toner
The toner design with a core-shell structure, utilizing specific monomer units, addresses the issue of irregular oxazoline group orientation, resulting in improved fluidity and charge stability.
Patent Information
- Application Number
- JP2020128076
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-29
- Publication Date
- 2024-09-17
- Estimated Expiration
- 2040-07-29
AI Technical Summary
Toner particles with a shell formed using a resin containing an oxazoline group exhibit insufficient fluidity due to irregular orientation of the oxazoline groups, leading to uneven charging and increased electrostatic adhesion forces.
A toner design with a core containing a resin A having a long-chain alkyl group and a shell containing a resin B with an oxazoline group, where the monomer units are within specific ratios, ensuring controlled orientation of the oxazoline groups to enhance fluidity and charge amount.
The toner achieves high charge amount and excellent fluidity, maintaining consistent charging properties even under varying temperature and humidity conditions.
Smart Images

Figure 0007551379000015 
Figure 0007551379000003 
Figure 0007551379000011
Abstract
Description
[Technical field]
[0001] The present invention relates to a toner used in an electrophotographic image forming apparatus. [Background technology]
[0002] In recent years, there has been an increasing demand for faster electrophotographic image forming apparatuses. In order to meet this demand, toners having excellent charging properties in a charging process have been developed.
[0003] A method of externally adding resin particles to toner particles is known for the purpose of improving the charging stability of the toner. However, the externally added resin particles are generally prone to detachment from the surface of the toner particles. When the resin particles detach from the surface of the toner particles during image formation, the toner particles tend to adhere to the surfaces of various members, and the charge amount of the toner tends to decrease.
[0004] Therefore, in order to improve the charge amount of the toner, a toner having toner particles in which an easily charged resin is fixed to the core surface of the toner particle to form a shell has been attracting attention. Patent Document 1 proposes a toner in which a shell is formed using a resin containing an oxazoline group, and describes that an unopened oxazoline group has a cyclic structure and exhibits strong positive charging properties. Therefore, a toner in which a shell is formed using a resin containing an oxazoline group can have a high charge amount. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent Publication 2017-151412 Summary of the Invention [Problem to be solved by the invention]
[0006] However, as a result of extensive investigations by the present inventors into the toner described in Patent Document 1, it has been found that the fluidity of the toner may be insufficient in some cases.
[0007] The present invention provides a toner that can have a high charge amount and also has excellent fluidity. [Means for solving the problem]
[0008] The present invention provides a toner having toner particles each having a core containing a resin component and a shell covering a surface of the core, The resin component contains a resin A having a monomer unit A represented by the following formula (1), a content ratio of the monomer unit A in the resin A is 2.0% by mass or more and 80.0% by mass or less, The shell contains a resin B having a monomer unit B represented by the following formula (2): death, The SP value of the resin A is A The SP value of the resin B is SP B Then, SP B -SP A , 0.00(J / cm 3 ) 0.5 More than 6.00(J / cm 3 ) 0.5 is less than or equal to A toner characterized by:
[0009] [ka]
[0010] (In formula (1), R 1 represents an alkyl group having 12 to 36 carbon atoms, and R 2 is hydrogen or a methyl group. 3 is hydrogen, a methyl group, or an ethyl group. Effect of the Invention
[0011] According to the present invention, it is possible to provide a toner that can have a high charge amount and also has excellent fluidity. [Brief description of the drawings]
[0012] [Figure 1] 2 is a schematic diagram of a cross section of a toner particle for explaining a supposed mechanism by which the effect of the present invention is exerted. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The expressions "xx or more and xx or less" or "xx to xx" expressing a numerical range mean a numerical range including the endpoints, that is, the lower limit and the upper limit, unless otherwise specified.
[0014] (Meth)acrylate means acrylate and / or methacrylate, and (meth)acrylic acid means acrylic acid and / or methacrylic acid.
[0015] When numerical ranges are stated in stages, the upper and lower limits of each numerical range can be combined in any way.
[0016] A monomer unit is a unit that constitutes a polymer, and refers to the form of a monomer (polymerizable monomer) that has reacted. For example, one section of carbon-carbon bonds in the main chain of a polymer in which a vinyl monomer has been polymerized is one monomer unit. A vinyl monomer can be represented by the following formula (Z), and a vinyl monomer unit is a structural unit of a polymer, and is in the form of a monomer represented by the following formula (Z) that has reacted. A monomer unit may also be simply referred to as a "unit."
[0017] [ka]
[0018] (In formula (Z), R Z1represents hydrogen or an alkyl group (preferably an alkyl group having 1 to 3 carbon atoms, more preferably a methyl group); R Z2 represents an optional substituent. The vinyl resin refers to a resin whose constituent unit is the vinyl monomer unit.
[0019] <Assumed mechanism by which the effects of the present invention manifest> FIG. 1 is a schematic diagram of a cross section of a toner particle for explaining a supposed mechanism for realizing the effects of the present invention.
[0020] Figure 1(A) is a schematic diagram of a cross section of a toner particle in which a monomer unit 3 containing an oxazoline group is contained in the shell 2, and a resin having a long-chain alkyl group is not contained in the core 1 of the toner particle. The oxazoline groups present in the shell 2 are oriented in irregular directions, which indicates that the toner particle is likely to have a large imbalance between strongly and weakly charged areas.
[0021] 1(B) is a schematic diagram of a cross section of a toner particle in which a monomer unit 3 containing an oxazoline group is contained in the shell 2, and the core 1 of the toner particle contains a resin having a long-chain alkyl group. The core of the toner particle contains a long-chain alkyl group 4, and a repulsive force 5 is generated between the long-chain alkyl group 4 and the oxazoline group present in the shell 2, which indicates that many of the oxazoline groups tend to face outward from the toner particle.
[0022] The present inventors speculate as follows about the mechanism by which the effects of the present invention are exerted.
[0023] When the core of the toner particle contains a resin A having a specific ratio of the monomer unit A represented by formula (1), the hydrophobicity of the core is easily maintained. 1This is because the oxazoline group in the shell is a long-chain alkyl group. This generates a repulsive force between the oxazoline group in the shell and the long-chain alkyl group in the toner core, and many of the oxazoline groups tend to face outward from the toner particles. As a result, it is presumed that the bias between the strongly charged and weakly charged parts of the toner particles is reduced, and the electrostatic adhesion of the toner is reduced, resulting in a toner with excellent fluidity.
[0024] In addition, when the shell of the toner particle contains resin B having monomer unit B represented by formula (2), a toner having a high charge amount is easily obtained. This is presumably because the oxazoline group in monomer unit B is a functional group that is easily charged.
[0025] <Background to the invention> Toner particles having a shell containing a resin containing an oxazoline group tend to have a high charge amount. The present inventors believe that this is because the polarity of the oxazoline group present in the shell is high. When the toner has a high charge amount, it tends to adhere quickly to a developing roller, a photoconductor, etc., and tends to be a toner that can output high image quality even in high-speed printing.
[0026] However, the present inventors have found through their investigations that toners having such a high charge amount may tend to have reduced fluidity. The reason why the fluidity tends to decrease is believed to be that the oxazoline groups in the shell tend to be oriented in an irregular direction, which increases the bias between the strongly charged and weakly charged parts in the toner particles. The reason why the oxazoline groups in the shell tend to be oriented in an irregular direction is believed to be that the direction in which the oxazoline groups are oriented is not controlled due to the small interaction between the core containing the resin component and the oxazoline groups in the shell (FIG. 1(A)). It is presumed that the bias in the charge in the toner particles increases the electrostatic adhesion of the toner, which reduces the fluidity of the toner.
[0027] Therefore, in order to provide a toner having a high charge amount and excellent fluidity, the present inventors have studied a toner in which the direction of the oxazoline group present in the shell is controlled and the electrostatic adhesion is appropriately maintained. As a result of intensive research, the inventors have arrived at the idea of using toner particles having a core containing a resin A having a monomer unit A of a (meth)acrylate having a long-chain alkyl group, and a shell containing a resin B having a monomer unit B containing an oxazoline group. When the shell contains a resin B containing an oxazoline group, the toner is likely to have a high charge amount. In addition, it is speculated that when the core contains a resin A having a monomer unit A having a long-chain alkyl group, a repulsive force is generated between the long-chain alkyl group present in the core and the oxazoline group present in the shell. It is speculated that this repulsive force makes it easier for many of the oxazoline groups to face toward the outside of the toner particles, and makes it difficult for the oxazoline groups in the shell to face in an irregular direction (FIG. 1(B)). As a result, it is presumed that the imbalance between strongly charged and weakly charged areas in the toner particles is reduced, and the electrostatic adhesion of the toner is reduced, resulting in a toner with excellent fluidity.
[0028] As a result of extensive investigation into the conditions under which a toner with excellent fluidity can be obtained, it was found that a desired toner can be obtained by having the above shell and containing a (meth)acrylate unit A having a long-chain alkyl group in the above resin A within a specific range. Such a toner has a high charge amount, and it is believed that sufficient repulsion occurs between the (meth)acrylate unit A having a long-chain alkyl group and the oxazoline group, and a toner with excellent fluidity can be obtained not only under normal temperature and normal humidity conditions but also under high temperature and high humidity conditions. It is also presumed that the repulsion that exhibits excellent fluidity becomes larger as the adhesion between the core and shell becomes stronger.
[0029] <Core> The toner particles have a core containing a resin component. In order to ensure that the core contains appropriate amounts of a release agent, a colorant, etc., the content of the resin component in the core is preferably 70.0 to 95.0% by mass.
[0030] The resin component contains a resin A having a monomer unit A represented by formula (1).
[0031] Resin A can be contained as a resin component of the toner by, for example, carrying out a polymerization reaction on a monomer composition containing polymerizable monomer A described later and using the resin obtained as a raw material for toner production.
[0032] The resin component is preferably a binder resin. That is, the toner has toner particles having a core containing a binder resin and a shell covering the surface of the core, and the binder resin preferably contains resin A.
[0033] <Resin A and Monomer Unit A> Resin A contains a monomer unit A represented by the above formula (1). 1 It is presumed that when R is an alkyl group having 12 to 36 carbon atoms, a repulsive force with the oxazoline group, which has a relatively high polarity, is easily generated, and a toner having excellent fluidity is easily obtained. 1 ) is also written as a long-chain alkyl group.
[0034] In addition, the content of the monomer unit A in the resin A is 2.0% by mass or more and 80.0% by mass or less. When the content of the monomer unit A in the resin A is 2.0% by mass or more, a toner having excellent fluidity is easily obtained. Therefore, it is 2.0% by mass or more, preferably 5.0% by mass or more, more preferably 10.0% by mass or more, more preferably 30.0% by mass or more, and even more preferably 50.0% by mass or more. Furthermore, when it is 80.0% by mass or less, the polarity of the resin A is not too low, and the adhesion between the resin A and the shell is easily maintained appropriately. As a result, a toner having excellent fluidity is easily obtained. Therefore, it is 80.0% by mass or less, preferably 75.0% by mass or less, and even more preferably 70.0% by mass or less.
[0035] In addition, R in formula (1)1 R is an alkyl group having 12 to 36 carbon atoms. 1 When the carbon number of the alkyl group of R1 is 12 or more, it is considered that the repulsion with the oxazoline group present in the shell is sufficiently large, and a toner having excellent fluidity is easily obtained. Therefore, the carbon number is 12 or more, preferably 16 or more, and more preferably 18 or more. Furthermore, when the carbon number of the alkyl group of R1 is 36 or less, the adhesion between the resin A and the shell is easily maintained appropriately, and a toner having excellent fluidity is easily obtained. Therefore, the carbon number is 36 or less, preferably 30 or less, more preferably 26 or less, and even more preferably 22 or less. Furthermore, it is preferable that the alkyl group having 12 to 36 carbon atoms is a linear alkyl group having 12 to 36 carbon atoms. Furthermore, it is preferable that R2 is hydrogen.
[0036] Resin A having monomer unit A can be incorporated as a monomer unit of resin A by vinyl polymerization of a (meth)acrylic acid ester having an alkyl group having 12 to 36 carbon atoms as a polymerizable monomer (hereinafter also referred to as polymerizable monomer A). That is, resin A is preferably a vinyl resin.
[0037] The polymerizable monomer A is a (meth)acrylate having an alkyl group having 12 to 36 carbon atoms.
[0038] Examples of (meth)acrylates having an alkyl group having 12 to 36 carbon atoms include (meth)acrylic acid esters having a linear alkyl group having 12 to 36 carbon atoms [stearyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate, heneicosanyl (meth)acrylate, behenyl (meth)acrylate, lignoceryl (meth)acrylate, ceryl (meth)acrylate, octacosyl (meth)acrylate, myricyl (meth)acrylate, doriaconta (meth)acrylate, etc.].
[0039] The polymerizable monomer A and the monomer unit A may be used alone or in combination of two or more kinds.
[0040] When the resin A has two or more kinds of monomer units A, the content of the monomer units A in the resin A is the sum of the respective contents.
[0041] <Monomer unit C> It is preferable that the resin A contains another monomer unit C which does not fall under the category of the monomer unit A.
[0042] Monomer unit C can be incorporated as a monomer unit of resin A by polymerizing (vinyl polymerization) a corresponding polymerizable monomer (hereinafter also referred to as polymerizable monomer C. Specific examples will be described later.) as a polymerizable monomer.
[0043] Moreover, the monomer unit C is preferably at least one monomer unit selected from the group consisting of a monomer unit represented by the following formula (3), a monomer unit represented by the following formula (4), and a monomer unit represented by the following formula (5).
[0044] [ka]
[0045] (In formula (3), R 4 represents hydrogen or an alkyl group having 1 to 4 carbon atoms; R 5 represents hydrogen or a methyl group. 6 represents a hydrogen or a methyl group.) By containing at least one monomer unit C selected from the group consisting of the above, the adhesion between the resin A in the toner core and the resin B in the shell is likely to be improved, making it easier to obtain a toner with excellent fluidity.
[0046] From the viewpoint of easily obtaining a toner having excellent fluidity, R 4 More preferably, R is a hydrogen atom or a linear alkyl group having 4 carbon atoms (i.e., an n-butyl group). 6More preferably, is a methyl group.
[0047] More preferably, the monomer unit C is at least one monomer unit selected from the group consisting of a monomer unit represented by formula (4) and a monomer unit represented by formula (5).
[0048] Further, the monomer unit C is more preferably a monomer unit represented by the formula (4).
[0049] In addition, the content of the monomer unit C in the resin A is preferably 25.0% by mass or more and 95.0% by mass or less. When the content is 25.0% by mass or more, the adhesion between the resin A in the toner core and the resin B in the shell is likely to be increased, and a toner with excellent fluidity is likely to be obtained. Therefore, it is preferably 25.0% by mass or more, and more preferably 40.0% by mass or more. When it is 95.0% by mass or less, the charge charged in the shell is unlikely to move excessively to the core of the toner particle, and a toner with a high charge amount is likely to be obtained. Therefore, it is preferably 95.0% by mass or less, more preferably 80.0% by mass or less, more preferably 70.0% by mass or less, and even more preferably 60.0% by mass or less.
[0050] Examples of the polymerizable monomer C other than the polymerizable monomer A capable of forming the resin A include the monomers listed below.
[0051] Styrenic monomers such as styrene, α-methylstyrene, and divinylbenzene, unsaturated carboxylic acid esters such as methyl acrylate, butyl acrylate, methyl methacrylate, 2-hydroxyethyl methacrylate, t-butyl methacrylate, and 2-ethylhexyl methacrylate, unsaturated carboxylic acids such as acrylic acid and methacrylic acid, unsaturated dicarboxylic acids such as maleic acid, unsaturated dicarboxylic anhydrides such as maleic anhydride, nitrile vinyl monomers such as acrylonitrile, halogen-containing vinyl monomers such as vinyl chloride, nitro vinyl monomers such as nitrostyrene, and monomers having two polymerizable unsaturated groups such as divinylbenzene and hexanediol diacrylate. These monomers can be used alone or in combination.
[0052] <Acid value of resin A> The acid value of the resin A is preferably 20.0 mgKOH / g or less. When the acid value of the resin A is 20.0 mgKOH / g or less, the reaction between the oxazoline group present in the shell and the carboxyl group in the resin A is unlikely to occur, and a toner having excellent fluidity is likely to be obtained. The mechanism of the effect on the toner caused by the reaction between the oxazoline group and the carboxyl group is considered to be as follows.
[0053] When an oxazoline group present in the shell reacts with a carboxyl group present in resin A, the oxazoline group and the carboxyl group form an amide ester bond. The portion where the amide ester bond is formed has a different charge amount from the portion where other oxazoline groups are present due to a change in structure. Furthermore, since the amide structure derived from the oxazoline group is covalently bonded to resin A, the amide structure faces toward resin A, that is, toward the inside of the toner particle. It is considered that the change in the structure of the oxazoline group and the fact that the amide structure derived from the oxazoline group faces toward the inside of the toner particle cause a bias in the charge amount in the toner particle, making it easier to obtain a toner with a large electrostatic adhesion force.
[0054] For the above reasons, the acid value of resin A is preferably 20.0 mgKOH / g or less, more preferably 15.0 mgKOH / g or less, more preferably 10.0 mgKOH / g or less, and even more preferably 8.0 mgKOH / g or less. The lower limit is not particularly limited, and is 0.0 mgKOH / g or more. That is, the acid value of resin A is preferably 0.0 mgKOH / g or more and 20.0 mgKOH / g or less. The acid value of resin A can be controlled by the type and / or amount of raw materials used in producing resin A.
[0055] <Other forms of Resin A> Resin A is preferably a vinyl resin. In addition, when resin A is a vinyl resin, resin A may be a part of a hybrid resin (a hybrid resin of resin A, which is a vinyl resin, and a resin other than a vinyl resin), which is bonded with a resin other than a vinyl resin, such as polyester. In that case, the content of resin A in the hybrid resin is 50.0% by mass or more. The content is more preferably 80.0% by mass or more, and even more preferably 95.0% by mass or more. Examples of the bond include a covalent bond.
[0056] Resin A may contain monomer unit B, which is a characteristic monomer unit of resin B and is represented by the above formula (2). In this case, the content of monomer unit B in resin A is preferably 9.9% by mass or less. When the content of monomer unit B in resin A is 9.9% by mass or less, the hydrophobicity of the core in the toner particle is easily maintained appropriately, and a toner having excellent fluidity is easily obtained. Therefore, it is preferably 9.9% by mass or less, more preferably 5.0% by mass or less, more preferably 1.0% by mass or less, more preferably 0.1% by mass or less, and even more preferably 0.0% by mass. 0.0% by mass means that resin A does not contain monomer unit B.
[0057] Other resins that can be used in combination as a resin component other than resin A are not particularly limited. Examples of other resins include polyester resin, polyamide resin, furan resin, epoxy resin, xylene resin, silicone resin, etc. Although multiple types of resins may be used by combining resin A with these resins, it is preferable that the content of resin A in the toner is 30.0% by mass or more and 90.0% by mass or less. When the content is 30.0% by mass or more, the repulsive force between the long-chain alkyl group and the oxazoline group is sufficiently generated, and a toner having excellent fluidity is easily obtained. Therefore, it is preferable that the content is 30.0% by mass or more, more preferably 40.0% by mass or more, more preferably 50.0% by mass or more, more preferably 70.0% by mass or more, and even more preferably 75.0% by mass or more. In addition, when it is 90.0% by mass or less, the charge amount of the toner is easily maintained appropriately. Therefore, it is preferable that the content is 90.0% by mass or less, and more preferably 85.0% by mass or less.
[0058] As described above, since a toner having excellent fluidity is easily obtained, the content of resin A in the resin components contained in the core according to the present invention is preferably 50.0% by mass or more. The content is more preferably 60.0% by mass or more, more preferably 75.0% by mass or more, and even more preferably 90.0% by mass or more. There is no particular upper limit, and it is 100.0% by mass. The content of 100.0% by mass means that the resin component contained in the core according to the present invention is only resin A.
[0059] The resin component may contain multiple types of resin A. When the resin component contains multiple types of resin A, the total mass of the resins corresponding to resin A is defined as the content of resin A.
[0060] When a polyester is used in combination with the resin component, for example, the polyester can be produced by carrying out a condensation polymerization reaction using a divalent carboxylic acid or a derivative thereof and a divalent alcohol as constituent components. Alternatively, the polyester may be obtained by carrying out a condensation polymerization reaction containing a monovalent or trivalent or higher carboxylic acid or a derivative thereof, and a monovalent or trivalent or higher alcohol as constituent components.
[0061] Examples of divalent carboxylic acids include aliphatic dicarboxylic acids such as maleic acid, fumaric acid, itaconic acid, oxalic acid, malonic acid, succinic acid, dodecylsuccinic acid, dodecenylsuccinic acid, adipic acid, azelaic acid, sebacic acid, and decane-1,10-dicarboxylic acid, and aromatic dicarboxylic acids such as phthalic acid, tetrahydrophthalic acid, hexahydrophthalic acid, tetrabromophthalic acid, tetrachlorophthalic acid, HET acid, himic acid, isophthalic acid, terephthalic acid, and 2,6-naphthalenedicarboxylic acid.
[0062] Furthermore, examples of the derivatives of divalent carboxylic acids include acid halides, esters and acid anhydrides of the above-mentioned aliphatic dicarboxylic acids and aromatic dicarboxylic acids.
[0063] Examples of trivalent or higher carboxylic acids and anhydrides thereof include trimellitic acid, trimellitic anhydride, pyromellitic acid, and pyromellitic anhydride.
[0064] Examples of dihydric alcohols include acyclic aliphatic diols such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, diethylene glycol, dipropylene glycol, triethylene glycol, and neopentyl glycol; and aromatic diols such as bisphenols such as bisphenol A and bisphenol F, alkylene oxide adducts of bisphenols, and aralkylene glycols such as xylylene glycol.
[0065] <shell> The shell contains a resin B having a monomer unit B represented by formula (2). As a method for incorporating the resin B as the shell of the toner particles, for example, a method of dispersing the toner cores in a solution in which the resin B is dispersed, and stirring and heating in that state can be mentioned.
[0066] <Resin B and Monomer Unit B> Resin B has a monomer unit B represented by formula (2). By having the monomer unit B, a toner having a high charge amount is easily obtained.
[0067] In addition, since a toner having a high charge amount is easily obtained, the toner of the present invention is preferably a positively charged toner, since resin B is a resin that is easily positively charged.
[0068] R in Equation (2) 3 is hydrogen, a methyl group, or an ethyl group. 3 is preferably a hydrogen atom or a methyl group. 3 When is hydrogen, a methyl group, or an ethyl group, the mobility of the oxazoline group represented by formula (2) is sufficiently maintained, so that the oxazoline group tends to uniformly face outward from the toner particle, and a toner having excellent fluidity is easily obtained.
[0069] Resin B having monomer unit B can be incorporated as a monomer unit of resin B by vinyl polymerization of a vinyl monomer having an oxazoline group as a polymerizable monomer (hereinafter also referred to as polymerizable monomer B). That is, resin B is preferably a vinyl resin.
[0070] The polymerizable monomer B is a vinyl monomer having an oxazoline group.
[0071] Examples of vinyl monomers having an oxazoline group include 2-vinyl-2-oxazoline and 2-isopropenyl-2-oxazoline.
[0072] The polymerizable monomer B and the monomer unit B may be used alone or in combination of two or more kinds.
[0073] When the resin B has two or more kinds of monomer units B, the content of the monomer units B in the resin B is the sum of the respective contents.
[0074] The content of the monomer unit B in the resin B is preferably 10.0% by mass or more and 95.0% by mass or less. When the content is 10.0% by mass or more, a toner having a high charge amount is easily obtained. Therefore, it is preferably 10.0% by mass or more, more preferably 30.0% by mass or more, more preferably 40.0% by mass or more, more preferably 50.0% by mass or more, and even more preferably 70.0% by mass or more. In addition, when it is 95.0% by mass or less, the oxazoline group in the resin B is easily directed to the outside of the toner particle, and a toner having excellent fluidity is easily obtained. Therefore, it is preferably 95.0% by mass or less, and more preferably 90.0% by mass or less.
[0075] <Monomer unit D> It is preferable that the resin B contains another monomer unit D which does not fall under the category of the monomer unit B.
[0076] Monomer unit D can be incorporated as a monomer unit of resin B by polymerizing (vinyl polymerization) a corresponding polymerizable monomer (hereinafter also referred to as polymerizable monomer D. Specific examples will be described later.) as a polymerizable monomer.
[0077] The monomer unit D is preferably at least one monomer unit selected from the group consisting of a monomer unit represented by the following formula (4) and a monomer unit represented by the following formula (6).
[0078] [ka]
[0079] (In formula (4), R 6 represents hydrogen or a methyl group. 7 represents hydrogen or an alkyl group having 1 to 4 carbon atoms; R 8 represents a hydrogen or a methyl group.) By containing at least one monomer unit D selected from the above group, the adhesion between the resin A in the core and the resin B in the shell is likely to be improved, making it easier to obtain a toner with excellent fluidity.
[0080] From the viewpoint of easily obtaining a toner having a high charge amount and excellent fluidity, R 6 More preferably, R is a methyl group. 7 is a methyl group, and R 8 More preferably, is a methyl group.
[0081] The monomer unit C is represented by the following formula (6), in which R 7 is a methyl group, and R 8 It is more preferable that the monomer unit is a methyl group.
[0082] From the viewpoint of easily obtaining a toner having a high charge amount and excellent fluidity, the content of monomer unit D in resin B is preferably 10.0% by mass or more and 70.0% by mass or less, more preferably 10.0% by mass or more and 50.0% by mass or less, more preferably 10.0% by mass or more and 30.0% by mass or less, and even more preferably 10.0% by mass or more and 20.0% by mass or less.
[0083] <Other forms of Resin B> In addition, the content of resin B in the toner is preferably 1.0% by mass or more and 10.0% by mass or less. When the content is 1.0% by mass or more, a toner having a high charge amount is easily obtained. Therefore, it is preferably 1.0% by mass or more, and more preferably 2.0% by mass or more. When it is 10.0% by mass or less, the content of resin B in the toner does not become too large, so that the toner is less likely to be overcharged, and a toner having a suitable charge amount is easily obtained. Therefore, it is preferably 10.0% by mass or less, more preferably 8.0% by mass or less, and even more preferably 5.0% by mass or less.
[0084] In addition, since a toner having a high charge amount is easily obtained, the content of resin B in the shell according to the present invention is preferably 50.0% by mass or more. More preferably, it is 75.0% by mass or more, and even more preferably, it is 90.0% by mass or more. There is no particular upper limit, and it is 100.0% by mass. The content of 100.0% by mass means that the shell according to the present invention is resin B.
[0085] In addition, the ratio of the mass of resin B contained in the shell according to the present invention to the mass of resin A contained in the core according to the present invention is preferably 1.0 mass% or more and 10.0 mass% or less. By containing resin A in the core and resin B in the shell at a mass ratio satisfying the above, a toner having a high charge amount and excellent fluidity is easily obtained, which is preferable. It is more preferably 3.0 to 7.0 mass%, and even more preferably 4.0 to 6.0 mass%.
[0086] The resin component may contain multiple types of resin B. When the resin component contains multiple types of resin B, the total mass of the resins corresponding to resin B is defined as the content of resin B.
[0087] Resin B may contain monomer unit A, which is a characteristic monomer unit of resin A and is represented by the above formula (1). In this case, the content of monomer unit A in resin B is preferably 1.9% by mass or less. When the content of monomer unit A in polymer B is 1.9% by mass or less, a toner having a high charge amount is easily obtained. Therefore, it is preferably 1.9% by mass or less, more preferably 0.1% by mass or less, and even more preferably 0.0% by mass. 0.0% by mass means that resin B does not contain monomer unit A.
[0088] Furthermore, as the shell resin, a resin other than the resin B having the monomer unit B may be used in combination. Examples of the resin other than the resin B include the following.
[0089] Examples of the resin include thermosetting resins such as melamine resin, urea resin, sulfonamide resin, glyoxal resin, guanamine resin, aniline resin, or derivatives of each of these resins, polyimide, maleimide polymer, bismaleimide, aminobismaleimide, or bismaleimide triazine, and thermoplastic resins such as vinyl resin and polyester not corresponding to resin B. These resins may be used alone or in combination of two or more kinds.
[0090] Examples of the polymerizable monomer D other than the polymerizable monomer B that can form the resin B include the monomers exemplified above as the polymerizable monomer C. These monomers can be used alone or in combination of two or more kinds.
[0091] SP value of resin B B Then, SP B is 21.50(J / cm 3 ) 0.5 More than 25.00(J / cm 3 ) 0.5 As a result of the studies by the present inventors, it is preferable that the SP B is 21.50(J / cm 3 ) 0.5When the charge amount was 21.50 (J / cm or more), a toner having a high charge amount was easily obtained. 3 ) 0.5 It is preferable that the temperature is 22.00 (J / cm 3 ) 0.5 More preferably, the SP B is 25.00 (J / cm 3 ) 0.5 When the charge amount is less than 25.00 (J / cm), the toner is less likely to be overcharged, and it is easy to obtain a toner having a suitable charge amount. 3 ) 0.5 It is preferable that the concentration is 24.50 (J / cm 3 ) 0.5 More preferably, it is 24.00 (J / cm 3 ) 0.5 It is even more preferable that:
[0092] The SP value of resin A is SP A The SP value of resin B is SP B Then, SP B -SP A is 0.00(J / cm 3 ) 0.5 More than 7.00(J / cm 3 ) 0.5 It is preferable that the above SP B -SP A is 0.00(J / cm 3 ) 0.5 If the charge ratio is more than 0.00 (J / cm), the adhesion between the resin A in the toner core and the resin B in the shell is appropriately maintained, and the charge generated in the shell is not excessively transferred to the core particles, making it easier to obtain a toner with a high charge amount. 3 ) 0.5 It is preferable that the J / cm2 is 1.00 or more. 3 ) 0.5 More preferably, it is 2.00 (J / cm 3 ) 0.5 More preferably, it is 7.00 (J / cm 3When the resin B in the toner core is 0.5 or less, the adhesion between the resin A in the toner core and the resin B in the shell is easily increased, and a toner having excellent fluidity is easily obtained. 3 ) 0.5 or less, and 6.00 (J / cm 3 ) 0.5 More preferably, it is 5.00 (J / cm 3 ) 0.5 It is even more preferable that:
[0093] The above SP A and SP B can be controlled by the type and / or amount of raw materials used.
[0094] <Various additives> If necessary, the toner may contain one or more additives selected from a colorant, a release agent, a magnetic material, a charge control agent, an external additive, and the like.
[0095] <Coloring agent> As the colorant, a black colorant, a yellow colorant, a magenta colorant, a cyan colorant, and the like can be used.
[0096] Examples of black colorants include carbon black.
[0097] Examples of yellow colorants include yellow pigments such as monoazo compounds, disazo compounds, condensed azo compounds, isoindolinone compounds, isoindoline compounds, benzimidazolone compounds, anthraquinone compounds, azo metal complexes, methine compounds, and allylamide compounds. Specific examples include CI Pigment Yellow 74, 93, 95, 109, 111, 128, 155, 174, 180, and 185.
[0098] Magenta colorants include magenta pigments such as monoazo compounds, condensed azo compounds, diketopyrrolopyrrole compounds, anthraquinone compounds, quinacridone compounds, basic dye lake compounds, naphthol compounds, benzimidazolone compounds, thioindigo compounds, and perylene compounds. Specific examples include CI Pigment Red 2, 3, 5, 6, 7, 23, 48:2, 48:3, 48:4, 57:1, 81:1, 122, 144, 146, 150, 166, 169, 177, 184, 185, 202, 206, 220, 221, 238, 254, and 269, and CI Pigment Violet Red 19.
[0099] Examples of cyan colorants include cyan pigments such as copper phthalocyanine compounds and their derivatives, anthraquinone compounds, basic dye lake compounds, etc. Specific examples include CI Pigment Blue 1, 7, 15, 15:1, 15:2, 15:3, 15:4, 60, 62, and 66.
[0100] In addition to the pigment, various dyes conventionally known as colorants can also be used.
[0101] The content of the colorant in the toner is preferably from 1.0% by mass to 20.0% by mass, and more preferably from 3.0% by mass to 15.0% by mass.
[0102] <Magnetic material> The toner of the present invention may contain a magnetic material to form a magnetic toner. The magnetic material may also function as a colorant.
[0103] Examples of magnetic materials include the following: iron oxides such as magnetite, hematite, and ferrite; metals such as iron, cobalt, and nickel; and alloys and mixtures of these metals with metals such as aluminum, cobalt, copper, lead, magnesium, tin, zinc, antimony, beryllium, bismuth, cadmium, calcium, manganese, selenium, titanium, tungsten, and vanadium.
[0104] The content of the magnetic material in the toner is preferably from 25.0% by mass to 60.0% by mass, and more preferably from 30.0% by mass to 50.0% by mass.
[0105] <Release agent> Examples of the release agent include the following:
[0106] Esters of monohydric alcohols and monocarboxylic acids, such as behenyl behenate, stearyl stearate, and palmityl palmitate; esters of dihydric carboxylic acids and monoalcohols, such as dibehenyl sebacate; esters of dihydric alcohols and monocarboxylic acids, such as ethylene glycol distearate and hexanediol dibehenate; esters of trihydric alcohols and monocarboxylic acids, such as glycerin tribehenate; esters of tetrahydric alcohols and monocarboxylic acids, such as pentaerythritol tetrastearate and pentaerythritol tetrapalmitate; dipentaerythritol hexastearate, dipentaerythritol Esters of hexahydric alcohols such as ritol hexapalmitate and monocarboxylic acids; esters of polyfunctional alcohols such as polyglycerin behenate and monocarboxylic acids; natural ester waxes such as carnauba wax and rice wax; petroleum-based hydrocarbon waxes and their derivatives such as paraffin wax, microcrystalline wax, petrolatum, etc.; hydrocarbon waxes and their derivatives produced by the Fischer-Tropsch process; polyolefin-based hydrocarbon waxes and their derivatives such as polyethylene wax and polypropylene wax; higher aliphatic alcohols; fatty acids such as stearic acid and palmitic acid; acid amide waxes, etc.
[0107] The wax content in the toner is preferably from 1.0% by mass to 30.0% by mass, and more preferably from 3.0% by mass to 20.0% by mass.
[0108] <Charge control agent> The charge control agent can be used without any particular limitation.
[0109] Examples of negative charge control agents include the following:
[0110] Metal compounds of aromatic carboxylic acids such as salicylic acid, alkylsalicylic acid, dialkylsalicylic acid, naphthoic acid, and dicarboxylic acids, or polymers or copolymers having the above-mentioned metal compounds of aromatic carboxylic acids. Polymers or copolymers having a sulfonic acid group, a sulfonate salt group, or a sulfonate ester group. Metal salts or metal complexes of azo dyes or azo pigments. Boron compounds, silicon compounds, calixarenes, etc. are included.
[0111] Examples of the positive charge control agent include quaternary ammonium salts, polymeric compounds having quaternary ammonium salts in the side chains; guanidine compounds; pyridine compounds; nigrosine compounds; and imidazole compounds.
[0112] The content of the charge control agent in the toner is preferably from 0.01% by mass to 5.00% by mass.
[0113] <External additives> As the external additive, the following external additives can be used.
[0114] Examples of the inorganic fine particles include silica particles and metal oxide particles (more specifically, alumina, titanium oxide, magnesium oxide, zinc oxide, strontium titanate, barium titanate, etc.), etc. Other examples include organic fine particles made of resin, silicone resin, melamine resin, etc., and organic-inorganic composite fine particles.
[0115] The external additive may be surface-treated. Examples of the surface treatment agent include silicone varnish, various modified silicone varnishes, unmodified silicone oils, various modified silicone oils, silane compounds, silane coupling agents, other organic silicon compounds, and organic titanium compounds. These surface treatment agents may be used alone or in combination.
[0116] <Toner manufacturing method> The toner of the present invention can be produced by, but is not limited to, a suspension polymerization method, a dissolution suspension method, an emulsion aggregation method, a pulverization method, etc. The toner of the present invention is a toner having a core containing a resin component and a shell covering the surface of the core, and a production method in which the core is prepared by the above-mentioned production method and then the shell is formed from the outside is preferable. Among them, a production method in which the core is produced by a pulverization method or a suspension polymerization method and then the shell is formed from the outside in a water system is more preferable.
[0117] <Various measurement methods, etc.> Various measurement methods etc. are described below.
[0118] <Observation of the presence or absence of shell in toner particles> The presence or absence of a shell in a toner particle can be observed by observing the cross-sectional shape of the toner particle. A specific method for observing the cross-sectional shape of a toner particle is as follows.
[0119] First, toner particles are sufficiently dispersed in a photocurable epoxy resin, and then the epoxy resin is cured by irradiating it with ultraviolet light to obtain a cured product. The obtained cured product is cut using a microtome equipped with a diamond blade to prepare a thin flake sample having a thickness of 100 nm. The sample is dyed with ruthenium tetroxide as necessary, and then a transmission electron microscope (TEM) (trade name: electron microscope Tecnai TF20XT, manufactured by FEI) is used to observe the cross section of the toner at an accelerating voltage of 120 kV to obtain a TEM image.
[0120] In the above observation method, when a shell is present and the core and shell are made of different components, the difference in the staining state or contrast due to element mapping is observed. The observation magnification is 20,000 times.
[0121] <Method for measuring the content of various monomer units in resin> The content of the monomer unit in the resin is measured by 1H-NMR under the following conditions.
[0122] Measuring device: FT NMR device JNM-EX400 (manufactured by JEOL Ltd.) Measurement frequency: 400MHz Pulse condition: 5.0μs Frequency range: 10500Hz Number of times: 64 Measurement temperature: 30℃ Sample: 50 mg of sample is added to deuterated chloroform (CDCl3) and dissolved in a thermostatic bath at 40°C. The resulting solution is filtered through a solvent-resistant membrane filter "Myshoridisc" (manufactured by Tosoh Corporation) with a pore size of 0.2 μm to obtain a sample solution. The sample solution is placed in a sample tube with an inner diameter of 5 mm and used for measurement.
[0123] Obtained 1 The H-NMR chart is analyzed to identify the structure of each monomer unit. Here, as an example, the measurement of the content ratio of monomer unit A in resin A according to the present invention will be described. 1 In the H-NMR chart, a peak that is independent of the peaks that are attributable to the components of the monomer unit A and other monomer units is selected, and the integral value S1 of this peak is calculated. The integral values of the other monomer units contained in the resin A are also calculated in the same manner.
[0124] When the monomer units constituting the resin A are the monomer unit A and one other monomer unit, the content of the monomer unit A is calculated using the above integral value S1 and the integral value S2 of the peak of the other monomer unit as follows: Here, n1 and n2 are the numbers of hydrogen atoms in the constituent elements to which the peaks of interest for each site belong.
[0125] Content of monomer unit A (mol%)= {(S1 / n1) / ((S1 / n1)+(S2 / n2))}×100 Even when two or more other monomer units are present, the content of the monomer unit A can be calculated in the same manner.
[0126] The content of the monomer unit B in the resin B according to the present invention is also measured by the same method as above.
[0127] In addition, when a polymerizable monomer that does not contain a hydrogen atom in any component other than the vinyl group is used, 13 Measure nuclei using C-NMR 13 C, and the measurement was performed in single pulse mode. 1 Calculate in the same manner using H-NMR.
[0128] <Detection of Resin B and Monomer Unit B Present on the Toner Particle Surface> To detect resin B present on the toner particle surface, a TOF-SIMS (TRIFT-IV, manufactured by ULVAC-PHI, Inc.) is used. The analysis conditions are as follows.
[0129] Sample preparation: Toner particles are deposited on an indium sheet.
[0130] Sample preparation: None Primary ion: Au + Acceleration voltage: 30 kV Charge neutralization mode: On Measurement mode: Positive Raster size: 100μm Accumulation time: 180 seconds By carrying out the above measurement, it is possible to detect resin B having monomer unit B present on the toner surface. By confirming the presence of the shell of the toner particles by observation and carrying out the measurement, it is possible to determine whether or not the shell contains resin B.
[0131] In addition, the content ratio of monomer unit B in resin B can also be calculated from the spectral intensity derived from the oxazoline group in the secondary ion mass spectrum (vertical axis: intensity, horizontal axis: mass number = m / z) obtained under the above conditions, using a calibration curve prepared based on samples with known concentrations.
[0132] <Measurement of resin weight average molecular weight (Mw)> The weight-average molecular weight (Mw) of the resin sample is measured by gel permeation chromatography (GPC) as follows.
[0133] First, the sample is dissolved in tetrahydrofuran (THF) at room temperature over 24 hours. Then, the resulting solution is filtered through a solvent-resistant membrane filter "Micron Disc" (manufactured by Tosoh Corporation) with a pore size of 0.2 μm to obtain a sample solution. Note that the sample solution is adjusted so that the sample of the components soluble in THF is 0.8% by mass. Using this sample solution, the measurement is carried out under the following conditions.
[0134] Apparatus: HLC8120 GPC (Detector: RI) (manufactured by Tosoh Corporation) Column: Seven columns of Shodex KF-801, 802, 803, 804, 805, 806, 807 (manufactured by Showa Denko K.K.) Eluent: Tetrahydrofuran (THF) Flow rate: 1.0 mL / min Oven temperature: 40.0 °C Sample injection volume: 0.10 mL When calculating the molecular weight of the sample, a molecular weight calibration curve prepared using a standard polystyrene resin (for example, trade names "TSK Standard Polystyrene F-850, F-450, F-288, F-128, F-80, F-40, F-20, F-10, F-4, F-2, F-1, A-5000, A-2500, A-1000, A-500", manufactured by Tosoh Corporation) is used.
[0135] <Calculation method of SP value> The SP values of the monomer units and the resin are determined as follows according to the calculation method proposed by Fedors.
[0136] For each monomer unit, the SP value of the monomer unit is based on the atoms or atomic groups in the molecular structure. From the table described in "polym. Eng. Sci., 14(2), 147-154(1974)", the evaporation energy (Δei) (cal / mol) and the molar volume (Δvi) (cm 3 / mol), (4.184×ΣΔei / ΣΔvi) 0.5 SP value (J / cm 3 ) 0.5 When calculating the SP value of units derived from alcohol-based and carboxylic acid-based monomers used in polyesters, the structure in which all hydroxyl groups and carboxylic acid groups are replaced with ester groups and one of the ester groups is removed is regarded as a monomer unit.
[0137] The SP value of a resin is calculated by calculating the evaporation energy (Δei) and molar volume (Δvi) of each monomer unit constituting the resin, and multiplying them by the molar ratio (j) of each monomer unit in the resin, using the following formula:
[0138] Resin SP value = {(Σj × ΣΔei) / (Σj × ΣΔvi)} 0.5 <Method for measuring the acid value of resin> The acid value is the weight (mg) of potassium hydroxide required to neutralize the acid contained in 1 g of a sample. The acid value of the resin in the present invention is measured in accordance with JIS K 0070-1992, and specifically, is measured according to the following procedure.
[0139] (1) Preparation of reagents Dissolve 1.0 g of phenolphthalein in 90 mL of ethyl alcohol (95% by volume), and add ion-exchanged water to make 100 mL to obtain a phenolphthalein solution.
[0140] Dissolve 7 g of special grade potassium hydroxide in 5 mL of water and add ethyl alcohol (95% by volume) to make 1 L. Place in an alkali-resistant container to avoid contact with carbon dioxide, etc., leave for 3 days, then filter to obtain potassium hydroxide solution. Store the resulting potassium hydroxide solution in an alkali-resistant container. The factor of the potassium hydroxide solution is determined by placing 25 mL of 0.1 mol / L hydrochloric acid in an Erlenmeyer flask, adding several drops of the phenolphthalein solution, and titrating with the potassium hydroxide solution, from the amount of potassium hydroxide solution required for neutralization. The 0.1 mol / L hydrochloric acid used is prepared in accordance with JIS K 8001-1998.
[0141] (2) Operation (A) Main Test 2.0 g of the melt-kneaded and pulverized toner sample is precisely weighed into a 200 mL Erlenmeyer flask, and 100 mL of a toluene / ethanol (2:1) mixed solution is added and dissolved over 5 hours. Next, several drops of the above phenolphthalein solution are added as an indicator, and titration is performed using the above potassium hydroxide solution. The end point of the titration is when the light red color of the indicator continues for 30 seconds.
[0142] (B) Blank test The titration is carried out in the same manner as above, except that no sample is used (i.e., only the toluene / ethanol (2:1) mixed solution is used).
[0143] (3) The obtained result is substituted into the following formula to calculate the acid value.
[0144] A = [(CB) × f × 5.61] / S Here, A is the acid value (mgKOH / g), B is the amount of potassium hydroxide solution added for the blank test (mL), C is the amount of potassium hydroxide solution added for the main test (mL), f is the factor of the potassium hydroxide solution, and S is the sample (g). EXAMPLES
[0145] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the examples, the parts are by weight unless otherwise specified.
[0146] <Production example of binder resin 1> The following materials were placed in a reaction vessel equipped with a reflux condenser, a stirrer, a thermometer, and a nitrogen inlet tube under a nitrogen atmosphere.
[0147] Toluene 100.0 parts Monomer composition 100.0 parts (The monomer composition is a mixture of behenyl acrylate, methacrylonitrile, and styrene in the ratio shown below.) Behenyl acrylate (monomer corresponding to monomer unit A) 50.0 parts Methacrylonitrile (other monomer) 30.0 parts Styrene (other monomer) 20.0 parts Polymerization initiator: 0.5 parts t-butyl peroxypivalate (NOF Corp.: Perbutyl PV) The inside of the reaction vessel was heated to 70°C while stirring at 200 rpm, and a polymerization reaction was carried out for 12 hours, to obtain a solution in which a polymer of the monomer composition was dissolved in toluene. Subsequently, the temperature of the solution was lowered to 25°C, and the solution was poured into 1000.0 parts of methanol while stirring, to precipitate the methanol insoluble matter. The obtained methanol insoluble matter was filtered, washed with methanol, and then vacuum dried at 40°C for 24 hours to obtain binder resin 1. The acid value of binder resin 1 was 0.0 mgKOH / g, and the SP value (SPA) calculated from the composition ratio was 20.75. In addition, when NMR measurement of binder resin 1 was performed, the monomer units constituting binder resin 1 were 50.0 mass% of units derived from behenyl acrylate, 30.0 mass% of units derived from methacrylonitrile, and 20.0 mass% of units derived from styrene.
[0148] <Production Examples of Binder Resins 2 to 20> As shown in Table 1, binder resins 2 to 20 were obtained in the same manner as in the production example of binder resin 1, except that the type and amount of monomer added were changed.
[0149] <Production Example of Binder Resin 22> A 5 L reaction vessel equipped with a thermometer (thermocouple), a dehydration tube, a nitrogen inlet tube, a fractionator, and a stirrer was set in an oil bath, and 1200 parts of propylene glycol, 1700 parts of terephthalic acid, and 3 parts of an esterification catalyst (tin (II) 2-ethylhexanoate) were added to the vessel. The temperature inside the vessel was then raised to 230°C using the oil bath, and the contents of the vessel were reacted (condensation reaction) for 15 hours under conditions of a nitrogen atmosphere and a temperature of 230°C. The vessel was then depressurized, and binder resin 22 (polyester) was obtained under conditions of a reduced pressure atmosphere (pressure 8.0 kPa) and a temperature of 230°C. The SP value of binder resin 22 was 22.10 (J / cm 3 )0.5 The acid value was 18.9 mgKOH / g. When the NMR measurement of the binder resin 22 was performed, the monomer units constituting the binder resin were 41.4 mass% of units derived from propylene glycol and 58.6 mass% of units derived from terephthalic acid.
[0150] The SP values of the obtained binder resins 1 to 22 (SP A ) and acid value are shown in Table 1. Furthermore, the monomer units constituting each binder resin and their content ratios obtained by carrying out NMR measurement of the obtained binder resins 1 to 21 are shown in Table 2. Binder resin 21 will be described later.
[0151] [Table 1]
[0152] The abbreviations in Tables 1 and 2 are as follows. BEA: Behenyl acrylate DOA: dodecyl acrylate SA: stearyl acrylate TRA: Triacontyl acrylate St: styrene MN: Methacrylonitrile BuA: n-butyl acrylate OcA: Octyl acrylate AA: Acrylic acid PG: Propylene glycol TPA: Terephthalic acid In Table 1, SP A The unit is (J / cm 3 ) 0.5 and the unit of the acid value of the binder resin is mgKOH / g.
[0153] In Table 1, binder resins 18 to 20 and 22 are not resins that correspond to resin A according to the present invention, but the SP values of each binder resin are A are listed in the column.
[0154] [Table 2]
[0155] <Production Examples of Oxazoline Group-Containing Resin B1 and Oxazoline Group-Containing Resin Solution B1> In a 1L four-neck flask equipped with a thermometer, a nitrogen inlet tube, a stirring device (stainless steel stirring blade), and a downflow condenser (heat exchanger), 30.0 parts of 2-vinyl-2-oxazoline, 60.0 parts of methyl methacrylate, 10.0 parts of n-butyl acrylate, 1.7 parts of azobisisobutyronitrile (AIBN), and 200 parts of ethyl acetate were placed. Nitrogen gas was then introduced into the flask through the nitrogen inlet tube, and the flask was placed in a nitrogen atmosphere (inert atmosphere). The flask contents were then heated to 235°C while stirring in the nitrogen atmosphere, and the flask was depressurized while maintaining the temperature, and the flask contents were reacted for 5 hours under conditions of a reduced pressure atmosphere (pressure 8.0 kPa) and a temperature of 235°C to obtain resin B1. In addition, NMR measurement of resin B1 revealed that the monomer units constituting resin B1 were 30.0% by mass of units derived from 2-vinyl-2-oxazoline, 60.0% by mass of units derived from methyl methacrylate, and 10.0% by mass of units derived from n-butyl acrylate.
[0156] Next, the resin B1 was dissolved in an aqueous 2-propanol solution having a concentration of 70% by mass to obtain an oxazoline group-containing resin solution B1 having a solid content concentration of 10% by mass.
[0157] <Production Examples of Oxazoline Group-Containing Resins B2 to B6 and Oxazoline Group-Containing Resin Solutions B2 to B6> As shown in Table 3, oxazoline group-containing resins B2 to B6 and oxazoline group-containing resin solutions B2 to B6 were obtained in the same manner as in the production examples of oxazoline group-containing resin B1 and oxazoline group-containing resin solution B1, except that the types and amounts of monomers used were changed.
[0158] The SPs of resins B1 to B6, including the oxazoline group-containing resin solutions "Epocross WS-300 (solid concentration: 10% by mass)" and "Epocross WS-700 (solid concentration: 25% by mass)" described below, are B The results are shown in Table 3. Table 4 shows the monomer units constituting each resin and their content ratios obtained by carrying out NMR measurements on oxazoline group-containing resins B1 to B6, EPOCROS WS-300, and EPOCROS WS-700.
[0159] [Table 3]
[0160] The abbreviations in Tables 3 and 4 are as follows. VOX: 2-vinyl-2-oxazoline IPOX: 2-isopropenyl-2-oxazoline MM: Methyl methacrylate BuA: n-butyl acrylate MN: Methacrylonitrile In Table 3, SP B The unit is (J / cm 3 ) 0.5 It is.
[0161] [Table 4]
[0162] <Production example of polyester 1> The following materials were added to an autoclave equipped with a pressure reducing device, a water separating device, a nitrogen gas introducing device, a temperature measuring device and a stirring device.
[0163] Terephthalic acid 32.3 parts (50.0 mol%) Bisphenol A-propylene oxide 2 mole adduct 67.7 parts (50.0 mole%) Potassium titanium oxalate (catalyst) 0.02 parts Subsequently, the reaction was carried out under a nitrogen atmosphere at normal pressure at 220°C until the desired molecular weight was reached. After cooling, the mixture was pulverized to obtain Polyester 1. Polyester 1 had an acid value of 8.0 mgKOH / g, a weight average molecular weight (Mw) of 12,000, and an SP value calculated from the composition ratio of 22.30 (J / cm 3 ) 0.5 It was.
[0164] An example of toner production is shown below.
[0165] <Toner 1 Manufacturing Example> (Core manufacturing) Binder resin 1 100.0 parts Colorant (Pigment Blue 15:3) 6.5 parts Hydrocarbon wax HNP-9 (manufactured by Nippon Seiro, melting point 74°C) 9.0 parts The above materials were premixed in a Henschel mixer (manufactured by Nippon Coke Company), and then melt-kneaded using a twin-screw kneading extruder (manufactured by Ikegai Iron Works Co., Ltd.: PCM-30 type).
[0166] The kneaded product thus obtained was cooled, coarsely pulverized with a hammer mill, and then pulverized with a mechanical pulverizer (Turbo Kogyo Co., Ltd.: T-250) to obtain a finely pulverized powder. The finely pulverized powder thus obtained was classified with a multi-division classifier utilizing the Coanda effect to obtain toner cores (toner particle cores) having a weight average particle size of 6.6 μm.
[0167] (Shell formation) A 1 L three-neck flask equipped with a thermometer and a stirring blade was placed in a water bath, and 300 parts of ion-exchanged water was placed in the flask. The temperature in the flask was then adjusted to 30° C. using the water bath. Next, 150 parts of an oxazoline group-containing resin B1 solution ("Epocross WS-300" manufactured by Nippon Shokubai Co., Ltd., solid content concentration: 10% by mass) were added to the flask. The amounts added in Table 5 indicate the amounts (unit: parts by mass) of oxazoline group-containing resin (solid content) added to 100 parts by mass of toner cores to be added later.
[0168] Then, 300 parts of the toner cores prepared by the above-mentioned procedure were added to the flask, and the contents of the flask were stirred for 1 hour at a rotation speed of 200 rpm. After that, 300 parts of ion-exchanged water was added to the flask, and 6 mL of an aqueous ammonia solution having a concentration of 1% by mass was added to the flask.
[0169] Next, the temperature inside the flask was raised to 55° C. at a rate of 0.5° C. / min while stirring the contents of the flask at a rotation speed of 150 rpm. Next, the temperature (55° C.) was maintained for 2 hours while stirring the contents of the flask at a rotation speed of 100 rpm.
[0170] Thereafter, an aqueous ammonia solution having a concentration of 1% by mass was added to the flask to adjust the pH of the flask content to 7. The resulting slurry was cooled to room temperature (about 25°C), washed, filtered, and subjected to solid-liquid separation, and then dried using a vacuum dryer to obtain toner particles 1. The content of the oxazoline group-containing resin in toner particles 1 was 4.6% by mass.
[0171] Next, silica fine particles (hydrophobized with hexamethyldisilazane, number average particle diameter of primary particles: 10 nm, BET specific surface area: 170 m) were added as an external additive to 100.0 parts by mass of toner particles 1. 2 The mixture was mixed for 15 minutes at 3000 rpm using a Henschel mixer (manufactured by Nippon Coke Corporation), to obtain toner 1.
[0172] <Production examples of toners 2-29, 31-35> As shown in Tables 5 and 6, toners 2 to 29 and 31 to 34 were obtained in the same manner as in the production example of toner 1, except that the type of binder resin and the type and amount of the oxazoline group-containing resin solution forming the shell were changed.
[0173] [Table 5]
[0174] (In Tables 5 and 6, the amount added indicates the amount (unit: parts by mass) of the oxazoline group-containing resin (solid content) added to 100 parts by mass of the toner core. Also, in Tables 5 and 6, SP B -SP A The unit is (J / cm 3 ) 0.5 It is.)
[0175] [Table 6]
[0176] In Table 6, binder resins 18 to 20 and 22 are not resins that correspond to resin A according to the present invention, but are SPs described in Table 1. A Using the value of SP B -SP A is calculated.
[0177] <Toner 30 manufacturing example> (Production of Core Slurry) Styrene 60.0 parts Coloring agent (CI Pigment Blue 15:3, Dainichi Seika Chemicals Co., Ltd.) 6.0 parts The above materials were placed in an attritor (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.), and further dispersed using zirconia particles having a diameter of 1.7 mm at 220 rpm for 5 hours to obtain a colorant dispersion liquid.
[0178] Styrene 10.0 parts Behenyl acrylate 30.0 parts Polyester 1 5.0 parts Hydrocarbon wax HNP-9 (manufactured by Nippon Seiro, melting point 74°C) 9.0 parts The above materials were mixed and added to the colorant dispersion liquid. The resulting mixture was kept at 60° C. and stirred at 500 rpm using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.) to dissolve and disperse uniformly, thereby preparing a polymerizable monomer composition.
[0179] Meanwhile, 850.0 parts of 0.10 mol / L Na3PO4 aqueous solution and 8.0 parts of 10% hydrochloric acid were added to a container equipped with a high-speed stirring device Clearmix (manufactured by M Technique Co., Ltd.), the rotation speed was adjusted to 15,000 rpm, and the temperature was heated to 70°C. 68.0 parts of 1.0 mol / L-CaCl2 aqueous solution were added to this to prepare an aqueous medium containing a calcium phosphate compound.
[0180] After the polymerizable monomer composition was added to the aqueous medium, 7.0 parts of t-butyl peroxypivalate, a polymerization initiator, was added, and the mixture was granulated for 10 minutes while maintaining a rotation speed of 15,000 rpm. After that, the high-speed agitator was replaced with a propeller agitator, and the mixture was reacted at 70°C for 5 hours under reflux, and then the liquid temperature was increased to 85°C and the mixture was reacted for another 2 hours.
[0181] After the polymerization reaction was completed, the obtained slurry was cooled and allowed to stand to allow the particles to settle, and a portion of the supernatant liquid was removed to obtain a core slurry having a solid content concentration of 25.0% by mass.
[0182] (Shell formation) A 1 L three-neck flask equipped with a thermometer and a stirring blade was set in a water bath, and 400.0 parts of the obtained core slurry was placed in the flask. The temperature in the flask was then adjusted to 30° C. using the water bath. Subsequently, 50 parts of an oxazoline group-containing resin dispersion ("Epocross WS-300" manufactured by Nippon Shokubai Co., Ltd., solid content concentration: 10.0% by mass) was added to the flask.
[0183] The contents of the flask were then stirred at a rotation speed of 200 rpm for 1 hour, and then 300 parts of ion-exchanged water was added to the flask. After adding 6 mL of an aqueous ammonia solution with a concentration of 1.0% by mass to the flask, the temperature in the flask was raised to 55°C at a rate of 0.5°C / min while stirring the contents of the flask at a rotation speed of 150 rpm. The temperature (55°C) was then maintained for 2 hours while stirring the contents of the flask at a rotation speed of 100 rpm.
[0184] Subsequently, an aqueous ammonia solution having a concentration of 1% by mass was added to the flask to adjust the pH of the content in the flask to 7. Subsequently, the obtained slurry was cooled to room temperature (about 25° C.).
[0185] Thereafter, while maintaining stirring, dilute hydrochloric acid was added until the pH reached 1.5 to dissolve the calcium phosphate compound, which was a dispersion stabilizer. The solid content was filtered off, thoroughly washed with ion-exchanged water, and then vacuum-dried at 40° C. for 24 hours to obtain toner particles.
[0186] For 100.0 parts by mass of the obtained toner particles, silica fine particles (hydrophobized with hexamethyldisilazane, number average particle size of primary particles: 10 nm, BET specific surface area: 170 m) were added as an external additive. 2 The mixture was mixed for 15 minutes at 3,000 rpm using a Henschel mixer (manufactured by Nippon Coke Corporation) to obtain toner 30.
[0187] <Production Example of Binder Resin 21> Further, production was carried out in the same manner as in the production example of the toner 30, except that the colorant, polyester 1, and hydrocarbon wax were removed from the process of producing the core slurry, and the dispersion stabilizer was dissolved, and the solid content was filtered, washed, and dried without forming a shell, to obtain binder resin 21. The SPA and acid value of the obtained binder resin 21 are shown in Table 1.
[0188] <Toner 35 Manufacturing Example> As shown in Table 6, toner 35 was obtained in the same manner as in the production example of toner 1, except that binder resin 21 was used.
[0189] SP of toners 1 to 35 obtained B -SP A The binder resin content in the toner, the oxazoline group-containing resin content in the toner, and the presence or absence of a shell in the toner particles are shown in Tables 5 and 6. Furthermore, when the above-mentioned TOF-SIMS analysis was performed on toners 1 to 35, resin B having monomer unit B was detected on the toner surfaces of toners 1 to 33 and 35.
[0190] <Example 1> Toner 1 was evaluated as follows. The evaluation results are shown in Table 7.
[0191] <Evaluation of toner fluidity> A modified laser printer (product name: LBP712Ci, manufactured by Canon) was used to evaluate the fluidity of the toner. The modification of the modified machine was to change the potential settings. The higher the fluidity of the toner, the faster the toner coats the developing roller (developing member), so the difference between the image density at the first rotation of the developing roller and the image density after the first rotation is smaller, and a good image without unevenness can be obtained. The potential settings were set so that when the following fluidity evaluation was performed on Toner 35 under a normal temperature and humidity environment, the image density difference was 0.20, and when the following charge amount evaluation was performed, the image density was 1.01. The cartridge used for the evaluation was a commercially available cartridge in which the toner was removed from the cartridge, the inside was cleaned with an air blower, and 100 g of Toner 1 was filled. The above cartridge was installed in the cyan station, and a dummy cartridge was installed in the other stations to perform the evaluation. Furthermore, various potential settings were changed so that development with positively charged toner was possible.
[0192] At 23°C and 60% RH (normal temperature and humidity), high whiteness paper (product name: GF-C081, Canon Inc., 81.4 g / m 2 ) was used to continuously print 10,000 images with a printing rate of 1%. After that, three fully solid images were continuously printed as sample images. For the third fully solid image obtained, the image density was measured at a portion 5 cm from the top and a portion 20 cm from the top in the center of the left and right sides of the image, and the flowability was evaluated using the difference between the measured image densities. The evaluation results are shown in Table 7. An X-rite exact advance (manufactured by X-rite) was used for the density measurements.
[0193] Furthermore, an evaluation cartridge filled with Toner 1 was prepared, and the same evaluation as above was performed using this cartridge under a 30°C, 80% RH environment (high temperature and high humidity environment). The evaluation results are shown in Table 7. Compared to the evaluation under normal temperature and humidity, it appears that the effect of toner fluidity on the above evaluation is more significant under a high humidity environment.
[0194] In the evaluation, when the difference in the image density between the normal temperature and normal humidity environment and the high temperature and high humidity environment was 0.20 or less, it was determined that the effect of the present invention was obtained.
[0195] <Evaluation of Toner Charge Amount> In the above-mentioned fluidity evaluation under normal temperature and humidity environment, after outputting three sheets of the full solid image, a check image having a 5 mm x 5 mm solid image was output in three places, the left, right, and center, 5 cm from the top of the image, with a leading edge margin of 5 mm and left and right margins of 5 mm. The image density of the three solid image parts of this check image was measured, and the average value of the image densities of the three places was calculated. The image density was measured using a Macbeth densitometer (manufactured by Macbeth Co., Ltd.), which is a reflection densitometer, using an SPI filter, and evaluation was performed based on the measurement results. In this evaluation, an image density of 1.00 or more was judged to be one in which the effect of the present invention was obtained. In this evaluation, when the charge amount of the toner is sufficiently high, a high image density is obtained.
[0196] <Examples 2 to 30> Toners 2 to 30 were evaluated in the same manner as in Example 1. The evaluation results are shown in Table 7. Incidentally, Examples 21 and 23 are described as reference examples.
[0197] <Comparative Examples 1 to 5> Toners 31 to 35 were evaluated in the same manner as in Example 1. The evaluation results are shown in Table 7.
[0198] [Table 7] [Explanation of symbols]
[0199] 1. Toner particle core 2. Shell of toner particles 3. A monomer unit having an oxazoline group contained in the shell of a toner particle 4 Long-chain alkyl groups contained in the resin contained in the core of the toner particles 5. Repulsion between the oxazoline group contained in the shell of the toner particle and the long-chain alkyl group contained in the core of the toner particle
Claims
1. A toner having toner particles each having a core containing a resin component and a shell covering a surface of the core, The resin component contains a resin A having a monomer unit A represented by the following formula (1), a content ratio of the monomer unit A in the resin A is 2.0% by mass or more and 80.0% by mass or less, The shell contains a resin B having a monomer unit B represented by the following formula (2), The toner is characterized in that, when the SP value of the resin A is SP A and the SP value of the resin B is SP B , SP B -SP A is 0.00 (J / cm 3 ) 0.5 or more and 6.00 (J / cm 3 ) 0.5 or less. 【Chemistry 1】 (In formula (1), R 1 represents an alkyl group having 12 to 36 carbon atoms; R 2 is hydrogen or a methyl group. 3 is hydrogen, a methyl group, or an ethyl group.
2. 2. The toner according to claim 1, wherein the content of the monomer unit B in the resin B is 10.0% by mass or more and 95.0% by mass or less.
3. 3. The toner according to claim 1, wherein the content of the resin A in the toner is 30.0% by mass or more.
4. 4. The toner according to claim 1, wherein the content of the resin B in the toner is 1.0% by mass or more and 10.0% by mass or less.
5. 5. The toner according to claim 1, wherein the acid value of the resin A is from 0.0 mgKOH / g to 20.0 mgKOH / g.
6. The SP B is 21.50 (J / cm 3 ) 0.5 25.00 (J / cm 3 ) 0.5 6. The toner according to claim 1, wherein:
7. The resin A further has a monomer unit C, The toner according to any one of claims 1 to 6, wherein the monomer unit C is at least one monomer unit selected from the group consisting of a monomer unit represented by the following formula (3), a monomer unit represented by the following formula (4), and a monomer unit represented by the following formula (5): 【Chemistry 2】 (In formula (3), R 4 represents hydrogen or an alkyl group having 1 to 4 carbon atoms; R 5 represents hydrogen or a methyl group. 6 represents hydrogen or a methyl group.)
8. The toner according to claim 7, wherein a content ratio of the monomer unit C in the resin A is 25.0% by mass or more and 95.0% by mass or less.
9. The resin B further has a monomer unit D, The toner according to any one of claims 1 to 8, wherein the monomer unit D is at least one monomer unit selected from the group consisting of a monomer unit represented by the following formula (4) and a monomer unit represented by the following formula (6): 【Chemistry 3】 (In formula (4), R 6 represents hydrogen or a methyl group. 7 represents hydrogen or an alkyl group having 1 to 4 carbon atoms; R 8 represents hydrogen or a methyl group.)
10. The toner according to claim 9, wherein the content of the monomer unit D in the resin B is 10.0% by mass or more and 70.0% by mass or less.
11. 11. The toner according to claim 1, wherein a content ratio of the monomer unit A in the resin A is 30.0% by mass or more.
12. 12. The toner according to claim 1, wherein a ratio of a mass of the resin B contained in the shell to a mass of the resin A contained in the core is 1.0 mass % or more and 10.0 mass % or less.
Citation Information
Patent Citations
Method of manufacturing toner
JP2013083854A
Toner
JP2014130243A
Toner for electrostatic latent image development
JP2017151412A
Toner and method for manufacturing the same
JP2019074655A
Toner
JP2019191315A