toner

The core-shell structured toner with silica particles on a polyester-styrene-acrylic resin surface addresses charge fluctuations, maintaining stable image quality and density by utilizing a charge buffering effect, even under harsh conditions.

JP7551409B2Active Publication Date: 2024-09-17CANON KK
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020152278
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-10
Publication Date
2024-09-17
Estimated Expiration
2040-09-10

AI Technical Summary

Technical Problem

Existing toners face issues with fluctuations in charge amount due to embedding and detachment of external additives, leading to decreased stability in image quality and density under varying environmental conditions, particularly in high temperature and humidity environments.

Method used

A core-shell structured toner with silica particles on the surface, where the core is made of polyester resin and the shell is made of styrene-acrylic resin, with specific pore diameter and volume ranges for silica particles, maintaining a constant charge amount through a charge buffering effect.

Benefits of technology

The toner maintains stable charge and image quality over long-term use, suppressing fogging and ensuring consistent density and halftone quality across different environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551409000006
    Figure 0007551409000006
  • Figure 0007551409000004
    Figure 0007551409000004
  • Figure 0007551409000003
    Figure 0007551409000003
Patent Text Reader

Abstract

To provide a toner that suppresses fluctuation of a charge amount due to durable use regardless of use environment to suppress fog even in long-term printing, thereby realizing excellent density stability and halftone quality.SOLUTION: A toner has toner particles and silica particles on the surface of the toner particles. On the surface of the toner particles, there is a surface formed of polyester resin and a surface formed of styrene-acrylic resin. The number average particle size of the silica particles is 15 nm or more and 60 nm or less. The average pore diameter of the silica particles is 5.0 nm or more and 20.0 nm or less. The total pore volume of the silica particles is 0.20 cm3 / g or more and 1.50 cm3 / g or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to toners used to form toner images by developing electrostatic latent images formed by methods such as electrophotography, electrostatic recording, and toner jet recording. [Background technology]

[0002] As the electrophotographic technology used in copiers, printers, facsimile receiving devices, etc. advances, the demands from users are becoming stricter year by year. In recent years, the market has expanded to cover a wider range of environments, and there is a strong demand for stable image quality that is not dependent on the environment, and for compact designs that can print for a long period of time. In order to satisfy the above requirements, it is necessary that (1) the developing property does not change during the long-term use in the electrophotographic process, and (2) the latent image is transferred onto the recording medium without being disturbed. Therefore, the toner is required to have a charge amount that does not change during the long-term use, and many improvements have been made to solve the above problems. From the viewpoint of maintaining the physical properties of the toner, a technique is known in which a relatively large external additive of about 100 nm is added to the toner to suppress deterioration of the toner due to the spacer effect. For example, Patent Document 1 discloses a technology in which monodispersed spherical particles of 50 nm to 150 nm are externally added to base particles having a shell layer made of a styrene acrylic modified polyester resin, thereby making the adhesive force between the smoothed base particle surface and the externally added particles uniform and suppressing separation, thereby further improving durability. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2013-003367 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, although the above toner certainly shows improved durability, it has been found that the embedding and detachment of external additive particles progresses toward the end of the long-term use, and the reduction in the number of external additive particles functioning on the toner particle surface is unavoidable, resulting in a problem of a change in the charge amount and a decrease in developability and transferability. The above problem is particularly noticeable when the toner is used in harsh environments such as high temperature and high humidity environments or low temperature and low humidity environments. It was also found that when the amount of external additives in the toner in the developing machine temporarily increases due to continuous output of high-print-ratio images, the charge amount fluctuates, resulting in problems such as reduced stability of image density and the occurrence of fogging. In other words, these problems are caused by the fact that there is still no way to maintain the charge amount when the amount of external additives in the toner in the developing machine changes due to long-term use or usage conditions. In order to obtain the image quality stability required by the market, a toner that can maintain a constant charge amount is still desired. The present disclosure provides a toner that suppresses fogging even in long-term printing by suppressing fluctuations in charge amount that occur with durable use regardless of the usage environment, and that provides excellent density stability and halftone quality. [Means for solving the problem]

[0005] 1. A toner having toner particles and silica particles on a surface of the toner particles, the toner particles have a surface formed of a polyester resin and a surface formed of a styrene-acrylic resin; the toner particles are toner particles having a core-shell structure having a core particle and a shell formed on a surface of the core particle, the core particles comprise a polyester resin; the shell comprises a styrene-acrylic resin; a surface of the toner particle formed of the polyester resin is present on the surface of the toner particle by a part of the polyester resin contained in the core particle being exposed on the surface of the toner particle, The number average particle size of the silica particles is 15 nm or more and 60 nm or less, The average pore diameter of the silica particles is 5.0 nm or more and 20.0 nm or less, The total pore volume of the silica particles is 0.20 cm 3 / g or more 1.50cm 3 / g or less. Effect of the Invention

[0006] According to the present disclosure, by suppressing fluctuations in charge amount that occur with durable use regardless of the usage environment, it is possible to provide a toner that suppresses fog even during long-term printing and has excellent density stability and halftone quality. [Brief description of the drawings]

[0007] [Figure 1] Schematic diagram of the charge amount measuring device DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] In the present disclosure, the expressions "XX or more and YY or less" and "XX to YY" representing a numerical range mean a numerical range including the endpoints, that is, the lower limit and the upper limit, unless otherwise specified. When numerical ranges are stated in stages, the upper and lower limits of each numerical range can be combined in any way. The present disclosure will be specifically described below.

[0009] The present disclosure provides a toner having toner particles and silica particles on a surface of the toner particles, the toner particles have a surface formed of a polyester resin and a surface formed of a styrene-acrylic resin; The number average particle size of the silica particles is 15 nm or more and 60 nm or less, The average pore diameter of the silica particles is 5.0 nm or more and 20.0 nm or less, The total pore volume of the silica particles is 0.20 cm 3 / g or more 1.50cm 3 / g or less.

[0010] The silica particles are porous silica particles having a specific average pore size and total pore volume. The silica particles have a unique property that the change in charge amount with respect to the amount of silica particles added shows an opposite tendency depending on whether the toner particle surface is made of polyester resin or styrene-acrylic resin. When the toner particle surface is made of polyester resin, the absolute value of the charge amount shows a decreasing tendency as the amount of silica particles added increases, whereas when the toner particle surface is made of styrene-acrylic resin, the absolute value of the charge amount shows an increasing tendency. As a result of extensive research into how to make the most of this property, it was discovered that adding the silica particles to toner particles having a surface formed of polyester resin and a surface formed of styrene-acrylic resin provides a charge buffering effect that enables the charge amount to be maintained approximately constant throughout durable use. The mechanism by which the charge buffering effect works is assumed to be as follows.

[0011] Porous silica particles having a specific pore size tend to retain water in the pores regardless of the environment due to the action of capillary action and, if there are residual silanol groups in the pores, the action of the residual silanol groups. In addition, polyester resins have a higher water absorption rate than styrene-acrylic resins. When the silica particles come into contact with and rub against the polyester resin on the surface of the toner particles, the water retained in the pores of the silica particles has a high affinity with the polyester resin, and therefore the charge generated by frictional charging tends to leak through the retained water. On the other hand, when the silica particles come into contact with and rub against the styrene-acrylic resin on the surface of the toner particles, the styrene-acrylic resin exhibits hydrophobicity, and the water retained in the pores moves easily. This movement is unlikely to occur, and the accumulation effect of charge due to friction comes into play.

[0012] When resin portions with charging tendencies opposite to those of silica particles coexist on the surface of a toner particle, it is presumed that a charge buffering effect is at work because the total charge amount converges to and is maintained at an approximately constant amount even if the amount of silica particles present on the surface of the toner particle increases or decreases. Therefore, in printers and copiers, even if the amount of silica particles on the toner surface inside the developing machine changes with repeated printing, the charge amount is maintained constant, which enables stable developability and transferability to be achieved throughout durable use, thereby enabling the achievement of a long life for high-quality image output.

[0013] The silica particles are porous silica particles having pores, an average pore diameter of 5.0 nm or more and 20.0 nm or less, and a total pore volume of 0.20 cm 3 / g or more 1.50cm 3 / g or less. The average pore diameter and the total pore volume are values ​​calculated by the BJH method. The total pore volume refers to the total pore volume measured by the BJH method in the pore diameter range of 1.7 nm or more and 300.0 nm or less.

[0014] By making the average pore diameter of the silica particles 5.0 nm or more, the water trapped in the pores can be efficiently adsorbed and desorbed, and when there is contact friction on the surface of the toner particles, charge accumulation and leakage functions according to the type of resin can be achieved. By setting the average pore diameter to 20.0 nm or less, it becomes possible to maintain the water trapped within the pores even in a low-temperature, low-humidity environment. The average pore size of the silica particles is preferably 7.0 nm or more and 15.0 nm or less.

[0015] The total pore volume of the silica particles is 0.20 cm 3 By setting the silica particle surface area to 1 / g or more, the charge buffering function due to the retained water trapped in the pores of the silica particles can be satisfactorily exhibited. The total pore volume is 1.50 cm 3 / g or less, the amount of water absorbed by the silica particles does not become excessive even in a high-temperature and high-humidity environment, a decrease in the charge amount can be prevented, and a stable charge amount can be maintained. The total pore volume of the silica particles is preferably less than 0.40 cm 3 / g or more 1.20cm 3 / g or less.

[0016] The number average particle size of the silica particles is 15 nm or more and 60 nm or less, preferably 15 nm or more and 49 nm or less, and more preferably 15 nm or more and 40 nm or less. By making the number-average particle diameter of the silica particles 15 nm or more, embedding of the silica particles due to the stress the toner receives inside the developing device is suppressed, and environmental characteristics and durability can be maintained. By setting the number-average particle size of the silica particles to 60 nm or less, it is possible to suppress the decrease in the amount of charge throughout durable use without impairing the frictional charging characteristics of the silica particles, and to maintain a constant amount of charge.

[0017] In a wet method for producing silica, the average pore size of the silica particles can be controlled by the temperature and pH during the reaction. In addition, in wet silica production methods, the total pore volume of silica particles can be controlled by the pH during the reaction, additives (for example, catalysts such as dimethylformaldehyde and formaldehyde), and the aging and drying conditions. The content of the silica particles is preferably 0.1 parts by mass or more and 10 parts by mass or less, more preferably 0.2 parts by mass or more and 5.0 parts by mass or less, and even more preferably 0.5 parts by mass or more and 3.0 parts by mass or less, relative to 100 parts by mass of the toner particles.

[0018] The silica particles are sol-gel silica particles obtained by a wet method, gel silica particles, and gas phase silica particles. Examples of the silica particles include fumed silica particles, fused silica particles, and deflagration silica particles obtained by the above-mentioned method. Among these, the silica particles are preferably wet silica such as sol-gel silica particles or gel silica particles, from the viewpoint of having an abundance of residual silanol groups and being particularly excellent in the adsorption and desorption properties of retained water.

[0019] The hydrophobicity of the silica particles is preferably 40% to 75%, more preferably 43% to 70%, and even more preferably 45% to 60%. When the hydrophobicity is within the above range, the silica particles have excellent adsorption and desorption properties for water retained in the pores, can maintain a suitable amount of charge even in a harsh environment, and are excellent in development properties such as transferability, fogging suppression, and density stability. The degree of hydrophobicity of the silica particles can be adjusted by subjecting the surfaces of the silica particles to a hydrophobic treatment.

[0020] The treating agent used for the hydrophobization treatment is not particularly limited, and any conventionally known silane or silazane compound can be used. Specific examples include the following: Dimethyldisilazane, hexamethyldisilazane, methyltrimethoxysilane, octyltrimethoxysilane, isobutyltrimethoxysilane, trimethylsilane, trimethylchlorosilane, trimethylethoxysilane, dimethyldichlorosilane, methyltrichlorosilane, allyldimethylchlorosilane, allylphenyldichlorosilane, benzyldimethylchlorosilane, bromomethyldimethylchlorosilane, α-chloroethyltrichlorosilane, β-chloroethyltrichlorosilane, chloromethyldimethyl Examples of suitable siloxanes include chlorosilanes, triorganosilyl mercaptans, trimethylsilyl mercaptans, triorganosilyl acrylates, vinyldimethylacetoxysilanes, dimethylethoxysilanes, dimethyldimethoxysilanes, diphenyldiethoxysilanes, 1-hexamethyldisiloxanes, 1,3-divinyltetramethyldisiloxanes, 1,3-diphenyltetramethyldisiloxanes, and dimethylpolysiloxanes having 2 to 12 siloxane units per molecule and having one hydroxyl group on each of the Si units located at the terminals.

[0021] Examples of silane compounds that exhibit positive charging include 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, and 3-(2-aminoethylamino)propyltrimethoxysilane. Examples of the silane include 3-(2-aminoethylamino)propyltriethoxysilane and 3-(2-aminoethylamino)propyltriethoxysilane. do. These may be used alone or in combination of two or more. Among these, hexamethyldisilazane is preferred. It is preferred that the silica particles are surface-treated with hexamethyldisilazane. Silica particles that have been wet-treated for hydrophobicity using hexamethyldisilazane are more preferred because the treatment is uniform and has excellent environmental stability.

[0022] As a hydrophobic treatment agent other than the above, silicone oil may be used, or silicone oil may be used in combination with the above silane or silazane compound. Examples of silicone oil include dimethyl silicone oil, methylphenyl silicone oil, α-methylstyrene modified silicone oil, chlorophenyl silicone oil, and fluorine modified silicone oil.

[0023] The silicone oil treatment method can be the following: Directly mix silica particles or silica particles treated with a silane coupling agent with silicone oil using a mixer such as a Henschel mixer. Spray silicone oil onto base silica particles. Alternatively, it is preferable to dissolve or disperse silicone oil in a suitable solvent, add silica particles, mix, and then remove the solvent.

[0024] Specific examples of the hydrophobic treatment agent include chlorosilanes such as methyltrichlorosilane, dimethyldichlorosilane, trimethylchlorosilane, phenyltrichlorosilane, diphenyldichlorosilane, t-butyldimethylchlorosilane, and vinyltrichlorosilane; tetramethoxysilane, methyltrimethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, diphenyldimethoxysilane, o-methylphenyltrimethoxysilane, p-methylphenyltrimethoxysilane, n-butyltrimethoxysilane, and i-butyltrimethoxysilane; , hexyltrimethoxysilane, octyltrimethoxysilane, decyltrimethoxysilane, dodecyltrimethoxysilane, tetraethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, phenyltriethoxysilane, diphenyldiethoxysilane, i-butyltriethoxysilane, decyltriethoxysilane, vinyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, γ-mercaptopropyltrimethoxysilane, alkoxysilanes such as dimethylsilane, γ-chloropropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-(2-aminoethyl)aminopropyltrimethoxysilane, and γ-(2-aminoethyl)aminopropylmethyldimethoxysilane; hexamethyldisilazane, hexaethyldisilazane, hexapropyldisilazane, hexabutyldisilazane, hexapentyldisilazane, hexahexyldisilazane, hexacyclohexyldisilazane, hexaphenyldisilazane, and divinyltetramethydisilane; silazanes such as dimethyldisilazane and dimethyltetravinyldisilazane; silicone oils such as dimethylsilicone oil, methylhydrogensilicone oil, methylphenylsilicone oil, alkyl-modified silicone oil, chloroalkyl-modified silicone oil, chlorophenyl-modified silicone oil, fatty acid-modified silicone oil, polyether-modified silicone oil, alkoxy-modified silicone oil, carbinol-modified silicone oil, amino-modified silicone oil, fluorine-modified silicone oil, and terminal-reactive silicone oil;Siloxanes such as hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, hexamethyldisiloxane, and octamethyltrisiloxane; fatty acids and metal salts thereof include long-chain fatty acids such as undecylic acid, lauric acid, tridecylic acid, dodecylic acid, myristic acid, palmitic acid, pentadecylic acid, stearic acid, heptadecylic acid, arachidic acid, montanic acid, oleic acid, linoleic acid, and arachidonic acid, and salts of the above fatty acids with metals such as zinc, iron, magnesium, aluminum, calcium, sodium, and lithium;

[0025] Among these, alkoxysilanes, silazanes, and straight silicone oils are preferably used because they are easy to carry out hydrophobic treatment. These hydrophobic treatment agents may be used alone or in combination of two or more kinds.

[0026] The toner of the present disclosure has a surface formed of a polyester resin and a surface formed of a styrene-acrylic resin on the surface of the toner particles, and thus can exhibit a charge buffering effect due to frictional charging with silica particles having a specific average pore diameter and total pore volume. The polyester resin present on the surface of the toner particles is not particularly limited, and any known polyester resin can be used.

[0027] The polyester resin is preferably a condensation polymer of one or more polyhydric alcohols and one or more polycarboxylic acids. As the alcohol for synthesizing the polyester resin, for example, dihydric alcohols (more specifically, diols or bisphenols, etc.) or trihydric or higher alcohols such as those shown below can be suitably used. As the carboxylic acid for synthesizing the polyester resin, for example, divalent carboxylic acids or trivalent or higher carboxylic acids, their acid anhydrides or The polyester resin is more preferably a condensation polymer of a dihydric alcohol, a divalent carboxylic acid, and a trivalent carboxylic acid (an acid anhydride or a lower alkyl ester thereof).

[0028] Suitable examples of diols include ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, neopentyl glycol, 2-butene-1,4-diol, 1,5-pentanediol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, dipropylene glycol, polyethylene glycol, polypropylene glycol, and polytetramethylene glycol. Suitable examples of bisphenols include bisphenol A, hydrogenated bisphenol A, an ethylene oxide adduct of bisphenol A, and a propylene oxide adduct of bisphenol A. The number of moles added of the ethylene oxide adduct of bisphenol A or the propylene oxide adduct of bisphenol A is preferably 1.0 mol to 10.0 mol, and more preferably 1.0 mol to 4.0 mol.

[0029] Suitable examples of trihydric or higher alcohols include sorbitol, 1,2,3,6-hexanetetrol, 1,4-sorbitan, pentaerythritol, dipentaerythritol, tripentaerythritol, 1,2,4-butanetriol, 1,2,5-pentanetriol, glycerol, diglycerol, 2-methylpropanetriol, 2-methyl-1,2,4-butanetriol, trimethylolethane, trimethylolpropane, and 1,3,5-trihydroxymethylbenzene.

[0030] Suitable examples of the divalent carboxylic acid include maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, phthalic acid, isophthalic acid, terephthalic acid, cyclohexanedicarboxylic acid, adipic acid, sebacic acid, azelaic acid, malonic acid, succinic acid, alkylsuccinic acid (more specifically, n-butylsuccinic acid, isobutylsuccinic acid, n-octylsuccinic acid, n-dodecylsuccinic acid, isododecylsuccinic acid, etc.), and alkenylsuccinic acid (more specifically, n-butenylsuccinic acid, isobutenylsuccinic acid, n-octenylsuccinic acid, n-dodecenylsuccinic acid, isododecenylsuccinic acid, etc.).

[0031] Examples of trivalent or higher carboxylic acids, their acid anhydrides, and their lower alkyl esters include 1,2,4-benzenetricarboxylic acid (trimellitic acid), 2,5,7-naphthalenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, 1,2,4-butanetricarboxylic acid, 1,2,5-hexanetricarboxylic acid, 1,3-dicarboxyl-2-methyl-2-methylenecarboxypropane, 1,2,4-cyclohexanetricarboxylic acid, tetra(methylenecarboxyl)methane, 1,2,7,8-octanetetracarboxylic acid, pyromellitic acid, empol trimer acid, and their acid anhydrides and lower alkyl esters.

[0032] The dihydric alcohol preferably includes a bisphenol. The acid value of the polyester resin is preferably 0.5 mgKOH / g or more and 20.0 mgKOH / g or less, and more preferably 1.0 mgKOH / g or more and 10.0 mgKOH / g or less. The glass transition temperature Tg of the polyester resin is preferably 50°C to 70°C.

[0033] The styrene-acrylic resin present on the surface of the toner particles is not particularly limited, and any known styrene-acrylic resin can be used. Styrene-acrylic resins are copolymers of one or more styrene monomers and one or more acrylic monomers. To synthesize styrene-acrylic resins, for example, Styrenic and acrylic monomers such as those shown below can be suitably used.

[0034] Suitable examples of the styrene-based monomer include styrene, alkylstyrene (more specifically, α-methylstyrene, p-ethylstyrene, 4-tert-butylstyrene, etc.), p-hydroxystyrene, m-hydroxystyrene, vinyltoluene, α-chlorostyrene, o-chlorostyrene, m-chlorostyrene, and p-chlorostyrene.

[0035] Suitable examples of the acrylic monomer include (meth)acrylic acid, (meth)acrylic acid alkyl esters, and (meth)acrylic acid hydroxyalkyl esters. Suitable examples of the (meth)acrylic acid alkyl ester include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, iso-propyl (meth)acrylate, n-butyl (meth)acrylate, iso-butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. Suitable examples of the (meth)acrylic acid hydroxyalkyl ester include 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. The styrene-acrylic resin is preferably a copolymer of a monomer containing styrene and an alkyl (meth)acrylate.

[0036] The toner particles preferably have a total area ratio (St-Ac+PES area ratio) of the surfaces formed of styrene-acrylic resin and polyester resin to the total area of ​​the toner particle surface of 90% or more, more preferably 95% or more, and the upper limit is preferably 100% or less. Furthermore, on the toner particle surface, the ratio of the area of ​​the surface formed by the styrene-acrylic resin to the total area of ​​the surfaces formed by the styrene-acrylic resin and the polyester resin (St-Ac area ratio) is preferably 40 area % or more and 80 area % or less, and more preferably 45 area % or more and 75 area % or less. The toner particle surface may have a surface formed of other components in addition to the styrene-acrylic resin and polyester resin. The surface formed of other components is not particularly limited, but is preferably 10% by area or less of the total area of ​​the toner particle surface, so that the charge buffering effect can be more effectively exhibited.

[0037] By making the St-Ac area ratio 40 area % or more and 80 area % or less, the charge amount can be further stabilized throughout durable use, regardless of the environment. Under normal printing conditions, as the toner in the developing unit undergoes continuous use, the silica particles present on the surface of the toner particles tend to become embedded in and detached from the toner particles due to the stress received from the rubbing member, and the amount of silica particles functioning on the surface of the toner particles tends to decrease.

[0038] Even if the number of silica particles functioning on the toner particle surface decreases, by setting the St-Ac area ratio to 40 area % or more, the charge buffering action provides excellent effectiveness in suppressing charge-up even in low temperature and low humidity environments. Furthermore, by setting the St-Ac area ratio to 80% or less, a charge buffering effect is achieved, and a decrease in the amount of charge in a high-temperature, high-humidity environment can be suppressed.

[0039] On the other hand, when high-resolution images are continuously output, silica particles tend to temporarily accumulate in the developing device, and the amount of silica particles present on the toner particle surface tends to increase. Even if the number of silica particles functioning on the toner particle surface increases, the St-Ac area ratio is reduced to 40 area % or less. By setting the St-Ac area ratio at 80% or less, charge-up can be suppressed. The St-Ac area ratio can be controlled by adjusting the particle size and the amount of resin particles added, which are fixed to the surface of the toner particles by a wet method or by external addition. The ratio of the area of ​​the surface formed by the polyester resin to the total area occupied by the surface formed by the styrene-acrylic resin and the surface formed by the polyester resin (PES area ratio) is preferably 20 area% or more and 60 area% or less, and more preferably 25 area% or more and 55 area% or less.

[0040] The toner of the present disclosure exhibits a charge buffering effect due to the difference in characteristic triboelectric charging characteristics between the porous silica particles and each of the polyester resin and styrene-acrylic resin on the surface of the toner particles, which is caused by the action of water retained in the pores. The toner may be a negatively charged toner or a positively charged toner. The control of the positive chargeability or negative chargeability can be achieved by the resin composition of the toner particle surface, the addition of a charge control agent, or the selection of a surface treatment agent for an external additive.

[0041] It is necessary that, on the surface of the toner particle, a surface formed of the polyester resin and a surface formed of the styrene-acrylic resin are clearly and independently present. A preferred embodiment is a method in which the toner particles have a core-shell structure, the composition of the core portion and the composition of the shell portion are selected from a styrene-acrylic resin and a polyester resin, respectively, and the shell portion is not completely covered, leaving part of the core exposed, thereby providing two surfaces. Specifically, applicable methods include a method of adding resin fine particles having a different composition to the core particles to form a shell, a method of fixing the added resin fine particles by further applying a mechanical impact, and a method of forming a film of the added resin fine particles by heating the added resin fine particles, etc.

[0042] Among these, a form in which the resin particles forming the shell are present in a state of being fused to each other and to the core particle is preferred because it provides an excellent charge buffering effect since the contact opportunity between the silica particles and the toner particle surface can be stably maintained. Whether the core component of the core-shell structure is a polyester resin or a styrene-acrylic resin, as long as there is an exposed portion of the core, a charge buffering effect can be obtained due to friction with the silica particles.

[0043] The toner particles preferably have a core-shell structure having a core particle and a shell formed on the surface of the core particle. It is preferable that the core particle contains a polyester resin, the shell contains a styrene-acrylic resin, and a part of the polyester resin contained in the core particle is exposed on the surface of the toner particle, so that the surface of the toner particle has a surface formed of the polyester resin. More preferably, the resin component contained in the core particle is a polyester resin, and the resin component contained in the shell is a styrene-acrylic resin. It is even more preferable that the resin component of the shell is composed only of a styrene-acrylic resin. It is also preferred that the core particles contain a styrene-acrylic resin, the shell contains a polyester resin, and a part of the styrene-acrylic resin contained in the core particles is exposed on the surface of the toner particles, so that the surface of the toner particles has a surface formed of the styrene-acrylic resin. More preferably, the resin component contained in the core particles is a styrene-acrylic resin, and the resin component contained in the shell is a polyester resin. It is even more preferred that the resin component of the shell is composed of only a polyester resin. A configuration in which the core particle contains a polyester resin and the shell contains a styrene-acrylic resin is preferred since the absolute value of the charge amount can be kept high and development stability tends to be further improved.

[0044] The core particles are particles prepared by the pulverization method, the suspension polymerization method, the dissolution suspension method, and the emulsion polymerization aggregation method. Children can be used. Among these, when particles obtained by a pulverization method are used for the core, it is preferable because the core resin can be easily exposed in the step of forming the shell layer, and a surface in which the core resin is clearly present can be formed.

[0045] The resin particles forming the shell preferably have a number-average particle size of 10 nm to 500 nm, more preferably 20 nm to 200 nm. Resin particles with a number-average particle size of 10 nm or more are likely to form a uniform and stable surface on the surface of the core particle. In addition, resin particles with a number-average particle size of 500 nm or less can control the layer thickness of the part formed by the resin particles to be uniform and even. The amount of the shell is preferably 0.20 parts by mass or more and 7.00 parts by mass or less, and more preferably 0.50 parts by mass or more and 2.00 parts by mass or less, relative to 100 parts by mass of the core particles.

[0046] The components of the toner particles will now be described. [Binding resin] The toner particles contain a binder resin. Since the toner particles have a surface formed of a styrene-acrylic resin and a surface formed of a polyester resin, the toner particles preferably have a styrene-acrylic resin and / or a polyester resin as a binder resin. The toner particles may contain other resins as binder resins. The other binder resins are not particularly limited, and for example, conventionally known resins such as vinyl resins, olefin resins, polyurethane resins, and polyamide resins can be used.

[0047] [Crosslinking agent] In order to control the molecular weight of the binder resin, a crosslinking agent may be added during polymerization of the polymerizable monomer. In the case of vinyl-based resins, examples thereof include aromatic divinyl compounds such as divinylbenzene and divinylnaphthalene; carboxylic acid esters having two double bonds such as ethylene glycol diacrylate, ethylene glycol dimethacrylate, 1,3-butanediol dimethacrylate, and 1,6-hexanediol diacrylate; divinyl compounds such as divinylaniline, divinyl ether, divinyl sulfide, and divinyl sulfone; and compounds having three or more vinyl groups.

[0048] In the case of polyester resin, a trivalent or higher polycarboxylic acid or polyol can be added. Examples of trivalent or higher polycarboxylic acids include trimellitic acid, pyromellitic acid, cyclohexanetricarboxylic acids, 2,5,7-naphthalenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, 1,2,4-butanetricarboxylic acid, 1,2,5-hexanetricarboxylic acid, 1,3-dicarboxyl-2-methylenecarboxylpropane, 1,3-dicarboxyl-2-methyl-methylenecarboxylpropane, tetra(methylenecarboxyl)methane, 1,2,7,8-octanetetracarboxylic acid, and anhydrides thereof. Examples of trihydric or higher polyols include sorbitol, 1,2,3,6-hexanetetol, 1,4-sorbitan, pentaerythritol, dipentaerythritol, tripentaerythritol, sucrose, 1,2,4-methanetriol, glycerin, 2-methylpropanetriol, 2-methyl-1,2,4-butanetriol, trimethylolethane, trimethylolpropane, and 1,3,5-trihydroxymethylbenzene. The amount of the crosslinking agent added is preferably 0.001 parts by mass or more and 10,000 parts by mass or less based on 100 parts by mass of the polymerizable monomer.

[0049] [wax] The toner particles may contain a wax. Examples of waxes include paraffin wax, microcrystalline wax, petroleum wax such as petrolatum and its derivatives, montan wax and its derivatives, hydrocarbon waxes and its derivatives by the Fischer-Tropsch process, polyolefin waxes such as polyethylene and polypropylene and their derivatives, natural waxes and their derivatives such as carnauba wax and candelilla wax, higher aliphatic alcohols, fatty acids such as stearic acid and palmitic acid, or compounds thereof, acid amide wax, ester wax, ketone, hydrogenated castor oil and its derivatives, vegetable wax, animal wax, and silicone resin. Hydrocarbon wax and ester wax are preferred. The derivatives include oxides, block copolymers with vinyl monomers, and graft modified products. The content of the wax is preferably 2.0 parts by mass or more and 20.0 parts by mass or less with respect to 100 parts by mass of the binder resin or the polymerizable monomer that produces the binder resin.

[0050] [Coloring agent] The toner particles may contain a colorant. The colorant is not particularly limited, and any known colorant can be used. Examples of yellow pigments that can be used include condensed azo compounds such as yellow iron oxide, navel yellow, naphthol yellow S, Hansa yellow G, Hansa yellow 10G, benzidine yellow G, benzidine yellow GR, quinoline yellow lake, permanent yellow NCG, and tartrazine lake, isoindolinone compounds, anthraquinone compounds, azo metal complexes, methine compounds, and allylamide compounds. Specific examples include the following. CI Pigment Yellow 12, 13, 14, 15, 17, 62, 74, 83, 93, 94, 95, 109, 110, 111, 128, 129, 147, 155, 168, 180, 185, 193. Orange pigments include the following: Permanent Orange GTR, Pyrazolone Orange, Balkan Orange, Benzidine Orange G, Induthrene Brilliant Orange RK, Induthrene Brilliant Orange GK.

[0051] Examples of red pigments include condensed azo compounds such as red iron oxide, permanent red 4R, lithol red, pyrazolone red, watching red calcium salt, lake red C, lake red D, brilliant carmine 6B, brilliant carmine 3B, eoxin lake, rhodamine lake B, and alizarin lake, diketopyrrolopyrrole compounds, anthraquinone compounds, quinacridone compounds, basic dye lake compounds, naphthol compounds, benzimidazolone compounds, thioindigo compounds, and perylene compounds. Specific examples include the following. CI Pigment Red 2, 3, 5, 6, 7, 23, 48:2, 48:3, 48:4, 57:1, 81:1, 122, 144, 146, 150, 166, 169, 177, 184, 185, 202, 206, 220, 221, 254. Examples of blue pigments include alkali blue lake, Victoria blue lake, phthalocyanine blue, metal-free phthalocyanine blue, phthalocyanine blue partial chloride, fast sky blue, copper phthalocyanine compounds such as indanthrene blue BG and their derivatives, anthraquinone compounds, basic dye lake compounds, etc. Specific examples include the following. CI Pigment Blue 1, 7, 15, 15:1, 15:2, 15:3, 15:4, 60, 62, 66.

[0052] Purple pigments include Fast Violet B and Methyl Violet Lake. Green pigments include Pigment Green B, Malachite Green Lake, and Final Yellow Green G. White pigments include zinc oxide, titanium oxide, and antimony white. , zinc sulfide. Examples of black pigments include carbon black, aniline black, non-magnetic ferrite, magnetite, and pigments toned to black using the above-mentioned yellow, red and blue colorants. These colorants can be used alone or in combination, or in the form of a solid solution. The content of the colorant is preferably 3.0 parts by mass or more and 15.0 parts by mass or less with respect to 100.0 parts by mass of the binder resin or the polymerizable monomer that produces the binder resin.

[0053] [Magnetic material] The toner can also be used as a magnetic toner, in which case the following magnetic materials are used. Iron oxides such as magnetite, maghemite, ferrite, or with other metal oxides; metals such as Fe, Co, Ni, or alloys of these metals with metals such as Al, Co, Cu, Pb, Mg, Ni, Sn, Zn, Sb, Ca, Mn, Se, Ti, and mixtures thereof. More specifically, iron oxide (Fe3O4), iron sesquioxide (γ-Fe2O3), zinc iron oxide (ZnFe2O4), copper iron oxide (CuFe2O4), neodymium iron oxide (NdFe2O3), barium iron oxide (BaFe 12 O 19 ), magnesium iron oxide (MgFe2O4), and manganese iron oxide (MnFe2O4). The above-mentioned magnetic materials can be used alone or in combination of two or more. Particularly suitable magnetic materials are fine powders of iron tetraoxide or gamma-iron sesquioxide.

[0054] The average particle diameter of these magnetic materials is preferably 0.1 μm or more and 2 μm or less, and more preferably 0.1 μm or more and 0.3 μm or less. The magnetic properties at an applied current of 795.8 kA / m (10 kOersted) are a coercive force (Hc) of 1.6 kA / m or more and 12 kA / m or less (20 Oersted or more and 150 Oersted or less), a saturation magnetization (σs) of 5 Am 2 / kg or more 200Am 2 / kg or less, preferably 50Am 2 / kg or more 100Am 2 / kg or less. The residual magnetization (σr) is 2Am 2 / kg or more 20Am 2 / kg or less is preferred. The content of the magnetic material is preferably from 10 to 200 parts by mass, more preferably from 20 to 150 parts by mass, relative to 100 parts by mass of the binder resin.

[0055] [Charge control agent] The toner particles may contain a charge control agent. Any known charge control agent can be used. In particular, a charge control agent that quickly increases the charge amount is preferred because it has excellent retention characteristics at an appropriate charge amount.

[0056] The following can be mentioned as the substances that control the toner particles to have a negative charge. metal compounds of aromatic carboxylic acids such as salicylic acid, alkylsalicylic acid, dialkylsalicylic acid, naphthoic acid, and dicarboxylic acids, or polymers or copolymers having metal compounds of the above aromatic carboxylic acids; Polymers or copolymers having sulfonic acid groups, sulfonate groups or sulfonate ester groups; Metal salts or metal complexes of azo dyes or azo pigments; Boron compounds, silicon compounds, calixarenes, etc.

[0057] As the polymer or copolymer having a sulfonate group or a sulfonate ester group, the following can be used. Styrene sulfonic acid, 2-acrylamido-2-methylpropane sulfonic acid, 2-methacrylamido-2-methylpropane sulfonic acid, vinyl sulfonic acid, methacryl sulfone Homopolymers of sulfonic acid group-containing vinyl monomers such as sulfonic acid, or copolymers of the vinyl monomers listed in the binder resin section and the above-mentioned sulfonic acid group-containing vinyl monomers.

[0058] The following can be mentioned as the substances that control the positive charge of the toner particles. Examples of the compound include quaternary ammonium salts, polymeric compounds having quaternary ammonium salts in the side chains, guanidine compounds, nigrosine compounds, and imidazole compounds. Examples of the resin-based charge control agent include melamine resin, guanamine resin, aniline resin, urea resin, polyurethane resin, sulfonamide resin, polyimide resin, and derivatives of these resins.

[0059] These charge control agents can be used alone or in combination of two or more. The amount of the charge control agent added is 0.01 to 10 parts by mass based on 100 parts by mass of the binder resin. It is preferable that it be .0 part by weight or less. However, if sufficient chargeability is ensured in the toner, it is not necessary to include a charge control agent.

[0060] [External additives] In addition to the silica particles, the toner may contain a fluidizing agent, a cleaning aid, and the like as so-called external additives in order to satisfy flowability, cleaning properties, and the like. The external additive can be any known external additive without any particular limitation.Specific examples of the external additive include inorganic fine particles such as silica particles or metal oxides (more specifically, alumina, titanium oxide, magnesium oxide, zinc oxide, zinc stearate, strontium titanate, calcium titanate, barium titanate, hydrotalcite, etc.), organic fine particles made of vinyl resin, silicone resin, melamine resin, etc., and organic-inorganic composite fine particles.

[0061] These may be used alone or in combination of two or more. The external additive may be surface-treated. Surface treatment agents include higher fatty acids, silicone varnishes, various modified silicone varnishes, unmodified silicone oils, various modified silicone oils, silane compounds, silane coupling agents, other organic silicon compounds, and organic titanium compounds, and may be used alone or in combination.

[0062] [Method of manufacturing toner particles] Hereinafter, a method for producing toner particles having a core-shell structure will be described as an example of a preferred embodiment in which a surface formed of a styrene-acrylic resin and a surface formed of a polyester resin are formed on the surface of a toner particle.

[0063] (Preparation of core particles) The core particles of the toner can be produced by any known method, such as a suspension polymerization method, a dissolution suspension method, an emulsion polymerization aggregation method, or a pulverization method.

[0064] When the core particles are obtained by the suspension polymerization method, first, a polymerizable monomer constituting a binder resin, and optionally a wax and a colorant, etc. are mixed to prepare a polymerizable monomer composition. Next, an aqueous medium containing a dispersion stabilizer is prepared and charged into a stirring tank equipped with a stirrer having high shear force, a polymerizable monomer composition is added thereto, and the polymerizable monomer composition is dispersed by stirring to form droplets of the polymerizable monomer composition. Subsequently, the polymerizable monomer in the droplets of the polymerizable monomer composition is polymerized to produce a binder resin and obtain core particles.

[0065] When core particles are obtained by the dissolution suspension method, a resin solution is prepared by uniformly dissolving or dispersing a binder resin, and if necessary, other materials such as wax, a polar resin, a colorant, and a charge control agent in an organic solvent. The obtained resin solution is dispersed in an aqueous medium and granulated, and the granulated particles are then dispersed in an aqueous medium. The organic solvent contained in the particles is removed to obtain core particles having a desired particle size.

[0066] When obtaining core particles by the emulsion aggregation method, first, fine particles of binder resin and fine particles of materials such as colorants are dispersed and mixed in an aqueous medium containing a dispersion stabilizer. A surfactant may be added to the aqueous medium. Then, an aggregating agent is added to aggregate the particles until the desired core particle diameter is obtained, and then or simultaneously with the aggregation, the resin fine particles are fused together. If necessary, the shape is controlled by heat to obtain the core particles.

[0067] When the core particles are produced by the pulverization method, the binder resin is mixed with components such as a colorant, a release agent, and a charge control agent as necessary. The resulting mixture is then melt-kneaded. The resulting melt-kneaded product is then pulverized, and the resulting pulverized product is classified. As a result, core particles having a desired particle size are obtained.

[0068] (Shell formation) Next, a shell is formed on the surface of the obtained core particle. A preferred example of a method for forming the shell will be described below. A dispersion of core particles and resin particles that form the shell is added to an aqueous medium whose pH has been adjusted. The resin fine particles adhere to the surface of the core particles in the aqueous medium. In order to uniformly adhere the resin fine particles to the surface of the core particles, it is preferable to highly disperse the core particles in the aqueous medium containing the resin fine particles. For this purpose, it is effective to add a surfactant or to strengthen the stirring force.

[0069] The surfactant includes anionic surfactants, cationic surfactants, amphoteric surfactants, and nonionic surfactants. Specific examples of such surfactants include anionic surfactants such as alkylbenzenesulfonates, α-olefinsulfonates, and phosphate esters; cationic surfactants of the amine salt type such as alkylamine salts, aminoalcohol fatty acid derivatives, polyamine fatty acid derivatives, and imidazolines, and quaternary ammonium salt type such as alkyltrimethylammonium salts, dialkyldimethylammonium salts, alkyldimethylbenzylammonium salts, pyridinium salts, alkylisoquinolinium salts, and benzethonium chloride; nonionic surfactants such as fatty acid amide derivatives and polyhydric alcohol derivatives; and amphoteric surfactants such as alanine, dodecyldi(aminoethyl)glycine, di(octylaminoethyl)glycine, and N-alkyl-N,N-dimethylammonium betaine. The surfactant may be used alone or in combination of two or more kinds.

[0070] The amount of the resin particles that form the shell is appropriately adjusted so as to achieve a desired coverage rate at which the core particles are exposed. Next, the aqueous medium containing the core particles and resin fine particles is heated to a temperature of 50° C. or more and 85° C. or less at a rate of 0.1° C. / min to 3° C. / min while being stirred.

[0071] Furthermore, in order to ensure that the formation of the shell proceeds satisfactorily, it is preferable to provide a retention time of 30 minutes or more and 8 hours or less. While the temperature of the aqueous medium is maintained at a high temperature, the resin fine particles are fixed to the surface of the core particles, or a film is formed by melting the resin fine particles. The shell can be formed in either a granular form in which resin particles are two-dimensionally connected, or in a film-like form by dissolution. The adhesion state of the resin particles can be either adhesion by melting the core particles or adhesion by melting the resin particles.

[0072] Subsequently, the dispersion of the core-shell particles is neutralized and then cooled to room temperature. The cooled dispersion of the core-shell particles is filtered, washed, and then dried to obtain toner particles having a core-shell structure in which the core particles are partially exposed.

[0073] Another example of a method for forming a shell by a dry process will be described. The core particles and the resin fine particles are mixed using a mixer (for example, FM Mixer (manufactured by Nippon Coke and Engineering Co., Ltd.)) to cause the resin fine particles to adhere to the surfaces of the toner core particles, thereby forming a shell. Furthermore, if necessary, the shell can be surface-treated using a Hybridization System (manufactured by Nara Machinery Works), Mechanofusion System (manufactured by Hosokawa Micron Corporation), Faculty (manufactured by Hosokawa Micron Corporation), Meteor Rainbow MR Type (manufactured by Nippon Pneumatic Co., Ltd.), etc.

[0074] [Toner manufacturing method] The above-mentioned silica particles and, if necessary, other external additives can be added to the toner particles to obtain a toner. Examples of external addition devices that can be used include a double cone mixer, a V-type mixer, a drum type mixer, a Super Mixer (manufactured by Kawata Corporation), an FM Mixer (manufactured by Nippon Coke & Engineering Co., Ltd.), a Nobilta (manufactured by Hosokawa Micron Corporation), a Hybridizer (manufactured by Nara Machinery Works, Ltd.), a Nauta Mixer, and a Mechano Hybrid.

[0075] The toner can be used as a one-component developer, but may also be mixed with a carrier to be used as a two-component developer. As the carrier, for example, magnetic particles made of a conventionally known material such as metals such as iron, ferrite, magnetite, and alloys of these metals with metals such as aluminum and lead can be used, and among these, it is preferable to use ferrite particles. Furthermore, as the carrier, a coated carrier in which the surface of a magnetic particle is coated with a coating agent such as a resin, or a resin dispersion type carrier in which a magnetic fine powder is dispersed in a binder resin may also be used. The carrier preferably has a volume average particle size of 15 μm or more and 100 μm or less, and more preferably has a volume average particle size of 25 μm or more and 80 μm or less.

[0076] The methods for measuring various physical properties will be described below. When measuring the physical properties of silica particles or toner particles from a toner to which silica particles have been externally added, the silica particles and other external additives can be separated from the toner and then measured. The toner is ultrasonically dispersed in methanol to separate the silica particles and other external additives, and then left to stand for 24 hours. The settled toner particles are separated from the silica particles and other external additives dispersed in the supernatant, and then collected, thoroughly washed, and dried to isolate the toner particles. The supernatant can also be repeatedly centrifuged using a centrifuge method to isolate the silica particles and other external additives.

[0077] <Number average particle size of primary particles of silica particles> The number average particle size of the primary silica particles is measured using a transmission electron microscope "JEM-2800" (JEOL Ltd.). The toner with silica microparticles added is observed, and the number average particle size is calculated by measuring the major axis of the primary particles of 100 randomly selected silica particles in a field of view magnified up to 200,000 times. The observation magnification is adjusted appropriately depending on the size of the silica particles. The silica particles can be distinguished from the external additives in the toner by STEM-EDS measurement under the following measurement conditions. JEM2800 transmission electron microscope: accelerating voltage 200 kV EDS detector: JED-2300T (JEOL, element area 100 mm2 ) EDS analyzer: Noran System 7 (Thermo Fisher Scientific) (Dick Co., Ltd.) X-ray storage rate: 10000~15000cps Dead time: The electron dose was adjusted to 20% to 30%, and EDS analysis was performed (100 times accumulation or measurement time 5 min).

[0078] <Hydrophobicity of Silica Particles> The hydrophobicity of the silica particles is measured using a powder wettability tester "WET-100P" (manufactured by Rhesca Corporation). A fluororesin-coated spindle-shaped rotor with a length of 25 mm and a maximum body diameter of 8 mm is placed in a cylindrical glass container with a diameter of 5 cm and a thickness of 1.75 mm. 70 ml of a water-containing methanol solution consisting of 50% by volume of methanol and 50% by volume of water is placed in the cylindrical glass container, after which 0.5 g of silica particles is added and the container is set in a powder wettability tester. Using a magnetic stirrer, add methanol to the liquid at a rate of 0.8 mL / min through the powder wettability tester while stirring at 3.3 revolutions / sec. Measure the transmittance with light of 780 nm wavelength, and the value expressed by the volume percentage of methanol (= (volume of methanol / volume of mixture) x 100) when the transmittance reaches 50% is taken as the degree of hydrophobicity. Adjust the initial volume ratio of methanol to water appropriately depending on the degree of hydrophobicity of the sample.

[0079] <Average pore size and total pore volume of silica particles> The average pore size and total pore volume of the silica particles are measured by a gas adsorption method in which nitrogen gas is adsorbed on the surface of a sample using a pore distribution measuring device Tristar 3000 (manufactured by Shimadzu Corporation). The measurement method follows the operation manual issued by Shimadzu Corporation. First, about 0.5 g of sample is placed in a sample tube and vacuum is applied at 100°C for 24 hours. After vacuum application is completed, the mass of the sample is precisely weighed to obtain a sample. From the obtained sample, the average pore size and the total pore volume in the pore size range of 1.7 nm to 300.0 nm can be obtained by the BJH method using the pore size distribution measuring device. The density value required for measurement is the true density value measured using a dry density meter Accupyc 1330 (manufactured by Shimadzu Corporation).

[0080] <Confirmation of the surfaces formed of polyester resin and the surfaces formed of styrene-acrylic resin, and the ratio of the total area of ​​the surfaces formed of styrene-acrylic resin and the surfaces formed of polyester resin to the total area of ​​the toner particle surface> The St-Ac+PES area ratio can be determined by dyeing toner particles with ruthenium, and analyzing an image of the dyed toner particles observed using a scanning electron microscope. A scanning electron microscope, JSM-7800F (manufactured by JEOL Ltd.), was used to analyze the reflected electron images of the dyed toner particles. The ease with which ruthenium is stained varies depending on the type of resin. For example, the rate at which ruthenium staining progresses is significantly different between polyester resin and styrene-acrylic resin. For this reason, in the backscattered electron image of the obtained toner particle surface, a difference in brightness occurs between the surface formed of polyester resin and the surface formed of styrene-acrylic resin, making it possible to recognize each of the surface formed of polyester resin and the surface formed of styrene-acrylic resin.

[0081] Image analysis is performed using image analysis software ("WinROOF" manufactured by Mitani Shoji Co., Ltd.) to perform binarization processing based on the brightness value of each pixel to obtain a binary image. In the obtained binary image, the total area attributable to the styrene-acrylic resin on the toner particle surface (hereinafter referred to as area St-Ac) and the total area attributable to the polyester resin (hereinafter referred to as area PES) are measured. When the toner particle surface has a surface formed of a resin other than the surface formed of the styrene-acrylic resin and the surface formed of the polyester resin, the difference in brightness This makes it possible to distinguish surfaces formed from other resins. In this case, by setting a threshold value of the brightness value attributable to the other resin, it is possible to measure the proportion of the area occupied by the surface formed of the other resin in the total area of ​​the toner particle surface.

[0082] The ratio of the total area of ​​the surfaces formed of the styrene-acrylic resin and the surfaces formed of the polyester resin to the total area of ​​the toner particle surfaces is calculated using the following formula. The area ratio is calculated for each of 100 toner particles, and the average value is used. The total area ratio (%) of the surfaces formed of styrene-acrylic resin and polyester resin to the total area of ​​the toner particle surface = "area St - Ac + area PES" / "total area of ​​the toner particle surface" x 100 When the resin present on the surface of the toner particle consists only of styrene-acrylic resin and polyester resin, the total area ratio of the surfaces formed of styrene-acrylic resin and polyester resin to the total area of ​​the toner particle surface is 100%.

[0083] <The ratio of the area of ​​the surface formed by styrene-acrylic resin to the total area of ​​the surface formed by styrene-acrylic resin and the surface formed by polyester resin> The above-described ruthenium dyeing of the toner particles and image analysis of the dyed toner particle surfaces are carried out, and the St-Ac area ratio is calculated according to the following formula. The area ratio is calculated for each of 100 toner particles, and the average value is used. The percentage of the area of ​​the surface formed by styrene-acrylic resin out of the total area of ​​the surface formed by styrene-acrylic resin and the surface formed by polyester resin (%) = "Area St-Ac" / "Area St-Ac + Area PES" x 100

[0084] <Measurement of toner particle size> The particle size of the toner particles can be measured by a capillary electric resistance method. For example, it can be measured and calculated using a "Coulter Counter Multisizer 3" and the accompanying dedicated software "Beckman Coulter Multisizer 3 Version 3.51" (manufactured by Beckman Coulter, Inc.). A precision particle size distribution measuring device using the pore electrical resistance method (product name: Coulter Counter Multisizer 3) and dedicated software (product name: Beckman Coulter Multisizer 3 Version 3.51, manufactured by Beckman Coulter, Inc.) are used. The aperture diameter is 100 μm, and measurements are made with an effective number of measurement channels of 25,000. The measurement data is then analyzed and calculated. The aqueous electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of approximately 1 mass %, for example ISOTON II (trade name) manufactured by Beckman Coulter. Before carrying out the measurements and analyses, the dedicated software is set up as follows. In the "Change Standard Measurement Method (SOM) screen" of the dedicated software, set the total count number in the control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using (standard particle 10.0 μm, Beckman Coulter). Press the threshold / noise level measurement button to automatically set the threshold and noise level. In addition, set the current to 1600 μA, the gain to 2, the electrolyte to ISOTON II (trade name), and check the aperture tube flush after measurement. In the "Pulse to particle size conversion setting screen" of the dedicated software, set the bin interval to logarithmic particle size, the particle size bin to 256 particle size bins, and the particle size range to 2 μm to 60 μm.

[0085] The specific measurement method is as follows. (1) Pour about 200 mL of the electrolyte solution into a 250 mL round-bottom glass beaker made exclusively for the Multisizer 3, set it on the sample stand, and stir the stirrer rod counterclockwise at 24 revolutions per second. Then, remove dirt and air bubbles from inside the aperture tube using the "Aperture Tube Flush" function of the dedicated software. (2) About 30 mL of the aqueous electrolyte solution is placed in a 100 mL flat-bottom glass beaker, and about 0.3 mL of a diluted solution of Contaminon N (trade name) (a 10% aqueous solution of a neutral detergent for cleaning precision measuring instruments, manufactured by Wako Pure Chemical Industries, Ltd.) diluted three times by mass with ion-exchanged water is added thereto. (3) An ultrasonic disperser with two built-in oscillators with an oscillation frequency of 50 kHz and a phase shift of 180 degrees, and an electrical output of 120 W (product name: Ultrasonic Dispersion System Tetora150, manufactured by Nikkaki Bios Co., Ltd.) Add a specified amount of ion-exchanged water and approximately 2 mL of Contaminon N (trade name) to the water tank. (4) The beaker (2) is set in the beaker fixing hole of the ultrasonic disperser, and the ultrasonic disperser is operated. Then, the height position of the beaker is adjusted so that the resonance state of the liquid surface of the electrolyte solution in the beaker is maximized. (5) While the electrolyte solution in the beaker in (4) is irradiated with ultrasonic waves, about 10 mg of toner (particles) is added little by little to the electrolyte solution and dispersed. Then, ultrasonic dispersion treatment is continued for another 60 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to be 10°C or higher and 40°C or lower. (6) Using a pipette, add the electrolytic solution (5) in which the toner (particles) is dispersed to the round-bottom beaker (1) placed in the sample stand, and adjust the measurement concentration to about 5%. Then, measurements are continued until the number of particles measured reaches 50,000. (7) The measurement data is analyzed using the dedicated software that comes with the device, and the weight average particle size (D4) is calculated. Note that when the dedicated software is set to Graph / Volume %, the "Average diameter" on the "Analysis / Volume Statistics (Arithmetic Mean)" screen is the weight average particle size (D4). When the dedicated software is set to Graph / Number %, the "Average diameter" on the "Analysis / Number Statistics (Arithmetic Mean)" screen is the number average particle size (D1).

[0086] <Acid value measurement> The acid value of resins, etc. is determined by the following procedure. The acid value is the number of milligrams of potassium hydroxide required to neutralize the acid contained in 1 g of sample. The basic procedure is based on JIS K0070-1992, but specifically, the measurement is performed according to the following procedure. (1) Preparation of reagents Dissolve 1.0 g of phenolphthalein in 90 ml of ethyl alcohol (95% by volume) and add ion-exchanged water to make 100 ml to obtain a phenolphthalein solution. Dissolve 7 g of special grade potassium hydroxide in 5 ml of water, and add ethyl alcohol (95% by volume) to make 1 L. Place in an alkali-resistant container to avoid contact with carbon dioxide and the like, leave for 3 days, then filter to obtain a potassium hydroxide solution. Store the resulting potassium hydroxide solution in an alkali-resistant container. The factor of the potassium hydroxide solution is determined by placing 25 ml of 0.1 mol / L hydrochloric acid in an Erlenmeyer flask, adding several drops of the phenolphthalein solution, and titrating with the potassium hydroxide solution, from the amount of the potassium hydroxide solution required for neutralization. The 0.1 mol / L hydrochloric acid used is prepared in accordance with JIS K 8001-1998. (2) Operation (A) Main Test 2.0 g of the crushed sample was precisely weighed into a 200 mL Erlenmeyer flask, and 100 mL of a mixed solution of toluene:ethanol (2:1) was added and dissolved for 5 hours. Next, several drops of the phenolphthalein solution were added as an indicator, and titration was performed using the potassium hydroxide solution. The end point of the titration was when the light red color of the indicator continued for about 30 seconds. (B) Blank test The titration is carried out in the same manner as above, except that no sample is used (i.e., only the toluene:ethanol (2:1) mixed solution is used). (3) The obtained result is substituted into the following formula to calculate the acid value. A = [(CB) × f × 5.61] / S Here, A is the acid value (mgKOH / g), B is the amount of potassium hydroxide solution added for the blank test (mL), C is the amount of potassium hydroxide solution added for the main test (mL), f is the factor of the potassium hydroxide solution, and S is the mass of the sample (g).

[0087] <Measurement of glass transition temperature (Tg) of resins, etc.> The glass transition temperature and the melting peak temperature are measured using a differential scanning calorimeter "Q2000" (manufactured by TA Instruments) in accordance with ASTM D3418-82. The melting points of indium and zinc are used for temperature correction of the device detection section, and the heat of fusion of indium is used for heat correction. Specifically, 3 mg of a sample such as a resin is precisely weighed and placed in an aluminum pan. Using an empty aluminum pan as a reference, measurement is performed under the following conditions. Heating rate: 10℃ / min Measurement start temperature: 30℃ End of measurement temperature: 180℃ Measurements are performed in the measurement range of 30 to 180°C at a heating rate of 10°C / min. The temperature is raised to 180°C once and held for 10 minutes, then cooled to 30°C, and then raised again. During this second heating process, the specific heat change is obtained in the temperature range of 30 to 100°C. The point at which the line midway between the baselines before and after the specific heat change appears and the differential thermal curve intersect is the glass transition temperature (Tg) of the resin. EXAMPLES

[0088] The present invention will be described in more detail below with reference to examples. The present invention is not limited to the following examples. In the following formulations, the number of parts is based on mass unless otherwise specified.

[0089] <Production Example of Silica Particle 1> A 1.5 L glass reaction vessel equipped with a stirrer, a dropping nozzle, and a thermometer was charged with 500 parts of methanol and 70 parts of water whose pH had been adjusted to 8.3 with 10% by mass aqueous ammonia, and mixed to obtain a catalyst solution. This alkaline catalyst solution was adjusted to 40° C., and then 100 parts of tetramethoxysilane (TMOS) and 20 parts of 1.0 mass % aqueous ammonia were simultaneously added dropwise over 60 minutes while stirring to obtain a hydrophilic silica particle dispersion. Thereafter, the obtained silica particle dispersion liquid was concentrated to a solid concentration of 40 mass % using a rotary filter R-Fine (manufactured by Kotobuki Industries Co., Ltd.) to obtain a silica particle dispersion liquid. To 250 parts of the concentrated silica particle dispersion, 40 parts of hexamethyldisilazane (HMDS) was added as a hydrophobic treatment agent, and the mixture was reacted at 130°C for 2 hours, cooled, and then dried by spray drying to obtain silica particles 1. The physical properties of the obtained silica particles 1 are shown in Table 1.

[0090] <Production Example of Silica Particles 2> In the manufacturing example of silica particles 1, the same steps were carried out except that the pH of the alkaline aqueous solution added to the catalyst solution was changed to 5.6, the adjustment temperature of the catalyst solution was changed to 30° C., and 20 parts of dimethylformamide (DMF) was added dropwise over 100 minutes in addition to the TMOS and 1.0 mass % ammonia water to be dropped, to obtain silica particles 2. The physical properties of the obtained silica particles 2 are shown in Table 1.

[0091] <Production Examples of Silica Particles 3 to 9> The same as silica particles 1 except that some of the manufacturing conditions for silica particles 1 were changed to the conditions shown in Table 1. Silica particles 3 to 9 were prepared using DMF (examples in which DMF was used were prepared in the same manner as silica particles 2). The physical properties are shown in Table 1. The pH of the water added to the catalyst solution was adjusted to 10% by mass ammonia. The solution was adjusted using NiO2 water and 10% by mass hydrochloric acid.

[0092] <Production Example of Silica Particles 10> Silica particles 10 were obtained by carrying out the same steps as in the manufacturing example of silica particles 1, except that hexamethyldisilazane (HMDS) added as a hydrophobizing agent was changed to 3-aminopropyltrimethoxysilane (APTMS). The physical properties of the obtained silica particles 10 are shown in Table 1.

[0093] <Production Examples of Silica Particles 11 and 12> The same as silica particles 1 except that some of the manufacturing conditions for silica particles 1 were changed to the conditions shown in Table 1. Silica particles 11 and 12 were prepared using DMF (Silica particles 11 was prepared in the same manner as silica particles 2). The physical properties are shown in Table 1. The pH of the water added to the catalyst solution was The solution was adjusted using 10% by mass of ammonia water and 10% by mass of hydrochloric acid.

[0094] <Production Example of Silica Particles 13> 100 parts of untreated fumed silica having a number average particle size of 12 nm was placed in a reaction vessel, and 2 parts of water were added under a nitrogen atmosphere, and 20 parts of 3-aminopropyltrimethoxysilane (APTMS) were added, and the mixture was heated and stirred at 200°C for 1 hour, and cooled after removing methanol. Subsequently, a crushing treatment was performed using a collision crushing device, and silica particles 13 were obtained. The physical properties of the obtained silica particles 13 are shown in Table 1.

[0095] <Production Example of Silica Particles 14> In the manufacturing example of silica particles 1, the pH of the alkaline aqueous solution added to the catalyst solution was changed to 6.6, the adjustment temperature of the catalyst solution was changed to 30°C, 30 parts of formaldehyde was added dropwise over 30 minutes in addition to the TMOS and 1.0 mass% ammonia water to be dropped, and the hydrophobizing agent was changed from hexamethyldisilazane (HMDS) to 3-aminopropyltrimethoxysilane (APTMS), to obtain silica particles 14. The physical properties of the obtained silica particles 14 are shown in Table 1.

[0096] [Table 1] The abbreviations in the table are as follows: HMDS: Hexamethyldisilazane APTMS: 3-aminopropyltrimethoxysilane

[0097] <Production of Polyester Resin 1> In a reaction vessel equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple, 47 mol parts of terephthalic acid, 35 mol parts of fumaric acid, 15 mol parts of dodecenylsuccinic acid, 60 mol parts of a propylene oxide 2-mol adduct of bisphenol A, and 40 mol parts of an ethylene oxide 2-mol adduct of bisphenol A were placed, and then 0.5 parts of dibutyltin oxide were added as a catalyst to 100 parts of the total amount of monomers. Next, the temperature was quickly raised to 180°C under normal pressure in a nitrogen atmosphere, and then water was distilled off while heating from 180°C to 210°C at a rate of 10°C / hour to carry out polycondensation. When the temperature reached 210° C., 1 mole of trimellitic anhydride was added, the pressure inside the reaction vessel was reduced to 5 kPa or less, and polycondensation was carried out under conditions of 210° C. and 5 kPa or less to obtain polyester resin 1. The physical properties of the obtained polyester resin 1 are shown in Table 2.

[0098] <Production of polyester resins 2 and 3> Polyester resins 2 and 3 were obtained in the same manner as in Production Example of Polyester Resin 1, except that the monomer composition was changed to the monomer composition shown in Table 2. The physical properties are shown in Table 2.

[0099] <Production of styrene-acrylic resin 1> In a reaction vessel equipped with a reflux condenser, a stirrer, a thermometer, and a nitrogen inlet tube, 100.0 parts of xylene, 80.0 parts of styrene, 20.0 parts of n-butyl acrylate, 0.3 parts of hexanediol diacrylate, and perbutyl O (10-hour half-life temperature 72.1°C (manufactured by NOF Corp.)) were added. 2.0 parts of the mixture was added, heated to 80° C., and stirred for 6 hours. The mixture was then heated to 100°C for 6 hours to remove the solvent, yielding a styrene-acrylic resin 1 for core resin. The glass transition temperature Tg of the resulting styrene-acrylic resin 1 was 60°C.

[0100] <Production of styrene acrylic modified polyester resin 1> Bisphenol A propylene oxide 2 mole adduct: 500 parts Terephthalic acid: 154 parts Fumaric acid: 45 parts Dibutyltin oxide: 3 parts The above materials were placed in a reaction vessel equipped with a reflux condenser, a stirrer, a thermometer, and a nitrogen inlet tube, and a polycondensation reaction was carried out at a temperature of 230°C for 8 hours. The polycondensation reaction was then continued for another hour at 8 kPa, and then cooled to 160°C. Next, 10 parts of acrylic acid was added while keeping the temperature at 160° C., and after mixing and maintaining the mixture for 20 minutes, a mixture of the following compounds was added dropwise using a dropping funnel over a period of 1 hour. Styrene: 315 parts n-Butyl acrylate: 65 parts Polymerization initiator (di-t-butyl peroxide): 9 parts After carrying out an addition polymerization reaction for 1 hour while maintaining the temperature at 160°C, the temperature was raised to 200°C and held at 10 kPa for 1 hour to produce styrene-acrylic modified polyester resin 1 with a styrene-acrylic copolymer molecular chain content of 35 mass%. The glass transition temperature Tg of the obtained styrene acrylic modified polyester resin 1 was 60°C.

[0101] [Table 2] The abbreviations in the table are as follows: BPA-PO: Bisphenol A propylene oxide 2 mol adduct BPA-EO: Bisphenol A with 2 mol of ethylene oxide

[0102] <Production of Core Particle 1> Polyester resin 1: 100 parts, hydrocarbon wax HNP-9 (manufactured by NOF Corporation, melting point 74°C) 5 parts, and colorant (CI Pigment Blue 15:3) 5 parts were mixed at a rotation speed of 2500 rpm using an FM mixer (manufactured by Nippon Coke and Engineering Co., Ltd.). The mixture was then melt-kneaded using a twin-screw extruder (PCM-30, manufactured by Ikegai Corporation). The kneaded mixture was then cooled. The cooled kneaded mixture was then pulverized using a turbo mill (manufactured by Freund Turbo Corporation). The pulverized mixture was then classified using a classifier (Elbow Jet EJ-LABO type, manufactured by Nittetsu Mining Co., Ltd.). As a result, core particles 1 having a weight average particle size (D4) of 6 μm were obtained.

[0103] <Production of Core Particle 2> Core particles 2 having a weight average particle size (D4) of 6 μm were obtained in the same manner as in the production of core particles 1, except that polyester resin 2 was added instead of polyester resin 1.

[0104] <Production of Core Particle 3> Core particles 3 having a weight average particle size (D4) of 6 μm were obtained in the same manner as in the production of core particles 1, except that polyester resin 3 was added instead of polyester resin 1.

[0105] <Production of Core Particle 4> Core particles 4 having a weight average particle size (D4) of 6 μm were obtained in the same manner as in the production of core particles 1, except that polyester resin 1 was replaced with styrene-acrylic resin 1.

[0106] <Production of Core Particle 5> A dispersion of core particles 5 was prepared by an emulsion polymerization flocculation method. (Preparation of Polyester Particle Dispersion) Polyester resin 1 200.0 parts -Ion-exchanged water 500.0 parts The above materials were placed in a stainless steel container, heated to 95°C in a hot bath, melted, and thoroughly stirred at 7800 rpm using a homogenizer (IKA Ultra Turrax T50) while adding 0.1 mol / L sodium bicarbonate to make the pH greater than 7.0. Then, a mixed solution of 3.0 parts of sodium dodecylbenzenesulfonate and 297.0 parts of ion-exchanged water was gradually added dropwise to emulsify and disperse the mixture, thereby obtaining a polyester particle dispersion. The particle size distribution of this polyester particle dispersion was measured using a particle size measuring device (LA-920, manufactured by Horiba, Ltd.), and the number average particle size of the polyester particle dispersion was found to be 0.25 μm, and no coarse particles exceeding 1 μm were observed.

[0107] (Preparation of Wax Particle Dispersion) -Ion-exchanged water 500.0 parts Fischer-Tropsch wax (Sasol C105, melting point: 80°C) 250.0 copies The above materials were placed in a stainless steel container, heated to 95°C in a hot bath, and melted. While thoroughly stirring at 7800 rpm using a homogenizer (IKA Ultra Turrax T50), 0.1N sodium bicarbonate was added to make the pH greater than 7.0. A mixed solution of 5.0 parts by mass of sodium dodecylbenzenesulfonate and 245.0 parts by mass of ion-exchanged water was then gradually added dropwise to emulsify and disperse. The particle size distribution of the wax particles contained in this wax particle dispersion was measured using a particle size measuring device (HORIBA, LA-920), and the number-average particle size of the wax particles contained was 0.35 μm, and no coarse particles exceeding 1 μm were observed.

[0108] (Preparation of Colorant Particle Dispersion) CI Pigment Blue 15:3 100.0 parts Sodium dodecylbenzenesulfonate 5.0 parts Ion-exchanged water 400.0 parts The above was mixed and dispersed using a sand grinder mill. The particle size distribution of the colorant particles contained in this colorant particle dispersion was measured using a particle size measuring device (LA-920, manufactured by Horiba, Ltd.), and the number-average particle size of the colorant particles contained was 0.2 μm, and no coarse particles exceeding 1 μm were observed.

[0109] (Production of Core Particle Dispersion) Polyester particle dispersion 500.0 parts Colorant particle dispersion 50.0 parts Wax particle dispersion 50.0 parts Sodium dodecylbenzenesulfonate 5.0 parts A reactor (1-liter flask, anchor blade with baffles) was charged with polyester resin particle dispersion 1, wax particle dispersion, and sodium dodecylbenzenesulfonate, and mixed uniformly. Meanwhile, a colorant particle dispersion was mixed uniformly in a 500 mL beaker, and this was gradually added to the reactor while stirring to obtain a mixed dispersion. 0.5 parts of aluminum sulfate aqueous solution (solid content) was added dropwise while stirring the obtained mixed dispersion to form aggregated particles. After the dropwise addition was completed, the system was purged with nitrogen and the temperature was maintained at 50° C. for 1 hour and then at 55° C. for 1 hour. The temperature was then raised to 90°C and held for 30 minutes. The temperature was then lowered to 63°C and held for 3 hours to form fused particles. After the specified time had elapsed, the temperature was lowered to 40°C at a rate of 0.5°C per minute to obtain a dispersion of core particles 5 having a weight average particle size (D4) of 6 µm.

[0110] <Production of Core Particle 6> A dispersion of core particles 6 was prepared by a dissolution suspension method. Polyester resin 1 100.0 parts CI Pigment Blue 15:3 (copper phthalocyanine) 5.0 parts Ester wax (behenyl behenate: melting point 72°C) 15.0 parts Methyl ethyl ketone 100.0 parts Ethyl acetate 100.0 parts The above materials were dispersed for 3 hours using an Attritor (manufactured by Mitsui Kinzoku Co., Ltd.) to obtain a colorant dispersion. Ta. On the other hand, 1.8 parts of tricalcium phosphate was added to 300.0 parts of ion-exchanged water heated to 60°C. The above-mentioned colorant dispersion was added to the above-mentioned aqueous medium, and the mixture was stirred at a stirring speed of 12,000 rpm for 15 minutes at 65°C under a N2 atmosphere using the TK homomixer to granulate colorant particles. Thereafter, the TK homomixer was changed to a conventional propeller stirrer, the stirring speed of the stirrer was maintained at 150 rpm, the internal temperature was raised to 95°C and maintained for 3 hours to remove the solvent from the dispersion, and a dispersion of core particles 6 having a weight average particle size (D4) of 6 μm was prepared.

[0111] <Production of Core Particle 7> Core particles 7 having a weight average particle size (D4) of 6 μm were obtained in the same manner as in the production of core particles 1, except that 0.7 parts of charge control agent BONTRON P-51 (manufactured by Orient Chemical Industries Co., Ltd.) was added in addition to the wax and colorant added.

[0112] <Preparation of Shell Resin Particles 1> A glass vessel equipped with a stirrer, reflux condenser, thermometer, and nitrogen inlet tube was placed in a water bath, and 500 parts of ion-exchanged water and 100 parts of anionic surfactant Neogen were added to the flask. 28.3 parts of RK (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) was added to the flask. Then, the temperature inside the flask was raised to 80° C. Then, two types of liquids (a first liquid and a second liquid) were each added dropwise to the flask content at 80° C. over a period of three hours. The first liquid was a mixture of 84 parts of styrene and 16 parts of butyl acrylate. The second liquid was a solution in which 1 part of potassium persulfate was dissolved in 50 parts of ion-exchanged water. The temperature inside the flask was then maintained at 80°C for an additional 2 hours to polymerize the contents of the flask. As a result, a dispersion containing shell resin particles 1 was obtained. The obtained shell resin particles 1 had a number average particle size of 50 nm and a Tg of 70°C.

[0113] <Preparation of Shell Resin Particles 2> In the preparation of shell resin particles 1, the amount of anionic surfactant NEOGEN RK (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) added was changed to 16.7 parts, and the monomer composition added as the first liquid was changed to 73.5 parts of styrene, 24.5 parts of butyl acrylate, and 2 parts of acrylic acid, and the same procedure was repeated to obtain a dispersion containing shell resin particles 2. The obtained shell resin particles 2 had a number average particle size of primary particles of 72 nm and a Tg of 61°C.

[0114] <Preparation of Shell Resin Particles 3 and 4> Dispersions containing shell resin particles 3 and 4 were obtained in the same manner as in preparing shell resin particles 1, except that the amount of anionic surfactant NEOGEN RK (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) added and the monomer composition were changed to the amounts shown in Table 3. The physical properties of the obtained shell resin particles 3 and 4 are shown in Table 3.

[0115] <Preparation of Shell Resin Particles 5> 1,200 parts polyester resin -500 parts deionized water The above materials were placed in a stainless steel container, heated to 95°C in a hot bath, and melted, and then 0.1 mol / L sodium bicarbonate was added while thoroughly stirring at 7800 rpm using a homogenizer (IKA: Ultra Turrax T50) to make the pH greater than 7.0. After that, a mixed solution of 3 parts of sodium dodecylbenzenesulfonate and 297 parts of ion-exchanged water was gradually added dropwise to emulsify and disperse the mixture, thereby obtaining a polyester resin particle dispersion. The particle size distribution of this polyester resin particle dispersion was measured using a particle size measuring device (LA-920, manufactured by Horiba, Ltd.). The number average particle size of the polyester resin particles was 24. 0 nm, and no coarse particles exceeding 1 μm were observed.

[0116] <Preparation of Shell Resin Particles 6> Shell resin microparticle dispersion 6 was obtained in the same manner as in preparation of shell resin particles 5, except that the polyester resin 1 was changed to styrene acrylic modified polyester resin 1. The number average particle size of the obtained styrene acrylic modified polyester resin particles was 250 nm, and no coarse particles exceeding 1 μm were observed.

[0117] [Table 3] The abbreviations in the table are as follows: St: styrene BA: n-butyl acrylate MA: Methyl acrylate AA: Acrylic acid 2-HEMA: 2-hydroxyethyl methacrylate

[0118] <Production of Toner 1> (Formation of core-shell particles) A three-neck flask equipped with a thermometer and a stirring blade was prepared, and the flask was set in a water bath. Then, 100 parts of ion-exchanged water was placed in the flask, and the temperature in the flask was kept at 30° C. using the water bath. Then, 10% by mass of hydrochloric acid was added to the flask, and the pH of the flask content was adjusted to 4. Next, the dispersion liquid containing the shell resin particles 1 prepared above was added to the flask in an amount such that the solid content was 1.00 parts. Next, 100 parts of the core particles 1 prepared by the above procedure were added to the flask, and the contents of the flask were thoroughly stirred. As a result, a dispersion liquid of the core particles 1 and the shell resin particles 1 was obtained in the flask. 100 parts of ion-exchanged water was added to the flask, and the content of the flask was heated to 50° C. at a rate of 1.0° C. / min while stirring at a rotation speed of 100 rpm. When the temperature inside the flask reached 50°C, add the anionic surfactant NEOGEN RK ( To the mixture was added 0.5 parts of ethyl acetate (manufactured by Ichi Kogyo Seiyaku Co., Ltd.), and the pH was adjusted to 7 by adding sodium hydrogen carbonate. Furthermore, the temperature of the flask content was increased at a rate of 1.0° C. / min to 85° C. while stirring the flask content at a rotation speed of 100 rpm, and the temperature was maintained at 85° C. for 2 hours. Thereafter, the flask content was cooled to room temperature, and a dispersion liquid containing toner particles 1 was obtained. The dispersion liquid containing the obtained toner particles 1 is filtered (solid-liquid separation), and the toner particles are mixed with ion-exchanged water. The mixture was washed by repeatedly redispersing and filtering, and then dried using a flash jet dryer to obtain toner particles 1. Toner particle 1 had a core-shell structure in which a part of the core particle was exposed, and the surface of the toner particle consisted of a surface formed of a polyester resin and a surface formed of a styrene-acrylic resin. The total area ratio of the surfaces formed of styrene-acrylic resin and polyester resin to the total area of ​​the toner particle surface of toner particle 1 was 100 (area %), and the total area ratio of the surfaces formed of styrene-acrylic resin to the total area of ​​the surfaces formed of styrene-acrylic resin and polyester resin was 60 (area %).

[0119] (External addition process) The obtained toner particles 1:100.0 parts and silica particles 1:1.0 parts were mixed in a Henschel mixer (FM-10 type manufactured by Mitsui Miike Chemical Engineering Co., Ltd.) to obtain toner 1 exhibiting negative charging properties. The physical properties are shown in Table 4.

[0120] <Production of Toner 2> Toner 2 exhibiting negative charging properties was produced in the same manner as in the production of toner 1, except that the amount of dispersion containing shell resin particles 1 added was changed to an amount that resulted in a solid content of 0.75 parts, and the silica particles 1 added in the (external addition step) were changed to silica particles 2. The St-Ac+PES area ratio of toner particles 2 was 100 (area%), and the St-Ac area ratio was 50 (area%). The physical properties are shown in Table 4.

[0121] <Production of toners 3-17, 20-25> Toners 3 to 17 and toners 20 to 25 were produced in the same manner as in the production of toner 1, except that the types and amounts of core particles and shell resin particles to be added, and the silica particles to be added in the external addition step were changed to those shown in Table 4. The physical properties are shown in Table 4. The dispersions of the core particles 5 and 6 added in the production of the toners 15 and 16 were added in amounts such that the solid content was 100 parts.

[0122] <Production of Toner 18> Toner 18 exhibiting positive charging properties was produced in the same manner as in the production of toner 1, except that 0.084 parts of a methylolmelamine aqueous solution (Milben Resin SM-607, manufactured by Showa Denko K.K.) was further added when the dispersion liquid containing shell resin particles 1 was added. The area ratio of St-Ac+PES in toner particle 18 was 90 (area %), and the area ratio of St-Ac was 60 (area %).

[0123] <Production of Toner 19> Toner 19 exhibiting positive charging properties was prepared in the same manner as Toner 18, except that the amount of methylolmelamine aqueous solution (Milben Resin SM-607, manufactured by Showa Denko KK) added was changed to 0.140 parts. The area ratio of St-Ac+PES of toner particle 19 was 88 (area %), and the area ratio of St-Ac was 60 (area %).

[0124] [Table 4]

[0125] In the table, PES stands for polyester resin, St-Ac stands for styrene-acrylic resin, and St-Ac-modified PES stands for styrene-acrylic-modified polyester resin. St-Ac+PES area ratio: The ratio of the total area of ​​the surfaces formed of styrene-acrylic resin and polyester resin to the total area of ​​the toner particle surface St-Ac area ratio: The ratio of the area of ​​the surface formed of styrene-acrylic resin to the total area of ​​the surfaces formed of styrene-acrylic resin and polyester resin on the surface of a toner particle

[0126] <Image evaluation> A Hewlett-Packard color laser beam printer (HP LaserJet Enterprise Color M652n) was used as the image forming device, and was modified so that the process speed was 300 mm / sec. An HP 656X genuine LaserJet toner cartridge (cyan) was used as the cartridge. The product toner was removed from the inside of the cartridge, and after cleaning with an air blower, 300 g of the toner to be evaluated was filled. The refilled toner cartridge was installed in the cyan station, and dummy cartridges were installed in the other stations, and the following image output test was carried out. In addition, the evaluation of the positive toners (toners 17 to 19, 24, and 25) was carried out in such a way that development with positively charged toners was possible. The seed potential setting was changed and the evaluation was performed in the same manner.

[0127] <Measurement of toner charge amount> In order to confirm the relationship between the results of the image output test and the toner charge amount, the toner was taken out from the developing container before and after each of the durability tests described below, and the toner charge amount was measured by the following method. 9.4 g of charge measurement carrier (F81-2535, Powdertech Co., Ltd.) is weighed into a 50 mL polyethylene container. Next, 0.6 g of the toner to be measured is weighed into the polyethylene container containing the carrier, and the cap is closed. Next, the container is placed on a shaker (Model-YS-LD: Yayoi Co., Ltd.) and shaken at 150 times / min for 2 minutes. Within one minute thereafter, about 0.4 g of the shaken sample is placed in a metal measurement container 2 with a 500 mesh screen 3 at the bottom, as shown in Figure 1, and the metal lid 4 is placed on the container. The mass of the entire measurement container 2 at this time is measured and this value is designated as W1 (g). Next, the potential of the electrometer 9 at this time is set to 0 V (volts). Next, the suction device 1 (at least the part in contact with the measurement container 2 is an insulator) sucks from the suction port 7, and the air flow control valve 6 is adjusted to make the pressure on the vacuum gauge 5 2.5 kPa (±0.1 kPa) within 10 seconds. Note that the time from measuring W1 to starting suction should be within 30 seconds. Suction is then continued for 3 minutes to remove the toner particles by suction. The potential on the electrometer 9 at this time is V (volts). Here, 8 is a capacitor with a capacity of C (μF). Next, the mass of the entire measurement container after suction is weighed, and this value is taken as W2 (g). The toner charge amount (mC / kg) of this sample is calculated using the following formula. Charge amount (mC / kg) = C × V / (W1-W2) The charge amount was measured using measurement samples that were taken from the toner in the developing container before and after durability tests in a low temperature and low humidity environment (temperature 15°C, humidity 10% RH: LL environment), a high temperature and high humidity environment (temperature 30°C / humidity 80% RH: HH environment), and a normal temperature and normal humidity environment (temperature 23°C, humidity 50% RH: NN environment), which will be described later. The evaluation of the positively charged toner was carried out in the same manner, except that the carrier for measuring the charge amount was changed from (F81-2535 manufactured by Powder Tech Co., Ltd.) to (F-150 manufactured by Powder Tech Co., Ltd.).

[0128] [Halftone image reproducibility] In a low temperature and low humidity environment (temperature 15°C, humidity 10% RH), a printout test of 30,000 sheets in total was conducted by repeating intermittent operation in which the printer was temporarily stopped every time two images with a print rate of 1% were printed. After the printout test was completed, the original halftone images of 30h, 80h and C0h were output, and each image was visually observed and the dot reproducibility was evaluated according to the following criteria. In addition, 30h in a halftone image is the hexadecimal value of 256 tones, with 00h being the 1st tone (white background) of 256 tones, and FFh being the 256th tone (solid area) of 256 tones, indicating an image that has been controlled. A: All halftone image dots are reproduced with high precision, resulting in a uniform image quality with no unevenness. B: Slight dot irregularities are observed in some halftone images, but the density unevenness is not noticeable. C: Dot irregularities were observed in some halftone images, and density unevenness was observed, but the unevenness was not noticeable in practical images. D: The dot reproducibility is poor in all halftone images, resulting in roughness and unevenness.

[0129] [Fog Evaluation] In a high temperature and humidity environment (temperature 30°C / humidity 80% RH), the print rate is 1%. A total of 30,000 printout tests were conducted by repeating intermittent operation in which the printer stopped after printing two sheets. After the printout test, a solid white image was output and the reflectance (%) of the solid white image was measured using a REFLECTOMETER MODEL TC-6DS (Tokyo Denshoku Co., Ltd.). The reflectance obtained was subtracted from the reflectance (%) of an unused printout paper (standard gloss paper) measured in the same manner, and the result was used for evaluation. The smaller the value, the more suppressed the image fog is. The solid white image was output in gloss paper mode on gloss paper (HP Brochure Paper 200g, Glossy, manufactured by HP, 200g / m 2 ) was used. (Evaluation Criteria) A: The deduction is less than 0.5% B: The deduction is between 0.5% and 1.5% C: The deduction is between 1.5% and 3.0%. D: The subtracted value is 3.0% or more.

[0130] [Image Density and Image Density Stability] In a normal temperature and humidity environment (temperature 23°C, humidity 50% RH), 5,000 images with a print rate of 1% were output in succession, and then 5,000 images with a high print rate of 25% were output in succession, for a total printout test of 10,000 sheets. At the beginning and end of the printout test, a sample image with a 20 mm square solid black image printed in the four corners and center of the paper was printed on GF-C081 (Canon Marketing Japan, 81.4 g / m 2 ) and output to the X-Rite 500 series (video The reflection density was measured using an Ojet X-Rite FT-IR 1000 (Ojet X-Rite Co., Ltd.) and the average image density of five points was calculated. The evaluation criteria for image density are as follows. A: Both the initial image density and the image density after durability test are less than 1.40±0.10 B: Both the initial image density and the image density after durability test are 1.40±0.10 or more and less than 0.15 C: Both the initial image density and the image density after durability test are 1.40±0.15 or more and less than 0.20 D: Both the initial image density and the image density after durability test are 1.40±0.20 or more The evaluation criteria for image density stability are as follows. A: The absolute difference between the initial image density and the image density after durability is less than 0.10 B: The absolute difference between the initial image density and the image density after durability is 0.10 or more and less than 0.15 C: The absolute difference between the initial image density and the image density after durability is 0.15 or more and less than 0.20 D: The absolute difference between the initial image density and the image density after durability is 0.20 or more

[0131] In Examples 1 to 19, the above evaluations were carried out using Toners 1 to 19, respectively. The evaluation results are shown in Table 5. Incidentally, Examples 10 and 12 were subjected to the above evaluation as reference examples.

[0132] [Comparative Examples 1 to 6] In Comparative Examples 1 to 6, the above evaluation was carried out using toners 20 to 25, respectively. The evaluation results are shown in Table 5.

[0133] [Table 5]

Claims

1. 1. A toner having toner particles and silica particles on a surface of the toner particles, the toner particles have a surface formed of a polyester resin and a surface formed of a styrene-acrylic resin; the toner particles are toner particles having a core-shell structure having a core particle and a shell formed on a surface of the core particle, the core particles comprise a polyester resin; the shell comprises a styrene-acrylic resin; a surface of the toner particle formed of the polyester resin is present on the surface of the toner particle by a part of the polyester resin contained in the core particle being exposed on the surface of the toner particle, The number average particle size of the silica particles is 15 nm or more and 60 nm or less, The average pore diameter of the silica particles is 5.0 nm or more and 20.0 nm or less, The total pore volume of the silica particles is 0.20 cm 3 / g or more 1.50cm 3 / g or less.

2. a ratio of a total area of ​​the surface of the toner particle formed of the styrene-acrylic resin and the surface of the polyester resin to a total area of ​​the surface of the toner particle is 90 area % or more; 2. The toner according to claim 1, wherein a ratio of an area of ​​the surface formed of the styrene-acrylic resin to a total area of ​​the surface formed of the styrene-acrylic resin and the surface formed of the polyester resin is 40 area % or more and 80 area % or less.

3. 3. The toner according to claim 1, wherein the silica particles have a number average particle size of 15 nm or more and 40 nm or less.

4. 4. The toner according to claim 1, wherein the silica particles are wet silica.

5. 5. The toner according to claim 1, wherein the silica particles have a hydrophobicity of 40% or more and 75% or less.

Citation Information

Patent Citations

  • Toner

    JP2008224939A

  • Toner

    JP2012150172A

  • Image forming method

    JP2013003367A

  • Toner for electrostatic charge image development, electrostatic charge image developer, toner cartridge, developer cartridge, process cartridge, image forming method, and image forming apparatus

    JP2016080886A

  • Toner for electrostatic charge image development

    JP2017156542A