Toner and its manufacturing method
By controlling the volume and dispersed particle diameters of charge control agents in toner particles, the issue of image defects is resolved, ensuring stable charging and clear image quality.
Patent Information
- Application Number
- JP2020153596
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-14
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-09-14
AI Technical Summary
Toner particles with poorly dispersed internal additives, particularly charge control agents, lead to image defects such as scattering and fogging due to uneven charge distribution and exposure issues.
Control the volume average particle diameter of toner particles and the number average dispersed particle diameter of charge control agents within specific ratios (Dc/Dt between 0.1 and 0.2, and Dc90/Dc10 less than 3.0) to ensure uniform dispersion and effective charge control.
Suppresses image defects like toner scattering and fogging, enabling stable charging and high-definition image formation by maintaining optimal charge control agent distribution.
Smart Images

Figure 0007553294000005 
Figure 0007553294000006 
Figure 0007553294000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a toner and a method for producing the toner. [Background technology]
[0002] Toners (toners for developing electrostatic images) used in image forming devices utilizing electrophotography, such as copying machines, multifunction machines, printers, and facsimile machines, usually contain binder resins, release agents, colorants, charge control agents, and the like in the toner particles, and these components are collectively called internal additives.
[0003] In small particle toners, if the dispersion state of the internal additives is poor, compositional deviations are likely to occur between each toner particle. If the dispersion state of the charge control agent among the internal additives is poor, the toner charge distribution becomes broad, causing problems such as scattering of toner particles and image defects such as fogging. On the other hand, if the charge control agent becomes over-dispersed, the charge control agent is no longer exposed to the toner particle surface, significantly reducing its function as a charge control agent, and the leak effect cannot be expected.
[0004] Patent Document 1 discloses that in a toner for a non-magnetic one-component development method, a specific charge control agent is used in the toner for the purpose of stabilizing the charging and transport of the toner over a long period of time, and that the dispersion state of the charge control agent is such that a specific relationship is established between the volume average particle size of the toner particles and the average dispersion diameter of the charge control agent used. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 10-20560 Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made in light of the above circumstances, and an object of the present invention is to provide a toner and a method for producing the toner that can suppress the occurrence of image defects such as toner particle scattering and fogging. [Means for solving the problem]
[0007] As a result of intensive research by the present inventors in order to solve the above-mentioned problems, they have found that in a toner having toner particles containing a binder resin, a colorant, and a charge control agent, the above-mentioned problems can be solved by controlling the volume average particle size of the toner particles, the number average dispersed particle size of the charge control agent, and the particle size distribution of the charge control agent as follows, and have completed the present invention.
[0008] That is, the toner according to the present invention is a toner having toner particles containing a binder resin, a colorant, and a charge control agent, and is characterized in that, when the volume average particle diameter of the toner particles is Dt and the number average dispersed particle diameter of the charge control agent is Dc, Dc / Dt is 0.1 or more and 0.2 or less, and when, in the particle size distribution of the charge control agent, the particle diameter of the particles whose cumulative number % from the small particle diameter side is 90% is Dc90, and the particle diameter of the particles whose cumulative number % from the small particle diameter side is 10% is Dc10, Dc90 / Dc10 is 3.0 or less.
[0009] Further, a method for producing a toner according to the present invention is a method for producing the toner, comprising a mixing step of mixing raw materials including a binder resin, a colorant, and a charge control agent, a melting and kneading step of melting and kneading the mixture obtained in the mixing step, a cooling and grinding step of cooling and solidifying the kneaded product obtained in the melting and kneading step and then grinding it, and a classification step of classifying the grinded product into first grinded particles, second grinded particles having a volume average particle size smaller than the first grinded particles, and third grinded particles having a volume average particle size larger than the first grinded particles, and recovering the first grinded particles as toner particles, wherein the segregation rate of the charge control agent defined by A / B×100 is 102% or more and 130% or less, where A is the amount of the charge control agent contained in the second grinded particles and B is the amount of the charge control agent contained in the first grinded particles. Effect of the Invention
[0010] According to the present invention, it is possible to suppress the occurrence of image defects such as scattering of toner particles and fogging. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a process diagram illustrating a first embodiment of a toner production method of the present invention. [Diagram 2] 3A to 3C are process diagrams illustrating a second embodiment of the toner production method of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The toner and the method for producing the toner according to the embodiment of the present invention will be described in detail below.
[0013] <Toner / toner particles> The toner of the present invention has toner particles containing at least a binder resin, a colorant, and a charge control agent, and may further contain optional components as necessary within the range not impairing the effects of the present invention.
[0014] In the toner of the present invention, when the volume average particle diameter of the toner particles is Dt and the number average dispersed particle diameter of the charge control agent is Dc, Dc / Dt is 0.1 or more and 0.2 or less, and when the particle diameter of the particles whose cumulative number % from the small particle diameter side is 90% in the particle size distribution of the charge control agent is Dc90, and the particle diameter of the particles whose cumulative number % from the small particle diameter side is 10% is Dc10, Dc90 / Dc10 is 3.0 or less.
[0015] If Dc / Dt is less than 0.1, the toner may be charged up, whereas if Dc / Dt is more than 0.2, the effect of the charge control agent may be reduced, resulting in fogging.
[0016] If Dc90 / Dc10 exceeds 3.0, the effect of the charge control agent is reduced and fogging may occur. Also, Dc90 / Dc10 is preferably 1.0 or more. If Dc90 / Dc10 is less than 1.0, the ratio of fine powder and coarse powder increases, and productivity may deteriorate.
[0017] When Dc / Dt and Dc90 / Dc10 satisfy the above conditions, the toner has the number average dispersed particle size of the charge control agent and the particle size distribution of the charge control agent controlled according to the volume average particle size of the toner particles, which makes it possible to suppress the scattering of toner particles and the occurrence of image defects such as fogging.
[0018] The volume average particle size of the toner particles is not particularly limited, but is preferably 3 μm or more and 15 μm or less, more preferably 4 μm or more and 9 μm or less, and even more preferably 5 μm or more and 8 μm or less. The toner particles having such a small particle size have an appropriate charge amount and can ensure sufficient fluidity. Therefore, the toner particles can be stably supplied to the photoconductor, and a clear and high-definition image can be formed, and the occurrence of contamination inside the machine due to the scattering of toner particles can be prevented.
[0019] <Binding resin> Examples of the binder resin include polyester-based resins, polystyrene-based resins such as styrene-acrylic-based resins, (meth)acrylic acid ester-based resins, polyolefin-based resins, polyurethane-based resins, and epoxy-based resins. One of these may be used alone, or two or more may be used in combination.
[0020] The polyester resin used for the binder resin is usually obtained by polycondensation reaction of one or more selected from a dihydric alcohol component and a trihydric or higher polyhydric alcohol component with one or more selected from a divalent carboxylic acid and a trivalent or higher polycarboxylic acid by a known method via an esterification reaction or an ester exchange reaction.
[0021] The conditions for the polycondensation reaction may be appropriately set depending on the reactivity of the monomer components, and the reaction may be terminated when the polymer has suitable physical properties. For example, the reaction temperature is about 170 to 250° C., and the reaction pressure is about 5 mmHg to normal pressure.
[0022] Examples of the dihydric alcohol component include alkylene oxide adducts of bisphenol A such as polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene(3.3)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene(2.0)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene(2.0)-polyoxyethylene(2.0)-2,2-bis(4-hydroxyphenyl)propane, and polyoxypropylene(6)-2,2-bis(4-hydroxyphenyl)propane; Examples of the diols include glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, neopentyl glycol, 1,4-butenediol, 1,5-pentanediol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, dipropylene glycol, polyethylene glycol, polypropylene glycol, and polytetramethylene glycol; bisphenol A; propylene adducts of bisphenol A; ethylene adducts of bisphenol A; and hydrogenated bisphenol A.
[0023] Examples of trihydric or higher polyhydric alcohol components include sorbitol, 1,2,3,6-hexanetetrol, 1,4-sorbitan, pentaerythritol, dipentaerythritol, tripentaerythritol, sucrose (cane sugar), 1,2,4-butanetriol, 1,2,5-pentanetriol, glycerol, 2-methylpropanetriol, 2-methyl-1,2,4-butanetriol, trimethylolethane, trimethylolpropane, and 1,3,5-trihydroxymethylbenzene.
[0024] In the present invention, the above dihydric alcohol components and trihydric or higher polyhydric alcohol components may be used alone or in combination of two or more.
[0025] Examples of divalent carboxylic acids include maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, phthalic acid, isophthalic acid, terephthalic acid, cyclohexanedicarboxylic acid, succinic acid, adipic acid, sebacic acid, azelaic acid, malonic acid, n-dodecenylsuccinic acid, n-dodecylsuccinic acid, n-octylsuccinic acid, isooctenylsuccinic acid, isooctylsuccinic acid, and acid anhydrides and lower alkyl esters thereof.
[0026] Examples of trivalent or higher polyvalent carboxylic acids include 1,2,4-benzenetricarboxylic acid, 1,2,5-benzenetricarboxylic acid, 2,5,7-naphthalenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, 1,2,4-butanetricarboxylic acid, 1,2,5-hexanetricarboxylic acid, 1,3-dicarboxyl-2-methyl-2-methylenecarboxypropane, 1,2,4-cyclohexanetricarboxylic acid, tetra(methylenecarboxyl)methane, 1,2,7,8-octanetetracarboxylic acid, pyromellitic acid, empol trimer acid, and acid anhydrides and lower alkyl esters thereof.
[0027] In the present invention, among the above divalent carboxylic acids and trivalent or higher polyvalent carboxylic acids, one kind may be used alone, or two or more kinds may be used in combination.
[0028] The polyester resin preferably has a weight average molecular weight of 3000 to 50000. If the weight average molecular weight of the polyester resin is less than 3000, the peelability on the high temperature side of the fixable region (non-offset region) may be poor. On the other hand, if the weight average molecular weight of the polyester resin is more than 50000, the low temperature fixability may be poor.
[0029] The polyester resin preferably has an acid value of 5 to 30 mgKOH / g. If the acid value of the polyester resin is less than 5 mgKOH / g, the electrostatic charge characteristics of the polyester resin may be reduced, and the charge control agent may be difficult to disperse in the polyester resin, which may adversely affect the electrostatic charge rise property and the electrostatic charge stability during continuous use. On the other hand, if the acid value of the polyester resin is more than 30 mgKOH / g, the electrostatic charge may become unstable due to high hygroscopicity.
[0030] <Charge control agent> As the charge control agent, a charge control agent for controlling a positive charge or a negative charge can be used.
[0031] Examples of charge control agents for controlling positive charges include nigrosine dyes and their derivatives, basic dyes, quaternary ammonium salts, quaternary phosphonium salts, aminopyrine, pyrimidine compounds, polynuclear polyamino compounds, aminosilanes, triphenylmethane derivatives, guanidine salts, and amidine salts.
[0032] On the other hand, examples of charge control agents for negative charging include oil-soluble dyes such as oil black and spiron black, metal-containing azo compounds, azo complex dyes, metal naphthenates, metal complexes and metal salts of salicylic acid and its derivatives (metals include chromium, zinc, zirconium, etc.), boron compounds, fatty acid soaps, long-chain alkyl carboxylates, and resin acid soaps.
[0033] The content of the charge control agent in the toner of the present invention is not particularly limited, but is preferably 0.1 to 3 parts by weight, and particularly preferably 0.2 to 2 parts by weight, per 100 parts by weight of the binder resin.
[0034] The adhesion strength of the charge control agent in the toner according to the present invention is preferably 30% to 80%, more preferably 35% to 75%, and even more preferably 50% to 65%. If the adhesion strength of the charge control agent is less than the lower limit, the effect of the charge control agent is reduced, which may cause charge-up. On the other hand, if the adhesion strength of the charge control agent exceeds the upper limit, fogging may worsen.
[0035] The adhesion strength of the charge control agent in the toner can be measured by determining the residual rate of the charge control agent when the toner is subjected to vibration. Specifically, it can be measured by a method that executes a step of quantitatively analyzing elements originating from the charge control agent present on the toner particles by fluorescent X-ray analysis or the like, a step of applying ultrasonic waves to the toner in water, and a step of quantitatively analyzing elements originating from the charge control agent on the toner particles after the ultrasonic waves are applied and calculating the residual rate of the charge control agent.
[0036] <Release agent> Examples of the release agent include petroleum waxes such as paraffin wax and its derivatives, microcrystalline wax and its derivatives; hydrocarbon synthetic waxes such as Fischer-Tropsch wax and its derivatives, polyolefin wax and its derivatives, polypropylene wax and its derivatives, polyolefin polymer wax (low molecular weight polyethylene wax, etc.) and its derivatives; vegetable waxes such as carnauba wax and its derivatives, rice wax and its derivatives, candelilla wax and its derivatives, and Japan wax; animal waxes such as beeswax and spermaceti; oil-based synthetic waxes such as fatty acid amides, phenol fatty acid esters and their derivatives; silicone polymers, higher fatty acids, etc. One of these may be used alone, or two or more may be used in combination. The derivatives include oxides, block copolymers of vinyl monomers and wax, and graft modified products of vinyl monomers and wax. The content of the release agent is not particularly limited, but it is more preferably 0.5 to 10 parts by weight relative to 100 parts by weight of the binder resin.
[0037] <Coloring agent> Examples of the coloring agent include black, yellow, magenta, and cyan pigments and dyes. Note that the color of the toner is not limited to these, and the toner may be colored in other colors, and a coloring agent corresponding to the color may be used.
[0038] Examples of black colorants include inorganic pigments such as carbon black and composite oxide black; and organic pigments such as aniline black.
[0039] Carbon black is classified into channel black, roller black, disc black, gas furnace black, oil furnace black, thermal black, acetylene black, etc., depending on the production method, etc., and an appropriate carbon black can be appropriately selected from these depending on the design characteristics of the toner to be obtained.
[0040] Examples of yellow colorants include organic pigments such as CI Pigment Yellow 1, CI Pigment Yellow 5, CI Pigment Yellow 12, CI Pigment Yellow 15, CI Pigment Yellow 17, CI Pigment Yellow 74, CI Pigment Yellow 93, CI Pigment Yellow 180, and CI Pigment Yellow 185, which are classified by the Color Index; nitro dyes such as CI Acid Yellow 1; and oil-soluble dyes such as CI Solvent Yellow 2, CI Solvent Yellow 6, CI Solvent Yellow 14, CI Solvent Yellow 15, CI Solvent Yellow 19, and CI Solvent Yellow 21.
[0041] Examples of magenta colorants include organic pigments such as CI Pigment Red 49, CI Pigment Red 57, CI Pigment Red 81, CI Pigment Red 122, CI Solvent Red 19, CI Solvent Red 49, CI Solvent Red 52, CI Basic Red 10, and CI Disperse Red 15, which are classified by the Color Index.
[0042] Examples of cyan colorants include organic pigments such as CI Pigment Blue 15, CI Pigment Blue 16, CI Solvent Blue 55, CI Solvent Blue 70, CI Direct Blue 25, CI Direct Blue 86, and KET.BLUE 111, which are classified by the Color Index.
[0043] <Other optional ingredients> Other optional components include, for example, magnetic materials such as magnetite powder, γ-hematite powder, and various ferrite powders, and among these, one type may be used alone or two or more types may be used in combination.
[0044] <Toner manufacturing method> [First embodiment] Fig. 1 is a process diagram showing a first embodiment of the toner production method of the present invention. The toner production method shown in Fig. 1 is a particle production method by a dry method, and includes a mixing step S1, a melt-kneading step S2, a cooling and pulverizing step S3, a classification step S4, and an external addition step S5.
[0045] (Mixing process S1) In the mixing step S1, a resin material (binder resin), a release agent, a charge control agent, a colorant, and a magnetic material are dry-mixed in a mixer to prepare a mixture. At this time, all of these raw materials may be mixed at once, but it is preferable to mix the raw materials other than the charge control agent and the colorant, mix the charge control agent, and then mix the colorant. By using the latter method, it becomes easier to adjust the particle size of the charge control agent in the kneaded product obtained in the melt-kneading step S2.
[0046] In particular, when a colorant and a magnetic material are added to the mixture, it is preferable to do the following.
[0047] First, a master batch containing a resin material and a colorant is prepared. This allows the colorant to be uniformly dispersed in the resin material (and thus the kneaded product). The master batch can be prepared, for example, by dry-mixing the resin material and the colorant in a mixer, melt-kneading the mixture in a kneader to obtain a kneaded product, and then pulverizing (coarsely pulverizing) the kneaded product in a pulverizer.
[0048] The mixing time is preferably about 60 to 180 seconds, more preferably about 90 to 150 seconds. The kneading temperature depends on the softening temperature of the resin material, but is preferably about 50 to 180°C, more preferably about 90 to 150°C.
[0049] Examples of mixers include Henschel type mixers such as Henschel Mixer (product name, manufactured by Mitsui Mining Co., Ltd.), Super Mixer (product name, manufactured by Kawata Corporation), and Mechano Mill (product name, manufactured by Okada Seiko Co., Ltd.), Ang Mill (product name, manufactured by Hosokawa Micron Corporation), Hybridization System (product name, manufactured by Nara Machinery Works, Ltd.), and Cosmo System (product name, manufactured by Kawasaki Heavy Industries, Ltd.).
[0050] Examples of the kneading machine include a kneader, a twin-screw extruder, a two-roll mill, a three-roll mill, a lab blast mill, etc. Specific examples of the kneading machine include single-screw or twin-screw extruders such as TEM-100B (trade name, manufactured by Toshiba Machine Co., Ltd.), PCM-65 / 87, and PCM-30 (all trade names, manufactured by Ikegai Corporation), and open-roll type kneading machines such as Kneadex (trade name, manufactured by Mitsui Mining Co., Ltd.).
[0051] Examples of the pulverizer include a hammer mill, a cutting mill, a speed mill, etc. The average particle size (for example, volume average particle size) of the master batch is usually about 1 to 5 mm.
[0052] Next, the master batch, the resin material, the release agent, and the magnetic material are mixed using the same mixer as above to obtain a first mixture. The mixing time is preferably about 60 to 200 seconds, and more preferably about 90 to 180 seconds.
[0053] Finally, the first mixture and the charge control agent are mixed using the mixer as described above to obtain a second mixture. The mixing time is preferably about 100 to 700 seconds, more preferably about 200 to 500 seconds.
[0054] By mixing the raw materials in this order to obtain a mixture, i.e., mixing the raw materials other than the charge control agent and then mixing the charge control agent to obtain a mixture, it is possible to prevent the needle-like particles of the charge control agent from being excessively pulverized in the mixture, which makes it easier to adjust the particle size of the charge control agent in the kneaded product obtained in the next melt-kneading step S2.
[0055] (Melting and kneading process S2) In the melt-kneading step S2, the second mixture produced in the mixing step S1 is melt-kneaded by a kneader to produce a kneaded product in which the release agent, charge control agent, colorant, and magnetic material are dispersed in the resin material.
[0056] In the melt-kneading step S2, a kneader similar to the kneader exemplified in the mixing step S1 can be used. Moreover, melt-kneading may be performed using a plurality of kneaders.
[0057] The temperature during melt kneading varies depending on the type of kneader used, but is preferably about 80 to 200° C., and more preferably about 100 to 150° C. By performing melt kneading at a temperature in this range, the release agent, charge control agent, colorant, and magnetic material can be more uniformly dispersed in the resin material.
[0058] By appropriately changing the mixing time in the mixing step S1, the type of kneader used in the melt-kneading step S2, the temperature during melt-kneading, etc., the average particle size of the charge control agent in the kneaded product can be adjusted to a desired value.
[0059] The mixing step S1 and the melt-kneading step S2 may be performed once each, or a set of both steps may be performed multiple times, or the mixing step S1 may be performed multiple times in succession before the melt-kneading step S2 is performed. The mixing step S1 may be performed again after the melt-kneading step S2, and the cooling and pulverizing step S3 and the classification step S4 may be performed after the final melt-kneading step S2. Furthermore, the pulverized material that has been subjected to the cooling and pulverizing step S3 and the classification step S4 may be used as the material in the mixing step.
[0060] In the mixing step S1, the particle size of the charge control agent can be controlled by changing the number of revolutions of the mixer, the rotation time, and the order of adding the materials. In this case, the charge control agent alone may be crushed separately in a mixer or the like and then used.
[0061] Similarly, in the pulverization and classification steps (S3 and S4) described below, the toner particle size can be controlled by changing the rotation speed, supply amount, air pressure, etc. of the pulverizer and classifier. By controlling either or both of the mixing step S1 and the pulverization and classification steps (S3 and S4), the desired toner particle size and charge control agent particle size can be obtained.
[0062] (Cooling and grinding process S3) In the cooling and pulverizing step S3, the kneaded product obtained in the melt-kneading step S2 is cooled and solidified, and then pulverized to obtain a pulverized product.
[0063] Specifically, the cooled and solidified kneaded material is coarsely pulverized to obtain a coarsely pulverized product, and then the coarsely pulverized product is finely pulverized to obtain a pulverized product. The volume average particle size of the coarsely pulverized product is preferably about 100 μm to 5 mm, and the volume average particle size of the pulverized product is preferably 15 μm or less.
[0064] The kneaded material can be pulverized using a pulverizer similar to that mentioned in the mixing step S1. In addition, the coarsely pulverized material can be finely pulverized using, for example, a jet pulverizer that uses a supersonic jet stream, or an impact pulverizer that introduces the coarsely pulverized material into a space formed between a rotor and a stator (liner) rotating at high speed to pulverize the material.
[0065] The pulverized product thus obtained typically contains toner particles (first pulverized particles), over-pulverized toner particles (second pulverized particles) having an average particle size (e.g., volume average particle size) smaller than the average particle size (e.g., volume average particle size) of the toner particles, and coarse toner particles (third pulverized particles) having an average particle size (e.g., volume average particle size) larger than the average particle size (e.g., volume average particle size) of the toner particles.
[0066] (Classification process S4) In the classification step S4, the pulverized product obtained in the cooling and pulverizing step S3 is classified by a classifier to remove over-pulverized toner particles (second pulverized particles) and coarse toner particles (third pulverized particles) to obtain toner particles (first pulverized particles). The over-pulverized toner particles and coarse toner particles (particularly the over-pulverized toner particles) can be collected and reused in a different or subsequent toner manufacturing process.
[0067] In the following, toner having toner particles before external additives are attached to the surface, such as these toner particles (first pulverized particles), will be referred to as non-additive toner, and toner having toner particles with external additives attached to the surface will be referred to as additive toner.
[0068] For classification, for example, a classifier that utilizes centrifugal force and wind force, such as a swirling wind classifier (rotary wind classifier), can be used.
[0069] As described above, by adjusting the average particle size of the charge control agent, the dispersion diameter of the charge control agent contained in the kneaded material becomes an appropriate size, and excessive pulverization of the kneaded material is suppressed, and as a result, the amount of charge control agent contained in the over-pulverized toner particles (second pulverized particles) (segregation rate of the charge control agent) is reduced. Therefore, even if the over-pulverized toner particles are continuously reused in the toner manufacturing process, the toner particles (recycled toner particles) obtained in the later rounds can fully maintain excellent charging properties.
[0070] The segregation rate of the charge control agent is defined as A / B × 100, where A is the amount of the charge control agent contained in the over-pulverized toner particles (second pulverized particles) and B is the amount of the charge control agent contained in the toner particles (first pulverized particles). For example, A and B can be measured by quantitatively analyzing elements derived from the charge control agent in both particles using fluorescent X-ray analysis, and the segregation rate can be calculated using the above formula.
[0071] In the present invention, the segregation rate of the charge control agent is preferably 102% or more and 130% or less, more preferably 104% or more and 120% or less, and even more preferably 106% or more and 115% or less. If the segregation rate of the charge control agent is less than the lower limit, the effect of the charge control agent may be reduced, which may cause charge-up. If the segregation rate of the charge control agent is more than the upper limit, fogging may be worsened.
[0072] The volume average particle size of the toner particles (first pulverized particles) to be collected is not particularly limited, but is preferably 3 μm or more and 15 μm or less, more preferably 3 μm or more and 9 μm or less, even more preferably 4 μm or more and 9 μm or less, and particularly preferably 5 μm or more and 8 μm or less. Toner particles having such a small particle size have an appropriate charge amount and can ensure sufficient fluidity. Therefore, the toner particles can be stably supplied to the photoconductor, and a clear and high-definition image can be formed, and the occurrence of contamination inside the machine due to scattering of toner particles can be prevented.
[0073] In addition, the content of toner particles having a number average particle size of 4 μm or less in the collected toner (fine powder content) is preferably less than 30%. If the content of toner particles having a number average particle size of 4 μm or less is above the upper limit, scattering inside the machine and fogging on paper may worsen. The content of toner particles having a number average particle size of 4 μm or less can be calculated, for example, by measuring the particle size distribution using a flow particle image analyzer (manufactured by Malvern Instruments, model: FPIA-3000).
[0074] (External addition process S5) In the external addition step S5, the toner particles obtained in the classification step S4 are mixed with an external additive to obtain a toner. The addition of the external additive improves the fluidity of the toner and the cleaning properties of the toner particles remaining on the photoreceptor surface, and prevents filming on the photoreceptor. Note that the toner particles themselves to which no external additive is added can also be used as the toner (non-additive toner).
[0075] Examples of the external additive include inorganic compounds such as silica, alumina, titania, zirconia, tin oxide, and zinc oxide, compounds such as acrylic acid esters, methacrylic acid esters, and styrene, copolymer resin fine particles of these compounds, fluororesin fine particles, silicone resin fine particles, higher fatty acids such as stearic acid, metal salts of higher fatty acids, carbon black, graphite fluoride, silicon carbide, and boron nitride. The external additive is preferably surface-treated with, for example, a silicone resin, a silane coupling agent, or the like.
[0076] The amount of the external additive added is not particularly limited and can be appropriately selected from a wide range, but is preferably 0.5 parts by weight or more and 5 parts by weight or less with respect to 100 parts by weight of the toner particles.
[0077] [Second embodiment] 2 is a process diagram showing a second embodiment of the toner manufacturing method of the present invention. In the second embodiment, the over-pulverized toner particles generated in the classification step S4 are returned to the mixing step S1 for reuse. Other than this point, the method is the same as the first embodiment.
[0078] The amount of the over-pulverized toner particles contained in the kneaded product is not particularly limited, but is preferably 5 to 40 parts by weight, and more preferably 10 to 35 parts by weight, relative to 100 parts by weight of the resin material. By adjusting the average particle size of the charge control agent in the mixing step S1 or the melt-kneading step S2 as described above, even when a relatively large amount of over-pulverized toner particles is added to the kneaded product, the resulting toner particles can sufficiently and reliably maintain excellent charging characteristics.
[0079] In addition, when the over-pulverized toner particles generated in the classification step S4 are returned to the mixing step S1 for reuse, it is preferable to mix the resin material, release agent, colorant, and magnetic material (raw materials other than the charge control agent and the over-pulverized toner particles) and then mix the charge control agent and the over-pulverized toner particles in this order to obtain a mixture. This makes it possible to prevent not only the needle-shaped particles of the charge control agent in the mixture, but also the particles of the charge control agent contained in the over-pulverized toner particles from being excessively pulverized. Therefore, it becomes easier to adjust the particle size of the charge control agent in the kneaded product obtained in the melt-kneading step S2.
[0080] Further, in the mixing step S1, fine toner particles having an average particle size (for example, a volume average particle size) smaller than the average particle size (for example, a volume average particle size) of the toner particles (toner particles to be used as a product) can be provided. Therefore, in addition to over-pulverized toner particles generated in the same toner manufacturing process as in this embodiment, the fine toner particles can be finely pulverized material obtained by collecting and separately pulverizing coarse toner particles generated in the same toner manufacturing process, over-pulverized toner particles generated in a different toner manufacturing process, finely pulverized material obtained by collecting and separately pulverizing coarse toner particles generated in a different toner manufacturing process, or a mixture thereof. The same effect as above can be obtained by using these fine toner particles. EXAMPLES
[0081] The present invention will be described below based on examples and comparative examples, but the present invention is not limited to these examples. First, the measurement methods used in the examples will be described.
[0082] <Method of measuring the volume average particle size (Dt) of toner particles> 20 mg of sample and 1 ml of sodium alkyl ether sulfate were added to 50 ml of electrolyte (Beckman Coulter, Inc., product name: ISOTON-II), and the mixture was dispersed for 3 minutes at a frequency of 20 kHz using an ultrasonic disperser (As One Corporation, tabletop dual-frequency ultrasonic cleaner, model: VS-D100) to obtain a measurement sample. The measurement sample was measured using a particle size distribution measuring device (Beckman Coulter, Inc., model: Multisizer3) under the conditions of aperture diameter: 100 μm, measurement particle number: 50,000 counts, and the volume average particle size was calculated from the volume particle size distribution of the sample particles.
[0083] <Method for measuring number average dispersed particle size (Dc) of charge control agent> The toner particles were melted at 180°C and cooled to obtain a cooled product. Next, the cooled product was cut using an ultramicrotome (manufactured by Leica Microsystems, product name: EM UC7) equipped with an ultrasonically vibrating knife to prepare a thin slice having a thickness of 100 nm. The cross section of the thin slice was then observed with a scanning transmission electron microscope (STEM, product name: S-4800, manufactured by Hitachi High-Technologies (now Hitachi High-Tech)). The dispersion diameter (circle equivalent diameter) was obtained from the obtained STEM image.
[0084] To measure the number of particles and the dispersed diameter, the images were binarized using image analysis software (product name: A-zo-kun, manufactured by Asahi Kasei Engineering Co., Ltd.), the number of charge control agents and the dispersed diameter were measured, and the number-average dispersed particle diameter of each sample was calculated.
[0085] <Method for measuring Dc10 and Dc90 in the particle size distribution of charge control agents> More than 1000 particles of the charge control agent in the cross-sectional image of the thin section obtained by the above method were measured using a vernier caliper or a scale to obtain the particle size distribution of the charge control agent. Note that this measurement may be performed using image processing software or the like. Next, the obtained particle sizes were arranged from the smallest particle size side, and the particle size of the particle that makes up 10% of the total number was defined as Dc10, and the particle size of the particle that makes up 90% of the total number was defined as Dc90, and the values of Dc10 and Dc90 were obtained.
[0086] <Method for measuring adhesion strength of charge control agent in toner> The adhesion strength of the charge control agent in the toner was measured by the following procedure. (1) 2.0 g of toner (external additive toner) is added to 40 ml of a 0.2% by mass aqueous solution of Triton (polyoxyethylene octylphenyl ether), and the mixture is stirred for 1 minute. (2) The aqueous solution is then irradiated with ultrasonic waves (output: 40 μA, for 2 minutes) using a homogenizer: US-300T (manufactured by Nippon Seiki Seisakusho Co., Ltd.). (3) The aqueous solution after the ultrasonic irradiation is left to stand for 3 hours, and the toner and the liberated charge control agent are separated. (4) After removing the supernatant, add approximately 50 ml of pure water to the precipitate and stir for 5 minutes. (5) The mixture is subjected to suction filtration using a membrane filter having a pore size of 1 μm (manufactured by Advantec Co., Ltd.). (6) The toner remaining on the filter is vacuum dried overnight. (7) Using an X-ray fluorescence analyzer (Rigaku Corporation, model: ZSX Primus II), the intensity of the element (K) in the charge control agent of 1 g of toner before and after the series of ultrasonic treatments (1) to (6) above was analyzed, and the adhesion strength of the charge control agent was calculated using the following formula.
[0087] Adhesion strength of charge control agent (%) = {(fluorescent X-ray intensity of K element after ultrasonic treatment) / (fluorescent X-ray intensity of K element before ultrasonic treatment)} x 100
[0088] <Method for measuring the segregation rate of charge control agent> Using a fluorescent X-ray analyzer (Rigaku Corporation, model: ZSX Primus II), elements derived from the charge control agent were quantitatively analyzed in the toner particles without external additives (the first pulverized particles described above) and the over-pulverized toner particles (the second pulverized particles described above).
[0089] Based on the amount (A) of the charge control agent contained in the over-pulverized toner particles (the above-mentioned second pulverized particles) and the amount (B) of the charge control agent contained in the toner particles (the above-mentioned first pulverized particles) measured by this quantitative analysis, the segregation rate (A / B x 100) of the charge control agent was calculated.
[0090] <Method for measuring the content (fine powder rate) of toner particles with a number-average particle size of 4 μm or less> The calculation was performed by measuring the particle size distribution using a flow particle image analyzer (manufactured by Malvern Instruments, model: FPIA-3000).
[0091] <How to evaluate image quality> The whiteness of the paper before printing was measured using a colorimeter (manufactured by Nippon Denshoku Industries Co., Ltd., model: ZE 6000), and the whiteness of the same location (unprinted area) was measured again after printing, and the difference was calculated as the fog on the paper.
[0092] From the results obtained, the image quality was evaluated according to the following criteria. ◎: Excellent (Can be used. Whiteness difference is 0 to less than 0.5) ○: Good (Can be used. Difference in whiteness is 0.5 or more and less than 1.0) △: Acceptable (Can be used. Whiteness difference is 1.0 or more and less than 1.5) ×: Not acceptable (Cannot be used. Difference in whiteness is 1.5 or more)
[0093] [Masterbatch production] In this embodiment, first, a master batch containing a part of the binder resin (L body) and a colorant is prepared by dry mixing the part of the binder resin and the colorant, followed by melt kneading.
[0094] In this embodiment, 100 parts by weight of L-form resin (glass transition point about 60°C, softening temperature about 70°C) and 10 parts by weight of carbon black (MA-77, manufactured by Mitsubishi Chemical Corporation) were mixed and dispersed in a Henschel mixer (manufactured by Mitsui Mining Co., Ltd.), and then melt-kneaded using an open-roll type kneader (Kneedex, manufactured by Mitsui Mining Co., Ltd.) The mixing conditions in the Henschel mixer were a rotation speed of 550 rpm and a time of 2 minutes.
[0095] [Mixing process, melt-kneading process] (1st manufacturing method) In the first production method, the toners of Example 4 and Comparative Example 4 were produced. In the first manufacturing method, the master batch, a part of the binder resin (H body), a release agent, a magnetic material, and a charge control agent are mixed, and then melted and kneaded to produce a kneaded product.Then, through a pulverization / classification process and an external addition process, the kneaded product is made into a toner.That is, in the first manufacturing method, the charge control agent is added at the same time as the binder resin and other materials (mixing 1).
[0096] In Example 4, 1 part by weight of a charge control agent (manufactured by Nippon Carlit Co., Ltd., LR-147A), 3.2 parts by weight of a microcrystalline wax (manufactured by Nippon Seiro Co., Ltd., Hi-Mic-1090), 1.5 parts by weight of a magnetic material (manufactured by Titanium Kogyo Co., Ltd., BL-220), and 60 parts by weight of an H-body resin were added to the above-mentioned master batch, and the mixture was mixed and dispersed in a Henschel mixer (manufactured by Mitsui Mining Co., Ltd.), and then melt-kneaded using a twin-screw extruder. The mixing conditions for the Henschel mixer were a rotation speed of 1200 rpm and a rotation time of 5 minutes. The operating conditions for the twin-screw extruder were a cylinder setting temperature of 110°C, a barrel rotation speed of 250 rpm, and a raw material supply rate of 10 kg / hour. On the other hand, in Comparative Example 4, the mixing conditions for the above-mentioned Henschel mixer were different, with a rotation speed of 800 rpm and a rotation time of 1 minute, and the timing of material input and kneading were the same as those in Example 4.
[0097] (Second manufacturing method) In the second production method, the toners of Examples 1 and 2, Examples 5 and 6, and Comparative Examples 2 and 3 were produced. In the second manufacturing method, the procedure for mixing materials is different from that of the first manufacturing method. After mixing the master batch, part of the binder resin (H body), release agent, and magnetic material, the charge control agent is added to the mixture and mixed again. After all the materials are mixed, the toner is produced through melt-kneading, pulverization, classification, and external addition. In other words, in the second manufacturing method, the other materials are mixed once, and then the charge control agent is added separately.
[0098] In Example 1, 3.2 parts by weight of microcrystalline wax (Hi-Mic-1090, manufactured by Nippon Seiro Co., Ltd.), 1.5 parts by weight of magnetic material (BL-220, manufactured by Titan Kogyo Co., Ltd.), and 60 parts by weight of H-body resin were added to the above-mentioned master batch, and mixed and dispersed (first mixing) in a Henschel mixer. The mixing conditions in the Henschel mixer were a rotation speed of 1500 rpm and a rotation time of 2.5 minutes.
[0099] One part by weight of a charge control agent (LR-147A, manufactured by Nippon Carlit Co., Ltd.) was added to the mixture (first mixing), and the mixture was mixed and dispersed again (second mixing) in the Henschel mixer. The mixing conditions in the Henschel mixer were a rotation speed of 1500 rpm and a rotation time of 2.5 minutes.
[0100] The mixture (second mixing) was melt-kneaded using a twin-screw extruder. The operating conditions of the twin-screw extruder were a cylinder set temperature of 110° C., a barrel rotation speed of 250 rpm, and a raw material supply rate of 10 kg / hour.
[0101] In Example 2, the mixing conditions were as follows: the rotation speed of the first mixer in the Henschel mixer was 1200 rpm, the rotation time was 2.5 minutes, and the rotation speed of the second mixer was 1200 rpm, the rotation time was 2.5 minutes. The timing of feeding the materials and the kneading were the same as in Example 1.
[0102] In Example 5, the mixing conditions were as follows: the rotation speed of the first mixer in the Henschel mixer was 1500 rpm, the rotation time was 3 minutes 20 seconds, and the rotation speed of the second mixer was 1200 rpm, the rotation time was 1 minute 20 seconds. The timing of adding the materials and the kneading were the same as in Example 1.
[0103] In Example 6, the mixing conditions were as follows: the rotation speed of the first mixer in the Henschel mixer was 1000 rpm, the rotation time was 1 minute 20 seconds, and the rotation speed of the second mixer was 1000 rpm, the rotation time was 2.5 minutes. The timing of adding the materials and the kneading were the same as in Example 1.
[0104] In Comparative Example 2, the mixing conditions were as follows: the rotation speed of the first mixer in the Henschel mixer was 700 rpm, the rotation time was 1 minute 40 seconds, and the rotation speed of the second mixer was 1000 rpm, the rotation time was 1 minute. The timing of feeding the materials and the kneading were the same as in Example 1.
[0105] In Comparative Example 3, the mixing conditions were as follows: the rotation speed of the first mixer in the Henschel mixer was 800 rpm, the rotation time was 2.5 minutes, and the rotation speed of the second mixer was 800 rpm, the rotation time was 50 seconds. The timing of adding the materials and the kneading were the same as in Example 1.
[0106] (Third manufacturing method) In the third production method, the toners of Example 3 and Comparative Example 1 were produced. In the third manufacturing method, the kneading process and the procedure for mixing materials are different from the first and second manufacturing methods. After mixing the binder resin (L type and H type), release agent, and magnetic material, the charge control agent is added to the mixture and mixed again. After that, colorants and, if necessary, over-pulverized toner are added and mixed again. After all the materials are mixed, the toner is produced through melt-kneading, pulverization, classification, and external addition. In other words, in the third manufacturing method, the other materials are mixed once without using a master batch, and then the charge control agent is added separately, and then the colorants, etc. are added.
[0107] In Example 3, 3.2 parts by weight of microcrystalline wax (Hi-Mic-1090, manufactured by Nippon Seiro Co., Ltd.), 1.5 parts by weight of magnetic material (BL-220, manufactured by Titan Kogyo Co., Ltd.), 60 parts by weight of H-body resin, and 40 parts by weight of L-body resin were mixed and dispersed in a Henschel mixer (first mixing). The mixing conditions in the Henschel mixer were a rotation speed of 1200 rpm and a rotation time of 2.5 minutes.
[0108] To the above mixture (first mixing), 1 part by weight of a charge control agent (LR-147A, manufactured by Nippon Carlit Co., Ltd.) was added, and the mixture was mixed and dispersed again (second mixing) in the Henschel mixer. The mixing conditions in the Henschel mixer were a rotation speed of 1200 rpm and a rotation time of 1 minute 15 seconds.
[0109] To the above mixture (second mixing), 10 parts by weight of a colorant (MA-77, manufactured by Mitsubishi Chemical Corporation) was added, and the mixture was mixed and dispersed again (third mixing) in the Henschel mixer. The mixing conditions in the Henschel mixer were a rotation speed of 1200 rpm and a rotation time of 5 minutes.
[0110] The mixture (from the third mixing) was melt-kneaded using a twin-screw extruder. The operating conditions of the twin-screw extruder were a cylinder temperature of 110° C., a barrel rotation speed of 250 rpm, and a raw material supply rate of 10 kg / hour.
[0111] In Comparative Example 1, the mixing conditions were as follows: the rotation speed of the first mixer in the Henschel mixer was 800 rpm, the rotation time was 1 minute, the rotation speed of the second mixer was 800 rpm, the rotation time was 1 minute, and the rotation speed of the third mixer was 800 rpm, the rotation time was 3 minutes 20 seconds. The timing of adding the materials and the kneading were the same as in Example 3.
[0112] In this embodiment, the colorant is mixed in the third mixing, but this is not limited thereto, and over-pulverized toner, etc. may be mixed in. In addition, in this embodiment, the same kneading conditions as those in the first and second manufacturing methods are used, but this is not limited thereto, and different kneading conditions may be used.
[0113] The mixing conditions using the Henschel mixer in these Examples and Comparative Examples are listed in the following Table 1. In Table 1, the unit of rotation speed is rpm, and the unit of time is seconds.
[0114] [Table 1]
[0115] [Cooling grinding process, classification process] The cooling and pulverizing step and the classification step are common to the first to third production methods. The resulting kneaded product was cooled with a cooling belt and then coarsely crushed in a speed mill equipped with a φ1 mm screen to obtain coarsely crushed products with particle sizes of 1 mm.
[0116] The coarsely crushed material obtained above was finely pulverized in a counter jet mill (product name: AFG, manufactured by Hosokawa Micron Corporation) to obtain finely pulverized particles having a volume average particle size of 6.2 μm.
[0117] The finely pulverized particles obtained above were classified using a rotary classifier (product name: TSP Separator, manufactured by Hosokawa Micron Corporation) to obtain fine particles (non-additive toner) having a volume average particle size of 6.7 μm.
[0118] The measurement results and evaluation results for the toners obtained in these Examples and Comparative Examples are shown in Table 2 below.
[0119] [Table 2]
[0120] As is clear from Table 2, the toners of Examples 1 to 6, in which Dc / Dt was 0.1 or more and 0.2 or less and Dc90 / Dc10 was 3.0 or less, were excellent in the image quality evaluation, and the occurrence of image defects such as fog was suppressed.
[0121] In contrast, Comparative Examples 1 to 4, which did not satisfy these requirements, were rated as "× (unacceptable)" in image quality, and were inferior to the Examples.
[0122] Next, toners of Examples 1-1 to 1-9 having Dc / Dt of 0.1 or more and 0.2 or less and Dc90 / Dc10 of 3.0 or less were manufactured by the following procedure, and the adhesion strength of the charge control agent, the segregation rate of the charge control agent, and the content rate (fine powder rate) of toner particles having a number average particle size of 4 μm or less were measured, and image quality was evaluated.
[0123] In Examples 1-1 to 1-9, toners were produced in the same manner as in Example 1, except that the amount of charge control agent added was changed by the second production method described above. In the second production method, the master batch, part of the binder resin (H body), release agent, and magnetic material were mixed, and then the charge control agent was added to the mixture and mixed again. After all the materials were mixed, the toner was produced through melt-kneading, pulverization, classification, and external addition.
[0124] [Example 1-1] In Example 1-1, 3.2 parts by weight of microcrystalline wax (Hi-Mic-1090, manufactured by Nippon Seiro Co., Ltd.), 1.5 parts by weight of magnetic material (BL-220, manufactured by Titan Kogyo Co., Ltd.), and 60 parts by weight of H-body resin were added to the above-mentioned master batch, and mixed and dispersed (first mixing) in a Henschel mixer. The mixing conditions in the Henschel mixer were a rotation speed of 1500 rpm and a rotation time of 2.5 minutes.
[0125] 0.05 parts by weight of a charge control agent (LR-147A, manufactured by Nippon Carlit Co., Ltd.) was added to the above mixture (first mixing), and the mixture was mixed and dispersed again (second mixing) in the Henschel mixer. The mixing conditions in the Henschel mixer were a rotation speed of 1500 rpm and a rotation time of 2.5 minutes.
[0126] The mixture (second mixing) was melt-kneaded using a twin-screw extruder. The operating conditions of the twin-screw extruder were a cylinder set temperature of 110° C., a barrel rotation speed of 250 rpm, and a raw material supply rate of 10 kg / hour.
[0127] The resulting kneaded product was cooled with a cooling belt and then coarsely crushed in a speed mill equipped with a φ1 mm screen to obtain coarsely crushed products with particle sizes of 1 mm.
[0128] The coarsely crushed material obtained above was finely pulverized in a counter jet mill (product name: AFG, manufactured by Hosokawa Micron Corporation) to obtain finely pulverized particles having a volume average particle size of 6.2 μm.
[0129] The finely pulverized particles obtained above were classified using a rotary classifier (product name: TSP Separator, manufactured by Hosokawa Micron Corporation) to obtain fine particles (non-additive toner) having a volume average particle size of 6.7 μm.
[0130] [Examples 1-2 to 1-9] A toner of Example 1-2 was obtained in the same manner as in Example 1-1, except that the amount of the charge control agent (manufactured by Nippon Carlit Co., Ltd., LR-147A) added was changed to 0.08 parts by weight. For Examples 1-3 to 1-9, the amount of charge control agent (LR-147A, manufactured by Nippon Carlit Co., Ltd.) added was changed to 0.1 parts by weight in Example 1-3, 0.15 parts by weight in Example 1-4, 0.5 parts by weight in Example 1-5, 1.0 parts by weight in Example 1-6, 2.0 parts by weight in Example 1-7, 2.5 parts by weight in Example 1-8, and 3.2 parts by weight in Example 1-9, and the respective toners were obtained in the same manner as in Example 1-1.
[0131] The measurement results and evaluation results for the toners obtained in Examples 1-1 to 1-9 are shown in Tables 3 and 4 below.
[0132] [Table 3]
[0133] [Table 4]
[0134] As is clear from Table 3, the toners of Examples 1-2 to 1-8, in which the adhesion strength of the charge control agent in the toner is 35% or more and 75% or less, had better image quality evaluations and suppressed the occurrence of image defects such as fog than the toners of Example 1-1 (adhesion strength: 33.7%) and Example 1-9 (adhesion strength: 78.1%). The toners of Examples 1-5 to 1-7, in which the adhesion strength of the charge control agent in the toner is 50% or more and 65% or less, had even better image quality evaluations and suppressed the occurrence of image defects such as fog than the toners of the other examples.
[0135] It is considered that the adhesion strength of the charge control agent is correlated with the particle size of the charge control agent, and that if the particle size of the charge control agent is large, the over-pulverized toner contains a large amount of the charge control agent, and the charge control agent in the toner particles is likely to be exposed to the toner surface, resulting in low adhesion strength.On the other hand, if the particle size of the charge control agent is small, the charge control agent is not exposed to the toner surface, and its effect as a charge control agent is reduced, resulting in high adhesion strength.
[0136] As is clear from Table 4, the toners of Examples 1-2 to 1-8, in which the segregation rate of the charge control agent is 102% or more and 130% or less, were superior in image quality evaluation and suppressed the occurrence of image defects such as fog, compared to the toners of Example 1-1 (segregation rate 101%) and Example 1-9 (segregation rate 142%). The toners of Examples 1-5 to 1-7, in which the segregation rate of the charge control agent is 106% or more and 115% or less, were even superior in image quality evaluation and suppressed the occurrence of image defects such as fog, compared to the toners of the other Examples.
[0137] Furthermore, the toners of Examples 1-3 to 1-8, in which the content of toner particles having a number-average particle size of 4 μm or less (fine-powder rate in the toner after classification) is less than 30%, had better image quality evaluations and suppressed the occurrence of image defects such as fogging than the toners of Example 1-1 (fine-powder rate: 40%) and Example 1-9 (fine-powder rate: 38%).
[0138] <Other embodiments> It should be noted that the embodiments disclosed herein are illustrative in all respects and are not intended to be limiting. Therefore, the technical scope of the present invention is not interpreted solely by the above-described embodiments, but is defined by the claims. The technical scope of the present invention includes all modifications within the scope and meaning equivalent to the claims.
Claims
1. A toner having toner particles including a binder resin, a colorant, and a charge control agent, the toner particles are ground toner particles; When the volume average particle diameter of the toner particles is Dt and the number average dispersed particle diameter of the charge control agent in the toner particles is Dc, Dc / Dt is 0.13 or more and 0.14 or less; In the particle size distribution of the charge control agent in the toner particles, when the dispersed particle size of particles having a cumulative number percentage of 90% from the small particle size side is Dc90 and the dispersed particle size of particles having a cumulative number percentage of 10% from the small particle size side is Dc10, Dc90 / Dc10 is 2.3 or more and 2.7 or less, The toner is characterized in that the adhesion strength of the charge control agent in the toner is 50% or more and 65% or less.
2. 2. The toner according to claim 1, The toner particles have a volume average particle size of 4 μm or more and 9 μm or less.
3. The toner according to claim 1 or 2, The toner is characterized in that the content of toner particles having a number average particle size of 4 μm or less in the toner is less than 30%.
4. A method for producing the toner according to any one of claims 1 to 3, comprising the steps of: a mixing step of mixing raw materials including the binder resin, the colorant, and the charge control agent; A melt-kneading step of melt-kneading the mixture obtained in the mixing step; A cooling and grinding step of cooling and solidifying the kneaded product obtained in the melt kneading step and then grinding it; a classification step of classifying the pulverized product obtained in the cooling and pulverizing step into first pulverized particles, second pulverized particles having a volume average particle size smaller than that of the first pulverized particles, and third pulverized particles having a volume average particle size larger than that of the first pulverized particles, and recovering the first pulverized particles as toner particles; A method for producing a toner, characterized in that, when the amount of the charge control agent contained in the second pulverized particles is A and the amount of the charge control agent contained in the first pulverized particles is B, a segregation rate of the charge control agent defined as A / B x 100 is 102% or more and 130% or less.
Citation Information
Patent Citations
Image forming method
JP1996240982A
Electrophotographic toner, its production and image forming method using the toner
JP1998020560A
Manufacture of toner
JP2001075307A
Electrostatic charge image developing toner, charge controlling agent used for the electrostatic charge image developing toner and method for manufacturing the same
JP2002372810A
Developer, image forming apparatus, image forming method, and developer container
JP2007249088A