unit mass of the oxide ceramic 20 when the pore diameter of the oxide ceramic 20 is 2 nm or less is 3 / g) is 0.01 cm 3 / g or more, preferably 0.02 cm 3 / g or more, 0.03cm 3 / g or more, 0.04cm 3 / g or more, 0.08cm 3 / g or more.

[0033] Although not particularly limited, the pore volume (cm ) per unit mass of the oxide ceramic 20 3 / g) is, for example, 10 cm 3 / g or less, preferably 5 cm 3 / g or less, 2cm 3 / g or less, 1cm 3 / g or less, 0.5cm 3 / g or less. With such a pore volume, the strength of the oxide ceramic 20 attached to the substrate 10 is maintained and falling off is suppressed.

[0034] The pore surface area (m2) of the oxide ceramic 20 per unit BET surface area of ​​the substrate, measured by the NLDFT method, when the pore diameter of the oxide ceramic 20 is 10 nm or less 2 / m 2 ) is 0.1m 2 / m 2 More than 0.2m is preferable. 2 / m 2 More than 0.5m 2 / m 2 More than 1m 2 / m 2 Over 2m 2 / m 2The above is more preferable. According to this configuration, the oxide ceramics 20 on the substrate 10 has pores of a certain surface area, that is, the oxide ceramics 20 is not densified and is preferably present as an aggregate of a plurality of particles. In this specification, the term "BET surface area" refers to a value obtained by analyzing an adsorption isotherm measured by a gas adsorption method using nitrogen (N2) gas as an adsorbate, according to "Method of measuring specific surface area of ​​powder (solid) by gas adsorption" defined in JIS Z 8830:2013 (ISO9277:2010), by the BET method.

[0035] The pore surface area (m2) of the oxide ceramic 20 per unit BET surface area of ​​the substrate, measured by the NLDFT method, when the pore diameter of the oxide ceramic 20 is 5 nm or less 2 / m 2 ) is 0.1m 2 / m 2 More than 0.2m is preferable. 2 / m 2 More than 0.5m 2 / m 2 More than 1m 2 / m 2 Over 2m 2 / m 2 More preferably, the pore surface area (m2) of the oxide ceramic 20 per unit BET surface area of ​​the substrate when the pore diameter of the oxide ceramic 20 is 2 nm or less is determined by the NLDFT method. 2 / m 2 ) is 0.1m 2 / m 2 More than 0.2m is preferable. 2 / m 2 More than 0.5m 2 / m 2 More than 0.7m 2 / m 2 More than 1m 2 / m 2 The above is more preferable.

[0036] The adhesion rate (wt%) of the oxide ceramics 20 in the entire composite material 100 is preferably 0.1 wt% or more, 0.2 wt% or more, 0.3 wt% or more, 0.5 wt% or more, or 1 wt% or more. On the other hand, the adhesion rate (wt%) of the oxide ceramics 20 is preferably 30 wt% or less, 20 wt% or less, 15 wt% or less, 10 wt% or less, 5 wt% or less, or 3 wt% or less. If the adhesion rate is too low, the surface exposed portion 12 of the substrate 10 increases on the surface of the composite material 10, which is not preferable. On the other hand, if the adhesion rate is too high, it is not preferable because the expression of the characteristics of the substrate 10 is suppressed. The adhesion rate of the oxide ceramics 20 can be calculated by the following formula (II). Adhesion rate of oxide ceramic (wt%) = weight of oxide ceramic (g) / (weight of non-oxide ceramic or diamond (g) + weight of oxide ceramic (g)) (II)

[0037] The weight of oxide ceramic 20 attached per unit BET surface area of ​​the substrate (g / m 2 ) is set to 0.001 g / m from the viewpoint of allowing the oxide ceramics 20 to adhere widely onto the substrate 10 and to perform suitable surface modification. 2 More than 0.002g / m 2 More than 0.003g / m 2 More than 0.005g / m 2 More than 0.007g / m 2 The adhesion weight (g / m) of the oxide ceramic 20 per unit BET surface area of ​​the substrate is preferably 100% or more. 2 ) is 1 g / m from the viewpoint of favorably exhibiting the characteristics of the base material 10. 2 Below 0.5g / m 2 Below, 0.1g / m 2 Below 0.05g / m 2 The following is preferred:

[0038] The deposition volume (nm) of oxide ceramics 20 per unit BET surface area of ​​the substrate 3 / nm 2 ) is set to 0.2 nm from the viewpoint of allowing the oxide ceramics 20 to adhere widely onto the substrate 10 and to perform suitable surface modification. 3 / nm 2 or more, 0.5nm3 / nm 2 Above, 1nm 3 / nm 2 Above, 1.5nm 3 / nm 2 Above, 2nm 3 / nm 2 More preferably, the deposition volume (nm 3 / nm 2 ) is set to 100 nm from the viewpoint of favorably exhibiting the characteristics of the base material 10. 3 / nm 2 Below, 80nm 3 / nm 2 Below, 50nm 3 / nm 2 Below, 30nm 3 / nm 2 Below, 20nm 3 / nm 2 The following is preferred:

[0039] In some preferred embodiments, when the separated phase of water and non-polar solvent and the powdered composite material 100 are stirred, 70 wt% or more (hereinafter also referred to as "the majority") of the composite material 100 is present in the aqueous phase, more preferably 75 wt% or more, 80 wt% or more. When the composite material 100 has the above-mentioned properties, it is found that the surface of the substrate tends to be modified by the oxide ceramics. That is, in a composite material having such properties, it is found that the oxide ceramics are attached to a certain or more part of the substrate surface. The above evaluation (hereinafter also referred to as "water-non-polar solvent preference evaluation") is, for example, first, the powdered composite material, water, and the non-polar solvent are placed in a container (e.g., a glass bottle, etc.) and stirred (e.g., shaken by hand, using a shaker, etc.). After that, the container is left to stand, and it is confirmed whether the majority of the composite material is present in the aqueous phase or the non-polar solvent phase. Such confirmation can be performed by visual inspection. The non-polar solvent used in the water-non-polar solvent preference evaluation can be any of hexane, heptane, octane, nonane, and decane. When evaluating the water-non-polar solvent preference, the solvent and the container of the composite material may be subjected to a dispersion treatment such as ultrasonic dispersion to such an extent that the surface properties are not changed due to the falling off of the oxide ceramics. In addition, the ratio of the composite material in the separated phase of water and non-polar solvent can be determined, for example, by removing either the water phase or the non-polar solvent phase (in other words, separating the water phase and the non-polar solvent phase), drying and removing the solvent of the other phase, measuring the weight of the composite material contained in that phase, and calculating the ratio of the weight to the weight of the total composite material (the weight of the entire composite material put into the container).

[0040] In some preferred embodiments, the composite material 100 may be used as a powder material, in which the composite material is contained in a powder form. More specifically, the composite material 100 exists in a powder form and is used as a powder material. The powder material may be used, for example, as a filler for a resin member such as a thermally conductive sheet.

[0041] In some preferred embodiments, the composite material 100 is used as a filler for a resin member. Conventionally, when a composite material having pores is used as a filler for a resin member, voids (typically air) remain in the pores in the composite material, which may impair the properties of the substrate (e.g., thermal conductivity, etc.). On the other hand, for pores with a pore diameter of 2 nm or less, components in the environment such as water vapor fill the micropores under normal conditions (typically in the atmosphere), so that the inhibition of the properties of the substrate by the pores is suppressed. In addition, the composite material 100 of this embodiment has a ratio of the surface area of ​​pores with a pore diameter of 2 nm or less to the surface area of ​​pores with a pore diameter of 10 nm or less in the composite material 100, which is determined by the NLDFT method, of 30% or more. Therefore, the inhibition of the properties of the substrate 10 can be suppressed by using the composite material disclosed herein as a filler for a resin member.

[0042] When the entire powder material is taken as 100 wt%, the powder material may contain, for example, 80 wt% or more of composite material 100, preferably 85 wt% or more of composite material 100, more preferably 90 wt% or more of composite material 100, even more preferably 95 wt% or more of composite material 100, and particularly preferably 98 wt% or more or 99 wt% or more of composite material 100.

[0043] In this embodiment, the average particle size of the composite material 100 in the powder material is not particularly limited and can be appropriately changed depending on the purpose and mode of use. The average particle size of the composite material 100 in the powder material is typically nano to millimeter size, for example, 0.05 μm or more, preferably 0.1 μm or more, 0.2 μm or more, or 0.5 μm or more. The average particle size of the composite material 100 in the powder material is not particularly limited, but is, for example, 1000 μm or less, preferably 100 μm or less, 50 μm or less, or 10 μm or less. In this specification, the "average particle size" refers to the particle size obtained by the arithmetic average of circle equivalent diameters obtained by image analysis of at least 100 particles in an image obtained using an optical microscope or a scanning electron microscope (SEM).

[0044] The composite material 100 disclosed herein is provided with a functional group (typically a hydroxyl group) on the surface due to the modifying effect of the oxide ceramics 20 (thereby improving wettability with other materials). Therefore, in some preferred embodiments, an abrasive containing the composite material 100 is provided. When the composite material 100 is used as an abrasive, the substrate 10 typically plays a role as so-called abrasive grains having the function of directly grinding a workpiece.

[0045] For example, a grinding wheel can be obtained by mixing an abrasive and a binder (typically, vitrified bond, resin bond, etc.) and firing the mixture. Conventionally, diamond and cubic nitride ceramics are preferably used as the abrasive grains contained in such abrasives. However, when these are used as they are, their affinity with the binder is low, so that a network with the binder is not formed well, and sufficient grinding wheel strength and abrasive grain retention are not obtained. Here, by using the composite material 100 according to this embodiment as an abrasive, the wettability of the abrasive grains in the abrasive and the binder can be increased. As a result, a network with the binder that bonds a plurality of abrasive grains to each other is preferably formed. Therefore, the abrasive containing the composite material 100 disclosed herein can provide a grinding wheel with a preferably improved grinding wheel strength.

[0046] When the entire abrasive is taken as 100 wt%, the abrasive may contain, for example, 80 wt% or more of composite material 100, preferably 85 wt% or more of composite material 100, more preferably 90 wt% or more of composite material 100, even more preferably 95 wt% or more of composite material 100, and particularly preferably 98 wt% or more or 99 wt% or more of composite material 100.

[0047] When the composite material 100 is used as an abrasive, the shape and average particle size of the composite material 100 can be appropriately determined according to the purpose and mode of use of the grindstone. The shape of the composite material 100 is not particularly limited, and may be, for example, spherical, plate-like, or irregular. For example, when the composite material 100 is used as an abrasive, the average particle size of the composite material 100 may be about 0.1 μm or more and 1000 μm or less, and is preferably about 1 μm or more and 100 μm or less. In addition, although not particularly limited, when the composite material 100 is used as an abrasive, the average aspect ratio (major axis / minor axis ratio) of the composite material 100 is preferably 1 or more and 2 or less, and more preferably 1.1 or more and 1.8 or less.

[0048] The applications of the composite material disclosed herein are not particularly limited, but the composite material can be suitably used in applications requiring wettability between the composite material and other materials, such as inorganic materials for heat dissipation components (e.g., heat dissipation sheets for electronics applications) and as abrasives.

[0049] The method for producing the composite material disclosed herein will be described below. The method for producing the composite material disclosed herein typically includes a resinate attachment step and a resinate decomposition step in this order. However, the method is not limited to this and may include other steps. Here, the method further includes a material preparation step prior to the resinate attachment step. Each step will be described below.

[0050] (1) Material preparation process In the material preparation step, a resinate containing a metal or metalloid as a raw material for the oxide ceramic, a non-oxide ceramic or diamond as a substrate, and a solvent are prepared. Note that the non-oxide ceramic and diamond are similar to those in the composite material described above, and therefore a description thereof will be omitted here.

[0051] The average particle size of the non-oxide ceramic or diamond prepared in the material preparation step is not particularly limited, but is, for example, 0.05 μm or more, preferably 0.1 μm or more, 0.2 μm or more, or 0.5 μm or more. The average particle size of the non-oxide ceramic or diamond is not particularly limited, but is, for example, 1000 μm or less, preferably 100 μm or less, 50 μm or less, or 10 μm or less.

[0052] The resinate may be a conventionally known organometallic compound resinate containing at least one element selected from the group consisting of Al, Si, Zr, Ti, Ce, Y, Fe, and Zn. In addition, the resinate is preferably one that forms at least one compound selected from the group consisting of alumina, silica, zirconia, titania, ceria, yttria, iron oxide, zinc oxide, and zeolite in the resinate decomposition step described below. More preferably, the resinate contains a compound that forms a mixture or composite oxide selected from the group consisting of amorphous alumina, γ-alumina, amorphous silica, and amorphous zirconia. This allows the resinate to be formed into an oxide ceramic, which is an aggregate of a plurality of particles having a suitable porous structure, and to be attached to the surface of the substrate in the resinate decomposition step described below.

[0053] The metal or metalloid component contained in the resinate is the same as that of the oxide ceramic of the composite material described above, and therefore the description is omitted here. The content of the metal or metalloid component in the resinate may be 70 wt% or less, and preferably 60 wt% or less, 50 wt% or less, 40 wt% or less, or 30 wt% or less, in terms of oxide ceramics. As a result, the content of the metal or metalloid component in the resinate is low, and the oxide ceramics preferably forms a porous structure. On the other hand, the content of the metal or metalloid component in the resinate may be 2 wt% or more, and preferably 5 wt% or more, or 10 wt% or more, in terms of oxide ceramics.

[0054] The thermal decomposition temperature of the resinate is not particularly limited, but may be 150° C. or higher in the air, and is preferably 200° C. or higher, 300° C. or higher, or 400° C. or higher. The thermal decomposition temperature of the resinate may be 1000° C. or lower in the air, and is preferably 900° C. or lower, 800° C. or lower, or 700° C. or lower.

[0055] The solvent prepared in the material preparation step may be an aqueous solvent or an organic solvent. As the aqueous solvent, water (e.g., pure water, deionized water, etc.) or a mixed solution mainly made of water (e.g., a mixed solution of water and a lower alcohol) can be used. In this specification, a "mixed solution mainly made of water" refers to a mixed solution in which 50 vol% or more of the mixed solution is water. On the other hand, as the organic solvent, alcohols such as methanol and ethanol, ketones such as acetone and methyl ketone, esters such as ethyl acetate, etc. can be used.

[0056] (2) Resinate attachment process In the resinate attachment step, the resinate containing the oxide ceramic prepared in the material preparation step is attached to the non-oxide ceramic or diamond substrate. Here, the sub-steps include (2-1) a mixing step and (2-2) a drying step.

[0057] (2-1) Mixing process In the mixing step, the resinate containing the oxide ceramic, the non-oxide ceramic or diamond as the substrate, and the solvent are mixed together to obtain a mixture in which the resinate and the substrate are uniformly present in the solvent.

[0058] In the mixing step, a conventionally known stirring device, mixing device, etc. may be used. The mixing time in the mixing step is not particularly limited as long as the resinate and the base material are uniformly present in the mixture. After the mixing step, a dispersion treatment such as ultrasonic dispersion may be performed to more suitably homogenize each component in the mixture.

[0059] The concentration of the substrate part in the mixture is not particularly limited, but if the concentration is too low, it is not preferable from the viewpoint of cost balance. Therefore, the concentration of the substrate part in the mixture is, for example, 10 g / l or more, preferably 100 g / l or more, or 300 g / l or more. On the other hand, if the concentration of the substrate part is too high, there is a risk of the composite material agglomerating. Therefore, the concentration of the substrate part in the mixture is, for example, 50000 g / l or less, preferably 10000 g / l or less, or 3000 g / l or less.

[0060] When the oxide ceramics in the resinate are converted, the ratio (wt%) of the oxide ceramics to the total amount of the oxide ceramics and the substrate in the mixture is preferably 0.1 wt% or more, 0.2 wt% or more, 0.3 wt% or more, 0.5 wt% or more, or 1 wt% or more. The ratio (wt%) of the oxide ceramics to the total amount of the oxide ceramics and the substrate in the mixture is preferably 30 wt% or less, 20 wt% or less, 15 wt% or less, 10 wt% or less, 5 wt% or less, or 3 wt% or less. If the ratio is too low, the oxide ceramics for expressing the functional group increasing effect may not be attached to the substrate. On the other hand, if the ratio is too high, the oxide ceramics may be excessively attached to the substrate, suppressing the expression of the characteristics of the substrate.

[0061] (2-2) Drying process In the drying step, the mixture obtained in the mixing step is dried to remove the solvent in the mixture, thereby obtaining a dried product having the resinate adhered to the surface of the base material.

[0062] In the drying step, a conventionally known drying means may be used, for example, a hot air dryer, a low-humid air dryer, a vacuum dryer, various infrared dryers, an electromagnetic induction dryer, a microwave dryer, dry air, etc., or drying promotion means such as air blowing, decompression, heating, etc., may be used alone or in combination. Such means may be appropriately selected depending on the type and amount of the solvent in the mixture.

[0063] The drying temperature in the drying step (such as the set temperature of the drying device) may be appropriately selected depending on the type and amount of the solvent in the mixture, and may be set to, for example, 60° C. to 150° C., typically 80° C. to 120° C. The drying time may also be appropriately selected depending on the type and amount of the solvent in the mixture, and is not particularly limited.

[0064] (3) Resinate decomposition process In the resinate decomposition step, the resinate in the dried material obtained in the drying step is decomposed. As a result, oxide ceramics are generated as a resinate decomposition product, which is an aggregate of multiple particles having a porous structure. Here, the resinate decomposition step (thermal decomposition of the resinate) is performed by heat treatment. The dried material may be crushed before the resinate decomposition step. This operation can more effectively suppress the aggregation of the composite material after the resinate decomposition step.

[0065] The temperature of the heat treatment in the resinate decomposition step is preferably 800°C or less, 780°C or less, 750°C or less, 720°C or less, or 700°C or less. In this temperature range, sintering of the oxide ceramics is suitably suppressed, and the specific surface area of ​​the oxide ceramics is increased. In other words, the oxide ceramics is suppressed from becoming non-porous, and an oxide ceramics that is an aggregate of multiple particles having a porous structure can be obtained. On the other hand, the lower limit of the heat treatment temperature is not particularly limited as long as it is equal to or higher than the decomposition temperature of the resinate, and is, for example, 200°C or more, and preferably 250°C or more, 300°C or more, or 350°C or more.

[0066] The atmosphere in the resinate decomposition step is not particularly limited as long as it can decompose the resinate. However, from the viewpoint of suitably removing organic component-derived residues (e.g., carbon, etc.) from the composite material, it is preferable to carry out the step in an oxidizing atmosphere (e.g., air, etc.).

[0067] The time for which the heat treatment is held at the top temperature in the resinate decomposition step is not particularly limited as long as the resinate can be completely decomposed, but the heat treatment can be carried out for, for example, about 0.1 to 2 hours.

[0068] After the heat treatment, the obtained composite material may be subjected to a crushing treatment. This makes the composite material in a powder form. Therefore, the obtained composite material can be suitably used as a powder material. The method for crushing the composite material in the crushing step is not particularly limited, and a conventionally known method can be used.

[0069] As described above, specific aspects of the technology disclosed herein include those described in the following sections.

[0070] Item 1: A composite material comprising a non-oxide ceramic or diamond, and a metal or semi-metal oxide ceramic attached to a surface of the non-oxide ceramic or diamond, wherein the oxide ceramic is an aggregate of a plurality of particles, the oxide ceramic has pores between the particles, and the maximum peak pore diameter in a differential pore volume distribution of the oxide ceramic calculated by a non-localized density functional (NLDFT) method is 5 nm or less.

[0071] Item 2: The pore surface area per unit mass of the oxide ceramics when the pore diameter of the oxide ceramics is 5 nm or less is 10 m 2 Item 2. The composite material according to item 1, wherein the elastic modulus is 1 / g or more.

[0072] Item 3: The composite material according to item 1 or 2, wherein the ratio of the surface area of ​​pores having a pore diameter of 2 nm or less to the surface area of ​​pores having a pore diameter of 10 nm or less in the oxide ceramic is 30% or more.

[0073] Item 4: The composite material according to any one of Items 1 to 3, wherein the oxide ceramic contains at least one compound selected from the group consisting of alumina, silica, zirconia, titania, ceria, yttria, iron oxide, zinc oxide, and zeolite.

[0074] Item 5: The composite material according to any one of Items 1 to 4, wherein the oxide ceramic contains a mixture or composite oxide selected from the group consisting of amorphous alumina, γ-alumina, amorphous silica, and amorphous zirconia.

[0075] Item 6: The composite material according to any one of Items 1 to 5, wherein the non-oxide ceramic is a nitride ceramic.

[0076] Item 7: The composite material according to item 6, wherein the nitride ceramic contains at least one compound selected from the group consisting of aluminum nitride and boron nitride.

[0077] Item 8: The composite material according to any one of Items 1 to 7, wherein when a separate phase of water and a nonpolar solvent is stirred with the composite material, 70 wt % or more of the composite material is present in the aqueous phase.

[0078] Item 9: A powder material comprising the composite material according to any one of items 1 to 8 in powder form.

[0079] Item 10: The composite material according to any one of items 1 to 9, which is a filler of a resin material.

[0080] Item 11: An abrasive comprising the composite material according to any one of items 1 to 10.

[0081] Item 12: A method for producing a composite material comprising a non-oxide ceramic or diamond and a metal or semi-metal oxide ceramic attached to the surface of the non-oxide ceramic or diamond, comprising the steps of: attaching a resinate containing a metal or semi-metal that is a raw material for the oxide ceramic to the non-oxide ceramic or diamond; and decomposing the resinate; wherein in the composite material, the oxide ceramic is an aggregate of a plurality of particles, and pores are present between the particles of the oxide ceramic; and the maximum peak pore size in the differential pore volume distribution of the oxide ceramic obtained by a non-localized density functional (NLDFT) method is 5 nm or less.

[0082] Item 13: The method for producing a composite material according to Item 12, wherein in the decomposition step, heat treatment is performed at 800° C. or less.

[0083] Test examples relating to the technology disclosed herein will be described below, but such test examples are not intended to limit the technology.

[0084] <Preparation of evaluation samples> In this test example, evaluation samples according to the following Examples 1 to 15 were prepared.

[0085] (Example 1) First, 10 ml of ethanol was added to 7.0 g (0.5 g in terms of silica) of an ethanol solution of tris(2-ethylhexanoic acid)ethoxysilane as a resinate (7.15 wt% in terms of silica, thermal decomposition temperature in air 350°C) and dissolved. 9.5 g of nonporous boron nitride powder (Tokuyama Corporation, S03) was added thereto and stirred. Then, a dispersion treatment was performed for 2 minutes using an ultrasonic cleaner to obtain a slurry-like mixture. The mixture was dropped with a dropper onto a release film placed on a hot plate at 80°C and dried. Furthermore, the release film was placed in a vacuum oven at 120°C and dried in the vacuum oven for 1 hour to obtain a dried product. The obtained dried product was lightly crushed in a mortar. After that, the dried product was fired in an air atmosphere at a temperature of 400°C, at a heating rate of 10°C / min, and for 0.5 hours to perform resinate decomposition. This resulted in a composite material in which 5 wt % of amorphous silica particles were attached to boron nitride. The composite material thus obtained was crushed in a mortar to obtain a powdered composite material as an evaluation sample according to Example 1.

[0086] (Example 2) The procedure was the same as in Example 1, except that the dried product was fired in an air atmosphere at a temperature of 700°C, at a heating rate of 5°C / min for 1 hour. As a result, a powdered composite material was obtained as an evaluation sample according to Example 2, in which 5 wt% of amorphous silica particles were attached to boron nitride.

[0087] (Example 3) The procedure was the same as in Example 2, except that silicon resinate (Si 13%, silica equivalent 27.8 wt%, decomposition temperature in air 617°C) was used as the Si resinate, and 12 ml of ethanol was added to 1.80 g of the Si resinate (silica equivalent 0.5 g) and dissolved. As a result, a powdered composite material was obtained as an evaluation sample according to Example 3, in which 5 wt% of amorphous silica particles were attached to the boron nitride.

[0088] (Example 4) The procedure was the same as in Example 3, except that 0.36 g of Si resinate (0.1 g in terms of silica) and 9.9 g of boron nitride powder were used. This resulted in a powdered composite material as an evaluation sample according to Example 4, in which 1 wt% of amorphous silica particles were attached to the boron nitride.

[0089] (Example 5) The procedure was the same as in Example 3, except that 0.72 g of Si resinate (0.2 g in terms of silica) and 9.8 g of boron nitride powder were used. This resulted in a powdered composite material as an evaluation sample for Example 5, in which 2 wt% of amorphous silica particles were attached to the boron nitride.

[0090] (Example 6) The procedure was the same as in Example 3, except that 3.60 g of Si resinate (1.0 g in terms of silica) and 9.0 g of boron nitride powder were used. This resulted in a powdered composite material as an evaluation sample according to Example 6, in which 10 wt% of amorphous silica particles were attached to the boron nitride.

[0091] (Example 7) First, 12 ml of ethanol was added to 1.08 g (0.2 g in terms of alumina) of aluminum ethyl acetoacetate diisopropylate (ALCH, manufactured by Kawaken Fine Chemicals) (18.47 wt% in terms of alumina, decomposition temperature in air 295°C) as Al resinate, and dissolved. 19.8 g of non-porous aluminum nitride powder (HF-01D, manufactured by Tokuyama Corporation) was added thereto and stirred. Then, dispersion treatment was performed for 2 minutes using an ultrasonic cleaner to obtain a slurry-like mixture. The mixture was dropped with a dropper onto a release film placed on a hot plate at 80°C and dried. Furthermore, the release film was placed in a vacuum oven at 120°C and dried in the vacuum oven for 1 hour to obtain a dried product. The obtained dried product was lightly crushed in a mortar. After that, the dried product was fired in an air atmosphere at a temperature of 400°C, at a heating rate of 10°C / min, and for 0.5 hours to perform resinate decomposition. As a result, a composite material in which 1 wt % of amorphous alumina particles were attached to aluminum nitride was obtained. The obtained composite material was crushed in a mortar to obtain a powdered composite material as an evaluation sample according to Example 7.

[0092] (Example 8) The procedure was the same as in Example 7, except that 5.4 g of Al resinate (1.0 g in terms of alumina) and 19.0 g of aluminum nitride powder were used. This resulted in a powdered composite material as an evaluation sample for Example 8, in which 5 wt% of amorphous alumina particles were attached to the aluminum nitride.

[0093] (Example 9) The powdered composite material according to Example 8, which had been fired and crushed, was further fired in an air atmosphere at a temperature of 650°C, at a heating rate of 10°C / min, for 0.5 hours. This resulted in a composite material in which 5 wt% of γ-alumina particles were attached to aluminum nitride. The resulting composite material was crushed in a mortar to obtain a powdered composite material as an evaluation sample according to Example 9.

[0094] (Example 10) First, 25 g of ethanol was added to 1.06 g (0.076 g in terms of silica) of an ethanol solution of tris(2-ethylhexanoic acid)ethoxysilane as a resinate (7.15 wt% in terms of silica, thermal decomposition temperature in air 350°C) and dissolved. 20 g of non-porous diamond powder (manufactured by Global Diamond Co., Ltd., FRM-DN 4-6) was added thereto and stirred. Then, a dispersion treatment was performed for 2 minutes using an ultrasonic cleaner to obtain a slurry-like mixture. The mixture was dropped with a dropper onto a release film placed on a hot plate at 80°C and dried. Furthermore, the release film was placed in a vacuum oven at 80°C and dried in the vacuum oven for 1 hour to obtain a dried product. The obtained dried product was lightly crushed in a mortar. After that, the dried product was fired in an air atmosphere at a temperature of 600°C, a heating rate of 10°C / min, and 0.5 hours to perform resinate decomposition. This resulted in a composite material in which 0.38 wt% of amorphous silica particles were attached to the diamond. The composite material thus obtained was then crushed in a mortar to obtain a powdered composite material as an evaluation sample according to Example 10.

[0095] (Example 11) First, 25 g of ethanol was added to 0.62 g (0.115 g in terms of alumina) of aluminum ethyl acetoacetate diisopropylate (Kawaken Fine Chemicals, ALCH) (18.47 wt% in terms of alumina, decomposition temperature in air 295°C) as Al resinate, and dissolved. 20 g of non-porous diamond powder (FRM-DN 4-6, Global Diamond Co., Ltd.) was added thereto and stirred. Then, dispersion treatment was performed for 2 minutes using an ultrasonic cleaner to obtain a slurry-like mixture. The mixture was dropped with a dropper onto a release film placed on a hot plate at 80°C and dried. Furthermore, the release film was placed in a vacuum oven at 80°C and dried in the vacuum oven for 1 hour to obtain a dried product. The obtained dried product was lightly crushed in a mortar. After that, the dried product was fired in an air atmosphere at a temperature of 600°C, a heating rate of 10°C / min, and 0.5 hours to perform resinate decomposition. This resulted in a composite material in which 0.57 wt% of γ-alumina particles were attached to the diamond. The composite material thus obtained was crushed in a mortar to obtain a powdered composite material as an evaluation sample according to Example 11.

[0096] (Example 12) The procedure was the same as in Example 1, except that the dried product was fired in an air atmosphere at a temperature of 900° C., at a heating rate of 5° C. / min for 1 hour. This resulted in a powdered composite material as an evaluation sample according to Example 12 in which 5 wt % of amorphous silica was attached to boron nitride.

[0097] (Example 13) The boron nitride powder (S03, manufactured by Tokuyama Corporation) used in Example 1 was used as an evaluation sample without adhering oxide ceramics.

[0098] (Example 14) The aluminum nitride powder (HF-01D, manufactured by Tokuyama Corporation) used in Example 7 was used as it was as an evaluation sample without adhering oxide ceramics.

[0099] (Example 15) The diamond powder (FRM-DN 4-6, manufactured by Global Diamond Co., Ltd.) used in Example 10 was used as an evaluation sample as it was, without adhering oxide ceramics.

[0100] <Evaluation test> The above composite material was subjected to the following evaluation tests.

[0101] (1) Pore analysis Each sample was pretreated in a vacuum at 250°C for 1 hour, and then subjected to a specific surface area measurement device (model number: Belsorp-max (registered trademark)) manufactured by Microtrack-Bell, Inc., to obtain a nitrogen adsorption isotherm at -196°C. The following analysis was then performed using analysis software (BELLMaster Version 7.3.2.0).

[0102] (1-1) Specific surface area analysis by BET method In each of Examples 1 to 12, the specific surface area of ​​the substrate (non-oxide ceramic or diamond) was analyzed by the BET method using the above-mentioned analysis software. 2 / g, the weight of oxide ceramics attached per unit BET surface area of ​​the substrate (g / m 2 ) and the deposition volume of oxide ceramics per unit BET surface area of ​​the substrate (nm 3 / nm 2 ) was calculated. Similarly, the BET specific surface area of ​​the substrate in Examples 13 to 15 measured by this method was taken as the value of the boron nitride powder, aluminum nitride powder, and diamond used in each Example. The BET specific surface area values ​​of the boron nitride powder, aluminum nitride powder, and diamond used in each Example were 1.3 m 2 / g, 3.2m 2 / g, 1.0m 2 / g. The densities of the attached oxide ceramics, amorphous alumina, γ-alumina, and amorphous silica, were 3.0 g / cm3, respectively. 3 , 3.7g / cm 3 , 2.2g / cm 3The results are shown in Table 1.

[0103] [Table 1]

[0104] (1-2) Pore volume analysis using NLDFT method In each of Examples 1 to 12, the pore size distribution was created under the following conditions using the above-mentioned analysis software. Curve Interpolation: Cubic Spline Curve Model: Cylinder Adsorbent: Metal oxide Fitting method: Tikhonov normalization, smoothing Using the obtained pore size distribution, the pore volume (cm) per unit mass of the composite material with pore sizes of 5 nm or less and 2 nm or less was calculated. 3 The pore volume per unit mass of the oxide ceramics (cm 3 / g) and the pore volume per unit BET surface area of ​​the powder (cm) consisting of the substrate in the composite material. 3 / m 2 ) was also calculated. Furthermore, the pore diameter of the maximum peak in the differential pore volume distribution was calculated. In Example 12, the obtained nitrogen adsorption isotherm was analyzed by the above-mentioned analysis software. s As a result of the analysis using the method, α s There was no clear inflection in the plot, so a second straight line could not be created. Therefore, Example 12 was determined to be non-porous, and is shown by a line. The results are shown in Table 1.

[0105] (1-3) Pore surface area analysis using NLDFT method In each of Examples 1 to 11, the pore surface area (m ) per unit mass of the composite material with pore sizes of 10 nm or less, 5 nm or less, 2 nm or less, and 1 nm or less was calculated using the pore size distribution obtained by the analysis in (1-2) above. 2 The pore surface area per unit mass of the oxide ceramics (m 2 / g) and the pore surface area per powder unit BET surface area (m2 / m 2 The results are shown in Table 2.

[0106] [Table 2]

[0107] As shown in Table 1, in Examples 1 to 11, the BET specific surface area of ​​the substrate in the composite material after the oxide ceramic was attached was increased compared to the BET specific surface area of ​​the substrate before the oxide ceramic was attached. On the other hand, in Example 12, the BET specific surface area of ​​the substrate in the composite material (here, boron nitride as a non-oxide ceramic) before the oxide ceramic was attached was 1.3 m 2 / g, while the BET specific surface area of ​​the substrate in the composite material after oxide ceramic deposition was 1.6 m 2 / g, there was little increase in the specific surface area before and after the attachment of the oxide ceramic. In addition, when comparing Example 1 and Example 12, the BET specific surface area of ​​the substrate in Example 12 was smaller than that of Example 1, even though the weight of the oxide ceramic attached was the same. This suggests that in Example 12, the oxide ceramic attached to the substrate (boron nitride as a non-oxide ceramic) was non-porous.

[0108] As shown in Table 1, it was confirmed that in all of Examples 1 to 11, the maximum peak pore diameter in the differential pore volume distribution of the oxide ceramics was 5 nm or less. Furthermore, in observations using a field emission scanning electron microscope (FE-SEM) described below, it was confirmed that the oxide ceramics existed as an aggregate of multiple particles in Examples 1 to 11 (see Figures 2 to 6), which revealed that in Examples 1 to 11, the oxide ceramics constituting the composite material were relatively densely assembled as an aggregate of multiple particles with small particle diameters. Therefore, it is considered that in the composite materials of Examples 1 to 11, functional groups are imparted to the surface of the substrate, and the surface is suitably modified. On the other hand, in Example 12, as described above, α s Analysis by the method confirmed that the material was non-porous.

[0109] As shown in Table 2, in each of Examples 1 to 11, the pore surface area per unit mass of the oxide ceramics in which the pore diameter of the oxide ceramics is 5 nm or less is 10 m 2 / g or more. This also supports the idea that in the composite materials according to Examples 1 to 11, the oxide ceramic is present as an aggregate of a plurality of particles.

[0110] Furthermore, as shown in Table 2, in Examples 1 to 11, the ratio of the surface area of ​​pores in the composite material with a pore diameter of 2 nm or less to the surface area of ​​pores in the composite material with a pore diameter of 10 nm or less (the item "2 nm or less / 10 nm or less" in Table 2) was 30% or more in all examples. This shows that, among the fine pores of 10 nm or less, the proportion of even finer pores of 2 nm or less is high in the pores in the composite materials of Examples 1 to 11. This also supports the idea that the oxide ceramics constituting the composite material are relatively densely assembled as an aggregate of multiple particles with small particle diameters.

[0111] (2) Water-nonpolar solvent preference evaluation For each of Examples 1 to 9 and Examples 12 to 14, approximately 200 mg of sample was placed in a glass bottle, 20 ml of pure water was added, the bottle was capped, and the bottle was shaken by hand. The bottle was then opened, 20 ml of n-hexane as a non-polar solvent was added, the bottle was capped again, and the bottle was shaken by hand. The glass bottle was then left to stand, and it was visually confirmed whether the majority of the sample (i.e., 70% or more) was present in the water phase or the non-polar solvent phase (hexane phase). For Examples 8 to 9 and 14, evaluation was performed in the same manner as described above, except that n-decane was used instead of n-hexane. The results are shown in Table 3.

[0112] [Table 3]

[0113] As shown in Table 3, it was confirmed that the majority of all samples in Examples 1 to 9 existed in the aqueous phase. This shows that the surface of the substrate was modified by the oxide ceramics, that is, the oxide ceramics were attached to a certain amount of the substrate surface (non-oxide ceramics in this case). On the other hand, it was confirmed that the majority of the samples in Examples 12 and 13 existed in the non-polar solvent phase. Note that in Example 14, the sample was present throughout the solvent when visually observed, and the boundary between the aqueous phase and the non-polar solvent phase (n-decane phase) in which the majority was present was unclear, so it was classified as "unclear."

[0114] (3) Surface morphology observation Each of Examples 1 to 15 was observed using a field emission scanning electron microscope (FE-SEM) manufactured by Hitachi High-Technologies Corporation. Backscattered electron images of some of the Examples are shown in Figures 2 to 9. Figure 2 is an FE-SEM image (50,000x) of Example 1. Figure 3 is an FE-SEM image (50,000x) of Example 2. Figure 4 is an FE-SEM image (50,000x) of Example 3. Figure 5 is an FE-SEM image (100,000x) of Example 8. Figure 6 is an FE-SEM image (100,000x) of Example 9. Figure 7 is an FE-SEM image (50,000x) of Example 12. Figure 8 is an FE-SEM image (50,000x) of Example 13. Figure 9 is an FE-SEM image (100,000x) of Example 14.

[0115] As shown in Figs. 8 and 9, the non-oxide ceramics (substrate) of Examples 13 and 14 in which no oxide ceramics are arranged have no irregularities on the surface, and are confirmed to be non-porous. Although illustrations are omitted here, the diamond (substrate) of Example 15 in which no oxide ceramics are arranged has no irregularities on the surface, and is confirmed to be non-porous. On the other hand, as shown in Figs. 2 to 6, in Examples 1 to 3, 8 and 9, fine irregularities were observed on the surface of the composite material, and it was confirmed that the oxide ceramics were attached to the surface of the substrate as an aggregate of multiple particles and had a porous structure, and similarly, the surface exposure of the substrate was confirmed. Furthermore, although illustrations are omitted here, the adhesion of the oxide ceramics as an aggregate of multiple particles, the formation of pores, and the surface exposure of the substrate were confirmed in Examples 4 to 7 and Examples 10 to 11. In Examples 1 to 11, by having a portion where the substrate is exposed on a part of the surface of the composite material, the characteristics of the substrate, for example, thermal conductivity, can be suitably expressed from the exposed portion.

[0116] As shown in FIG. 7, in Example 12, in which the oxide ceramics were highly densified, it was confirmed that the oxide ceramics were spheroidized on the (0001) surface (FIG. 7) of the non-oxide ceramics (boron nitride), which is stable and has few functional groups. This is believed to be because the oxide ceramics were repelled by the (0001) surface of the boron nitride during the densification process by sintering the oxide ceramics, resulting in the spheroidized form shown in FIG. 7. When the oxide ceramics exist in a spheroidized state as shown in FIG. 7, the oxide ceramics tend to easily fall off from the surface of the substrate. On the other hand, in Example 12, it was confirmed that the oxide ceramics were concentrated in a band shape on the end surface of the non-oxide ceramics (lower right of FIG. 7). This is believed to be because the end surface of the boron nitride constituting the non-oxide ceramics is an area with many functional groups compared to the (0001) surface, and has a high affinity with the oxide ceramics. In addition, when the oxide ceramics are concentrated on the end surface of the substrate, as shown in Example 12 (FIG. 7), it is not preferable because it inhibits the expression of the characteristics of the substrate (especially thermal conductivity). Moreover, the surface of the substrate becomes excessively exposed, which is undesirable since it reduces the effect of surface modification.

[0117] (4) Three-point bending strength evaluation 9g of the composite material of Example 10 or Example 11 or the diamond powder of Example 15 as the abrasive (abrasive grain), 10.6g of vitrified raw powder (TOMATEC Corporation, TMX-501F Bi2O3-ZnO-B2O3-SiO2-based glass), 0.14g of pore former (Sekisui Chemical Co., Ltd., Techpolymer MB30X-8Y), 4g of binder (Kyoeisha Chemical Co., Ltd., Oricox #2435E), and 1.5g of ethanol were mixed using a mixer (Thinky Corporation, Awatori Rentaro AR-550L-2) to form a paste. This was dried at 100°C for 4 hours, and then crushed in a mortar to obtain a grindstone clay. Five molded bodies of 55mm x 6.5mm x 4mm were produced by pressing 3.0g of this clay. These were heated to 400°C in air over 5 hours, held for 2 hours, further heated to 570°C over 1 hour 40 minutes, held for 2 hours, and then cooled to room temperature over 4 hours. As a result, five rectangular grindstone test pieces for each of Examples 10, 11, and 15 were obtained. Using the grindstone test pieces for Examples 10, 11, and 15, a three-point bending test was performed on the grindstone test pieces to measure bending strength. Note that the test machine used was EZTest (manufactured by Shimadzu Corporation), and the measurement was performed under the conditions of a distance between lower supports: 30 mm, and a speed: 0.5 mm / min. In addition, the three-point bending strength measurement was performed on five grindstone test pieces for each example (i.e., n=5), and the arithmetic average value was calculated. The results are shown in Table 4.

[0118] [Table 4]

[0119] As shown in Table 4, comparing Examples 10, 11, and 15, Examples 10 and 11, in which oxide ceramics were attached to the diamond surface, showed better results in three-point bending strength than Example 15, in which oxide ceramics were not attached. As mentioned above, in the abrasives used in Examples 10 and 11, the diamond surface was modified by the oxide ceramics attached to the diamond surface. This is thought to have improved the wetting of the abrasive grains (diamond) and the vitrified bond, favorably forming a network that bonds the abrasive grains and the vitrified bond, and improving the three-point bending strength of the grinding wheel.

[0120] Although specific examples of the present disclosure have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and alterations of the specific examples exemplified above. [Explanation of symbols]

[0121] 10 Base material part 11 Pore 12 Surface exposure 20 Oxide Ceramics 100 Composite materials

Claims

1. 1. A composite material comprising a non-oxide ceramic or diamond and a metal or metalloid oxide ceramic attached to a surface of the non-oxide ceramic or diamond, The oxide ceramic is an aggregate of a plurality of particles, The oxide ceramic has pores between the particles, The maximum peak pore diameter in the differential pore volume distribution of the oxide ceramics obtained by a nonlocalized density functional (NLDFT) method is 5 nm or less; Composite material.

2. The pore surface area per unit mass of the oxide ceramics when the pore diameter of the oxide ceramics is 5 nm or less is 10 m 2 / g or more; 2. The composite material of claim 1.

3. The ratio of the surface area of ​​pores having a pore diameter of 2 nm or less to the surface area of ​​pores having a pore diameter of 10 nm or less of the oxide ceramics is 30% or more.

3. A composite material according to claim 1 or 2.

4. The oxide ceramic contains at least one compound selected from the group consisting of alumina, silica, zirconia, titania, ceria, yttria, iron oxide, zinc oxide, and zeolite.

3. A composite material according to claim 1 or 2.

5. The oxide ceramic comprises a mixture or composite oxide selected from the group consisting of amorphous alumina, γ-alumina, amorphous silica, and amorphous zirconia; 3. A composite material according to claim 1 or 2.

6. The non-oxide ceramic is a nitride ceramic.

3. A composite material according to claim 1 or 2.

7. The nitride ceramic contains at least one compound selected from the group consisting of aluminum nitride and boron nitride.

7. The composite material of claim 6.

8. 3. The composite material according to claim 1, wherein when the composite material is mixed with a separate phase of water and a non-polar solvent, 70 wt % or more of the composite material is present in the aqueous phase.

9. The composite material according to claim 1 or 2 is in powder form. powder material.

10. A filler for resin materials, 3. A composite material according to claim 1 or 2.

11. The composite material according to claim 1 or 2 is included. Abrasive material.

12. 1. A method for producing a composite material comprising a non-oxide ceramic or diamond and a metal or metalloid oxide ceramic attached to a surface of the non-oxide ceramic or diamond, comprising the steps of: a step of depositing a resinate containing a metal or metalloid that is a raw material for the oxide ceramic onto the non-oxide ceramic or the diamond; and decomposing the resinate, In the composite material, the oxide ceramic is an aggregate of a plurality of particles, The oxide ceramic has pores between the particles, The maximum peak pore diameter in the differential pore volume distribution of the oxide ceramics obtained by a nonlocalized density functional (NLDFT) method is 5 nm or less; Manufacturing methods for composite materials.

13. In the decomposition step, heat treatment is performed at 800° C. or less. A method for producing the composite material according to claim 12.

Citation Information

Patent Citations

  • Surface-covered cubic crystal boron nitride abrasive grain with excellent resistance to coming-off for use on vitrified bond grinding wheel

    JP1995108461A

  • Metal nitride particle coated with silica, and manufacturing method thereof

    JP2015101510A