Ground glass-like heat-regulating thermoplastic molded product
A thermoplastic resin molded product with a silicate particle coating layer integrated through extrusion molding addresses the challenge of maintaining transparency and achieving a matte feel and frosted glass appearance.
Patent Information
- Application Number
- JP2023067663
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-18
- Publication Date
- 2024-10-30
AI Technical Summary
Conventional molded products using spherical particles or fillers lose surface gloss while maintaining transparency, failing to impart a matte feel or frosted glass look effectively.
A thermoplastic resin molded product with a coating layer containing dispersed silicate particles, integrated with a substrate layer through extrusion molding, maintains transparency and achieves a frosted glass appearance.
The product eliminates surface gloss while retaining transparency, providing a good matte feel and a clear ground glass look.
Smart Images

Figure 2024154059000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermoplastic resin molded article having a ground-glass appearance. [Background technology]
[0002] Extrusion molded products having a ground-glass-like appearance are widely used, for example, for partitions, lighting covers, signs, etc. In general, they are obtained by extrusion molding in which specific fine particles are dispersed in a transparent resin and extruded into a sheet.
[0003] At this time, it is necessary to diffuse the fine particles dispersed in the transparent resin or to make them protrude from the sheet surface.
[0004] As a method for obtaining a ground-glass appearance in a plastic molded product, Patent Document 1 discloses a technology for eliminating the gloss of plastic and imparting a matte finish by using spherical fine particles with high heat resistance and a high refractive index. Patent Document 2 discloses that a polyester resin composition obtained by blending a spherical fine powder of polymethyl methacrylate and a fine powder of calcium carbonate with a polyester resin causes light diffusion in the molded product, resulting in a molded product with a ground-glass appearance.
[0005] Furthermore, Patent Document 3 proposes an acrylic laminate in which spherical fine particles having a volatile content of 1.5% or less are blended on one or both sides of a substrate made of an acrylic resin. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 01-297465 [Patent Document 2] Japanese Patent Application Publication No. 11-001606 [Patent Document 3] Patent Publication No. 2000-153586 Summary of the Invention [Problem to be solved by the invention]
[0007] However, in conventional molded products using spherical microparticles or fillers, it was not possible to sufficiently eliminate surface gloss and impart a matte or frosted glass feel while maintaining the transparency of acrylic resins, polyester resins, polystyrene resins, polycarbonate resins, and the like.
[0008] The present invention has been made in consideration of the above circumstances, and has an object to provide a thermoplastic resin molded article that can be imparted with a ground glass look while maintaining the transparency of the plastic. [Means for solving the problem]
[0009] The present invention includes the following inventions. [1] A ground-glass-like thermoplastic molded product having a coating layer on at least one main surface of a substrate layer containing a thermoplastic resin, the coating layer being made of a resin composition in which 100 parts by weight of thermoplastic resin (A) is dispersed with 0.1 to 10 parts by weight of silicate particles (B). [2] A ground-glass-like thermoplastic molded product according to [1], in which the substrate layer and the covering layer are laminated together by extrusion molding. [3] the thermoplastic resin substrate layer is at least one selected from the group consisting of polyethylene terephthalate resin, polystyrene resin, polymethyl methacrylate resin and polycarbonate resin; In the coating layer, the thermoplastic resin (A) is at least one resin selected from the group consisting of polyethylene terephthalate resin, polystyrene resin, polymethyl methacrylate resin, and polycarbonate resin; The ground-glass-like thermoplastic molded article according to [1], wherein the silicate of the silicate particles (B) is mica. [4] The ground-glass texture thermoplastic molded product according to [1], wherein the molded product has a thickness of 0.1 mm to 30 mm. [5] The ground-glass-like thermoplastic molded product according to [1], wherein the average particle size of the silicate is 10 μm or more. [6] The ground-glass-like thermoplastic molded product according to [1], wherein the amount of the silicate particles (B) is 0.2 to 7 parts by weight per 100 parts by weight of the thermoplastic resin (A) of the coating layer. [7] A thermoplastic resin; a resin composition in which 0.1 to 10 parts by weight of silicate particles (B) are dispersed in 100 parts by weight of a thermoplastic resin (A); A method for producing the ground glass texture thermoplastic molded article according to [1], comprising laminating and integrating the above. [8] A masterbatch for ground glass-like thermoplastic molded products, comprising 100 parts by weight of a thermoplastic resin (A) and 1 to 200 parts by weight of silicate particles (B). Effect of the Invention
[0010] According to the present invention, it is possible to eliminate surface gloss while maintaining the transparency of the resin, and to impart a good matte feel or a good ground glass texture to a molded article. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a schematic cross-sectional view of a ground-glass style thermoplastic molded article of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The ground glass thermoplastic molded article of the present invention has a coating layer on one or two main surfaces of the substrate layer. It is preferable that the coating layer is on two main surfaces. The thermoplastic molded article of the present invention is preferably in the form of a sheet, but may also have other shapes, such as complex shapes such as containers. The thermoplastic resin in the substrate layer and the thermoplastic resin in the coating layer are preferably the same, but may be different.
[0013] The thickness of the molded article may be 0.1 mm to 30 mm or 0.3 mm to 10 mm. The thickness of the molded article may be 0.2 mm or more, 0.4 mm or more, 0.6 mm or more, 0.8 mm or more, 1 mm or more, 1.2 mm or more, 1.4 mm or more, 1.6 mm or more, 1.8 mm or more, 2 mm or more, 2.2 mm or more, 2.4 mm or more, 2.6 mm or more, 2.8 mm or more, or 3 mm or more. The thickness of the molded article may be 25 mm or less, 20 mm or less, 15 mm or less, 12 mm or less, 10 mm or less, 9 mm or less, 8 mm or less, 7 mm or less, 6 mm or less, 5 mm or less, 4 mm or less, or 3.5 mm or less.
[0014] The molded article preferably has a total light transmittance of 55% or more, 60% or more, 65% or more, 70% or more, 75% or more, 80% or more, 85% or more, or 90% or more when the thickness is 2 mm to 5 mm (for example, 2 mm, 3 mm, 4 mm or 5 mm, particularly 3.0 mm). The total light transmittance may be 56% or more, 58% or more, 60% or more, 62% or more, 64% or more, 66% or more, 68% or more, 70% or more, 72% or more, 74% or more, 76% or more, 78% or more, 80% or more, 82% or more, 84% or more, 86% or more, 88% or more, 90% or more, 92% or more, or 94% or more. The total light transmittance may be 100% or less, 98% or less, 96% or less, 94% or less, 92% or less, 90% or less, or 88% or less.
[0015] The total light transmittance of the molded article can be measured in accordance with JIS K 7136: 2000. For the measurement, for example, a haze meter (model TC-H3DPK) manufactured by Tokyo Denshoku Co., Ltd. can be used. [Formula] Total light transmittance (Tt) = Linear transmittance (Tp) + Diffuse transmittance (Td)
[0016] The haze of the molded product may be 5-90, 10-85, 10-80, or 20-80, or 40-75. The haze of a molded product can be measured in accordance with JIS K 7136, for example, using a haze meter (model TC-H3DPK) manufactured by Tokyo Denshoku Co., Ltd. [Formula] HAZE=(Diffuse transmittance (Td) / Total light transmittance (Td))*100
[0017] The gloss of the molded article may be 10 or more, 20 or more, 30 or more, 40 or more, 50 or more, 60 or more, 70 or more, or 80 or more, and may be 150 or less, 140 or less, 130 or less, 120 or less, 110 or less, 100 or less, 90 or less, or 80 or less. It is preferable that the upper and lower main surfaces of the molded article have different gloss values, but the gloss values of the upper and lower main surfaces may be the same.
[0018] The gloss can be measured according to the gloss measurement method of JIS Z 8741: 1997. For measuring the gloss, for example, a GMX-202 model manufactured by Murakami Color Research Laboratory Co., Ltd. can be used.
[0019] FIG. 1 is a schematic cross-sectional view showing a ground-glass thermoplastic molded article of the present invention. The molded article 10 has coating layers 1 and 3 on each of the two main surfaces (i.e., the upper and lower surfaces) of the substrate layer 2. The coating layers 1 and 3 may be the same or different. For example, the coating layers 1 and 3 may have the same thickness, the same particle concentration, and / or the same surface (e.g., a matte surface). Alternatively, for example, the coating layers 1 and 3 may have different thicknesses, different particle concentrations, and / or different surfaces (e.g., one coating layer has a matte finish and the other coating layer has a glossy finish). The molded article may have only one coating layer (not shown).
[0020] The thickness of the substrate layer may be 0.1 to 50 mm, 0.2 to 30 mm, or 0.3 to 20 mm. The thickness of the coating layer may be 0.01 to 10 mm, 0.02 to 5 mm, 0.05 to 2 mm, or 0.1 to 1 mm. It is preferable that the total thickness of the coating layer is 40% or less, 30% or less, or 20% or less of the thickness of the molded article.
[0021] [Thermoplastic resin (hereinafter sometimes referred to as "resin")] Resins are used in the substrate layer and the cover layer, and preferably the resin in the substrate layer and the resin in the cover layer are the same, but they may be different.
[0022] Examples of the resin include acrylonitrile-butadiene-styrene resin, low-density polyethylene resin, high-density polyethylene resin, polystyrene resin, polypropylene resin, acrylonitrile-styrene resin, cellulose acetate resin, ethylene-vinyl acetate resin, acrylic-acrylonitrile-styrene resin, acrylic-chlorinated polyethylene resin, ethylene-vinyl alcohol resin, fluororesin, polymethyl methacrylate resin, polyacetal resin, polyamide resin, polyethylene terephthalate resin, polycarbonate resin, polysulfone resin, polyethersulfone resin, methylpentene resin, polyarylate resin, polybutylene terephthalate resin, resin containing an alicyclic structure-containing ethylenically unsaturated monomer unit (e.g., cycloolefin polymer resin), polyphenylene sulfide resin, polyphenylene oxide resin, polyether ether ketone resin, etc. The resin may be used alone or in combination of two or more kinds.
[0023] The resin is preferably a resin having excellent transparency and excellent moldability at a predetermined processing temperature, and more preferably a thermoplastic resin having a total light transmittance of 85% or more or 90% or more at a thickness of 3.0 mm. At least one resin selected from polyethylene terephthalate resin, polystyrene resin, polycarbonate resin, and polymethyl methacrylate resin is preferable. By using a thermoplastic resin having excellent transparency, the ground glass tone tends to become clearer. Two or more of these resins may be used in combination as long as the transparency and mechanical properties are not impaired.
[0024] [Silicate particles] The silicate particles (hereinafter sometimes referred to as "particles") are silicate particles. The silicate may be a hydrated silicate. Examples of the silicate include clay, mica, calcium silicate, glass (fibers, beads, etc.), etc. The silicate particles may be used alone or in combination of two or more kinds.
[0025] Examples of clays are calcined clay and kaolin clay. Examples of glasses are C-glass, D-glass, E-glass, S-glass, and T-glass.
[0026] The silicate is preferably mica. The mica may be natural mica or synthetic mica. Examples of mica include sericite (silicite), muscovite (white mica), phlogopite (gold mica), and synthetic mica. Among them, synthetic mica is preferable.
[0027] Synthetic mica is generally a colorless, transparent, pure crystal. Synthetic mica may be mica in which hydroxyl groups (OH) are replaced with fluorine atoms (F). In synthetic mica, the iron content may be 100 ppm or less, or 50 ppm or less. In synthetic mica, the amount of heavy metals may be 1 ppm or less, or 0.1 ppm or less.
[0028] Mica particles (especially synthetic mica particles) are thin and plate-like, thermally and chemically stable, and have a high aspect ratio (ratio of particle size to thickness) (for example, aspect ratio is 10 to 100, 20 to 80, or 30 to 70). Therefore, by orienting the mica particles in a molded product, it is possible to improve mechanical properties such as low warpage, high rigidity, and low shrinkage, and to impart insulation properties, vibration damping properties, etc. Furthermore, it is possible to impart glossiness due to interface reflection with the base resin, so it is widely used in the fields of home appliances, heavy electrical machinery, electric wires, etc. Mica is obtained by refining, pulverizing, and classifying mica ore, and the higher the aspect ratio, the more likely it is that specific properties in terms of physical properties will be expressed.
[0029] The average particle size of the particles may be 1 to 100 μm, 2 to 80 μm, 3 to 70 μm, 4 to 60 μm, 5 to 55 μm, or 7 to 50 μm. Alternatively, the average particle size of the particles is preferably 45 μm or less, 40 μm or less, 35 μm or less, 30 μm or less, 25 μm or less, 20 μm or less, 15 μm or less, or 10 μm or less. When the amount is within the above range, a high haze and a good ground glass texture are obtained. The average particle size of the particles may be 1 μm or more, 3 μm or more, 5 μm or more, or 10 μm or more.
[0030] The average particle size of the particles can be measured using an optical microscope (200 to 500 times magnification). The median size (D50) obtained by creating a particle size distribution from the particle sizes of any number of particles (for example, 100 or 200 particles) can be used as the average particle size.
[0031] In the coating layer, the amount of particles is preferably 0.1 to 10 parts by weight or 0.3 to 5 parts by weight based on 100 parts by weight of the thermoplastic resin (A). When the amount is within the above range, the haze is high and a good ground glass texture is obtained. More preferably, it is 0.2 to 8 parts by weight or 0.3 to 3 parts by weight, for example, 1 to 2.5 parts by weight. Alternatively, the lower limit of the amount of particles may be 0.1 parts by weight, 0.2 parts by weight, 0.3 parts by weight, 0.5 parts by weight, 0.8 parts by weight, 1 part by weight, 1.5 parts by weight, 2 parts by weight, 3 parts by weight, 4 parts by weight, 5 parts by weight, 6 parts by weight, 7 parts by weight, 8 parts by weight, or 9 parts by weight, and the upper limit of the amount of particles may be 10 parts by weight, 9 parts by weight, 8 parts by weight, 7 parts by weight, 6 parts by weight, 5 parts by weight, 4 parts by weight, 3 parts by weight, 2 parts by weight, 1.5 parts by weight, 1 part by weight, 0.5 parts by weight, or 0.2 parts by weight, relative to 100 parts by weight of the thermoplastic resin (A).
[0032] Since it is easy to impart a ground glass look, it is preferable that the difference between the refractive index of the particles and the refractive index of the thermoplastic resin is small. The difference between the refractive index of the particles and the refractive index of the thermoplastic resin is preferably 0.005 to 0.08, more preferably 0.008 to 0.03. When the amount is within the above range, the haze is high and a good ground glass look is obtained. The refractive index difference may be 0.006 or more, 0.007 or more, 0.008 or more, 0.009 or more, 0.01 or more, 0.011 or more, 0.012 or more, 0.013 or more, 0.014 or more, 0.015 or more, 0.02 or more, 0.025 or more, 0.03 or more, 0.035 or more, 0.04 or more, 0.045 or more, or 0.05 or more; It may be 0.07 or less, 0.065 or less, 0.06 or less, 0.055 or less, 0.05 or less, 0.045 or less, 0.04 or less, 0.035 or less, 0.03 or less, 0.025 or less, 0.02 or less, 0.019 or less, 0.018 or less, 0.017 or less, 0.016 or less, 0.015 or less, 0.014 or less, 0.013 or less, or 0.012 or less.
[0033] The refractive index of thermoplastic resin was measured using a multi-wavelength Abbe refractometer (ATAGO DR-M4 model). First, a small amount of contact liquid (1-bromonaphthalene) was dropped onto the surface of a test piece made by injection molding, and the edge of the test piece was brought into contact with the surface of the prism with the light source facing the light source. After that, the field was adjusted until all colors disappeared, and the boundary between the bright field and the dark field was aligned with the intersection of the crosshairs of the eyepiece to measure the refractive index. A halogen lamp with a wavelength of 589 nm was used as the light source.
[0034] The refractive index of particles was measured using the Becke method. First, the particles were placed on a slide glass and a known refractive index liquid was dropped onto it. Then, after thoroughly mixing the particles and the refractive index liquid, the outline of the particles was observed from above using an optical microscope while shining light on them. If the outline was not visible, it was determined that the refractive index of the refractive index liquid and the particles were equal.
[0035] In addition, there is no problem with the observation by the optical microscope as long as the magnification allows the outline of the particles to be confirmed, but for particles with a diameter of 5 μm, a magnification of about 500 times is appropriate. By the above operation, the closer the refractive index of the particle and the refractive index of the refractive liquid, the harder it is to see the outline of the particle, so the refractive index of the refractive liquid in which the outline of the particle is difficult to see was determined to be equal to the refractive index of the particle.
[0036] In addition, if there is no difference in the appearance of a particle between two types of refractive index liquids with a refractive index difference of 0.002, the intermediate value of these two types of refractive index liquids was determined to be the refractive index of the particle. For example, when testing with refractive index liquids of 1.554 and 1.556, if there is no difference in the appearance of a particle in both refractive index liquids, the intermediate value of these refractive index liquids, 1.555, was determined to be the refractive index of the particle.
[0037] [Other ingredients] Other components may be included in the substrate layer, the coating layer and the masterbatch. Other components, for example, additives, include neutralizing agents, antioxidants, ultraviolet absorbers, lubricants, antistatic agents, antiblocking agents, processing aids, colorants (inorganic pigments, organic pigments, pigment dispersants, etc.), foaming agents, nucleating agents, plasticizers, flame retardants, brightness enhancers, antibacterial agents, light diffusing agents, etc. These additives may be used alone or in combination of two or more. The additives may be present in an amount of 50% by weight or less, 0.1 to 30% by weight, or 1 to 20% by weight based on the substrate layer, the coating layer, and the masterbatch.
[0038] [Master batch] The coating layer may be prepared using a masterbatch that includes a thermoplastic resin and a high concentration of silicate particles. It may contain 100 parts by weight of thermoplastic resin (A) and 1 to 200 parts by weight, 1 to 150 parts by weight, 1 to 100 parts by weight, 1 to 70 parts by weight, or 1 to 50 parts by weight of silicate particles (B). In the masterbatch, the concentration of the silicate particles may be 0.01% or more, 0.05% or more, 0.1% or more, 0.5% or more, 1% or more, 2% or more, 3% or more, or 5% or more by weight, and may be 70% or less, 65% or less, 60% or less, 55% or less, 50% or less, 45% or less, 40% or less, 35% or less, 30% or less, 25% or less, 20% or less, 15% or less, 10% or less, 5% or less, 3% or less, 2% or less, or 1% or less by weight, based on the masterbatch.
[0039] <Masterbatch manufacturing method> The masterbatch can be prepared by mixing the silicate particles with a thermoplastic resin at a temperature at which the thermoplastic resin melts, such that the silicate particles are dispersed in the thermoplastic resin.
[0040] The components constituting the master batch (thermoplastic resin, silicate particles, and other components as required) are mixed in various forms such as bulk, pellets, chips, etc., to a predetermined mixing ratio, and then premixed as required, and then put into a melt kneader and heated to the melting point of the thermoplastic resin or higher to melt knead. The mixture is then extruded into a strand shape and cut into granules (pellets or chips) to obtain a master batch. The size (maximum length) may generally be 0.1 to 100 mm or 0.5 to 50 mm.
[0041] The premixing may be a dry blend using a premixer such as a ribbon blender, a Henschel mixer, or a V blender. The melt kneading may be performed using a melt kneader equipped with a heating mechanism such as a Banbury mixer, a mixing roll, a single-screw or twin-screw extruder, or a kneader. The melt kneader may be equipped with a filter having an opening of 1 mm or less, for example, 0.01 to 0.5 mm, particularly 0.05 to 0.3 mm.
[0042] <Method of manufacturing molded products> A molded article can be manufactured by laminating and integrating a thermoplastic resin (substrate layer) and a resin composition (coating layer) in which silicate particles are dispersed in a thermoplastic resin. The resin composition constituting the coating layer (coating layer composition) is preferably manufactured by adding a thermoplastic resin to a master batch. To form the substrate layer and the coating layer, the feed material for the substrate layer (thermoplastic resin) and the feed material for the coating layer (thermoplastic resin and silicate particles) are melted (melt-kneaded). Before being melted, the feed material for the coating layer may be mixed with the resin and particles, if necessary, to uniformly disperse the particles in the resin.
[0043] The method for producing the molded article of the present invention is not particularly limited. Methods for producing the molded article include extrusion molding, compression molding, casting molding, and injection molding. The method for producing the molded article is preferably co-extrusion (co-extrusion molding). According to the co-extrusion method, the fluidity of each layer can be matched and made uniform during lamination, so that the adhesion between layers is good and there is little molding distortion.
[0044] The term "coextrusion" refers to a method in which two or more materials are extruded through a single die with two or more orifices arranged in it, so that the extrudates merge with each other into a layered structure. Coextrusion systems use at least two extruders feeding a common die assembly. The number of extruders depends on the number of different materials that make up the molded article (e.g., a coextruded sheet). A different extruder may be used for each different material. Thus, a three-layer coextrusion may require up to three extruders, but fewer extruders may be used if two or more layers are made of the same material.
[0045] The co-extrusion method generally uses two or more extruders, a large diameter extruder for the substrate layer resin and a small diameter extruder for the coating layer resin, and generally integrates and co-extrudes through an extrusion die head. Examples of combinations of a large diameter extruder for the substrate layer resin and a small diameter extruder for the coating layer resin include a combination of 120mm and 50mm, a combination of 90mm and 45mm, and a combination of 40mm and 20mm. The thickness of the substrate layer and the coating layer is generally adjusted by adjusting the extrusion rate of each extruder and the gap between the rolls installed at the exit of the extrusion die. When the layer is passed between the two rolls, the surfaces of the two rolls may be different. For example, the roll in contact with the coating layer may be a roll made of rubber, a roll with a rubber layer on metal, or a roll with a metal film on rubber, while the roll in contact with the substrate layer may be a roll made of metal with a flat surface. In this way, the surface of the coating layer may be given a matte appearance.
[0046] This can be achieved by adjusting the temperature of each extruder in order to match the fluidity of the substrate layer resin and the coating layer resin during co-extrusion. The feed material used for the coating layer is preferably a pellet obtained by uniformly mixing the resin and particles in advance using a blender or the like and melt-kneading the mixture in an extruder.
[0047] In the coextrusion method, the temperature of the cylinder and die head of each extruder is equal to or higher than the melting point of the thermoplastic resin, and although it depends on the melting point of the thermoplastic resin, it may usually be 200°C or higher or 230°C or higher, and 350°C or lower or 300°C or lower. EXAMPLES
[0048] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the following, parts, % or ratios refer to parts by weight, % by weight or ratios by weight unless otherwise specified.
[0049] [Example 1] Polymethylmethacrylate resin (MFR: 2, total light transmittance: 93%), synthetic mica (particle size: 40 μm), and ethylene bis(stearic acid amide) were mixed in a tumbler in a ratio of 88.95:11.0:0.05 and granulated at 240°C using a 65 mmφ twin-screw extruder to obtain a master batch. The polymethyl methacrylate resin and the obtained master batch were blended in a ratio of 100.0:10.0 using a Henschel mixer to prepare a coating layer composition. The obtained coating layer composition was co-extruded with a 50 mmφ single screw extruder, and the polymethyl methacrylate resin was co-extruded with a 120 mmφ single screw extruder for the substrate layer. The die had two types and three layers, and the thickness of the substrate layer was adjusted to 1.5 mm and the thickness of the coating layer was adjusted to 0.1 mm, to obtain a molded product. The extrusion temperature of the coating layer portion was 225 to 260°C, the extrusion temperature of the substrate layer portion was 200 to 265°C, and the temperature of the die portion was 260°C.
[0050] [Example 2] A molded product was obtained in the same manner as in Example 1, except that the thickness of the substrate layer was adjusted to 0.5 mm and the thickness of the coating layer was adjusted to 0.05 mm.
[0051] [Example 3] A molded article was obtained in the same manner as in Example 1, except that 0.002 part of blue dye (CI Solvent Blue 97) was added to the substrate layer.
[0052] [Example 4] A molded article was obtained in the same manner as in Example 2, except that 0.002 part of blue dye (CI Solvent Blue 97) was added to the substrate layer.
[0053] The molded articles obtained in the examples were evaluated for the following.
[0054] [Total light transmittance] The molded articles obtained in the examples were measured for total light transmittance in accordance with JIS K7361.
[0055] [HAZE] The molded articles obtained in the examples were measured for haze in accordance with JIS K7136.
[0056] [Gross] The molded articles obtained in the examples were measured for glossiness at 60° reflection using a gloss meter in accordance with JIS Z 8741:1997.
[0057] [Ground glass] The molded articles obtained in the examples were visually inspected and evaluated for ground glass properties according to the following criteria. ◯: Good ground glass properties. ×: No ground glass properties
[0058] The thicknesses of the substrate layer and the coating layer are shown in Table 1, and the evaluation results are shown in Table 2.
[0059] [Table 1]
[0060] [Table 2] [Industrial Applicability]
[0061] According to the present invention, it is possible to obtain a molded article which has no surface gloss and has a good matte feel or a good ground glass texture while maintaining the transparency of the resin. [Explanation of symbols]
[0062] 10 Molded products 1,3 Covering layer 2. Board Layer
Claims
1. A ground-glass-like thermoplastic molded product having a coating layer on at least one main surface of a substrate layer containing a thermoplastic resin, the coating layer being made of a resin composition in which 100 parts by weight of a thermoplastic resin (A) is dispersed with 0.1 to 10 parts by weight of silicate particles (B).
2. 2. The ground-glass texture thermoplastic molded article according to claim 1, wherein the substrate layer and the covering layer are integrally laminated by extrusion molding.
3. the substrate layer is at least one selected from the group consisting of polyethylene terephthalate resin, polystyrene resin, polymethyl methacrylate resin, and polycarbonate resin; In the coating layer, the thermoplastic resin (A) is at least one resin selected from a polyethylene terephthalate resin, a polystyrene resin, a polymethyl methacrylate resin, and a polycarbonate resin; 2. The ground-glass texture thermoplastic molded article according to claim 1, wherein the silicate of the silicate particles (B) is mica.
4. 2. The ground-glass texture thermoplastic molded article according to claim 1, wherein the thickness of the molded article is 0.1 mm to 30 mm.
5. 2. The ground-glass style thermoplastic molded article according to claim 1, wherein the silicate has an average particle size of 10 μm or more.
6. 2. The ground-glass-like thermoplastic molded article according to claim 1, wherein the amount of the silicate particles (B) is 0.2 to 7 parts by weight per 100 parts by weight of the thermoplastic resin (A) of the coating layer.
7. A thermoplastic resin; a resin composition in which 0.1 to 10 parts by weight of silicate particles (B) are dispersed in 100 parts by weight of a thermoplastic resin (A); The method for producing the ground-glass texture thermoplastic molded article according to claim 1, comprising laminating and integrating the above.
8. A masterbatch for ground-glass style thermoplastic molded products comprising 100 parts by weight of a thermoplastic resin (A) and 1 to 200 parts by weight of silicate particles (B).
Citation Information
Patent Citations
JP153586A
Molded synthetic resin article
JP1989297465A
Polyester resin composition
JP1999001606A