Carrier core material, and electrophotographic development carrier and electrophotographic developer using the same
A ferrite-based carrier core material with controlled convexity, circularity, and magnetization addresses development memory and conveyance issues, ensuring stable and high-quality electrophotographic image production.
Patent Information
- Application Number
- JP2021044299
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-18
- Publication Date
- 2024-09-19
- Estimated Expiration
- 2041-03-18
AI Technical Summary
Existing electrophotographic carriers face issues with development memory and insufficient developer conveyance due to uneven particle surfaces, leading to poor image quality and stability over time.
A carrier core material with specific convexity, circularity, and residual magnetization ranges, composed of ferrite particles with controlled composition and surface coating, is developed to enhance developer transport and reduce development memory.
The carrier core material effectively suppresses development memory and maintains stable developer conveyance, ensuring high-quality image formation even during long-term use.
Smart Images

Figure 0007554144000004 
Figure 0007554144000006 
Figure 0007554144000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a carrier core material, and a carrier for electrophotographic development and a developer for electrophotography each using the same. [Background technology]
[0002] For example, in image forming devices using electrophotography such as facsimiles, printers, and copiers, a toner is attached to an electrostatic latent image formed on the surface of a photoconductor to make it visible, and this visible image is transferred to paper or the like, and then fixed by applying heat and pressure. From the viewpoint of achieving high image quality and colorization, so-called two-component developers containing a carrier and a toner are widely used as developers.
[0003] In a development method using a two-component developer, the carrier and toner are mixed and stirred in a development device, and the toner is charged to a predetermined amount by friction. The developer is then supplied to a rotating development roller, a magnetic brush is formed on the development roller, and the toner is electrically transferred to a photoconductor via the magnetic brush, thereby making the electrostatic latent image on the photoconductor visible. After the toner transfer, the carrier is peeled off from the development roller and mixed with the toner again in the development device. For this reason, the characteristics of the carrier require a transfer characteristic to the development roller, a magnetic characteristic to form a magnetic brush, a charging characteristic to impart a desired charge to the toner, and durability in repeated use.
[0004] Such carriers are generally made of magnetic particles such as magnetite and various ferrites, the surfaces of which are coated with resin. The magnetic particles serving as the carrier core material are required to have good magnetic properties as well as good triboelectric properties with respect to the toner. Various shapes of carrier core materials that satisfy such properties have been proposed.
[0005] For example, in order to suppress development memory (the phenomenon in which the influence of a previous image appears in a subsequent image), it has been proposed to use manganese (Mn) ferrite particles containing specific amounts of strontium (Sr) and silicon (Si) and having a specific range of maximum peak-valley depth Rz and its standard deviation σ as a carrier core material (Patent Document 1). Also, a carrier core material having a specific composition, containing a specific amount of Sn and having a specific range of saturation magnetization σs has been proposed (Patent Document 2). Also proposed is a ferrite core material with an extremely deformed shape, such as a rock candy shape and / or an oyster shell shape (Patent Document 3). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2017-031031 A [Patent Document 2] JP 2020-144310 A [Patent Document 3] JP 2007-148452 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, by increasing the maximum peak-valley depth Rz of the particles, in other words, by promoting the unevenness of the particle surface, when the surface of the carrier core material is resin-coated, part of the carrier core material is exposed to the surface, reducing the electrical resistance of the resin-coated carrier and suppressing the occurrence of development memory to some extent; however, there is a risk that the amount of developer pumped up to the developing roller and transported to the development area (hereinafter sometimes referred to as the "amount of developer transported") will be insufficient.
[0008] The present invention has been made in consideration of such conventional problems, and its object is to provide a carrier core material that can suppress development memory and is less likely to cause a decrease in the amount of developer transported.
[0009] Another object of the present invention is to provide a carrier for electrophotography and a developer for electrophotography which are capable of stably forming images of good quality even after long-term use. [Means for solving the problem]
[0010] One embodiment of the carrier core material according to the present invention that achieves the above object is a carrier core material composed of ferrite particles, the carrier core material having a convexity calculated from the following formula (1) of 0.800 or more and 0.920 or less, and a residual magnetization σ r is 1.0Am 2 / kg > 3.0Am 2 / kg or less. Convexity = convex hull perimeter / perimeter (1) (In the formula, the convex hull perimeter is the length obtained by connecting the convex parts in the projected image of the core material particle, and the perimeter is the perimeter of the projected image of the core material particle)
[0011] In the carrier core material having the above-mentioned configuration, the circularity calculated from the following formula (2) is preferably 0.850 or more and 0.890 or less. Circularity = (ISO circle area equivalent diameter) / (perimeter ellipse equivalent diameter) (2)
[0012] In the carrier core material having the above structure, the maximum height Rz is preferably 1.70 μm or more and 2.10 μm or less.
[0013] In the carrier core material having the above-mentioned configuration, the ferrite particles are represented by the composition formula (Mn X Fe 3-X )O4 (where 0≦X<3) is the main component, Ca is contained in an amount of 0.01 mol % or more and 0.50 mol % or less, and Sn is contained in an amount of 0.01 mol % or more and 0.50 mol % or less.
[0014] According to the present invention, there is also provided a carrier for electrophotographic development, characterized in that the surface of any one of the carrier core materials described above is coated with a resin.
[0015] Furthermore, according to the present invention, there is provided an electrophotographic developer comprising the above-described electrophotographic development carrier and a toner.
[0016] In the present invention, the convexity and residual magnetization σ r The circularity and maximum height Rz were measured using the measuring device and under the measuring conditions described in the Examples below.
[0017] In this specification, the terms "ferrite particles," "carrier core material," "electrophotographic development carrier," and "toner" each mean an aggregate (powders) of individual particles. In this specification, unless otherwise specified, "to" is used to mean that the numerical values before and after it are included as the lower and upper limits. Effect of the Invention
[0018] According to the carrier core material of the present invention, development memory is suppressed and a decrease in the amount of transported developer is suppressed.
[0019] Furthermore, by using a developer containing the carrier core material according to the present invention, it is possible to stably form images of good quality even after long-term use. [Brief description of the drawings]
[0020] [Figure 1] 2 is a SEM photograph of the carrier core material of Example 1. [Diagram 2] 4 is a SEM photograph of the carrier core material of Example 2. [Diagram 3] 1 is a SEM photograph of the carrier core material of Comparative Example 22. [Figure 4] 1 is a SEM photograph of the carrier core material of Comparative Example 23. [Diagram 5] 1 is a schematic diagram showing an example of a developing device using an electrophotographic developer according to the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] One of the major features of the carrier core material according to the present invention is that the convexity calculated from the above formula (1) is 0.800 or more and 0.920 or less. The convexity approaches "1.000" as the number of convex parts on the particle surface of the carrier core material decreases. If the convexity of the carrier core material is less than 0.800, although many convex parts exist on the particle surface of the carrier core material, each of the convex parts is too fine, and when the particle surface of the carrier core material is coated with a resin, the surface shape of the core material does not remain on the surface of the coating resin, and the surface becomes smooth. This reduces the ability to scrape off toner attached to the surface of the developing roller and the ability to impart charge to the toner. On the other hand, if the convexity exceeds 0.920, the convex parts on the particle surface of the carrier core material are few, and when the particle surface of the carrier core material is coated with a resin, the surface of the coating resin becomes smooth, resulting in the same problems as when the convexity is less than 0.800. Therefore, in the present invention, the convexity of the carrier core material is set to the above range. A more preferable range of the convexity of the carrier core material is 0.890 or more and 0.920 or less. The convexity of the carrier core material can be adjusted by controlling, for example, the firing temperature, the oxygen concentration, the Ca and Sn contents, and the like during main firing.
[0022] Another major feature of the carrier core material according to the present invention is the residual magnetization σ r is 1.0Am 2 / kg > 3.0Am 2 / kg or less. The residual magnetization σ of the carrier core material r is 1.0Am 2 If the carrier density is less than 1 / kg, the amount of developer transported may decrease. r 3.0Am 2 If the residual magnetization of the carrier core exceeds σ / kg, the developer may not be peeled off smoothly from the developing roller after the toner has been consumed during development. r The residual magnetization σ of the carrier core material is set to the above range. r A more preferred range is 1.1 Am 2 / kg or more 2.5Am 2 / kg or less. Residual magnetization σ of the carrier core material rcan be adjusted, for example, by controlling the oxygen concentration during cooling in the main firing or the oxidation treatment temperature.
[0023] The circularity of the carrier core material of the present invention calculated from the formula (2) is preferably 0.850 or more and 0.890 or less. The circularity approaches "1.000" as the projected shape of the carrier core material particles becomes more circular. If the circularity of the carrier core material is less than 0.850, the particle shape of the carrier core material becomes too distorted, and deterioration over time such as cracking and chipping of the particles is likely to progress. On the other hand, if the circularity of the carrier core material exceeds 0.890, the particles become too spherical, which may cause a decrease in the scraping action of the carrier on the developing roller surface and a decrease in toner transportability. The circularity of the carrier core material can be adjusted, for example, by controlling the baking temperature, oxygen concentration, Ca and Sn contents, etc. during the main baking.
[0024] The maximum height Rz of the carrier core material of the present invention is preferably 1.70 μm or more and 2.10 μm or less. If the maximum height Rz of the carrier core material is less than 1.70 μm, there is a risk of development memory or insufficient developer transport amount. On the other hand, if the maximum height Rz of the carrier core material exceeds 2.10 μm, there is a risk of particle cracking or chipping. The maximum height Rz of the carrier core material is more preferably in the range of 1.74 μm or more and 2.05 μm or less. The maximum height Rz of the carrier core material can be adjusted, for example, by controlling the firing temperature, oxygen concentration, Ca and Sn contents, etc. during main firing.
[0025] The ferrite particles constituting the carrier core material of the present invention are represented by the composition formula (Mn X Fe 3-X)O4 (where 0≦X<3) is the main component, and it is preferable that Ca (calcium) is contained at 0.01 mol% or more and 0.50 mol% or less, and Sn (tin) is contained at 0.01 mol% or more and 0.50 mol% or less, relative to the total number of moles of Mn (manganese) and Fe (iron). By containing Ca and Sn in the above amounts, the electrical properties, magnetic properties, and shape properties of the carrier core material can be adjusted to desired ranges. The preferred Ca content range is 0.10 mol% or more and 0.40 mol% or less. The preferred Sn content range is 0.10 mol% or more and 0.35 mol% or less.
[0026] The apparent density AD (g / cm 3 ) is preferably in the range of 1.80 or more and 2.80 or less, and more preferably in the range of 2.00 or more and 2.50 or less.
[0027] The fluidity FR (sec / 50 g) of the carrier core material of the present invention is preferably in the range of 20 to 50, more preferably in the range of 24 to 40. When the fluidity FR is in this range, the stress between the particles constituting the carrier core material is small, and wear of the resin coating layer is suppressed.
[0028] The volume average particle diameter (D 50 ) is preferably in the range of 20 μm or more and 60 μm or less, and more preferably in the range of 25 μm or more and 40 μm or less. The ratio of the carrier core material having a particle size of 22 μm or less is preferably 5.0% or less, and more preferably 1.5% or less. The carrier core material of the present invention has a convexity of 0.800 or more and 0.920 or less, and a circularity of 0.850 or more and 0.890 or less, and is an approximately spherical irregular-shaped particle different from a true sphere. However, since the convexity and circularity are in the above ranges, the particle size can be controlled by a sieve or the like, and the volume average particle size (D 50 ) and the ratio of particles with a particle size of 22 μm or less can be easily adjusted to a preferred range, and carrier adhesion and the like can be effectively suppressed.
[0029] The electrical resistance of the carrier core material of the present invention at a voltage of 1000 V is 5.0×10 5It is preferably Ω or more, and more preferably 1.0×10 6 Ω or more. Electrical resistance is 5.0×10 5 By setting the electric resistance to Ω or more, charge injection into the carrier core material is effectively suppressed, and carrier adhesion is suppressed. Note that this electric resistance value is determined by the method for measuring static electric resistance in the examples described later.
[0030] The magnetic properties of the carrier core material of the present invention are preferably in the following ranges. These magnetic properties are measured by the method of measuring magnetic properties in the examples described later. First, the saturation magnetization σ s (Am 2 / kg) is preferably in the range of 50 to 90, and more preferably in the range of 70 to 80. s 90Am 2 If the toner density exceeds 100 / kg, the magnetic brush formed on the outer periphery of the developing roller becomes hard and the density of the magnetic brush becomes low, which may result in an insufficient amount of developer being transported to the developing area.
[0031] Also, the magnetic field is 79.58×10 3 Magnetization σ when A / m (1,000 Oersted) is applied 1k (Am 2 / kg) is preferably in the range of 40 to 80, more preferably in the range of 50 to 65. c (×10 3 / (4π)A / m) is preferably in the range of 10.0 or more and 32.0 or less.
[0032] The average length RSm (μm) of the carrier core material is preferably in the range of 4.0 to 10.0, more preferably in the range of 6.0 to 8.0, and the skewness Rsk of the carrier core material is preferably in the range of -0.50 to 0.00, more preferably in the range of -0.30 to -0.10.
[0033] The pore volume PV (cm) of the carrier core material according to the present invention 3 / g) is preferably in the range of 0.002 or more and 0.100 or less, and more preferably in the range of 0.004 or more and 0.020 or less. If the pore volume PV is too large, the magnetization per particle of the carrier core material decreases, which may cause new problems such as carrier adhesion.
[0034] The BET specific surface area (m 2 The true density (g / cm3) of the carrier core material of the present invention is preferably in the range of 0.05 to 0.50, more preferably in the range of 0.08 to 0.20. 3 ) is preferably in the range of 4.20 or more and 5.20 or less, and more preferably in the range of 4.50 or more and 4.95 or less.
[0035] Although there is no particular limitation on the method for producing the carrier core material of the present invention, the production method described below is preferable.
[0036] First, the raw materials such as Fe component raw material, Mn component raw material, Ca component raw material, Sn component raw material, and conventionally known additives are weighed out as necessary. As the Fe component raw material, Fe2O3, etc. can be suitably used. As the Mn component raw material, MnCO3, Mn3O4, etc. can be used. As the Ca component raw material, CaCO3, Ca(NO3)2, etc. can be suitably used. As the Sn component raw material, SnO2, SnO, etc. can be used.
[0037] Next, the raw materials are put into the dispersion medium to prepare a slurry. Water is suitable as the dispersion medium used in the present invention. In addition to the above-mentioned calcination raw materials, a binder, a dispersant, etc. may be mixed into the dispersion medium as necessary. For example, polyvinyl alcohol can be used as the binder. The amount of the binder to be mixed is preferably about 0.1% by mass to 2% by mass in the slurry. In addition, for example, ammonium polycarboxylate or methacrylic acid-based polymer can be used as the dispersant. The amount of the dispersant to be mixed is preferably about 0.1% by mass to 2% by mass in the slurry. In addition, a reducing agent such as carbon black, a pH adjuster such as ammonia, a lubricant, a sintering accelerator, etc. may be mixed. The solid content concentration of the slurry is preferably in the range of 50% by mass to 90% by mass. More preferably, it is 60% by mass to 80% by mass. If it is 60% by mass or more, there are few pores in the particles in the granulated product, and insufficient sintering during firing can be prevented.
[0038] The weighed raw materials may be mixed, pre-fired, and deagglomerated, and then poured into a dispersion medium to prepare a slurry. The pre-fire temperature is preferably in the range of 750°C to 1000°C. If it is 750°C or higher, partial ferritization by pre-fired progresses, the amount of gas generated during firing is small, and solid-state reactions progress sufficiently, so it is preferable. On the other hand, if it is 1000°C or lower, sintering by pre-fired is weak, and the raw materials can be sufficiently pulverized in the subsequent slurry pulverization process, so it is preferable. In addition, air is preferable as the atmosphere during pre-fired.
[0039] Next, the slurry prepared as described above is wet-pulverized. For example, wet-pulverization is performed for a predetermined time using a ball mill or a vibration mill. The average particle size of the raw material after pulverization is preferably 5 μm or less, more preferably 1 μm or less. It is preferable that media of a predetermined particle size is contained inside the vibration mill or ball mill. Examples of the media material include iron-based chrome steel and oxide-based zirconia, titania, alumina, etc. The form of the pulverization process may be either continuous or batchwise. The particle size of the pulverized product is adjusted by the pulverization time, rotation speed, material and particle size of the media used, etc.
[0040] The pulverized slurry is then spray-dried to form granules. Specifically, the slurry is introduced into a spray dryer, such as a spray drier, and sprayed into the atmosphere to form spherical granules. The atmospheric temperature during spray drying is preferably in the range of 100°C to 300°C. This results in spherical granules with a particle size of 10 μm to 200 μm. Next, if necessary, the obtained granules are classified using a vibrating sieve to produce granules with a predetermined particle size range.
[0041] Next, the granulated material is put into a furnace heated to a predetermined temperature and sintered by a general method for synthesizing ferrite particles to generate ferrite particles. The sintering temperature is preferably in the range of 1050°C to 1350°C. More preferably, it is in the range of 1100°C to 1300°C. If the sintering temperature is 1050°C or lower, phase transformation is unlikely to occur and sintering is unlikely to proceed. If the sintering temperature exceeds 1350°C, excessive sintering may cause excessive grains to be generated. The heating rate up to the sintering temperature is preferably in the range of 250°C / h to 500°C / h. The holding time at the sintering temperature is preferably 2 hours or more. The unevenness of the ferrite particle surface can also be adjusted by the oxygen concentration in the sintering process. Specifically, the oxygen concentration is set to 0.05% to 10%. Also, the oxidation state of the ferrite phase may be adjusted by setting the oxygen concentration during cooling lower than the oxygen concentration during sintering. Specifically, the oxygen concentration is set to the range of 0.05% to 21%. The oxygen concentration during the heating, sintering and cooling steps is preferably controlled within the range of 0.05% to 21%. The oxygen concentration during the heating step is more preferably within the range of 0.6% to 5%.
[0042] The fired product thus obtained is disintegrated as necessary. Specifically, for example, the fired product is disintegrated by a hammer mill or the like. The disintegration process may be either continuous or batchwise. After the disintegration process, classification may be performed to adjust the particle size to a predetermined range as necessary. As a classification method, a conventionally known method such as wind classification or sieve classification may be used. After primary classification by a wind classifier, the particle size may be adjusted to a predetermined range by a vibrating sieve or ultrasonic sieve. Furthermore, after the classification process, non-magnetic particles may be removed by a magnetic field separator. The particle size of the ferrite particles is preferably 25 μm or more and less than 50 μm.
[0043] Thereafter, if necessary, the classified ferrite particles may be heated in an oxidizing atmosphere to form an oxide film on the particle surface to increase the resistance of the ferrite particles (resistance increasing treatment). The oxidizing atmosphere may be either air or a mixed atmosphere of oxygen and nitrogen.
[0044] The ferrite particles prepared as described above are used as the carrier core material of the present invention. In order to obtain the desired charging properties, the outer periphery of the carrier core material is coated with a resin to form a carrier for electrophotographic development.
[0045] The resin that coats the surface of the carrier core material may be any of the conventionally known resins, such as polyethylene, polypropylene, polyvinyl chloride, poly-4-methylpentene-1, polyvinylidene chloride, ABS (acrylonitrile-butadiene-styrene) resin, polystyrene, (meth)acrylic resin, polyvinyl alcohol resin, as well as thermoplastic elastomers such as polyvinyl chloride, polyurethane, polyester, polyamide, and polybutadiene, and fluorosilicone resin.
[0046] To coat the surface of the carrier core material with a resin, a solution or dispersion of the resin may be applied to the carrier core material. As the solvent for the coating solution, one or more of the following may be used: aromatic hydrocarbon solvents such as toluene and xylene; ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; cyclic ether solvents such as tetrahydrofuran and dioxane; alcohol solvents such as ethanol, propanol, and butanol; cellosolve solvents such as ethyl cellosolve and butyl cellosolve; ester solvents such as ethyl acetate and butyl acetate; and amide solvents such as dimethylformamide and dimethylacetamide. The resin component concentration in the coating solution is generally in the range of 0.001% by mass to 30% by mass, particularly 0.001% by mass to 2% by mass.
[0047] The resin can be coated onto the carrier core material by, for example, a spray-drying method, a fluidized bed method, a spray-drying method using a fluidized bed, a dipping method, etc. Among these, the fluidized bed method is particularly preferred because it can be efficiently coated with a small amount of resin. In the case of the fluidized bed method, for example, the amount of resin coating can be adjusted by the amount of resin solution sprayed and the spraying time.
[0048] The particle size of the carrier is generally preferably in the range of 25 μm or more and less than 50 μm, particularly preferably in the range of 25 μm or more and 40 μm or less, in terms of volume average particle size.
[0049] The electrophotographic developer according to the present invention is obtained by mixing the carrier and toner prepared as described above. There is no particular limitation on the mixture ratio of the carrier and toner, and it may be appropriately determined based on the development conditions of the developing device to be used. In general, the toner concentration in the developer is preferably in the range of 1% by mass or more and 15% by mass or less. If the toner concentration is less than 1% by mass, the image density becomes too thin, while if the toner concentration exceeds 15% by mass, toner scattering occurs in the developing device, which may cause problems such as dirt inside the device or toner adhesion to the background part of the transfer paper. A more preferable toner concentration is in the range of 3% by mass or more and 10% by mass or less.
[0050] The toner may be produced by a conventional method such as a polymerization method, a pulverization classification method, a melt granulation method, a spray granulation method, etc. Specifically, a toner containing a colorant, a release agent, a charge control agent, etc. in a binder resin mainly composed of a thermoplastic resin can be suitably used.
[0051] Generally, the particle size of the toner is preferably in the range of 5 μm to 15 μm, more preferably 7 μm to 12 μm, in terms of the volume average particle size measured by a Coulter counter.
[0052] If necessary, a modifier may be added to the toner surface. Examples of the modifier include silica, alumina, zinc oxide, titanium oxide, magnesium oxide, polymethyl methacrylate, etc. These may be used alone or in combination of two or more.
[0053] The carrier and toner can be mixed using a conventionally known mixing device, such as a Henschel mixer, a V-type mixer, a tumbler mixer, or a hybridizer.
[0054] Although there is no particular limitation on the developing method using the developer of the present invention, a magnetic brush development method is preferable. Fig. 5 shows a schematic diagram of an example of a developing device that performs magnetic brush development. The developing device shown in Fig. 5 includes a rotatable developing roller 3 incorporating multiple magnetic poles, a regulating blade 6 that regulates the amount of developer on the developing roller 3 that is transported to a developing section, two screws 1 and 2 that are arranged in parallel in the horizontal direction and stir and transport the developer in opposite directions, and a partition plate 4 that is formed between the two screws 1 and 2 and allows the developer to move from one screw to the other screw at both ends of the screws and prevents the developer from moving at any other than both ends.
[0055] The two screws 1 and 2 have helical blades 13 and 23 formed on shafts 11 and 21 at the same inclination angle, and are rotated in the same direction by a driving mechanism (not shown) to transport the developer in opposite directions. The developer moves from one screw to the other at both ends of the screws 1 and 2. This causes the developer, which is made up of toner and carrier, to constantly circulate and be stirred inside the device.
[0056] Meanwhile, the developing roller 3 is a metal cylindrical body with a surface roughness of several μm, and has a fixed magnet with five magnetic poles arranged in order as magnetic pole generating means: a developing magnetic pole N1, a transporting magnetic pole S1, a peeling magnetic pole N2, a pumping magnetic pole N3, and a blade magnetic pole S2. When the cylindrical body of the developing roller 3 rotates in the direction of the arrow, the developer is pumped up from the screw 1 to the developing roller 3 by the magnetic force of the pumping magnetic pole N3. The developer carried on the surface of the developing roller 3 is regulated in layer by a regulating blade 6, and then transported to the development area.
[0057] In the development area, a bias voltage in which an AC voltage is superimposed on a DC voltage is applied from a transfer voltage power source 8 to the development roller 3. The DC voltage component of the bias voltage is set to a potential between the background portion potential and the image portion potential on the surface of the photoconductor drum 5. The background portion potential and the image portion potential are set to potentials between the maximum and minimum values of the bias voltage. The peak-to-peak voltage of the bias voltage is preferably in the range of 0.5 kV to 5 kV, and the frequency is preferably in the range of 1 kHz to 10 kHz. The waveform of the bias voltage may be any of a square wave, a sine wave, a triangular wave, and the like. This causes the toner and carrier to vibrate in the development area, and the toner adheres to the electrostatic latent image on the photoconductor drum 5 to develop it.
[0058] The developer on the developing roller 3 is then transported inside the device by the transport magnetic pole S1, peeled off from the developing roller 3 by the peeling electrode N2, and circulated again within the device by the screws 1 and 2, where it is mixed and stirred with the developer not being used for development. Then, new developer is supplied from the screw 1 to the developing roller 3 by the pumping pole N3.
[0059] In the embodiment shown in FIG. 5, the developing roller 3 has five magnetic poles. However, it is of course possible to increase the number of magnetic poles to eight, ten, or twelve in order to further increase the amount of developer movement in the development area or to further improve the pumping performance, etc. EXAMPLES
[0060] Example 1 As raw materials, 43.35 kg of Fe2O3 (average particle size: 0.6 μm), 20.52 kg of Mn3O4 (average particle size: 3.4 μm), 244 g of CaCO3 (average particle size: 0.6 μm), and 293 g of SnO2 (average particle size: 5.6 μm) were dispersed in 21.75 kg of pure water, and 191.6 g of carbon black was added as a reducing agent, 389.6 g of polycarboxylate ammonium dispersant as a dispersant, and 45.5 g of ammonia water as a pH adjuster to obtain a mixture. This mixture was pulverized using a wet ball mill (media diameter 3 mm) to obtain a mixed slurry. This mixed slurry was sprayed into hot air at about 210° C. using a spray dryer to obtain dried granules with a particle size of 10 μm to 75 μm. Fine particles with a particle size of 25 μm or less were removed from the granules using a sieve. The granulated material was placed in an electric furnace and heated to 1300°C at an oxygen concentration of 1.0% over 5.5 hours. It was then fired at 1300°C for 2.5 hours at an oxygen concentration of 0.4% to 1.0%. It was then cooled at an oxygen concentration of 0.4% over 5.5 hours. The obtained sintered product was disintegrated with a hammer mill ("Hammer Crusher NH-34S" manufactured by Sansho Industry Co., Ltd., screen opening: 0.3 mm) and classified with a vibrating sieve to obtain sintered particles with a volume average particle size of 35.5 μm. The obtained sintered particles were subjected to an oxidation treatment by being held at a temperature of 465° C. in air for 1 hour, and a carrier core material according to Example 1 was obtained. The apparent density, fluidity, volume average particle size (average particle size), magnetic properties, pore volume, BET specific surface area, static resistance, circularity, and convexity of the obtained carrier core material were measured by the methods described below. The carrier core materials of the following examples and comparative examples were also measured by the same methods. Figure 1 shows an SEM photograph of the carrier core material of Example 1.
[0061] Example 2 As raw materials, 43.36 kg of Fe2O3 (average particle size: 0.6 μm), 17.72 kg of Mn3O4 (average particle size: 3.4 μm), 233 g of CaCO3 (average particle size: 0.6 μm), and 280 g of SnO2 (average particle size: 5.6 μm) were dispersed in 20.84 kg of pure water, and 164.9 g of carbon black was added as a reducing agent, 447.1 g of polycarboxylate ammonium dispersant as a dispersant, and 43.5 g of ammonia water as a pH adjuster to obtain a mixture. This mixture was pulverized using a wet ball mill (media diameter 2 mm) to obtain a mixed slurry. This mixed slurry was sprayed into hot air at about 140° C. using a spray dryer to obtain dried granules with a particle size of 10 μm to 75 μm. Fine particles with a particle size of 25 μm or less were removed from the granules using a sieve. The granulated material was placed in an electric furnace and heated to 1300°C at an oxygen concentration of 1.0% over 5 hours. It was then fired by holding at 1300°C for 3 hours at an oxygen concentration of 0.4% to 1.0%. It was then cooled at an oxygen concentration of 0.4% over 6 hours. The obtained sintered product was disintegrated using a hammer mill ("Hammer Crusher NH-34S" manufactured by Sansho Industry Co., Ltd., screen opening: 0.3 mm) and classified using a vibrating sieve to obtain sintered particles with a volume average particle size of 35 μm. The obtained sintered particles were subjected to an oxidation treatment by being held at a temperature of 480° C. in air for 1 hour, thereby obtaining a carrier core material according to Example 2. An SEM photograph of the carrier core material of Example 2 is shown in FIG. 2.
[0062] Example 3 As raw materials, 43.35 kg of Fe2O3 (average particle size: 0.6 μm), 20.52 kg of Mn3O4 (average particle size: 3.4 μm), 244 g of CaCO3 (average particle size: 0.6 μm), and 293 g of SnO2 (average particle size: 5.6 μm) were dispersed in 21.75 kg of pure water, and 191.6 g of carbon black was added as a reducing agent, 389.6 g of polycarboxylate ammonium dispersant as a dispersant, and 45.5 g of ammonia water as a pH adjuster to obtain a mixture. Except for this, calcined particles having a volume average diameter of 36.0 μm were obtained in the same manner as in Example 2. The obtained calcined particles were subjected to an oxidation treatment by holding them at a temperature of 460° C. under air for 1 hour, and a carrier core material according to Example 3 was obtained.
[0063] Example 4 Burned particles having a volume average diameter of 36.0 μm were obtained in the same manner as in Example 3. The obtained burned particles were subjected to an oxidation treatment by being held at a temperature of 480° C. in the air for 1 hour, thereby obtaining a carrier core material according to Example 4.
[0064] Example 5 Except for carrying out the calcination by holding at 1270°C with an oxygen concentration of 0.4% to 1.0% for 3 hours, calcined particles having a volume average diameter of 35.3 μm were obtained in the same manner as in Example 3. The calcined particles thus obtained were subjected to an oxidation treatment by holding at a temperature of 440°C in the atmosphere for 1 hour, thereby obtaining a carrier core material according to Example 5.
[0065] Example 6 Burned particles having a volume average diameter of 35.3 μm were obtained in the same manner as in Example 5. The obtained burned particles were subjected to an oxidation treatment by being held at a temperature of 460° C. in the air for 1 hour, thereby obtaining a carrier core material according to Example 6.
[0066] Example 7 Burned particles having a volume average diameter of 35.3 μm were obtained in the same manner as in Example 5. The obtained burned particles were subjected to an oxidation treatment by being held at a temperature of 480° C. in the air for 1 hour, thereby obtaining a carrier core material according to Example 7.
[0067] Example 8 Sintered particles having a volume average diameter of 35.4 μm were obtained in the same manner as in Example 3, except that the firing was performed by holding at 1250° C. with an oxygen concentration of 0.4% to 1.0% for 3 hours. The obtained fired particles were subjected to an oxidation treatment by holding at a temperature of 440° C. in the atmosphere for 1 hour, and a carrier core material according to Example 8 was obtained.
[0068] Example 9 Burned particles having a volume average diameter of 35.4 μm were obtained in the same manner as in Example 8. The obtained burned particles were subjected to an oxidation treatment by being held at a temperature of 460° C. in the air for 1 hour, thereby obtaining a carrier core material according to Example 9.
[0069] Example 10 Burned particles having a volume average diameter of 35.4 μm were obtained in the same manner as in Example 8. The obtained burned particles were subjected to an oxidation treatment by being held at a temperature of 480° C. in the air for 1 hour, thereby obtaining a carrier core material according to Example 10.
[0070] Example 11 Sintered particles having a volume average diameter of 35.9 μm were obtained in the same manner as in Example 3, except that the firing was performed by holding at 1230° C. with an oxygen concentration of 0.4% to 1.0% for 3 hours. The obtained fired particles were subjected to an oxidation treatment by holding at a temperature of 440° C. in the atmosphere for 1 hour, and a carrier core material according to Example 11 was obtained.
[0071] Example 12 Burned particles having a volume average diameter of 35.4 μm were obtained in the same manner as in Example 11. The obtained burned particles were subjected to an oxidation treatment by being held at a temperature of 460° C. in the air for 1 hour, thereby obtaining a carrier core material according to Example 12.
[0072] Example 13 Burned particles having a volume average diameter of 35.4 μm were obtained in the same manner as in Example 11. The obtained burned particles were subjected to an oxidation treatment by being held at a temperature of 480° C. in the air for 1 hour, thereby obtaining a carrier core material according to Example 13.
[0073] Example 14 As raw materials, 43.35 kg of Fe2O3 (average particle size: 0.6 μm), 20.52 kg of Mn3O4 (average particle size: 3.4 μm), 244 g of CaCO3 (average particle size: 0.6 μm), and 293 g of SnO2 (average particle size: 5.6 μm) were dispersed in 21.75 kg of pure water, and 191.6 g of carbon black was added as a reducing agent, 389.6 g of polycarboxylate ammonium dispersant as a dispersant, and 45.5 g of ammonia water as a pH adjuster to obtain a mixture. Except for this, calcined particles having a volume average particle size of 35.5 μm were obtained in the same manner as in Example 2. The obtained calcined particles were subjected to an oxidation treatment by holding them at a temperature of 460 ° C. under air for 1 hour, and a carrier core material according to Example 14 was obtained.
[0074] Example 15 Burned particles having a volume average diameter of 35.5 μm were obtained in the same manner as in Example 14. The obtained burned particles were subjected to an oxidation treatment by being held at a temperature of 480° C. in the air for 1 hour, thereby obtaining a carrier core material according to Example 15.
[0075] Example 16 Sintered particles having a volume average diameter of 35.2 μm were obtained in the same manner as in Example 14, except that the firing was performed by holding at 1270° C. with an oxygen concentration of 0.4% to 1.0% for 3 hours. The obtained fired particles were subjected to an oxidation treatment by holding at a temperature of 440° C. in the atmosphere for 1 hour, and a carrier core material according to Example 16 was obtained.
[0076] Example 17 Burned particles having a volume average diameter of 35.2 μm were obtained in the same manner as in Example 16. The obtained burned particles were subjected to an oxidation treatment by being held at a temperature of 460° C. in the air for 1 hour, thereby obtaining a carrier core material according to Example 17.
[0077] Example 18 Calcined particles having a volume average diameter of 35.2 μm were obtained in the same manner as in Example 16. The calcined particles obtained were subjected to an oxidation treatment by being held at a temperature of 480° C. in the air for 1 hour, thereby obtaining a carrier core material according to Example 18.
[0078] Example 19 Sintered particles having a volume average diameter of 36.2 μm were obtained in the same manner as in Example 14, except that the firing was performed by holding at 1250° C. with an oxygen concentration of 0.4% to 1.0% for 3 hours. The obtained fired particles were subjected to an oxidation treatment by holding at a temperature of 440° C. in the atmosphere for 1 hour, and a carrier core material according to Example 19 was obtained.
[0079] Example 20 Burned particles having a volume average diameter of 36.2 μm were obtained in the same manner as in Example 19. The obtained burned particles were subjected to an oxidation treatment by being held at a temperature of 460° C. in the air for 1 hour, thereby obtaining a carrier core material according to Example 20.
[0080] Example 21 Burned particles having a volume average diameter of 36.2 μm were obtained in the same manner as in Example 19. The obtained burned particles were subjected to an oxidation treatment by being held at a temperature of 480° C. in the air for 1 hour, thereby obtaining a carrier core material according to Example 21.
[0081] Example 22 Sintered particles having a volume average diameter of 35.8 μm were obtained in the same manner as in Example 14, except that the firing was carried out by holding at 1230° C. with an oxygen concentration of 0.4% to 1.0% for 3 hours. The obtained fired particles were subjected to an oxidation treatment by holding at a temperature of 440° C. in air for 1 hour, thereby obtaining a carrier core material according to Example 22. An SEM photograph of the carrier core material of Comparative Example 22 is shown in FIG.
[0082] Example 23 Sintered particles having a volume average diameter of 35.8 μm were obtained in the same manner as in Example 20. The obtained sintered particles were subjected to an oxidation treatment by being held at a temperature of 460° C. in air for 1 hour, thereby obtaining a carrier core material according to Example 23. An SEM photograph of the carrier core material of Comparative Example 23 is shown in FIG.
[0083] Example 24 Burned particles having a volume average diameter of 35.8 μm were obtained in the same manner as in Example 20. The obtained burned particles were subjected to an oxidation treatment by being held at a temperature of 480° C. in the air for 1 hour, thereby obtaining a carrier core material according to Example 24.
[0084] Comparative Example 1 Burned particles having a volume average diameter of 36.0 μm were obtained in the same manner as in Example 3. The obtained burned particles were not subjected to an oxidation treatment, and a carrier core material according to Comparative Example 1 was obtained.
[0085] Comparative Example 2 Burned particles having a volume average diameter of 36.0 μm were obtained in the same manner as in Example 3. The obtained burned particles were subjected to an oxidation treatment by being held at a temperature of 420° C. in the air for 1 hour, thereby obtaining a carrier core material according to Comparative Example 2.
[0086] Comparative Example 3 Burned particles having a volume average diameter of 36.0 μm were obtained in the same manner as in Example 3. The obtained burned particles were subjected to an oxidation treatment by being held at a temperature of 440° C. in the atmosphere for 1 hour, to obtain a carrier core material according to Comparative Example 3.
[0087] Comparative Example 4 Burned particles having a volume average diameter of 35.3 μm were obtained in the same manner as in Example 5. The obtained burned particles were not subjected to an oxidation treatment, and a carrier core material according to Comparative Example 4 was obtained.
[0088] Comparative Example 5 Burned particles having a volume average diameter of 35.3 μm were obtained in the same manner as in Example 5. The obtained burned particles were subjected to an oxidation treatment by being held at a temperature of 420° C. in the air for 1 hour, to obtain a carrier core material according to Comparative Example 5.
[0089] Comparative Example 6 Burned particles having a volume average diameter of 35.4 μm were obtained in the same manner as in Example 8. The obtained burned particles were not subjected to an oxidation treatment, and a carrier core material according to Comparative Example 6 was obtained.
[0090] Comparative Example 7 Burned particles having a volume average diameter of 35.4 μm were obtained in the same manner as in Example 8. The obtained burned particles were subjected to an oxidation treatment by being held at a temperature of 420° C. in the air for 1 hour, to obtain a carrier core material according to Comparative Example 7.
[0091] Comparative Example 8 Burned particles having a volume average diameter of 35.9 μm were obtained in the same manner as in Example 11. The obtained burned particles were not subjected to an oxidation treatment, and a carrier core material according to Comparative Example 8 was obtained.
[0092] Comparative Example 9 Burned particles having a volume average diameter of 35.9 μm were obtained in the same manner as in Example 11. The obtained burned particles were subjected to an oxidation treatment by being held at a temperature of 420° C. in the atmosphere for 1 hour, to obtain a carrier core material according to Comparative Example 9.
[0093] Comparative Example 10 Burned particles having a volume average diameter of 35.5 μm were obtained in the same manner as in Example 14. The obtained burned particles were not subjected to an oxidation treatment, and a carrier core material according to Comparative Example 10 was obtained.
[0094] Comparative Example 11 Burned particles having a volume average diameter of 35.5 μm were obtained in the same manner as in Example 14. The obtained burned particles were subjected to an oxidation treatment by being held at a temperature of 420° C. in the air for 1 hour, to obtain a carrier core material according to Comparative Example 11.
[0095] Comparative Example 12 Burned particles having a volume average diameter of 35.5 μm were obtained in the same manner as in Example 14. The obtained burned particles were subjected to an oxidation treatment by being held at a temperature of 440° C. in the air for 1 hour, thereby obtaining a carrier core material according to Comparative Example 12.
[0096] Comparative Example 13 Burned particles having a volume average diameter of 35.2 μm were obtained in the same manner as in Example 16. The obtained burned particles were not subjected to an oxidation treatment, and a carrier core material according to Comparative Example 13 was obtained.
[0097] Comparative Example 14 Burned particles having a volume average diameter of 35.2 μm were obtained in the same manner as in Example 14. The obtained burned particles were subjected to an oxidation treatment by being held at a temperature of 420° C. in the air for 1 hour, to obtain a carrier core material according to Comparative Example 14.
[0098] Comparative Example 15 Burned particles having a volume average diameter of 36.2 μm were obtained in the same manner as in Example 19. The obtained burned particles were not subjected to an oxidation treatment, and a carrier core material according to Comparative Example 15 was obtained.
[0099] Comparative Example 16 Burned particles having a volume average diameter of 36.2 μm were obtained in the same manner as in Example 19. The obtained burned particles were subjected to an oxidation treatment by being held at a temperature of 420° C. in the air for 1 hour, to obtain a carrier core material according to Comparative Example 16.
[0100] Comparative Example 17 Burned particles having a volume average diameter of 35.8 μm were obtained in the same manner as in Example 22. The obtained burned particles were not subjected to an oxidation treatment, and a carrier core material according to Comparative Example 17 was obtained.
[0101] Comparative Example 18 Sintered particles having a volume average diameter of 35.8 μm were obtained in the same manner as in Example 22. The obtained sintered particles were subjected to an oxidation treatment by being held at a temperature of 420° C. in the atmosphere for 1 hour, to obtain a carrier core material according to Comparative Example 18.
[0102] Comparative Example 19 As raw materials, 23.95 kg of Fe2O3 (average particle size: 0.6 μm) and 8.98 kg of Mn3O4 (average particle size: 3.4 μm) were dispersed in 11.32 kg of pure water, and 99.83 g of carbon black as a reducing agent, 199.7 g of polycarboxylate ammonium dispersant as a dispersant, and 23.1 g of ammonia water as a pH adjuster were added to form a mixture. This mixture was pulverized using a wet ball mill (media diameter 2 mm) to obtain a mixed slurry. This mixed slurry was sprayed into hot air at about 140° C. using a spray dryer to obtain dried granules having particle sizes of 10 μm to 75 μm. The granulated material was placed in an electric furnace and heated to 1300°C at an oxygen concentration of 1.0% over 5 hours. It was then fired by holding at 1300°C for 3 hours at an oxygen concentration of 0.4% to 1.0%. It was then cooled at an oxygen concentration of 0.4% over 6 hours. The obtained sintered product was disintegrated with a hammer mill ("Hammer Crusher NH-34S" manufactured by Sansho Industry Co., Ltd., screen opening: 0.3 mm) and classified with a vibrating sieve to obtain sintered particles with a volume average particle size of 35.7 μm. The obtained sintered particles were subjected to an oxidation treatment by being held at a temperature of 400° C. in air for 1 hour to obtain a carrier core material according to Comparative Example 19.
[0103] Comparative Example 20 As raw materials, 23.23 kg of Fe2O3 (average particle size: 0.6 μm), 8.71 kg of Mn3O4 (average particle size: 3.4 μm), and 108 g of CaCO3 (average particle size: 0.6 μm) were dispersed in 10.82 kg of pure water, and 95.8 g of carbon black as a reducing agent, 194.8 g of polycarboxylate ammonium dispersant as a dispersant, and 22.6 g of ammonia water as a pH adjuster were added to obtain a mixture. This mixture was pulverized using a wet ball mill (media diameter 2 mm) to obtain a mixed slurry. This mixed slurry was sprayed into hot air at about 140° C. using a spray dryer to obtain dried granules having particle sizes of 10 μm to 75 μm. The granulated material was placed in an electric furnace and heated to 1300°C at an oxygen concentration of 1.0% over 5 hours. It was then fired by holding at 1300°C for 3 hours at an oxygen concentration of 0.4% to 1.0%. It was then cooled at an oxygen concentration of 0.4% over 6 hours. The obtained sintered product was pulverized using a hammer mill ("Hammer Crusher NH-34S" manufactured by Sansho Industry Co., Ltd., screen opening: 0.3 mm) and classified using a vibrating sieve to obtain sintered particles with a volume average particle size of 36.0 μm. The obtained sintered particles were subjected to an oxidation treatment by being held at a temperature of 460° C. in air for 1 hour, to obtain a carrier core material according to Comparative Example 20.
[0104] Comparative Example 21 As raw materials, 23.23 kg of Fe2O3 (average particle size: 0.6 μm), 8.71 kg of Mn3O4 (average particle size: 3.4 μm), 108 g of CaCO3 (average particle size: 0.6 μm), and 130 g of SnO2 (average particle size: 5.6 μm) were dispersed in 10.82 kg of pure water, and 95.8 g of carbon black as a reducing agent, 194.8 g of polycarboxylate ammonium dispersant as a dispersant, and 22.7 g of ammonia water as a pH adjuster were added to obtain a mixture. This mixture was pulverized using a wet ball mill (media diameter 2 mm) to obtain a mixed slurry. This mixed slurry was sprayed into hot air at about 140° C. using a spray dryer to obtain dried granules having particle sizes of 10 μm to 75 μm. The granulated material was placed in an electric furnace and heated to 1300°C at an oxygen concentration of 1.0% over 5 hours. It was then fired by holding at 1300°C for 3 hours at an oxygen concentration of 0.4% to 1.0%. It was then cooled at an oxygen concentration of 0.4% over 6 hours. The obtained sintered product was disintegrated with a hammer mill ("Hammer Crusher NH-34S" manufactured by Sansho Industry Co., Ltd., screen opening: 0.3 mm) and classified with a vibrating sieve to obtain sintered particles with a volume average particle size of 35.3 μm. The obtained sintered particles were subjected to an oxidation treatment by being held at a temperature of 460° C. in air for 1 hour, and a carrier core material according to Comparative Example 21 was obtained.
[0105] Comparative Example 22 As raw materials, 14.52 kg of Fe2O3 (average particle size: 0.6 μm), 5.44 kg of Mn3O4 (average particle size: 3.4 μm), 111 g of SrCO3 (average particle size: 0.6 μm), and 91 g of SnO2 (average particle size: 5.6 μm) were dispersed in 6.9 kg of pure water, and 60.5 g of carbon black as a reducing agent, 121 g of polycarboxylate ammonium dispersant as a dispersant, and 14 g of ammonia water as a pH adjuster were added to make a mixture. This mixture was pulverized using a wet ball mill (media diameter 3 mm) to obtain a mixed slurry. This mixed slurry was sprayed into hot air at about 210° C. using a spray dryer to obtain dried granules with a particle size of 10 μm to 75 μm. Fine particles with a particle size of 25 μm or less were removed from the granules using a sieve. The granulated material was placed in an electric furnace and heated to 1300°C at an oxygen concentration of 1.0% over 4.5 hours. Then, sintering was performed by holding at 1300°C with an oxygen concentration of 0.4% to 1.0% for 3 hours. Then, cooling was performed at an oxygen concentration of 0.5% over 6 hours. The obtained sintered material was disintegrated with a hammer mill ("Hammer Crusher NH-34S" manufactured by Sansho Industry Co., Ltd., screen opening: 0.3 mm) and classified using a vibrating sieve to obtain sintered particles with a volume average particle size of 35.6 μm. The obtained sintered particles were subjected to an oxidation treatment by holding at a temperature of 480°C in the atmosphere for 1 hour, and a carrier core material according to Comparative Example 22 was obtained.
[0106] Comparative Example 23 As raw materials, 14.52 kg of Fe2O3 (average particle size: 0.6 μm), 5.44 kg of Mn3O4 (average particle size: 3.4 μm), 111 g of SrCO3 (average particle size: 0.6 μm), and 91 g of SnO2 (average particle size: 5.6 μm) were dispersed in 6.9 kg of pure water, and 60.5 g of carbon black as a reducing agent, 121 g of polycarboxylate ammonium dispersant as a dispersant, and 14 g of ammonia water as a pH adjuster were added to make a mixture. This mixture was pulverized using a wet ball mill (media diameter 3 mm) to obtain a mixed slurry. This mixed slurry was sprayed into hot air at about 210° C. using a spray dryer to obtain dried granules with a particle size of 10 μm to 75 μm. Fine particles with a particle size of 25 μm or less were removed from the granules using a sieve. The granulated material was placed in an electric furnace and heated to 1300°C at an oxygen concentration of 1.0% over 4.5 hours. Then, sintering was performed by holding at 1300°C with an oxygen concentration of 0.4% to 1.0% for 3 hours. Then, cooling was performed at an oxygen concentration of 0.4% over 6 hours. The obtained sintered material was disintegrated with a hammer mill ("Hammer Crusher NH-34S" manufactured by Sansho Industry Co., Ltd., screen opening: 0.3 mm) and classified using a vibrating sieve to obtain sintered particles with a volume average particle size of 36.5 μm. The obtained sintered particles were subjected to an oxidation treatment by holding at a temperature of 400°C in the atmosphere for 1 hour, and a carrier core material according to Comparative Example 23 was obtained.
[0107] Comparative Example 24 As raw materials, 20.80 kg of Fe2O3 (average particle size: 0.6 μm) and 8.12 kg of Mn3O4 (average particle size: 3 μm) were dispersed in 11.50 kg of water, and 180.0 g of polycarboxylate ammonium dispersant, 10.0 g of ammonia water as a pH adjuster, and 63.0 g of carbon black as a reducing agent were added. The mixture was then pulverized using a wet ball mill (media diameter 2 mm) to obtain a mixed slurry. This mixed slurry was sprayed into hot air at about 210° C. using a spray dryer to obtain a dried granulated powder. At this time, granulated powders other than those having the desired particle size distribution were removed using a sieve. The granulated powder was placed in an electric sintering furnace and sintered at a temperature of 1200°C for a holding time of 2.5 hours. It was then cooled at an oxygen concentration of 1.30% for 5.5 hours. The sintered product was disintegrated using a hammer mill ("Hammer Crusher NH-34S" manufactured by Sansho Industry Co., Ltd., screen opening: 0.3 mm) and classified using a vibrating sieve to obtain sintered particles with a volume average particle size of 34.0 μm. The sintered particles were subjected to an oxidation treatment by holding them at a temperature of 410°C in the atmosphere for 1 hour, to obtain a carrier core material according to Comparative Example 24.
[0108] Comparative Example 25 As raw materials, 28.94 kg of Fe2O3 (average particle size: 0.6 μm), 11.30 kg of Mn3O4 (average particle size: 2 μm), and 264 g of CaCO3 (average particle size: 0.6 μm) were dispersed in 13.71 kg of water, 250.8 g of polycarboxylate ammonium dispersant and 111.6 g of carbon black as a reducing agent were added, and the mixture was pulverized using a wet ball mill (media diameter 3 mm) to obtain a mixed slurry. This mixed slurry was sprayed into hot air at about 210° C. using a spray dryer to obtain a dried granulated powder. At this time, granulated powders other than those having the desired particle size distribution were removed using a sieve. The granulated powder was placed in an electric sintering furnace and sintered at a temperature of 1150°C for a holding time of 2.5 hours. It was then cooled at an oxygen concentration of 0.50% for 5.5 hours. The sintered product was disintegrated using a hammer mill ("Hammer Crusher NH-34S" manufactured by Sansho Industry Co., Ltd., screen opening: 0.3 mm) and classified using a vibrating sieve to obtain sintered particles with a volume average particle size of 34.3 μm. The sintered particles were subjected to an oxidation treatment by holding them at a temperature of 445°C in the atmosphere for 1 hour, to obtain a carrier core material according to Comparative Example 25.
[0109] Comparative Example 26 As raw materials, 15.00 kg of Fe2O3 (average particle size: 0.6 μm) and 5.86 kg of Mn3O4 (average particle size: 2 μm) were dispersed in 5.22 kg of water, 129.8 g of polycarboxylate ammonium dispersant and 170.0 g of SrCO3 (average particle size: 0.6 μm) were added, and the mixture was pulverized using a wet ball mill (media diameter 3 mm) to obtain a mixed slurry. This mixed slurry was sprayed into hot air at about 210° C. using a spray dryer to obtain a dried granulated powder. At this time, granulated powders other than those having the desired particle size distribution were removed using a sieve. The granulated powder was placed in an electric sintering furnace and sintered at a temperature of 1225°C for a holding time of 2.5 hours. It was then cooled at an oxygen concentration of 0.35% for 5.5 hours. The sintered product was disintegrated using a hammer mill ("Hammer Crusher NH-34S" manufactured by Sansho Industry Co., Ltd., screen opening: 0.3 mm) and classified using a vibrating sieve to obtain sintered particles with a volume average particle size of 35.6 μm. The sintered particles were subjected to an oxidation treatment by holding them at a temperature of 500°C in the atmosphere for 1 hour, to obtain a carrier core material according to Comparative Example 26.
[0110] Comparative Example 27 As raw materials, 14.34 kg of Fe2O3 (average particle size: 0.6 μm), 4.62 kg of Mn3O4 (average particle size: 2 μm), and 1.04 kg of MgO were mixed. This mixture was pelletized using a roller compactor. The obtained pellets were pre-fired in a rotary firing furnace at 850 °C under atmospheric conditions. The pellets were pulverized for 6 hours using a dry bead mill to obtain pre-fired powder. The pre-fired powder obtained was dispersed in 7.12 kg of water, to which 149.5 g of CaCO3 and 219.7 g of an aqueous solution containing 21% methacrylic acid-based polymer were added, and the mixture was pulverized using a wet ball mill (media diameter 3 mm) to obtain a mixed slurry. The solid content of this slurry was 73.5%, and the cumulative distribution 50% particle size D of the raw materials in the slurry was 1.06 kg. 50 is 1.5μm, cumulative distribution 90% particle size D 90 was 5.3 μm. This mixed slurry was sprayed into hot air at about 210° C. using a spray dryer to obtain a dried granulated powder. At this time, granulated powders other than those having the desired particle size distribution were removed using a sieve. This granulated powder was placed in an electric sintering furnace and sintered at a temperature of 1250°C for a holding time of 3 hours. It was then cooled over 6 hours at an oxygen concentration of 0.75%. The resulting sintered material was disintegrated using a hammer mill ("Hammer Crusher NH-34S" manufactured by Sansho Industry Co., Ltd., screen opening: 0.3 mm) and classified using a vibrating sieve to obtain sintered particles with a volume average particle size of 35.2 μm. The resulting sintered particles were not subjected to an oxidation treatment, and a carrier core material according to Comparative Example 27 was obtained.
[0111] Comparative Example 28 Sintered particles having a volume average diameter of 35.8 μm were obtained in the same manner as in Comparative Example 27. The obtained sintered particles were subjected to an oxidation treatment by being held at a temperature of 360° C. in the atmosphere for 1 hour, thereby obtaining a carrier core material according to Comparative Example 28.
[0112] (Apparent density) The apparent density of the carrier core material was measured in accordance with JIS Z 2504.
[0113] (Flow rate) The fluidity of the carrier core material was measured in accordance with JIS Z 2502.
[0114] (Volume average particle size (average particle size) and percentage of particles with a particle size of 22 μm or less) The volume average particle size and the proportion of particles with particle sizes of 22 μm or less of the carrier core material were measured using a laser diffraction particle size distribution measuring device ("Microtrac Model 9320-X100" manufactured by Nikkiso Co., Ltd.).
[0115] (Magnetic properties) Using a room temperature dedicated vibrating sample magnetometer (VSM) ("VSM-P7" manufactured by Toei Kogyo Co., Ltd.), the external magnetic field was set to 0 to 79.58 × 10 4 A / m (10,000 Oersted) is continuously applied for one cycle to measure the saturation magnetization σ s , residual magnetization σ r , coercive force H c and 79.58 x 10 3 Magnetization σ in a magnetic field of A / m (1000 Oersted) 1k (Am 2 / kg) were measured.
[0116] (Static Electrical Resistance) Two 2 mm thick brass plates with electrolytically polished surfaces were used as electrodes, arranged with a distance of 2 mm between the electrodes. 200 mg of carrier core material was placed in the gap between the two electrodes, and then a 240 mm diameter copper foil was placed behind each electrode. 2 With a magnet placed between the electrodes to form a bridge of the powder to be measured, DC voltages of 100 V, 500 V, and 1000 V were applied between the electrodes, and the current flowing through the carrier core material was measured using the four-terminal method to obtain the resistance value.
[0117] (Pore volume) The evaluation device used was a POREMASTER-60GT manufactured by Quantachrome. Specifically, the measurement conditions were as follows: Cell Stem Volume: 0.5ml, Head pressure: 20PSIA, Surface tension of mercury: 485.00 erg / cm 2 , Contact angle of mercury: 130.00degrees, High pressure measurement mode: Fixed Rate, Motor Speed: 1, High pressure measurement range: 20.00~10000.00PSI The measurement was performed by weighing 1,500 g of the sample and filling it into a 0.5 ml (cc) cell. The pore volume was calculated by subtracting the volume A (ml / g) at 60 PSI from the volume B (ml / g) at 10,000 PSI.
[0118] (BET specific surface area) Using a BET single-point specific surface area measuring device ("Macsorb HM model-1208" manufactured by Mountec Co., Ltd.), 8,500 g of the sample was filled into a cell with a volume of 5 mL, and the sample was degassed at 200°C for 30 minutes and then measured.
[0119] (true density) The true density of the carrier core material was measured using "ULTRA PYCNOMETER 1000" manufactured by Quantachrome.
[0120] (Method of measuring maximum peak-valley depth Rz and average length RSm) The surface was observed with a 100x objective lens using an ultra-deep color 3D shape measuring microscope ("VK-X100" manufactured by Keyence Corporation). Specifically, the carrier core material was first fixed to a flat adhesive tape with a surface, and the measurement field of view was determined with a 100x objective lens, after which the focus was adjusted to the adhesive tape surface using the autofocus function. A laser beam was irradiated from the vertical direction (Z direction) to the flat adhesive tape surface on which the carrier core material was fixed, and the surface was scanned in the X and Y directions. In addition, data in the Z direction was obtained by connecting the lens height positions when the intensity of the reflected light from the surface was at its maximum. The position data in the X, Y, and Z directions were connected to obtain the 3D shape of the carrier core material surface. The auto-photography function was used to capture the 3D shape of the carrier core material surface. Each parameter was measured using particle roughness inspection software (Mitani Shoji). First, as a pretreatment, particle recognition and shape selection were performed on the three-dimensional shape of the obtained carrier core surface. Particle recognition was performed in the following manner. Of the three-dimensional shape obtained by photography, the maximum value in the Z direction was set to 100%, the minimum value was set to 0%, and the range between the maximum value and the minimum value was divided into 100 equal parts. The area corresponding to 100 to 35% of this was extracted, and the outline of the independent area was recognized as the particle outline. Next, particles such as coarse, small, and associated particles were excluded by shape selection. By performing this shape selection, it is possible to reduce errors during the curvature correction performed later. Specifically, particles with an area equivalent diameter of 28 μm or less, 38 μm or more, and an acicular ratio of 1.15 or more were excluded. Here, the acicular ratio is a parameter calculated from the ratio of the maximum length / diagonal width of the particle, and the diagonal width represents the shortest distance between two straight lines when a particle is sandwiched between two straight lines parallel to the maximum length. Next, the portion to be used for analysis was extracted from the three-dimensional surface shape. First, a square with a side length of 15.0 μm was drawn with the center of gravity determined from the particle outline recognized by the above method as its center. 21 parallel lines were drawn within the square, and 21 roughness curves that fell on those line segments were extracted.
[0121] Since the carrier core material is approximately spherical, the roughness curve has a certain curvature as the background. Therefore, to correct the background, an optimal quadratic curve was fitted and subtracted from the roughness curve. In this case, a low-pass filter was applied with a strength of 1.5 μm, and the cutoff value λ was set to 80 μm.
[0122] The maximum peak-valley depth Rz was calculated as the sum of the height of the highest peak and the depth of the deepest valley in the roughness curve. The average value of 50 particles was used as the average value of each parameter to calculate the maximum height Rz.
[0123] The average length RSm is calculated by averaging the length of each element, which is defined as a combination of a valley and a peak in the roughness curve. The average value of 50 particles is used to calculate the average length RSm.
[0124] The above-described measurements of the maximum height Rz and average length RSm are performed in accordance with JIS B0601 (2001 edition).
[0125] (Skewness Rsk) The skewness Rsk was calculated by applying the roughness curve to the following formula 1.
[0126]
number
[0127] Here, in the formula 1, Rn represents the difference from the average line of the nth peak or valley in a reference length of 15 μm, and the root mean square height Rq is calculated by the formula shown in the following formula 2.
[0128]
number
[0129] Here, the larger the value of the obtained skewness Rsk, the more biased it is toward the valley region.
[0130] (Circularity (Average ISO Circulariy)) The evaluation device used was an injection type image analysis particle size distribution meter (Jasco International Co., Ltd., model: IF-3200). Specifically, 0.07 g of the sample was weighed out and dispersed in a screw cap bottle (volume 9 ml) containing 9 ml of polyethylene glycol 400, and then the measurement was performed. (Measurement conditions) Spacer thickness: 150μm Sampling: 20% Analysis type: Relative measurement Measurement amount: 0.95ml Analysis: Dark Detect Threshold: 169 (fill holes) O-Roughness filter: 0.5 Filter by: ISO Area Diameter: Min 33, Max 37, Inner Range (Analysis conditions) Analysis filter criteria I: ISO Circulariy: Min 0.81, Max 0.87, Inner range The analysis was performed using analysis filter condition I to obtain the average ISO circularity.
[0131] (Average Convexity) The evaluation device used was an injection type image analysis particle size distribution meter (Jasco International Co., Ltd., model: IF-3200). Specifically, 0.07 g of the sample was weighed out and dispersed in a screw cap bottle (volume 9 ml) containing 9 ml of polyethylene glycol 400, and then the measurement was performed. (Measurement conditions) Spacer thickness: 150μm Sampling: 20% Analysis type: Relative measurement Measurement amount: 0.95ml Analysis: Dark Detect Threshold: 169 (fill holes) O-Roughness filter: 0.5 Filter by: ISO Area Diameter: Min 5, Max 100, Inner Range (Analysis conditions) Analysis Filter Condition II: Convexity: Min 0, Max 0.93, Inner range The average convexity was calculated using analysis filter condition II.
[0132] (Development memory) The surface of the obtained carrier core material was coated with resin to prepare a carrier. Specifically, 450 parts by mass of silicone resin and 9 parts by mass of (2-aminoethyl)aminopropyltrimethoxysilane were dissolved in 450 parts by mass of toluene as a solvent to prepare a coating solution. This coating solution was applied to 50,000 parts by mass of the carrier core material using a fluidized bed type coating device, and heated in an electric furnace at a temperature of 300°C to obtain a carrier. In the following, carriers were obtained in the same manner for all examples and comparative examples. The obtained carrier and toner having an average particle size of about 5.0 μm were mixed for a predetermined time using a pot mill to obtain a two-component electrophotographic developer. In this case, the carrier and toner were adjusted so that the weight of the toner / (weight of the toner and carrier)=5 / 100. The developer was obtained in the same manner for all the following examples and comparative examples. The obtained developer was put into a developing device (peripheral speed of the developing roller Vs: 406 mm / sec, peripheral speed of the photosensitive drum Vp: 205 mm / sec, distance between the photosensitive drum and the developing roller: 0.3 mm) having a structure shown in FIG. 5, and an image in which a solid image portion and a non-image portion are adjacent to each other in the longitudinal direction of the photosensitive drum, followed by a wide area of intermediate tones, was obtained initially and after 200,000 sheets of image formation, and the image density of the area where the solid image of the first rotation of the developing roller was developed and the area where it was not developed was measured using a reflection densitometer (model number TC-6D manufactured by Tokyo Denshoku Co., Ltd.), and the difference was calculated and evaluated according to the following criteria. "○": Less than 0.006 "△": 0.006 or more and less than 0.020 "×": 0.020 or more
[0133] (Transport amount) 80 g of the two-component developer was placed in a small developing device (roller diameter: 16 mm, grooved roller, non-magnetic regulating plate gap: 0.6 mm) and stirred for 3 minutes at a roller rotation speed of 250 rpm. After that, a circular hole was cut out on the developing roller, measuring 4 cm wide and 1 cm long, with an area of 3.785 cm2. 2 The developer in the patch was sucked and collected in the filter using a filter-equipped suction device. The weight of the filter before and after collection was measured, the weight difference of the filter was calculated, and the transport amount per unit area was calculated using the following formula. (Developer transport volume)÷3.785cm 2 = Transport volume per unit area "〇": 50mg / □cm 2 End "×": 50mg / □cm 2 less than
[0134] [Table 1]
[0135] As shown in Table 1, in the developers using the carriers of Examples 1 to 24, the development memory was suppressed, and the developer transport amount was also good.
[0136] In contrast, the residual magnetization σ r is 1.0Am 2 The amount of developer transported was small in the developers using the carriers of Comparative Examples 1 to 28, which had a maximum height Rz of less than 1.70 μm. Development memory also occurred in the developers using the carriers of Comparative Examples 24, 25, 27, and 28, which had a maximum height Rz of less than 1.70 μm. Development memory also occurred in the developer using the carrier of Comparative Example 23, which had a large maximum height Rz of 2.27 μm. [Industrial Applicability]
[0137] According to the carrier core material of the present invention, development memory is suppressed and a decrease in the amount of transported developer is suppressed. [Explanation of symbols]
[0138] 3 Developing roller 5 Photoconductor drum
Claims
1. A carrier core material composed of ferrite particles, The convexity calculated from the following formula (1) is 0.800 or more and 0.920 or less, residual magnetization σ r is 1.0 Am 2 / kg and above 3.0 Am 2 / kg or less A carrier core material comprising: Convexity = convex hull perimeter / perimeter (1) (In the formula, the convex hull perimeter is the length obtained by connecting the convex parts in the projected image of the core particle, and the perimeter is the perimeter of the projected image of the core particle.)
2. 2. The carrier core material according to claim 1, wherein the circularity calculated from the following formula (2) is 0.850 or more and 0.890 or less. Circularity=(ISO circle area equivalent diameter) / (circumferential ellipse equivalent diameter) (2)
3. 3. The carrier core material according to claim 1, wherein the maximum height Rz is 1.70 μm or more and 2.10 μm or less.
4. The ferrite particles have a composition formula (Mn X Fe 3-X ) O 4 (wherein 0≦X<3) is the main component, Ca is contained in an amount of 0.01 mol% or more and 0.50 mol% or less, The Sn content is 0.01 mol% or more and 0.50 mol% or less, The carrier core material according to any one of claims 1 to 3,
5. 5. A carrier for electrophotographic development, comprising the carrier core material according to claim 1, the surface of which is coated with a resin.
6. 6. An electrophotographic developer comprising the carrier for electrophotographic development according to claim 5 and a toner.
Citation Information
Patent Citations
Amorphous ferrite carrier and electrophotographic developer using the ferrite carrier
JP2007148452A
Magnetic carrier and two-component developer
JP2014006513A
Carrier core material, carrier for electrophotographic development using the same, and developer for electrophotography
JP2016184130A
Carrier core material and method for forming the material
JP2016200669A
Ferrite particle, carrier for developing electrophotography and developing agent for electrophotography using the same
JP2017031031A