Articles made from ceramics

JP7557048B2Active Publication Date: 2024-09-26THE SWATCH GRP RES & DEVELONMENT LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023511635
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-09-25
Filing Date
2021-07-28
Publication Date
2024-09-26
Estimated Expiration
2041-07-28

Smart Images

  • Figure 0007557048000003
    Figure 0007557048000003
  • Figure 0007557048000002
    Figure 0007557048000002
  • Figure 0007557048000001
    Figure 0007557048000001
Patent Text Reader

Abstract

The present invention relates to an article made of a material consisting of multiple ceramic phases, the material including a major ceramic phase containing nitrides and / or carbonitrides of one or more elements selected from Ti, Zr, Hf, V, Nb, and Ta, and at least one minor ceramic phase. The proportion of the major ceramic phase is 60 to 98% by weight. In the minor ceramic phase, a single minor ceramic phase is formed by zirconium silicide and / or aluminum silicide, or several minor ceramic phases are formed by carbides of one or more elements selected from Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, and W, and zirconium oxide and / or aluminum oxide, respectively. The total proportion of the minor ceramic phase is 2 to 40% by weight. The present invention also relates to a method for producing the article.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an article, in particular an outer part or a part of a movement of a watch (e.g. wristwatch, pocket watch), made of a composite material consisting only of ceramic phases. The present invention further relates to a method for producing the same. [Background technology]

[0002] Many external components are made from composite ceramic materials, which have the advantage, among other things, of being very hard and therefore scratch resistant. The literature describes composite materials which mainly contain oxides such as alumina to which carbides have been added. They consist, for example, of a composite material containing 70% by weight of Al2O3 and 30% by weight of TiC, used as a reinforcing material. These composite materials are characterized by little or no metallic luster compared to other materials such as stainless steel or ceramels, which can be a disadvantage in decorative articles where such a luster is desired.

[0003] Materials based on titanium nitride or titanium carbonitride are also known. These materials are very difficult to densify due to their very high melting points, for example 2930°C for TiN, associated with a low diffusion coefficient. It is therefore necessary to resort to rapid sintering methods, also known as flash, such as SPS sintering (spark plasma sintering) or pressure sintering (sinter-HIP), or to densification methods under very high pressures and temperatures after sintering, such as HIP (hot isostatic pressing). Furthermore, these sintering processes do not allow parts with complex geometries to be obtained. A solution to this problem involves, for example, the preparation of ceramels based on TiN or TiCN with the addition of metallic elements that act as metallic binders. Thus, thanks to the addition of a few percent of nickel or cobalt, densification at lower temperatures, typically in the range of 1500°C, is possible. However, these elements have the problem of being highly allergenic, which limits their use in articles that are not intended to come into contact with the skin. Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention aims to solve the above-mentioned problems by providing a ceramic material, also called a composite material, with a composition and manufacturing method optimized to meet the following criteria: - Avoid the use of allergenic elements such as nickel and cobalt. - High metallic luster (65≦L*≦85). - Densification can be carried out at atmospheric pressure, vacuum or partial gas pressure without relying on high pressure to maintain the shape of the article blank upon completion of sintering. -Preferably K IC is 2.5MPa m 1 / 2 As described above, while having sufficient toughness, the hardness is 500 HV30 or more, preferably 800 HV30 or more, and more preferably 1000 HV30 or more. [Means for solving the problem]

[0005] To this end, the invention relates to an article made of a material consisting of several ceramic phases, which comprises a majority ceramic phase comprising nitrides and / or carbonitrides of one or more elements selected from group IVB, i.e. Ti, Zr and Hf, and group VB, i.e. V, Nb and Ta, and at least one minor ceramic phase. The proportion of the majority ceramic phase is between 60 and 98% by weight. In the minor ceramic phase, a single minor ceramic phase is formed by zirconium silicide and / or aluminum silicide, or several minor ceramic phases are formed by carbides of one or more elements selected from group IVB (Ti, Zr, Hf), group VB (V, Nb, Ta) and group VIB (Cr, Mo, W) and zirconium oxide and / or aluminum oxide, respectively. The total proportion of said at least one minor ceramic phase is between 2 and 40% by weight.

[0006] The composites thus produced have, after polishing, a metallic luster similar to that observed in stainless steels or ceramels with nickel or cobalt as metal binders. These composites have the other advantage of being free of allergenic elements such as Ni. They are also non-magnetic, yet hard and tough enough to produce external parts. They can also be shaped to obtain "near-net" parts by traditional powder metallurgy processes such as pressing or injection molding, or by various processes dedicated to the production of three-dimensional parts, such as 3D printing. Parts of more or less complex shape can finally be consolidated at atmospheric pressure, under vacuum or partial gas pressure, i.e. without resorting to significant pressure, at temperatures between 1400 and 1900 °C.

[0007] Additionally, articles made from this ceramic material have the advantage of being beautiful in color in chunks, ranging from yellow to reddish pink, depending on the composition.

[0008] Other characteristics and advantages of the invention will become apparent from reading the following description of preferred embodiments, given by way of example with reference to the attached drawings, in which: [Brief description of the drawings]

[0009] [Figure 1] 1 shows a timepiece with a middle part made of a ceramic material according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention relates to an article made of a composite material consisting of only ceramic phases. The article can be a decorative article such as a component of a watch, jewelry, wristlet, etc., and generally can be an external part of a portable element such as the shell of a mobile phone. In the field of a watch, the article can be an external part such as a middle, a base, a bezel, a crown, a bridge, a push piece, a wristlet link, a dial, hands, dial indexes, etc. For illustration purposes, FIG. 1 shows a middle made of the ceramic material according to the invention. The article can also consist of parts of a movement, such as a plate or a vibration weight.

[0011] The ceramic material includes a major phase constituted by nitrides and / or carbonitrides of one or more elements selected from Ti, Zr, Hf, V, Nb, and Ta, and one or more kinds of minor phases. The ceramic material can be either zirconium silicide and / or aluminum silicide, or a combination of carbides of one or more elements selected from Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, and W with zirconium oxide (Zr) and / or aluminum oxide (Al). Preferably, the major phase is constituted by titanium nitride and / or titanium carbonitride. Preferably, the minor phase is constituted by either zirconium silicide and / or aluminum silicide, or a combination of tungsten carbide and / or vanadium carbide with zirconium oxide and / or aluminum oxide, respectively.

[0012] The proportion of the majority phase is 60-98% by weight, and the proportion of all minority phases is 2-40% by weight. Preferably, the proportion of the majority phase is 65-97% by weight, preferably 70-96% by weight, more preferably 75-95% by weight. The proportion of all minority phases that complement the majority phase is preferably 3-35% by weight, more preferably 4-30% by weight, more preferably 5-25% by weight. When the majority phase contains nitrides and carbonitrides of one or more elements selected from Ti, Zr, Hf, V, Nb, and Ta, the proportions of the nitrides and carbonitrides are preferably 20-70% by weight, more preferably 25-60% by weight, based on the entire ceramic material. When the ceramic material contains two minor phases, which are carbides of one or more elements selected from Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, and W, and oxides (Al2O3 and / or ZrO2), the proportions of these phases are preferably 3 to 35% by weight, and more preferably 5 to 25% by weight, based on the total ceramic material.

[0013] The ceramic article is made by sintering starting from a mixture of powders. The manufacturing method comprises the following steps: a) preparing a mixture of different ceramic powders, optionally in a moist environment. These starting powders preferably have a d50 of less than 45 μm. Optionally, the mixture can be carried out in a grinder, which reduces the d50 of the particles of the powder after grinding to a size in the range of a few μm (<5 μm). The proportion of powders of nitrides and / or carbonitrides of one or more elements selected from Ti, Zr, Hf, V, Nb and Ta is 60-98% by weight, preferably 65-97% by weight, more preferably 70-96% by weight, more preferably 75-95% by weight, based on all of these powders. The proportion of powders of zirconium silicide and / or aluminum silicide, or powders of carbides of Ti, Zr, Hf, V, Nb, Ta, Cr, Mo and W, and powders of zirconium oxide and / or aluminum oxide is 2-40% by weight, preferably 3-35% by weight, more preferably 4-30% by weight, more preferably 5-25% by weight. For example, the ratio of the powder mixture to the total of 100% by weight is - 75-85% by weight of TiN or TiCN, 15-25% by weight of ZrSi2 - 85-95% by weight of TiN or TiCN, 5-15% by weight of ZrSi2 - 75-85% by weight of TiN or TiCN, 5-15% by weight of WC or VC, 5-15% by weight of ZrO2 or Al2O3 The composition may be any of the following weight percentages: TiN 40-55%, TiCN 25-35%, WC or VC 5-15%, and ZrO2 5-15%.

[0014] b) Optionally, a second mixture can be made comprising the above mixture and an organic binder system (paraffin, polyethylene, etc.). c) Forming a blank by imparting the mixture with the shape of the desired article, for example by injection molding, pressing or 3D printing.

[0015] d) Sintering the blank under partial gas pressure, in vacuum or at atmospheric pressure at a temperature between 1200 and 2100°C, preferably between 1400 and 1900°C, for a time between 10 min and 20 h, preferably between 15 min and 3 h. This step can be preceded by a debinding step in the temperature range between 60 and 500°C, if the mixture contains a binder system. Although the composition of the invention allows sintering under low pressure, the invention does not exclude carrying out by SPS (spark plasma sintering) or sintered HIP, with or without a subsequent HIP (hot isostatic pressing) consolidation.

[0016] The blank thus obtained is cooled and polished, and may be machined prior to polishing to obtain the desired article.

[0017] The article obtained by this method of manufacture contains major and minor phases in weight percentages close to those of the starting powder. However, there may be slight variations in composition and proportions between the base powder and the material obtained by sintering, for example after contamination or transformation during sintering. For example, carbides may react with nitrides to form carbonitrides.

[0018] The article has a luminance component L*, which represents the manner in which a material reflects light, of 60 to 85, preferably 65 to 80, and more preferably 70 to 75 in the CIELAB color space (based on standards CIE Number 15, ISO 7724 / 1, DIN 5033 Teil 7, ASTM E-1164). Preferably, the article is yellow in color, with an a* component (red component) of +1 to +7 and a b* component (yellow component) of +20 to +35. Preferably, the article is reddish-pink in color, with an a* component of +2 to +15 and a b* component of +2 to +10.

[0019] The ceramic material has a hardness HV30 of 500 or more, preferably 800 to 1800, depending on the type and proportion of the constituents. IC , but 2MPa m 1 / 2More than 2.5MPa m, preferably 1 / 2 This value is greater than or equal to 8 MPa m 1 / 2 This toughness is determined based on measuring the crack length at the four ends of the diagonal of the hardness indentation according to the following formula:

[0020]

number

[0021] where P is the applied load [N], a is the semi-diagonal [m] and l is the measured crack length [m].

[0022] The following examples are used to illustrate the methods and resulting materials according to the present invention.

[0023] A mixture of seven powders was prepared in a mill in the presence of a solvent. The mixture was made without a binder. The mixture was milled under vacuum or at 60 mbar (6000 N / m) at a temperature depending on the composition of the powder. 2 The samples were compacted by pressing and sintering under a flow of argon or nitrogen at 1000 K. After sintering, the samples were polished. Table 1 below shows the composition, sintering parameters, and mechanical properties (HV30, K IC ) and Lab colorimetric values. Values ​​in italics and bold indicate hardnesses greater than 800 Vickers and toughnesses greater than 2.5 MPa m 1 / 2 and an L* index of greater than 70 or, for those with a high degree of yellowness, a b* index of greater than 20.

[0024] A hardness measurement of HV30 was performed on the surface of the sample, and the viscosity was determined as described above based on the hardness measurement.

[0025] Lab colorimetry was measured on the polished samples using a KONICA MINOLTA CM-5 spectrophotometer under the following conditions: SCI (specular component included) and SCE (specular component excluded) measurements were performed in the MAV measurement area with a slope of 8 and a diameter of 8 mm.

[0026] Example 1 The ceramic material consists of a ceramic composite containing titanium nitride (TiN) as the majority phase and up to 20 wt. % zirconium silicide (ZrSi2) as the minor phase. In contrast to traditional sintering, the composite is densified according to the present invention by spark plasma sintering (SPS). The measured hardness is 1328 Vickers (HV30) and the toughness is 4.3 MPa m 1 / 2 It was.

[0027] Example 2 The ceramic material consists of a ceramic composite containing titanium nitride (TiN) as the majority phase and up to 10 wt% zirconium silicide (ZrSi2) as the minority phase. The 90TiN-10ZrSi2 composite was densified by both SPS and traditional sintering. When it was sintered by traditional sintering, a decrease in hardness was observed compared to SPS sintering, decreasing from 1302 to 863 Vickers, but maintaining good toughness (4.2 MPa m 1 / 2 4.4MPa m 1 / 2 ). On the other hand, traditional sintering resulted in a much better brightness with a higher luminance index (L*) (66.2 vs. 74.5). Traditional sintering also resulted in a yellower color with a slightly higher value of the yellow component b*.

[0028] Example 3 The ceramic material consists of a ceramic composite containing titanium carbonitride (TiCN) as the majority phase and up to 10 wt% zirconium silicide (ZrSi2) as the minority phase. The 90TiCN-10ZrSi2 composite achieved the most pronounced yellow color with a b* value reaching 27.29, although the hardness was reduced to 590 Vickers.

[0029] Example 4 This ceramic material is a ceramic composite material with titanium nitride (TiN) as the majority phase and tungsten carbide (WC) and aluminum oxide (Al2O3) as the minor phases, with a weight ratio of 80TiN-10WC-10Al2O3. Densified by traditional sintering and obtained without pressure input, this composite material has a hardness of 938 Vickers and a toughness of 3.6 MPa while maintaining a beautiful metallic luster (L*=72.8). 1 / 2 , and had an intense yellow color with a* of 1.7 and b* of 26.2.

[0030] Example 5 The ceramic material consists of a ceramic composite with titanium nitride (TiN) as the majority phase and tungsten carbide (WC) and zirconium dioxide (ZrO2) as minor phases in the ratio 80TiN-10WC-10ZrO2 by weight. The composite has a maximum hardness of 1187 Vickers and a measured luminance L* of 72.9. The color of such a ceramic composite is yellow, and the values ​​of the indices a* and b* are 1.48 and 26.0, respectively. Thus, thanks to the replacement of aluminum oxide (example 4) by zirconium dioxide, the hardness can be increased by 249 Vickers.

[0031] Example 6 The ceramic material consists of a ceramic composite with titanium nitride (TiN) as the majority phase and vanadium carbide (VC) and zirconium dioxide (ZrO2) as the minor phases in a ratio of 80TiN-10VC-10ZrO2 by weight. The composite has a hardness of 1275 Vickers and a measured luminance L* of 71.8. The color of such a ceramic composite is yellow, with a* and b* values ​​of 2.9 and 23.4, respectively. Thus, thanks to the replacement of tungsten carbide (example 5) with vanadium carbide, it was possible to increase the hardness by about 7%.

[0032] Example 7 The ceramic material consists of a ceramic composite containing titanium nitride (TiN) and titanium carbonitride (TiCN) as the majority phases and tungsten carbide (WC) and zirconium dioxide (ZrO2) as the minor phases in the ratio 48TiN-32TiCN-10WC-10ZrO2 by weight. Such a composite was reddish-pink in color with a* and b* indices of 7.52 and 8.02, respectively. The measured hardness was very high, i.e., 1727 Vickers, almost the same as that obtained by SPS sintering. This increase is directly attributable to the addition of tungsten carbide.

[0033] [Table 1]

Claims

1. An article made of a ceramic material consisting of several ceramic phases, the ceramic material is composed of a majority ceramic phase including nitrides and / or carbonitrides of one or more elements selected from Ti, Zr, Hf, V, Nb, and Ta, and a single minority ceramic phase formed by zirconium silicide and / or aluminum silicide; the proportion of said majority ceramic phase is 60 to 98 weight percent; The total proportion of the minority ceramic phase is 2 to 40% by weight. An article characterized by:

2. the proportion of said majority ceramic phase is 65 to 97 weight percent; The total percentage of the minority ceramic phase is 3 to 35% by weight.

2. The article of claim 1.

3. the proportion of said majority ceramic phase is between 70 and 96% by weight; The total proportion of the minority ceramic phase is 4 to 30% by weight.

2. The article of claim 1.

4. the proportion of said majority ceramic phase is 75 to 95 weight percent; The total percentage of the minority ceramic phase is 5 to 25% by weight.

2. The article of claim 1.

5. When the majority ceramic phase contains nitrides and carbonitrides of one or more elements selected from Ti, Zr, Hf, V, Nb, and Ta, the proportion of the nitrides and carbonitrides is 20 to 70% by weight based on the total ceramic material.

2. The article of claim 1.

6. The proportion of the nitride and carbonitride is 25 to 60% by weight based on the total weight of the ceramic material.

6. The article of claim 5.

7. The majority ceramic phase comprises titanium nitride and / or titanium carbonitride.

2. The article of claim 1.

8. In the CIELAB color space, the L* component is 60 to 85, or 65 to 80.

2. The article of claim 1.

9. The color is yellow, and in the CIELAB color space, the a* component is +1 to +7, and the b* component is +20 to +35.

2. The article of claim 1.

10. The color is reddish pink, and in the CIELAB color space, the a* component is +2 to +15, and the b* component is +2 to +10.

2. The article of claim 1.

11. HV30 hardness is 500 or more 2. The article of claim 1.

12. HV30 hardness is 800 to 1800 2. The article of claim 1.

13. Toughness KIC is 2MPa・m 1 / 2 or more, or 2.5 MPa m 1 / 2 That's all.

2. The article of claim 1.

14. The ceramic material is, relative to a total of 100% by weight, A majority ceramic phase containing 75 to 85 wt% TiN or TiCN, and ZrSi 2 a minority ceramic phase containing 15 to 25 weight percent of A majority ceramic phase containing 85 to 95 wt% TiN or TiCN, and ZrSi 2 Minor ceramic phase containing 5-15 wt% Either of the following is the allocation:

2. The article of claim 1.

15. Timekeeping parts 2. The article of claim 1.

16. An outer part selected from the group consisting of a middle part, a base part, a bezel, a push part, a crown, a wristlet link, a dial, a needle and a dial index, or a part of a movement selected from the group consisting of a plate, a bridge and a vibration weight.

16. The article of claim 15.

17. 1. A method of manufacturing an article, comprising the steps of: a) producing a mixture consisting of 60-98% by weight of powder of nitrides and / or carbonitrides of one or more elements selected from Ti, Zr, Hf, V, Nb and Ta, and 2-40% by weight in total of at least one powder formed by zirconium silicide and / or aluminum silicide, b) forming a blank by imparting the shape of the article to the mixture; and c) sintering the blank at a temperature of 1200-2100° C., or 1400-1900° C., for 30 minutes to 20 hours, or 15 minutes to 3 hours. A method comprising:

18. The proportion of the powder mixture in step a) is, relative to the total of 100% by weight, TiN or TiCN 75 to 85% by weight, ZrSi 2 15 to 25% by weight, or TiN or TiCN 85 to 95% by weight, ZrSi 2 5 to 15% by weight Either of the following is the allocation:

20. The method of claim 17 .

Citation Information

Patent Citations

  • Technology for preparing composite ceramic material and coproducing sulfuric acid by using phosphor gypsum and red mud

    CN108752005A

  • Sintered silicon nitride having electrically conductive coating film and production thereof

    JP1989131086A

  • Composite powder and production thereof

    JP1989294514A

  • Electrical conductive sialon sintered body, production thereof and die for drawing

    JP1990157169A

  • Gold-colored sintered compact

    JP1998007464A