Method for recovering lithium precursors

The method of converting positive electrode active materials into carbon-based solids under inert gas and water washing effectively recovers lithium precursors with high purity and yield, addressing the inefficiencies of existing wet extraction methods.

JP7566015B2Active Publication Date: 2024-10-11
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022520241
Authority / Receiving Office
JP · JP
Patent Type
Patents
Priority Date
2019-10-02
Filing Date
2020-09-18
Publication Date
2024-10-11
Estimated Expiration
2040-09-18

AI Technical Summary

Technical Problem

Existing methods for recovering lithium precursors from positive electrode active materials result in low purity and yield, with excessive impurity generation due to wet extraction processes.

Method used

A method involving the conversion of a positive electrode active material mixture into a carbon-based solid material under an inert gas atmosphere, followed by a water washing process to separate lithium precursor, is employed. This process includes reacting the mixture at temperatures between 740°C and 1,200°C, using carbon-based materials like carbon black or activated carbon, and performing dry mixing in a fluidized bed reactor.

Benefits of technology

High-purity lithium precursor is obtained with high yield and efficiency, avoiding aggregation and by-product formation, as lithium oxide is selectively separated without additional pulverization steps.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566015000005
    Figure 0007566015000005
  • Figure 0007566015000006
    Figure 0007566015000006
  • Figure 0007566015000001
    Figure 0007566015000001
Patent Text Reader

Abstract

The method for recovering lithium precursors according to an embodiment of the present invention involves preparing a positive electrode active material mixture containing a lithium composite oxide. The positive electrode active material mixture is reacted with a carbon-based solid material under an inert gas atmosphere to form a preliminary precursor mixture containing lithium oxide. The preliminary precursor mixture is washed with water to separate the lithium precursor. This allows for the recovery of lithium precursors in high yield and with high efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for recovering a lithium precursor, and more particularly to a method for recovering a lithium precursor from a positive electrode active material mixture. [Background technology]

[0002] Secondary batteries are batteries that can be repeatedly charged and discharged, and have been widely applied to portable electronic communication devices such as camcorders, mobile phones, and notebook computers with the development of the information and communication and display industries. Examples of secondary batteries include lithium secondary batteries, nickel-cadmium batteries, nickel-hydrogen batteries, etc. Among them, lithium secondary batteries have been actively developed and applied because of their high operating voltage and high energy density per unit weight, as well as their advantages in terms of charging speed and weight reduction.

[0003] The lithium secondary battery may include an electrode assembly including a positive electrode, a negative electrode, and a separator, and an electrolyte impregnated in the electrode assembly. The lithium secondary battery may further include, for example, a pouch-shaped exterior material that contains the electrode assembly and the electrolyte.

[0004] The positive electrode active material of the lithium secondary battery may be a lithium composite oxide, which may further contain a transition metal such as nickel, cobalt, or manganese.

[0005] The lithium composite oxide as the positive electrode active material can be produced by reacting a lithium precursor with a nickel-cobalt-manganese (NCM) precursor containing nickel, cobalt and manganese.

[0006] The use of the high-cost valuable metals in the positive electrode active material accounts for more than 20% of the manufacturing cost. In addition, in recent years, as interest in environmental protection has increased, research into methods for recycling positive electrode active materials has been progressing. In order to recycle the positive electrode active material, it is necessary to regenerate the lithium precursor from the waste positive electrode with high efficiency and high purity.

[0007] For example, Korean Patent Publication No. 2015-0002963 discloses a method for recovering lithium using a wet method. However, since cobalt, nickel, etc. are extracted and lithium is recovered from the remaining waste liquid by wet extraction, the recovery rate may be excessively low and a large amount of impurities may be generated from the waste liquid. Summary of the Invention [Problem to be solved by the invention]

[0008] An object of the present invention is to provide a method for recovering a lithium precursor from a positive electrode active material mixture with high purity, high yield and high efficiency. [Means for solving the problem]

[0009] A method for recovering a lithium precursor according to an exemplary embodiment of the present invention includes the steps of preparing a cathode active material mixture including a lithium composite oxide, reacting the cathode active material mixture with a carbon-based solid material under an inert gas atmosphere to form a pre-precursor mixture including a lithium oxide, and washing the pre-precursor mixture with water to separate the lithium precursor.

[0010] In an exemplary embodiment, the step of forming the pre-precursor mixture may be performed at a temperature of 740° C. or greater.

[0011] In an exemplary embodiment, the step of forming the pre-precursor mixture may be performed at a temperature between 840°C and 1,200°C.

[0012] In an exemplary embodiment, in forming the pre-precursor mixture, up to 1 / 10th the weight of lithium carbonate relative to lithium oxide may be produced.

[0013] In an exemplary embodiment, the carbon-based solid material can include at least one selected from the group consisting of carbon black, activated carbon, carbon fiber, carbon nanotubes, graphene, natural graphite, artificial graphite, hard carbon, and coke.

[0014] In an exemplary embodiment, the inert gas may include argon or nitrogen.

[0015] In an exemplary embodiment, forming the pre-precursor mixture may include dry mixing the positive electrode active material mixture and the carbon-based solid material.

[0016] In an exemplary embodiment, the dry mixing may be carried out by a fluidized bed reactor.

[0017] In an exemplary embodiment, the step of forming the preliminary precursor mixture may involve reacting the positive electrode active material mixture with the carbonaceous solid material in a weight ratio of 4:1 to 9:1.

[0018] In an exemplary embodiment, the water washing process can include converting at least a portion of the lithium oxide to lithium hydroxide.

[0019] In an exemplary embodiment, the pre-precursor mixture further comprises a transition metal-containing compound, and the water washing process produces an aqueous lithium hydroxide solution and the transition metal-containing compound can precipitate.

[0020] In an exemplary embodiment, the water washing process may be carried out in a carbon dioxide-free (CO2-free) atmosphere.

[0021] In an exemplary embodiment, the lithium composite oxide may be represented by Formula 1 below.

[0022] [ka]

[0023] In Chemical Formula 1, M is selected from the group consisting of Mn, Na, Mg, Ca, Ti, V, Cr, Cu, Zn, Ge, Sr, Ag, Ba, Zr, Nb, Mo, Al, Ga, and B; <x≦1.1、2≦y≦2.02、0.5≦a≦1、0≦b≦0.5であってもよい。

[0024] In an exemplary embodiment, the positive electrode active material mixture can be obtained from spent lithium secondary batteries.

[0025] In an exemplary embodiment, the step of preparing the positive electrode active material mixture may include a step of separating a positive electrode, which includes a positive electrode current collector, a positive electrode active material, a binder, and a conductive material, from the used lithium secondary batteries, and a step of crushing or treating the separated positive electrode with an organic solvent to remove the positive electrode current collector.

[0026] In an exemplary embodiment, the inert gas atmosphere may be free of oxidizing and reducing gases. Effect of the Invention

[0027] According to an exemplary embodiment of the present invention, a high-purity lithium precursor can be obtained in high yield and efficiency by reacting a positive electrode active material mixture with a carbon-based solid material under an inert gas atmosphere.

[0028] The reaction of the positive electrode active material with the carbonaceous solid material produces lithium oxide, which may not agglomerate under the temperature conditions of the reaction, allowing efficient isolation of the lithium precursor without an additional grinding step. [Brief description of the drawings]

[0029] [Figure 1]FIG. 1 is a schematic flow chart illustrating a method for regenerating a lithium precursor according to an exemplary embodiment. [Diagram 2] FIG. 2 is an X-ray diffraction (XRD) graph to confirm the formation of lithium oxide according to an exemplary embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] In an exemplary embodiment of the present invention, a method for recovering a lithium precursor is provided, which comprises reacting a positive electrode active material mixture containing a lithium composite oxide with a carbonaceous solid material under an inert gas atmosphere and washing the mixture with water, thereby recovering the lithium precursor with high yield and high efficiency.

[0031] Hereinafter, embodiments of the present invention will be described in more detail with reference to the drawings. However, these embodiments are merely illustrative of the present invention and are not intended to limit the present invention.

[0032] As used herein, the term "precursor" is used to refer collectively to a compound containing a specific metal to provide the specific metal contained in the electrode active material.

[0033] FIG. 1 is a schematic flow chart illustrating a method for regenerating a lithium precursor according to an exemplary embodiment.

[0034] As shown in FIG. 1, a positive electrode active material mixture containing a lithium composite oxide can be prepared (e.g., step S10). The positive electrode active material mixture can include a lithium-containing compound obtained or regenerated from an electric element or a chemical element. The positive electrode active material mixture can further include various lithium-containing compounds, such as lithium oxide, lithium carbonate, and lithium hydroxide, as non-limiting examples.

[0035] According to an exemplary embodiment, the positive electrode active material mixture may be obtained from a used lithium secondary battery. The used lithium secondary battery may include a lithium secondary battery that is substantially unable to be reused (charged or discharged), for example, a lithium secondary battery whose life span has been exhausted and whose charge / discharge efficiency has been significantly reduced, or a lithium secondary battery that has been destroyed by impact or chemical reaction.

[0036] The waste lithium secondary battery may include an electrode assembly including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, and the positive electrode and the negative electrode may include a positive electrode active material layer and a negative electrode active material layer coated on a positive electrode current collector and a negative electrode current collector, respectively.

[0037] For example, the positive electrode active material included in the positive electrode active material layer may include an oxide containing lithium and a transition metal.

[0038] In some embodiments, the positive electrode active material may be an NCM-based lithium oxide containing nickel, cobalt, and manganese. The NCM-based lithium oxide as the positive electrode active material may be prepared by reacting a lithium precursor and an NCM precursor (e.g., an NCM oxide) with each other, for example, by a co-precipitation reaction.

[0039] However, the embodiments of the present invention can be applied not only to the cathode material containing the NCM-based lithium oxide, but also to any lithium-containing cathode material.

[0040] As a result, according to an embodiment of the present invention, a method for regenerating lithium oxide (Li2O) or lithium hydroxide (LiOH) as a lithium precursor with high selectivity can be provided.

[0041] For example, the positive electrode can be separated from the used lithium secondary battery to recover the used positive electrode. The positive electrode includes a positive electrode current collector (e.g., aluminum (Al)) and a positive electrode active material layer as described above, and the positive electrode active material layer may include a conductive material and a binder in addition to the positive electrode active material described above.

[0042] The conductive material may include, for example, a carbon-based material such as graphite, carbon black, graphene, carbon nanotubes, etc. The binder may include, for example, a resin material such as vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethylmethacrylate, etc.

[0043] The positive electrode active material mixture can be prepared from the recovered positive electrode. In some embodiments, the positive electrode active material mixture can be produced in powder form by a physical method such as a grinding process. The positive electrode active material mixture can include a lithium-transition metal oxide powder as described above, for example, an NCM-based lithium oxide powder (e.g., Li(NCM)O2).

[0044] In some embodiments, the recovered positive electrode may be heat-treated before the pulverization treatment. This can promote detachment of the positive electrode current collector during the pulverization treatment, and can at least partially remove the binder and conductive material. The temperature of the heat treatment may be, for example, about 100 to 500°C, preferably about 350 to 450°C.

[0045] In some embodiments, the positive electrode active material mixture can be obtained after immersing the recovered positive electrode in an organic solvent, for example, by immersing the recovered positive electrode in an organic solvent to separate and remove the positive electrode current collector, and selectively extracting the positive electrode active material by centrifugation.

[0046] Through the above process, the positive electrode current collector components, such as aluminum, are substantially completely separated and removed, and the positive electrode active material mixture in which the content of carbonaceous components derived from the conductive material and binder is removed or reduced can be obtained.

[0047] For example, the lithium composite oxide may include an oxide containing lithium and a transition metal, such as nickel, cobalt, or manganese.

[0048] In some embodiments, the lithium composite oxide can be represented by Formula 1 below.

[0049] [ka]

[0050] In Chemical Formula 1, M is selected from the group consisting of Mn, Na, Mg, Ca, Ti, V, Cr, Cu, Zn, Ge, Sr, Ag, Ba, Zr, Nb, Mo, Al, Ga, and B; <x≦1.1、2≦y≦2.02、0.5≦a≦1、0≦b≦0.5であってもよい。

[0051] According to an exemplary embodiment, a lithium composite oxide having a Ni content of 0.5 molar ratio or more can be effectively converted to lithium oxide.

[0052] The positive electrode active material mixture may be reacted with a carbon-based solid material under an inert gas atmosphere to form a pre-precursor mixture (e.g., step S20). The pre-precursor mixture may include lithium oxide.

[0053] The positive electrode active material mixture and the carbon-based solid material may react at a temperature of 740° C. or more. In this temperature range, the lithium composite oxide contained in the positive electrode active material mixture may be converted to lithium oxide. For example, if the reaction temperature is less than 740° C., lithium oxide may not be formed, and lithium carbonate may be formed.

[0054] In an exemplary embodiment, the positive electrode active material mixture and the carbonaceous solid material may be reacted at a temperature of 740° C. or more. In this case, the amount of lithium carbonate produced by the reaction may be 1 / 10 or less of the weight of the lithium oxide. This may increase the lithium recovery yield of the process. Preferably, the reaction may be carried out at a temperature of 840° C. or more. In this case, substantially no lithium carbonate may be produced. In this specification, "substantially no production" may mean that lithium carbonate is formed in an amount of 1 part by weight or less per 100 parts by weight of lithium oxide.

[0055] In some embodiments, the reaction temperature between the positive electrode active material mixture and the carbon-based solid material may be 1,200° C. or less. If the reaction temperature exceeds 1,200° C., the positive electrode active material mixture, the transition metal-containing mixture, the lithium oxide, etc. may react with each other to form by-products. As a result, the purity and yield of the lithium precursor may decrease.

[0056] In an exemplary embodiment, the carbon-based solid material may include a crystalline or amorphous carbon material. For example, the carbon-based solid material may include at least one selected from the group consisting of carbon black, activated carbon, carbon fiber, carbon nanotubes, graphene, natural graphite, artificial graphite, hard carbon, and coke. Preferably, carbon black or activated carbon can effectively react with the positive electrode active material mixture. The carbon-based solid material may be oxidized when reacting with the lithium composite oxide, and may promote decomposition of the lithium composite oxide.

[0057] In an exemplary embodiment, the inert gas may include argon or nitrogen. For example, the inside of a reactor in which the positive electrode active material mixture and the carbon-based solid material react may be purged with the inert gas. Thus, the inside of the reactor may be formed into an inert gas atmosphere. For example, the purging may include purging.

[0058] In some embodiments, the inert gas atmosphere may not include an oxidizing gas or a reducing gas. For example, the inside of the reactor may include an atmosphere filled only with the inert gas. This can suppress the formation of by-products, such as lithium carbonate formed by the reaction of carbon dioxide gas, which is a reducing gas, with the lithium component.

[0059] For example, the oxidizing gas may include oxygen gas, and the reducing gas may include hydrogen gas, carbon monoxide gas, carbon dioxide gas, and the like.

[0060] In an exemplary embodiment, the positive electrode active material mixture and the carbon-based solid material may be dry mixed. For example, no liquid material such as a solvent may be added to the reactor. The positive electrode active material mixture and the carbon-based solid material may be stirred in the reactor.

[0061] In an exemplary embodiment, the reactor may include a fluidized bed reactor. For example, the dry mixing may be performed in a fluidized bed reactor. The positive electrode active material mixture and the carbon-based solid material may be introduced into the fluidized bed reactor and reacted in the fluidized bed reactor.

[0062] For example, the inert gas may be injected into the lower portion of the fluidized bed reactor and passed through the bottom of the positive active material mixture, forming a cyclone at the lower portion of the fluidized bed reactor and effectively mixing the positive active material mixture and the carbon-based solid material.

[0063] In an exemplary embodiment, the positive electrode active material mixture and the carbon-based solid material may be mixed in a weight ratio of 4:1 to 9:1. If the amount of the positive electrode active material mixture used is less than 4:1, the yield of lithium oxide may be reduced. If the amount of the positive electrode active material mixture used is more than 9:1, the conversion of the positive electrode active material mixture to lithium oxide may be insufficient. Preferably, the positive electrode active material mixture and the carbon-based solid material may be mixed in a weight ratio of 5:1 to 9:1.

[0064] In an exemplary embodiment, the preliminary precursor mixture can further include a transition metal-containing mixture. The transition metal-containing mixture can include a transition metal, a transition metal-containing oxide, etc. The transition metal can include nickel, cobalt, manganese, etc.

[0065] The transition metal component of the transition metal-containing mixture may be derived from the lithium composite oxide. For example, the transition metal component may be separated in a reaction in which the lithium composite oxide is converted to lithium oxide to form the transition metal-containing mixture. In this case, the lithium composite oxide may be decomposed to form lithium oxide and the transition metal-containing mixture.

[0066] The pre-precursor mixture may be washed with water (e.g., step S30). The washing with water may separate the lithium oxide in the pre-precursor mixture and provide it as a lithium precursor.

[0067] In an exemplary embodiment, the water washing process can dissolve at least a portion of the lithium oxide in water and convert it to lithium hydroxide, e.g., lithium hydroxide is water soluble and an aqueous lithium hydroxide solution can be produced.

[0068] In this case, lithium oxide can be selectively separated from the preliminary precursor mixture. Components other than lithium oxide in the preliminary precursor mixture can be precipitated at the bottom of the aqueous solution (the bottom of the reactor). For example, the transition metal-containing mixture can be precipitated.

[0069] The transition metal-containing mixture can be separated by filtration to obtain a lithium precursor containing high purity lithium hydroxide.

[0070] For example, the aqueous lithium hydroxide solution can be separated and the water evaporated or crystallized by recrystallization, fractional crystallization, etc. to recover the lithium precursor in the form of lithium hydroxide or lithium oxide.

[0071] In some embodiments, the precipitated transition metal-containing mixture can be treated with an acid solution to form a precursor of each transition metal in the form of an acid salt. In one embodiment, sulfuric acid can be used as the acid solution. In this case, NiSO4, MnSO4, and CoSO4 can be recovered as the transition metal precursors.

[0072] In some embodiments, the water washing process can be performed under conditions where carbon dioxide (CO2) is excluded. For example, the water washing process can be performed in a CO2-free atmosphere (e.g., an air atmosphere from which CO2 has been removed), thereby preventing regeneration of lithium carbonate.

[0073] In one embodiment, the water provided during the water rinsing process can be purged with a CO2-depleted gas (eg, nitrogen purging) to provide a CO2-free atmosphere.

[0074] In the comparative example, when the lithium composite oxide is reduced with hydrogen, lithium hydroxide may be formed. The melting point of lithium hydroxide is 462°C, and the formed lithium hydroxide may be partially melted under the temperature condition of the hydrogen reduction treatment (450 to 700°C). Therefore, the lithium hydroxides may aggregate with each other or with the transition metal-containing mixture during the cooling process after the hydrogen reduction treatment. In this case, it is necessary to pulverize the aggregated lithium hydroxide in order to effectively separate the lithium hydroxide.

[0075] According to an exemplary embodiment, the lithium component of the lithium composite oxide can be converted to lithium oxide. The melting point of lithium oxide is about 1,438° C., and the lithium composite oxide and the carbon-based solid material can react at a temperature below the melting point of lithium oxide. This allows the lithium oxide to be efficiently separated without agglomeration and without an additional grinding process.

[0076] Hereinafter, experimental examples including specific examples and comparative examples will be presented to aid in understanding the present invention, but these experimental examples are merely illustrative of the present invention and do not limit the scope of the appended claims. It is clear to those skilled in the art that various changes and modifications can be made to these examples within the scope of the scope and technical ideas of the present invention, and it is natural that these changes and modifications fall within the scope of the appended claims.

[0077] Experimental Example 1 After separating the positive electrode from the waste lithium secondary battery, the current collector in the positive electrode was removed to prepare a positive electrode active material mixture.

[0078] The positive electrode has a composition of about LiNi 0.8 Co 0.1 Mn 0.1 The positive electrode active material layer was formed by using a positive electrode active material of O2, a conductive material of Denka Black, and a PVDF binder in a weight ratio of 92:5:3.

[0079] FIG. 2 shows the results of X-ray diffraction spectroscopy (XRD) of the positive electrode active material mixture at room temperature (30° C.).

[0080] The positive electrode active material mixture (25 g) and carbon black (5 g) with a particle size of about 0.5 μm were added to a reactor purged with argon gas, and reacted at temperatures of 500 to 900°C for 60 minutes each while stirring. The results of XRD analysis (X-Ray Diffraction Spectroscopy) of the samples reacted at each temperature are shown in Figure 2. As shown in Figure 2, lithium oxide began to be observed from 740°C.

[0081] Experimental Example 2 After separating the positive electrode from the waste lithium secondary battery, the current collector in the positive electrode was removed to prepare a positive electrode active material mixture.

[0082] The positive electrode has a composition of about LiNi 0.6 Co 0.2 Mn 0.2 The cathode active material layer was formed by mixing the cathode active material of O2, the conductive material of Denka Black, and the PVDF binder in a weight ratio of 92:5:3. The cathode active material mixture (25 g) and carbon black (3 g) with a particle size of about 0.5 μm were added and heated to 600°C and 900°C while stirring.

[0083] Samples were extracted in which the positive electrode active material mixture and carbon black were reacted at temperatures of 600° C. and 900° C., respectively. The content of lithium compounds in the samples was determined by XRD analysis and crystal structure analysis using the Rietveld method, and the fractions of each material phase were calculated. The fractions are shown in Table 1 below.

[0084] [Table 1]

[0085] As shown in Table 1, it was confirmed that Li2CO3 substance was produced at 600°C, but only Li2O substance was produced at 900°C.

Claims

1. A method for producing a positive electrode active material mixture comprising: preparing a positive electrode active material mixture comprising a lithium composite oxide containing nickel, cobalt, and manganese; reacting the cathode active material mixture with a carbon-based solid material under an inert gas atmosphere to form a pre-precursor mixture including lithium oxide; and washing the pre-precursor mixture with water to separate the lithium precursor.

11. A method for recovering a lithium precursor, wherein the step of forming a pre-precursor mixture is carried out at 840° C. to 1,200° C., and the inert gas atmosphere is free of reducing gases.

2. 2. The method for recovering a lithium precursor according to claim 1, wherein in the step of forming the preliminary precursor mixture, lithium carbonate is produced in an amount equal to or less than 1 / 10 by weight of lithium oxide.

3. 2. The method for recovering a lithium precursor according to claim 1, wherein the carbon-based solid material comprises at least one selected from the group consisting of carbon black, activated carbon, carbon fiber, carbon nanotubes, graphene, natural graphite, artificial graphite, hard carbon, and coke.

4. 2. The method for recovering lithium precursor according to claim 1, wherein the inert gas comprises argon or nitrogen.

5. 2. The method of claim 1, wherein the step of forming a preliminary precursor mixture comprises dry mixing the positive electrode active material mixture and the carbon-based solid material.

6. The method for recovering lithium precursor according to claim 5, wherein the dry mixing is carried out by a fluidized bed reactor.

7. 2. The method for recovering a lithium precursor according to claim 1, wherein the step of forming a preliminary precursor mixture comprises reacting the positive electrode active material mixture with the carbon-based solid material in a weight ratio of 4:1 to 9:

1.

8. 2. The method for recovering a lithium precursor according to claim 1, wherein the water washing treatment comprises converting at least a portion of the lithium oxide to lithium hydroxide.

9. The pre-precursor mixture further comprises a transition metal-containing mixture; The method for recovering a lithium precursor according to claim 1 , wherein the water washing treatment produces an aqueous lithium hydroxide solution, and the transition metal-containing mixture precipitates.

10. The washing process is carried out in a carbon dioxide-free (CO 2 2. The method for recovering a lithium precursor according to claim 1, wherein the method is carried out in a nitrogen atmosphere (N-free atmosphere).

11. The method for recovering a lithium precursor according to claim 1 , wherein the lithium composite oxide is represented by the following chemical formula 1: 【Chemistry 1】 (In Chemical Formula 1, M is selected from the group consisting of Mn, Na, Mg, Ca, Ti, V, Cr, Cu, Zn, Ge, Sr, Ag, Ba, Zr, Nb, Mo, Al, Ga, and B, and 0<x≦1.1, 2≦y≦2.02, 0.5≦a≦1, and 0≦b≦0.5.)

12. The method for recovering lithium precursors according to claim 1 , wherein the positive electrode active material mixture is obtained from waste lithium secondary batteries.

13. The step of preparing the positive electrode active material mixture includes the steps of separating a positive electrode from the waste lithium secondary battery, the positive electrode including a positive electrode current collector, a positive electrode active material, a binder and a conductive material; and removing the positive electrode current collector by crushing or treating the separated positive electrode with an organic solvent.

14. 2. The method for recovering a lithium precursor according to claim 1, wherein the inert gas atmosphere does not contain an oxidizing gas.

Citation Information

Patent Citations

  • Method for recovering lithium and cobalt from lithium cobaltate

    JP2004011010A

  • Method for recovering lithium

    JP2011094227A

  • Method for recovering lithium

    JP2011094228A

  • Method of regenerating lithium precursor from used lithium secondary battery

    KR101897134B1

  • Method of recycling active metal of lithium secondary battery

    KR102020238B1