Toner for developing electrostatic latent images and electrophotographic image forming method
Ultrasonic dispersion treatment of toner particles with specific circularity and particle size conditions addresses uneven hiding performance in toners with white pigments, enhancing image quality and cleaning efficiency.
Patent Information
- Application Number
- JP2019208356
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-11-19
- Publication Date
- 2024-09-17
- Estimated Expiration
- 2039-11-19
AI Technical Summary
Existing toners with white pigments suffer from uneven hiding performance between the leading and trailing edges of prints due to minute toner particles slipping through the cleaning mechanism, leading to image defects and reduced concealability.
The toner particles are subjected to ultrasonic dispersion treatment in water to achieve specific conditions: average circularity of 0.920 to 0.970 and a reduced number of particles with a size of 2.0 μm or less, ensuring good fluidity and effective cleaning performance.
This approach enhances the toner's hiding properties by minimizing slip-through and image defects, maintaining consistent concealability across the print edge, and improving cleaning efficiency.
Smart Images

Figure 0007551290000001 
Figure 0007551290000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a toner for developing electrostatic latent images and a method for forming electrophotographic images, and more particularly to a toner for developing electrostatic latent images having a white pigment and excellent concealing properties, and a method for forming electrophotographic images using the toner. [Background technology]
[0002] In recent years, in the field of toner for developing electrostatic latent images (hereinafter also referred to as "toner") used in electrophotographic image formation, development has been carried out in response to various demands from the market. In particular, the number of types of recording media used for printing has been increasing, and there is a high demand from the market for the compatibility of printing machines with recording media.
[0003] For example, when printing on special recording media such as colored paper, black paper, aluminum-deposited paper, and transparent film, the color characteristics of the recording media affect the printing, so sufficient color development cannot be obtained with only colored toners that exhibit yellow (Y), magenta (M), cyan (C), and black (K), etc. For this reason, a technology has been proposed that conceals the color of the recording media by forming a toner image containing a white pigment (hereinafter also referred to as "white toner") in the bottom layer (see, for example, Patent Documents 1 and 2).
[0004] In order to ensure the concealment of the recording medium, it is common to place more white toner on the recording medium than the four color toners of YMCK, and it is known that this is achieved by increasing the pigment loading and the amount of white toner placed (see, for example, Patent Document 3).
[0005] However, when the white pigment is highly filled or the amount of the white pigment is increased to increase the hiding power, the white pigment, for example, titanium oxide, is easily exposed on the surface of the toner particles, and the weight of each toner particle also increases, which increases the load on the cleaning unit and causes the problem of different hiding power at the leading and trailing edges of the print. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2002-311648 A [Patent Document 2] JP 2016-45418 A [Patent Document 3] JP 2007-33719 A Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention has been made in consideration of the above problems and circumstances, and an object of the present invention is to provide a toner for developing electrostatic latent images that contains a white pigment and has excellent hiding properties, and an electrophotographic image forming method using the same.
[0008] In order to solve the above problem, the inventors have investigated the causes of the above problem and have found that the phenomenon in which the concealment differs between the leading and trailing ends of a print is due to the fact that minute toner particles with a particle size of 2.0 μm or less cannot be cleaned, slip through and remain on the photosensitive drum, which causes minute defects on the image and reduces the concealment of the image. Furthermore, they have found that the amount of this slip-through is closely related not only to the amount of minute toner particles with a particle size of 2.0 μm or less, but also to the circularity of the toner particles, which led to the present invention. That is, the above-mentioned problems of the present invention are solved by the following means.
[0009] 1. A toner for developing electrostatic latent images, which is made of toner particles containing at least a white pigment, and when the toner particles are subjected to ultrasonic dispersion treatment in water, the toner particles satisfy the following conditions ( 3) Filled with, true density is 1. 5 0~2. 0 0g / cm 3 A toner for developing electrostatic latent images, characterized in that conditions( 3 ): Average circularity is 0.9 3 The particle size is within the range of 0 to 0.950, and the number of particles with a particle size of 2.0 μm or less is 30% or less by number.。
[0012] 2 1. In the section A method for forming an electrophotographic image, comprising using the toner for developing an electrostatic latent image described above. Effect of the Invention
[0013] According to the above-mentioned means of the present invention, it is possible to provide a toner for developing electrostatic latent images, which contains a white pigment and has excellent hiding properties, and an electrophotographic image forming method using the toner. Although the mechanism by which the effects of the present invention are expressed or the mechanism of action has not been clarified, it is speculated as follows.
[0014] It was found that when ultrasonic dispersion is applied to white toner, which causes the phenomenon of different hiding power at the leading and trailing edges of printing, the number of tiny toner particles (hereinafter referred to as "toner fine particles") with a diameter of 2.0 μm or less increases, and fine particles other than the target particle size are present during toner manufacturing. The increased toner fine particles are thought to be fine particles that are easily detached from the toner due to stress.
[0015] From the viewpoint of cleaning performance of white toner, when the average circularity of toner particles is high, 0.920 or more, it is believed that the toner has good fluidity and toner spent on the drum due to toner accumulation in the cleaning area can be suppressed. Also, when the average circularity of toner particles is 0.970 or less, the toner particles become slightly distorted compared to perfect circles, the toner itself has many contact points, and the amount of toner particles that can adhere to the uneven parts of the toner increases, so the toner can be wiped off with the cleaning blade, and toner slip-through is suppressed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The toner for developing electrostatic latent images of the present invention is a toner for developing electrostatic latent images that is composed of toner particles containing at least a white pigment, and is characterized in that, when subjected to ultrasonic dispersion treatment in water, the toner particles satisfy the above-mentioned condition (1) or condition (2). This characteristic is a technical characteristic common to or corresponding to each of the following embodiments (configurations).
[0017] As an embodiment of the present invention, it is preferable that the toner particles satisfy the condition (3) when subjected to the ultrasonic dispersion treatment in water, because this can suppress the occurrence of toner filming and obtain good cleaning properties. In addition, the true density is 1.30 to 2.20 g / cm 3 It is preferable that the content is within the range from 0.01 to 0.15 since high hiding power can be obtained. Further, the present invention is preferably an electrophotographic image forming method using the toner for developing electrostatic latent images of the present invention.
[0018] The present invention, its components, and embodiments for carrying out the present invention will be described in detail below. In this application, except for the case of "more than", "to" is used to mean that the numerical values before and after it are included as the lower and upper limits.
[0019] In the present invention, the toner base particles to which an external additive has been added are referred to as toner particles, and an aggregate of toner particles is referred to as toner. Generally, the toner base particles can be used as they are as toner particles, but in the present invention, the toner base particles to which an external additive has been added can be used as toner particles. In the present invention, the term "(meth)acrylic resin" means an acrylic resin or a methacrylic resin, and the term "(meth)acrylic acid" means acrylic acid or methacrylic acid.
[0020] <<Outline of the toner for developing electrostatic latent images of the present invention>> The toner for developing electrostatic latent images of the present invention is a toner for developing electrostatic latent images that is composed of toner particles containing at least a white pigment, and is characterized in that, when subjected to ultrasonic dispersion treatment in water, the toner particles satisfy the following condition (1) or condition (2):
[0021] Condition (1): The average circularity is within a range of 0.920 to 0.950, and the number of particles having a particle size of 2.0 μm or less is 30% or less by number. Condition (2): The average circularity is within a range of more than 0.950 and 0.970, and the number of particles having a particle size of 2.0 μm or less is 15% by number or less.
[0022] With this configuration, it is possible to provide a toner for developing electrostatic latent images, which contains a white pigment and has excellent hiding power, and an electrophotographic image forming method using the toner.
[0023] Since toner particles have a strong adhesive property, they usually remain attached to the toner surface, but it is believed that they are detached from the toner due to stress during cleaning. As described above, since the white pigment is exposed in large amounts on the toner surface, these detached toner particles have a low charge amount and a high adhesive force, so they are transferred back to the photoconductor drum, where they cannot be cleaned and slip through, causing minute defects on the image and reducing the concealment of the image.
[0024] Furthermore, as mentioned above, this phenomenon is also related to the circularity of the toner particles. When the average circularity of the toner after ultrasonic dispersion treatment is within the range of 0.920 to 0.950, if the toner fine particles are 30% or less by number, or when the average circularity is within the range of more than 0.950 to 0.970, if the toner fine particles are 15% or less by number, they will adhere to the uneven parts of the toner and will not detach even under stress during cleaning, and will be transported to the waste toner together with the toner, thereby providing satisfactory performance.
[0025] When the average circularity is within the range of 0.920 to 0.950, even if there are more toner particles, they are less likely to detach even under stress during cleaning. This is presumably because toner particles with a lower circularity have more contact points with the toner itself, and a larger amount of toner particles can adhere to the uneven parts of the toner.
[0026] With regard to the relationship between the average circularity of the toner particles after the ultrasonic dispersion treatment and the content of the toner fine particles, it is more preferable that the toner particles satisfy the following condition (3). Condition (3): The average circularity is within a range of 0.930 to 0.950, and the number of particles having a particle size of 2.0 μm or less is 30% or less by number.
[0027] [Ultrasonic dispersion processing] The average circularity and the number % of particles with a particle size of 2.0 μm or less of the toner particles according to the present invention are obtained by ultrasonic dispersion treatment in water. Specifically, ultrasonic dispersion treatment is performed as follows, and the average circularity and the content (number %) of toner fine particles are measured.
[0028] (Ultrasonic dispersion treatment method in water) 3 g of toner is moistened with 40 g of a 0.2% by weight aqueous solution of polyoxyethyl phenyl ether in a 100 mL plastic cup, and ultrasonic energy is applied for 1 minute using an ultrasonic homogenizer "US-1200" (manufactured by Nippon Kikai Co., Ltd.) so that the value of the ammeter that shows the vibration indication value attached to the main device indicates 60 μA (50 W).
[0029] [Toner fine particle content] The content (number %) of fine particles (toner fine particles) of 2.0 μm or less can be measured using “FPIA-3100” (manufactured by Sysmex Corporation).
[0030] Specifically, after the toner is mixed with an aqueous solution containing a surfactant, measurements are taken using the "FPIA-3100" under the measurement conditions of HPF (high magnification imaging) mode at an appropriate concentration of 3,000 to 10,000 HPF detections. Within this range, the same reproducible measurement values can be obtained. The particle size is calculated from the projected area equivalent diameter, the particle sizes of each particle are added together, and the proportion of particles with a particle size of 2.0 μm or less (number %) relative to the total number of particles is evaluated.
[0031] [Average particle size] The average particle size of the toner particles is preferably within the range of 4.0 to 10.0 μm, more preferably within the range of 4.0 to 7.0 μm, as the arithmetic mean determined from the measurement of the projected area equivalent diameter using the above-mentioned "FPIA-3100." By being within the above range, the transfer efficiency is increased, the image quality of halftones is improved, and the image quality of thin lines, dots, etc. is improved.
[0032] [Average circularity] The average circularity can be measured using an FPIA-3100 (manufactured by Sysmex Corporation). Specifically, after the toner is mixed with an aqueous solution containing a surfactant, the measurement is performed using the FPIA-3100 under the measurement conditions of HPF (high magnification imaging) mode at an appropriate concentration of 3,000 to 10,000 HPF detections. Within this range, the same reproducible measurement value can be obtained. The average circularity is calculated from the circularity defined by the following formula. Circularity = (perimeter of a circle with the same projected area as the particle image) / (perimeter of the projected particle image) The average circularity is calculated by adding up the circularity of each particle and dividing the sum by the total number of particles.
[0033] [True density] The true density of the toner for developing electrostatic latent images of the present invention is 1.30 to 2.20 g / cm 3 It is preferable that the range is 1.30 g / cm 3 If it is more than 2.20 g / cm, high hiding power can be ensured. 3 If the average particle size is less than 1.30 g / cm, high electrostatic charge can be obtained, which is preferable. Also, from the viewpoint of the weight per particle and the hiding power, the average particle size is 1.30 to 2.20 g / cm. 3 It is preferably in the range of 1.50 to 2.00 g / cm. 3 is within the range. The true density of the toner can be controlled by changing conditions such as the part by mass of the white pigment in the method for producing a toner for developing an electrostatic latent image, which will be described later.
[0034] (True density measurement) Using a Shimadzu Micromeritics dry density meter Accupic II 1340TC (gas displacement method), 5 g of toner was measured at 10 cm 3 The measurement can be carried out by placing the sample in a cell, repeating the measurement five or more times, and calculating the average value.
[0035] <<Details of the toner for developing electrostatic latent images of the present invention>> The toner for developing electrostatic latent images of the present invention is a toner for developing electrostatic latent images that is composed of toner particles containing at least a white pigment, and is characterized in that, when subjected to ultrasonic dispersion treatment in water, the toner particles satisfy the above-mentioned condition (1) or condition (2). The toner for developing electrostatic images of the present invention has toner base particles containing a white pigment, a binder resin, and a release agent, and may further contain a charge control agent or an external additive, if necessary.
[0036] [White pigment] Examples of the white pigment include inorganic pigments (e.g., heavy calcium carbonate, light calcium carbonate, titanium oxide, aluminum hydroxide, titanium white, talc, calcium sulfate, barium sulfate, zinc oxide, magnesium oxide, magnesium carbonate, amorphous silica, colloidal silica, white carbon, kaolin, calcined kaolin, delaminated kaolin, aluminosilicate, sericite, bentonite, smexite, etc.) and organic pigments (e.g., polystyrene resin particles, urea formalin resin particles, etc.). From the viewpoint of hiding power, the white pigment is preferably an inorganic pigment.
[0037] Examples of the white pigment also include pigments having a hollow structure, such as hollow resin particles and hollow silica. From the viewpoint of chargeability and hiding power, the white pigment is preferably titanium oxide. Titanium oxide may have any crystal structure, such as anatase type, rutile type, or brookite type. Titanium oxide can be obtained by a manufacturing method such as a sulfuric acid method or a chlorine method.
[0038] [Toner base particles] The toner base particles according to the present invention are not particularly limited as long as they contain the white pigment, and any known toner base particles can be used. In particular, however, it is preferable that the toner base particles contain at least a binder resin, and that the binder resin contains at least a crystalline resin.
[0039] (Binding resin) As the binder resin contained in the toner base particles according to the present invention, for example, when the toner base particles are produced by a pulverization method, a dissolution suspension method, an emulsion aggregation method, or the like, various known resins such as vinyl resins such as styrene resins, (meth)acrylic resins, styrene-(meth)acrylic copolymer resins, and olefin resins, polyester resins, polyamide resins, carbonate resins, polyethers, polyvinyl acetate resins, polysulfones, epoxy resins, polyurethane resins, and urea resins can be used. These can be used alone or in combination of two or more. In the present invention, it is preferable to use a vinyl resin from the viewpoint of the chargeability of the toner.
[0040] (Crystalline Resin) It is preferable that the binder resin constituting the toner base particles contains a crystalline resin, in order to facilitate melting of the toner particles and to achieve energy saving during fixing to a recording medium. The crystalline resin is a resin having crystallinity. Examples thereof include crystalline polyester resins and crystalline vinyl resins. Among them, crystalline polyester resins are preferable, and aliphatic crystalline polyester resins are more preferable.
[0041] The crystalline polyester resin can be produced by a general polyester polymerization method in which an acid component and an alcohol component are reacted. Examples of the polymerization method include direct polycondensation and transesterification, and the polymerization method is appropriately selected depending on, for example, the type of monomer.
[0042] The crystalline polyester resin can be produced at a polymerization temperature of, for example, 180 to 230°C. If necessary, the pressure in the reaction system is reduced, and the monomer is reacted while removing water and alcohol generated by condensation. If the monomer is not soluble or compatible at the reaction temperature, a high-boiling point solvent may be added as a solubilizing agent to dissolve the monomer. The polycondensation reaction is carried out while distilling off the solubilizing agent. If a monomer with poor compatibility is present in the copolymerization reaction, for example, the monomer with poor compatibility may be condensed in advance with the acid or alcohol to be polycondensed with the monomer, and then polycondensed with the main component. In addition, other binder resins may be contained, examples of which include styrene-(meth)acrylic resins, polyester resins, and partially modified polyester resins.
[0043] The styrene-(meth)acrylic resin has a molecular structure of a radical polymer of a compound having a radically polymerizable unsaturated bond, and can be synthesized, for example, by radical polymerization of the compound. The compound may be one or more kinds, and examples thereof include styrene and its derivatives, and (meth)acrylic acid and its derivatives.
[0044] Examples of the styrene and its derivatives include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, p-methoxystyrene, p-phenylstyrene, p-chlorostyrene, p-ethylstyrene, pn-butylstyrene, p-tert-butylstyrene, pn-hexylstyrene, pn-octylstyrene, pn-nonylstyrene, pn-decylstyrene, pn-dodecylstyrene, 2,4-dimethylstyrene and 3,4-dichlorostyrene.
[0045] Examples of the (meth)acrylic acid and derivatives thereof include methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, cyclohexyl acrylate, phenyl acrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate, hexyl methacrylate, 2-ethylhexyl methacrylate, β-hydroxyacrylate, propyl γ-aminoacrylate, stearyl methacrylate, dimethylaminoethyl methacrylate, and diethylaminoethyl methacrylate.
[0046] The polyester resin has a molecular structure of a condensation polymerization product of a polycarboxylic acid and a polyhydric alcohol, and can be synthesized, for example, by condensation polymerization of these.
[0047] The polycarboxylic acid may be one or more kinds. Examples of the polycarboxylic acid include aliphatic dicarboxylic acids, aromatic dicarboxylic acids, dicarboxylic acids having a double bond, trivalent or higher carboxylic acids, their anhydrides, and their lower alkyl esters. The dicarboxylic acids having a double bond are radically cross-linked through the double bond, and therefore are suitable from the viewpoint of preventing hot offset during fixing in toner particles.
[0048] Examples of the aliphatic dicarboxylic acids include oxalic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid.
[0049] Examples of the aromatic dicarboxylic acids include phthalic acid, isophthalic acid, terephthalic acid, naphthalene-2,6-dicarboxylic acid, malonic acid and mesaconic acid.
[0050] Examples of the dicarboxylic acid having a double bond include maleic acid, fumaric acid, 3-hexenedioic acid, and 3-octenedioic acid. Among them, fumaric acid or maleic acid is preferred from the viewpoint of cost.
[0051] Examples of the trivalent or higher carboxylic acid include 1,2,4-benzenetricarboxylic acid, 1,2,5-benzenetricarboxylic acid and 1,2,4-naphthalenetricarboxylic acid. The polyhydric alcohol may be one or more kinds. Examples of the polyhydric alcohol include aliphatic diols and trihydric or higher alcohols. Among them, aliphatic diols are preferred from the viewpoint of obtaining a crystalline polyester resin described later, and linear aliphatic diols having 7 to 20 carbon atoms in the main chain are more preferred.
[0052] When the aliphatic diol is the linear aliphatic diol, the crystallinity of the polyester is maintained and the drop in the melting temperature of the polyester is suppressed. Therefore, it is preferable from the viewpoint of obtaining the two-component developer having excellent toner blocking resistance, image storage stability, and low-temperature fixing property. In addition, when the carbon number of the main chain part of the linear aliphatic diol is 7 to 20, it is preferable from the viewpoint of suppressing the melting point of the product when polycondensed with the aromatic dicarboxylic acid to a low value and realizing low-temperature fixing. In addition, in practical use, the material is easily available. From these viewpoints, it is more preferable that the carbon number of the main chain part is 7 to 14.
[0053] Examples of aliphatic diols suitable for use in the synthesis of the crystalline polyester resin include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol and 1,14-eicosanedecanediol. Among these, 1,8-octanediol, 1,9-nonanediol or 1,10-decanediol is preferred from the viewpoint of availability.
[0054] Examples of the trihydric or higher alcohol include glycerin, trimethylolethane, trimethylolpropane and pentaerythritol.
[0055] A chain transfer agent may be added to the monomer components used in synthesizing the binder resin to adjust the molecular weight of the resulting resin. The chain transfer agent may be one or more types, and is used in an amount that can achieve the above-mentioned object within the range in which the effects of the present embodiment are achieved. Examples of the chain transfer agent include mercaptans such as 2-chloroethanol, octyl mercaptan, dodecyl mercaptan, and t-dodecyl mercaptan, and styrene dimer.
[0056] (Release agent) As the release agent, various known waxes can be used. Examples of waxes include polyolefin waxes such as polyethylene wax and polypropylene wax, branched-chain hydrocarbon waxes such as microcrystalline wax, long-chain hydrocarbon waxes such as paraffin wax and sazol wax, dialkyl ketone waxes such as distearyl ketone, carnauba wax, montan wax, ester waxes such as behenic acid behenate, trimethylolpropane tribehenate, pentaerythritol tetrabehenate, pentaerythritol diacetate dibehenate, glycerin tribehenate, 1,18-octadecanediol distearate, trimellitic acid tristearyl, and distearyl maleate, and amide waxes such as ethylenediamine behenylamide and trimellitic acid tristearylamide.
[0057] The content of the release agent is preferably within a range of 0.1 to 30 parts by mass, and more preferably within a range of 1 to 10 parts by mass, relative to 100 parts by mass of the binder resin.
[0058] (Charge control agents, etc.) The charge control agent is not particularly limited as long as it is a substance that can provide a positive or negative charge through frictional charging, and various known positive charge control agents and negative charge control agents can be used. For example, it is preferable to use an azo-based metal complex, a metal complex or a metal salt of salicylic acid or alkylsalicylic acid. The content of the charge control agent is preferably within a range of 0.01 to 30 parts by mass, and more preferably within a range of 0.1 to 10 parts by mass, relative to 100 parts by mass of the binder resin. The toner may also contain other ingredients known in the art, such as anti-offset agents, such as low molecular weight propylene, low molecular weight polyethylene, waxes, and the like.
[0059] [External additives] From the viewpoint of improving the charging performance, fluidity or cleaning property of the toner, known particles such as inorganic fine particles or organic fine particles or lubricants can be added as external additives to the surface of the toner base particles.
[0060] Preferable examples of inorganic fine particles used as external additives include fine particles containing silica, titania, alumina, strontium titanate, etc. If necessary, these fine particles may be subjected to a hydrophobic treatment.
[0061] As the organic fine particles, spherical organic fine particles having a number average primary particle size of about 10 to 2000 nm can be used. Specifically, organic fine particles made of homopolymers such as styrene and methyl methacrylate, or copolymers thereof can be used.
[0062] The lubricant is used for the purpose of further improving the cleaning property and transfer property, and examples of the lubricant include metal salts of higher fatty acids such as salts of stearic acid such as zinc, aluminum, copper, magnesium, calcium, etc., salts of oleic acid such as zinc, manganese, iron, copper, magnesium, etc., salts of palmitic acid such as zinc, copper, magnesium, etc., salts of linoleic acid such as zinc, calcium, etc., salts of ricinoleic acid such as zinc, calcium, etc. Various types of these external additives may be used in combination.
[0063] Examples of the method for adding the external additives include methods using various known mixing devices such as a Turbula mixer, a Henschel mixer, a Nauta mixer, and a V-type mixer.
[0064] <<Method for producing toner for developing electrostatic images>> The method for producing the toner for developing electrostatic images of the present invention is not particularly limited, and includes known methods such as a kneading and pulverizing method, a suspension polymerization method, an emulsion aggregation method, a dissolution suspension method, a polyester elongation method, and a dispersion polymerization method. Among these, the kneading and pulverizing method is preferred from the viewpoint of manufacturability, which allows easy high pigment loading.
[0065] [Kneading and grinding method] The kneading and grinding method is a method in which various materials such as a white pigment are mixed, and then the materials are melted and kneaded using a kneader, an extruder, or the like, and the resulting molten and kneaded product is coarsely ground, and then ground using a jet mill or the like, and then passed through an air classifier to obtain toner particles having a desired particle size. More specifically, the kneading and pulverizing method is divided into a kneading step of kneading the toner forming materials including the white pigment and the binder resin, and a pulverizing step of pulverizing the kneaded mixture. If necessary, the method may include other steps such as a cooling step of cooling the kneaded mixture formed in the kneading step.
[0066] Toner particles are obtained by dispersing internal additives such as binder resin, white pigment, and release agent added as required by kneading and melting them in a twin-screw extruder or the like, pulverizing and classifying them by fine pulverizing means, heat-treating the surface of the toner particles under a hot air stream, and then adding and mixing external additives and charge adjusters as required. The circularity of the toner particles can be controlled by heat-treating them. For example, particles with the desired circularity can be obtained by adjusting the contact time with hot air as part of the heat treatment. This process is also called the "circularization process."
[0067] [Emulsification aggregation method] The emulsion aggregation method is a method for producing toner particles by mixing a dispersion of binder resin particles (hereinafter also referred to as "binder resin particles") dispersed with a surfactant or a dispersion stabilizer with a dispersion of white pigment particles (hereinafter also referred to as "white pigment particles") as necessary, aggregating them to a desired toner particle size, and further controlling the shape by fusing the binder resin particles together. Here, the binder resin particles may optionally contain a release agent, a charge control agent, etc. As a preferred method for producing the toner according to the present invention, an example of obtaining toner particles having a core-shell structure by using an emulsion aggregation method will be described below.
[0068] (1) A step of preparing a white pigment particle dispersion in which white pigment particles are dispersed in an aqueous medium (2) A step of preparing a resin particle dispersion (core / shell resin particle dispersion) in which binder resin particles, optionally containing internal additives, are dispersed in an aqueous medium. (3) A step of mixing a white pigment particle dispersion and a core resin particle dispersion to obtain a resin particle dispersion for aggregation, and aggregating and fusing the white pigment particles and binder resin particles in the presence of an aggregating agent to form aggregated particles as core particles (aggregation and fusion step). (4) A process of adding a dispersion of resin particles for shell containing binder resin particles for the shell layer to a dispersion containing core particles, and aggregating and fusing the particles for the shell layer to the surface of the core particles to form toner base particles having a core-shell structure (aggregation and fusion process). (5) This step is carried out as necessary. In the aging step, the associated particles obtained in the aggregation and fusion step are aged by thermal energy until they reach a desired shape to form toner particles. Specifically, the aging treatment is carried out by heating and stirring the system in which the associated particles are dispersed, and adjusting the heating temperature, stirring speed, heating time, etc., until the shape of the associated particles reaches a desired circularity. (6) A process of filtering the toner base particles from the toner base particle dispersion (toner base particle dispersion) and removing surfactants and the like (cleaning process) (7) Step of drying the toner base particles (drying step) (8) A step of adding an external additive to the toner base particles (an external additive treatment step). Toner particles having a core-shell structure can be obtained by first preparing core particles by aggregating and fusing binder resin particles for core particles and white pigment particles, and then adding binder resin particles for the shell layer to the dispersion of the core particles to aggregate and fuse the binder resin particles for the shell layer to the surface of the core particles to form a shell layer that covers the surface of the core particles. However, for example, toner particles formed from a single layer of particles can also be produced in the same manner without adding a dispersion of resin particles for shell in the above step (4).
[0069] [Two-component developer for electrostatic latent images] The toner for developing electrostatic images of the present invention can be used as a non-magnetic one-component developer, but can also be suitably employed in a two-component developer for developing electrostatic latent images containing a carrier.
[0070] (Career) The carrier particles are made of a magnetic material. Examples of the carrier particles include coated carrier particles having a core particle made of the magnetic material and a layer of a coating material that coats the surface of the core particle, and resin-dispersed carrier particles having a fine powder of a magnetic material dispersed in a resin. The carrier particles are preferably coated carrier particles from the viewpoint of suppressing adhesion of the carrier particles to the photoreceptor.
[0071] (Carrier core (core particles)) The core particles are made of a magnetic material, for example, a material that is strongly magnetized in a direction by a magnetic field. The magnetic material may be one or more types, and examples include ferromagnetic metals such as iron, nickel, and cobalt, alloys or compounds containing these metals, and alloys that become ferromagnetic when heat-treated.
[0072] Examples of the ferromagnetic metal or compound containing the same include iron, ferrite represented by the following formula (a), and magnetite represented by the following formula (b), in which M represents one or more monovalent or divalent metals selected from the group consisting of Mn, Fe, Ni, Co, Cu, Mg, Zn, Cd, and Li.
[0073] Formula (a): MO·Fe2O3 Formula (b): MFe2O4 Examples of alloys that become ferromagnetic when subjected to the above heat treatment include Heusler alloys such as manganese-copper-aluminum and manganese-copper-tin, and chromium dioxide.
[0074] The core particles are preferably various ferrites, because the specific gravity of the coated carrier particles is smaller than the specific gravity of the metal constituting the core particles, and therefore the impact force of stirring in the developing device can be reduced.
[0075] (Carrier coat resin) The carrier coat resin (coating material) may be one or more kinds. The coating material may be a known resin used for coating the core particles of the carrier particles. The coating material is preferably a resin having a cycloalkyl group from the viewpoint of reducing the moisture adsorption of the carrier particles and increasing the adhesion of the coating layer to the core particles. Examples of the cycloalkyl group include a cyclohexyl group, a cyclopentyl group, a cyclopropyl group, a cyclobutyl group, a cycloheptyl group, a cyclooctyl group, a cyclononyl group, and a cyclodecyl group.
[0076] Among these, a cyclohexyl group or a cyclopentyl group is preferred, and a cyclohexyl group is more preferred from the viewpoint of adhesion between the coating layer and the ferrite particles. The weight average molecular weight Mw of the resin is, for example, 10,000 to 800,000, and more preferably 100,000 to 750,000. The content of the cycloalkyl group in the resin is, for example, 10 to 90 mass %. The content of the cycloalkyl group in the resin can be measured, for example, by pyrolysis-gas chromatography / mass spectrometry (P-GC / MS) or 1 This can be determined by H-NMR or the like.
[0077] [Two-component developer] The two-component developer can be prepared by appropriately mixing toner particles and carrier particles so that the toner particle content (toner concentration) is 4.0 to 8.0% by mass. Examples of mixing equipment that may be used for the blending include a Nauta mixer, a W-cone and a V-blender.
[0078] [Image forming method] The image forming method of the present invention is characterized by using the toner for developing electrostatic images of the present invention, and can be suitably used in image forming methods using a general electrophotographic system.
[0079] For example, an electrostatic latent image formed electrostatically on an image carrier is visualized by charging a developer with a frictional charging member in a developing device to obtain a white toner image, which is then transferred onto a recording medium.Then, the white toner image transferred onto the recording medium is fixed to the recording material by a fixing process using a contact heating method, thereby obtaining a white visible image.
[0080] Examples of the fixing method include a so-called contact heating method, which includes a heat and pressure fixing method, a heat roll fixing method, and a pressure contact heat fixing method in which fixing is performed by a rotating pressure member containing a fixedly arranged heater.
[0081] In the fixing method of the heat roll fixing system, a fixing device is used that is composed of an upper roller with a heat source inside a metal cylinder made of iron or aluminum with a surface coated with fluororesin, and a lower roller made of silicone rubber. A linear heater is used as the heat source, and the surface temperature of the upper roller is heated to about 120 to 200°C by this heater. Pressure is applied between the upper roller and the lower roller, and the lower roller is deformed by this pressure, forming a nip.
[0082] The recording medium (also referred to as recording material, recording paper, recording paper, etc.) may be a commercially available product, and may be, for example, any product capable of holding a toner image formed by a known image forming method using an image forming apparatus, etc. Examples of recording media that can be used include plain paper ranging from thin paper to thick paper, coated printing paper such as high-quality paper, art paper, and coated paper, commercially available Japanese paper and postcard paper, plastic film for overhead projectors, cloth, aluminum vapor deposition film, PET film, and synthetic paper. The embodiments to which the present invention can be applied are not limited to the above-described embodiments, and can be modified as appropriate without departing from the spirit of the present invention. EXAMPLES
[0083] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. In the examples, the terms "parts" and "%" are used, but they represent "parts by mass" or "% by mass" unless otherwise specified.
[0084] <<Preparation of Toner>> [Preparation of toner base particles] <Preparation of toner base particles 1> Binder resin: styrene-n-butyl acrylate copolymer (Mw: 51000, Mn: 4000, Mw / Mn: 26) 100 parts by weight White pigment: Titanium oxide ET-500W (manufactured by Ishihara Sangyo Kaisha, Ltd.) 60 parts by weight Release agent: Paraffin wax (HNP-9: manufactured by Nippon Seiro Co., Ltd.) 10 parts by weight A continuous two-roll open-roll kneader "Kneedex" (manufactured by Mitsui Mining Co., Ltd., roll outer diameter: 14 cm, effective roll length: 80 cm) was used.
[0085] The operating conditions of the continuous two-roll open-roll mixer were: high-rotation roll (front roll) peripheral speed 75 r / min (32.97 m / min), low-rotation roll (back roll) peripheral speed 50 r / min (21.98 m / min), roll gap at the end of the kneaded material supply port side 0.1 mm. The heating medium temperature and cooling medium temperature in the rolls were 135°C on the raw material input side of the high-rotation roll and 90°C on the kneaded material discharge side, and 35°C on the raw material input side of the low-rotation roll and 35°C on the kneaded material discharge side. The supply rate of the raw material mixture was 10 kg / hour, and the average residence time was about 6 minutes.
[0086] The obtained kneaded material was cooled to below 20°C while being rolled with a cooling roll, and the cooled molten kneaded material was coarsely pulverized to 3 mm using a Rotoplex (manufactured by Toa Machinery Co., Ltd.), and then pulverized using a fluidized tank jet mill "AFG-400" (manufactured by Alpine Co., Ltd.) and classified using a rotor type classifier "TTSP" (manufactured by Alpine Co., Ltd.) so that the average particle size of the toner particles containing the external additives described below was 7.0 μm.
[0087] Thereafter, in the circularization process, a hot air sphering device (Surfusing System SFS-3 type: manufactured by Nippon Pneumatic Mfg. Co., Ltd.) was used to perform hot air treatment under conditions of an inlet temperature of 200°C and a contact time with hot air of 0.01 seconds so that the average circularity of the toner particles became 0.937, thereby obtaining toner base particles 1.
[0088] <Preparation of toner base particles 2 to 12 and 15 to 20> In preparing toner base particle 1, the mass parts of the white pigment, the inlet temperature of the hot air treatment in the circularization step, and the contact time with the hot air were changed as shown in Table I, and the toner particles were classified to have an average particle size of 7.0 μm. Toner base particles 2 to 12 and 15 to 20 were prepared in the same manner as in preparing toner base particle 1.
[0089] <Preparation of toner base particles 13> (Preparation of Resin Particle Dispersion) First, a resin particle dispersion was prepared as follows.
[0090] Styrene 308 parts by weight n-Butyl acrylate 100 parts by mass Acrylic acid 4 parts by mass Dodecanethiol 3 parts by mass Propanediol diacrylate 1.5 parts by weight The above components were mixed and dissolved, and the resulting mixture was poured into an aqueous solution of 4 parts of anionic surfactant (Neogen SC, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) dissolved in 550 parts of ion-exchanged water to form an emulsion in a flask. After mixing for 10 minutes, an aqueous solution of 6 parts of ammonium persulfate dissolved in 350 parts of ion-exchanged water was poured into the mixture, followed by nitrogen replacement. The flask was then heated in an oil bath with stirring until the contents reached 75°C, and emulsion polymerization was continued for 5 hours.
[0091] In this manner, a resin particle dispersion (1) was obtained, which was a styrene-acrylic resin dispersion (resin particle concentration: 40% by mass) in which resin particles having an average particle size of 195 nm and a weight-average molecular weight (Mw) of 41,000 were dispersed.
[0092] (Preparation of White Pigment Particle Dispersion) White pigment (titanium oxide ET-500W (Ishihara Sangyo Kaisha, Ltd.)) 30 parts by weight Anionic surfactant (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., Neogen RK) 0.3 parts by mass Ion-exchanged water 100 parts by weight A 0.1 mol / L aqueous solution of hydrogen chloride was added to ion-exchanged water to adjust the pH to 4.5, after which a white pigment and an anionic surfactant were added and dispersed in a round stainless steel flask for 5 minutes using a homogenizer (Ultra-Turrax T50, manufactured by IKA Corporation) to obtain a white pigment particle dispersion (1).
[0093] (Preparation of Release Agent Particle Dispersion) Paraffin wax (HNP-9: manufactured by Nippon Seiro Co., Ltd.) 100 parts by weight Anionic surfactant (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., Neogen RK) 1.5 parts by mass Ion-exchanged water 400 parts by weight The above components were dispersed in a round stainless steel flask using a homogenizer (Ultra Turrax T50: manufactured by IKA) for 20 minutes, and then dispersed using a pressure discharge type homogenizer to prepare a release agent particle dispersion liquid (1) in which the release agent was dispersed.
[0094] (Preparation of toner base particles 13) Resin particle dispersion (1) 250 parts by mass Release agent particle dispersion (1) 25 parts by weight White pigment particle dispersion (1) 175 parts by weight Anionic surfactant (TeycaPower) 1.0 parts by weight Ion-exchanged water 100 parts by weight
[0095] The above raw materials were placed in a cylindrical stainless steel container, and dispersed and mixed for 5 minutes using a homogenizer (IKA, Ultra Turrax T50) with the homogenizer rotation speed set to 4000 rpm and shear force applied. Next, 1.5 parts of a 10% nitric acid aqueous solution of polyaluminum chloride was gradually added dropwise, and the homogenizer rotation speed was set to 5000 rpm while stirring, and the temperature was raised at a rate of 0.5°C / min, and the particle size of the aggregated particles was appropriately measured using a "Multisizer 3" (Beckman Coulter). The heating time was adjusted so that the average particle size of the toner particles containing the external additive described below was 7.0 μm, and then 2 parts by mass of a 40% aqueous solution of 3-hydroxy-2,2'-iminodisuccinic acid tetrasodium was added to stop the particle size growth. Furthermore, the internal temperature was raised to 85°C, and the heating time was adjusted using a "FPIA-3100" (Sysmex) so that the average circularity of the toner particles was 0.968. Thereafter, the reaction liquid was cooled to room temperature at a rate of 10° C. / min, and the reaction liquid was repeatedly filtered and washed, and then dried to obtain toner base particles 13.
[0096] <Preparation of Toner Base Particles 14> Toner base particles 14 were prepared in the same manner as in the preparation of toner base particles 13, except that the amount of white pigment particle dispersion (1) was changed from 175 parts by mass to 210 parts by mass.
[0097] [External addition process] For the toner base particle 1 prepared as described above, 0.8 parts by mass of small-diameter silica microparticles "RX-200" (fumed silica, HMDS (hexamethyldisilazane) treated, number average particle size 12 nm, manufactured by Nippon Aerosil Co., Ltd.) were added as an external additive to 100 parts by mass of the toner base particle, and added to a Henschel mixer model "FM20C / I" (manufactured by Nippon Coke and Engineering Co., Ltd.), and the mixing speed (rotation speed) was set so that the blade tip peripheral speed was 60 m / s, and the mixture was stirred for 1 minute, and then the rotation speed was set to 40 m / s and the mixture was stirred for 19 minutes to produce toner 1. Toners 2 to 20 were prepared by varying the blade tip peripheral speed from 60 m / s to the mixing speeds shown in Table I.
[0098] The product temperature during external addition mixing was set to 40°C ± 1°C. When it reached 41°C, cooling water was flowed into the outer bath of the Henschel mixer at a flow rate of 5 L / min, and when it reached 39°C, cooling water was flowed at 1 L / min, thereby controlling the temperature inside the Henschel mixer.
[0099] [Measurement of toner characteristics] For each of the produced toners 1 to 20, the average circularity, the number of toner particles having a particle size of 2.0 μm or less (number %) after ultrasonic (US) dispersion, the average particle size of the toner particles, and the true density of the toner were measured by the methods described above. The details of the toner are shown in Table I. In the following Tables 1 and 2, "the present invention" in the remarks column for Toner Nos. 3 to 9, 11, 13 and 14 will be read as "Reference Example."
[0100] [Table 1]
[0101] "evaluation" For each of the toners 1 to 20 prepared above, the concealing property and the cleanability were evaluated, and further, the toner filming on the photoreceptor and the maximum image density difference were evaluated.
[0102] <Concealment> Using an image forming device "bizhub PRESSPRO C1100" (manufactured by Konica Minolta) modified for white toner output, vertical stripe images were printed on a Tencolor 152 (g / m) A3 sheet in landscape mode in an environment with a temperature of 23°C and a humidity of 50%. 2 ) with a monochrome toner amount of 10g / m 2 A copy test was conducted to ensure that the results were as follows:
[0103] The leading and trailing edge images of the output solid image were measured using a reflection densitometer "FD-7" (Konica Minolta, Inc.) and the CIE1976 (L * a * b * ) color system, L *The hiding power (whiteness) was evaluated based on the value, and the difference was calculated. If the value was rated as .circle-solid., .smallcircle., or .DELTA., the sample was deemed to be acceptable since it had no practical problems.
[0104] ◎: L at the front and rear ends * The difference is 5 or less ○: L at the front and rear ends * The difference is greater than 5 and less than 10 △: L at the front and rear ends * The difference is greater than 10 and less than or equal to 15 ×: L at the front and rear ends * The difference is higher than 15
[0105] <Toner filming on the photoreceptor> Using the image forming apparatus, 100,000 copies of a character chart equivalent to a printing rate of 5% were printed, and then the surface of the photoconductor was visually observed and a halftone image was printed, and the toner filming on the photoconductor was evaluated based on the following evaluation criteria. If the result was ⊚ or ◯, the product was deemed to be acceptable since there was no practical problem.
[0106] ◎: No streak defects are observed in the halftone image along the photoconductor axis. ○: 1 to 4 axial image streak defects less than 1 cm in length in the photoconductor axial direction and less than 1 mm in width in the paper feed direction are visible in the halftone image. ×: Five or more image streak defects of less than 1 cm in length in the photoconductor axial direction and less than 1 mm in width in the paper feed direction are visually observed in a halftone image. Table I shows the number of image streak defects in the axial direction of the photoreceptor that are less than 1 cm in length and less than 1 mm in width in the paper feed direction.
[0107] <Maximum image density difference> A4 quality paper (65g / m 2 A test image with five 3cm-wide vertical solid band images was printed continuously on a paper substrate (durability printing) for 100,000 copies, and the entire solid image was output using an evaluation device after the durability printing. The image density of the output solid image was measured at six points in total, five points corresponding to the bands during durability testing and one point corresponding to the non-bands, using a Macbeth reflection densitometer "RD-918". The maximum image density difference was then calculated using the following formula.
[0108] Maximum image density difference = ("Image density at the point with the highest image density among the five image densities at the portion corresponding to the band portion during durability test" - "Image density at the portion corresponding to the non-band portion") Based on the calculated maximum image density difference, a value of 0.12 or less was judged to be practical and pass the test according to the following criteria.
[0109] Here, if the maximum image density difference is small, it can be considered that the cleaning ability is high and the occurrence of image defects due to toner slipping through is small. If the maximum image density difference is 0.12 or less, there is no problem in practical use, so it is judged as passing. The table shows the maximum image density difference.
[0110] ◎: Maximum image density difference is 0.03 or less ○: Maximum image density difference is greater than 0.03 and equal to or less than 0.08 △: Maximum image density difference is greater than 0.08 and less than 0.12 ×: Maximum image density difference is greater than 0.12
[0111] [Table 2]
[0112] From Table II, when the toner of the present invention is used, the concealment properties (L * It can also be seen that when the toner of the present invention is used, there is little toner filming and little difference in maximum image density, and cleaning properties are also excellent.
Claims
1. A toner for developing an electrostatic latent image, which comprises toner particles containing at least a white pigment, and when the toner particles are subjected to ultrasonic dispersion treatment in water, the toner particles satisfy the following condition (3) and have a true density of 1.50 to 2.00 g / cm 3 A toner for developing electrostatic latent images, characterized in that Condition (3): The average circularity is within a range of 0.930 to 0.950, and the number of particles having a particle diameter of 2.0 μm or less is 30% or less by number.
2. 2. An electrophotographic image forming method, comprising using the toner for developing an electrostatic latent image according to claim 1.
Citation Information
Patent Citations
Electrostatic charge image developing toner, electrostatic charge image developer, electrostatic charge image developer unit and image forming method
JP2002311648A
Dry toner, method for manufacturing the same, developing method and transfer method
JP2003177568A
Toner, developer, developing device and image forming apparatus
JP2005257976A
Toner for electrostatic latent image development and image forming method
JP2006284922A
Toner for electrostatic image development, developer for electrostatic image development and image forming method