Method for manufacturing laminate and image display panel

The laminate structure with controlled thickness and peeling forces addresses the poor workability of thin polarizing plates with retardation layers, enhancing manufacturing efficiency and yield in image display devices.

JP7566663B2Active Publication Date: 2024-10-15NITTO DENKO CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021028303
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-25
Publication Date
2024-10-15
Estimated Expiration
2041-02-25

AI Technical Summary

Technical Problem

Existing image display devices face challenges with poor workability during the manufacturing process due to the bonding of thin polarizing plates with retardation layers, which are desired for flexibility and thinness.

Method used

A laminate structure is developed comprising a surface protection film, polarizing plate with a retardation layer, adhesive layer, and release film, with specific thickness and peeling force requirements to enhance workability, including a polarizing plate thickness of 70 μm or less and a release film thickness of 40 μm or more, ensuring a controlled peeling force ratio.

Benefits of technology

The laminate structure significantly improves the workability in the manufacturing process of image display panels by ensuring easy and controlled peeling, reducing defects and enhancing the manufacturing yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566663000003
    Figure 0007566663000003
  • Figure 0007566663000004
    Figure 0007566663000004
  • Figure 0007566663000005
    Figure 0007566663000005
Patent Text Reader

Abstract

To provide a laminate including a polarizing plate having a thin-type retardation layer, the laminate excellent in workability at a manufacturing process of an image display panel.SOLUTION: A laminate includes a surface protective film, a polarizing plate having a polarizer and a protective layer, a retardation layer, an adhesive layer and a release film in this order. A thickness of a laminated part from the polarizing plate to the adhesive layer is 70 μm or less. A thickness of the release film is 40 μm or more. A peel force Fr of the release film against the adhesive layer is 0.04 N / 25 mm or less. A peel force Fp of the surface protective film against the polarizing plate is larger than the Fr and at most 0.1 N / 25 mm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a laminate and an image display panel. [Background technology]

[0002] Image display devices, such as liquid crystal display devices and electroluminescence (EL) display devices (e.g., organic EL display devices, inorganic EL display devices), are rapidly becoming widespread. A polarizing plate and a retardation plate are typically used in the image display panel mounted on the image display device. In practice, a retardation layer-attached polarizing plate in which a polarizing plate and a retardation plate are integrated is widely used (e.g., Patent Document 1). In recent years, there has been a strong demand for thinner image display devices. In addition, the possibility of curving, bending, folding, and rolling up image display devices has been studied. As a retardation layer-attached polarizing plate used in such image display devices, a thin retardation layer-attached polarizing plate is demanded. However, when such a retardation layer-attached polarizing plate is attached to the image display panel body, the workability may be poor. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 3325560 Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention has been made to solve the above-mentioned problems in the conventional art, and a main object of the present invention is to provide a laminate including a thin polarizing plate with a retardation layer, which has excellent workability in the manufacturing process of an image display panel. [Means for solving the problem]

[0005] According to an embodiment of the present invention, there is provided a laminate comprising a surface protective film, a polarizing plate including a polarizer and a protective layer, a retardation layer, a pressure-sensitive adhesive layer, and a release film in this order, wherein the thickness of a laminated portion from the polarizing plate to the pressure-sensitive adhesive layer is 70 μm or less, the thickness of the release film is 40 μm or more, the peeling force Fr of the release film to the pressure-sensitive adhesive layer is 0.04 N / 25 mm or less, and the peeling force Fp of the surface protective film to the polarizing plate is greater than Fr and is 0.1 N / 25 mm or less. In one embodiment, the surface protective film has a thickness of 60 μm or more. In one embodiment, the thickness of the surface protection film is greater than the thickness of the laminated portion. In one embodiment, in the polarizing plate, a protective layer is arranged only on the side of the polarizer on which the retardation layer is not arranged. In one embodiment, the polarizer has a thickness of 8 μm or less. In one embodiment, the retardation layer is a layer in which a liquid crystal compound is aligned and fixed. In one embodiment, the laminate has a warpage of 5% or less. According to another embodiment of the present invention, there is provided a method for manufacturing an image display panel, the method including, in this order, preparing the laminate, bonding the laminate with the release film peeled off from the pressure-sensitive adhesive layer to an image display panel body, and peeling off the surface protective film from the polarizing plate. Effect of the Invention

[0006] According to the embodiment of the present invention, by using a laminate having a surface protective film and a release film that satisfy a predetermined peel strength for a retardation layer-attached polarizing plate, the workability in the manufacturing process of an image display panel can be significantly improved. [Brief description of the drawings]

[0007] [Figure 1]FIG. 1 is a schematic cross-sectional view showing an outline of the configuration of a laminate according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing an example of a warped state of a laminate precursor. [Figure 3A] 1A to 1C are diagrams illustrating an example of a manufacturing process for a composite substrate according to one embodiment. [Figure 3B] This is a continuation of Figure 3A. [Figure 3C] This is a continuation of Figure 3B. [Figure 3D] This is a continuation of Figure 3C. [Figure 3E] This is a continuation of Figure 3D. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.

[0009] (Definition of terms and symbols) The definitions of terms and symbols used in this specification are as follows. (1) Refractive index (nx, ny, nz) "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the direction perpendicular to the slow axis in the plane (i.e., the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-plane phase difference (Re) "Re(λ)" is the in-plane retardation measured with light of wavelength λ nm at 23° C. For example, "Re(550)" is the in-plane retardation measured with light of wavelength 550 nm at 23° C. Re(λ) is calculated by the formula: Re(λ)=(nx-ny)×d, where d(nm) is the thickness of the layer (film). (3) Retardation in the thickness direction (Rth) "Rth(λ)" is the retardation in the thickness direction measured with light of wavelength λ nm at 23° C. For example, "Rth(550)" is the retardation in the thickness direction measured with light of wavelength 550 nm at 23° C. Rth(λ) is calculated by the formula: Rth(λ)=(nx-nz)×d, where d(nm) is the thickness of the layer (film). (4) Nz coefficient The Nz coefficient is calculated by Nz=Rth / Re. (5)Angle When angles are referred to herein, the angles include both clockwise and counterclockwise angles relative to a reference direction, so for example, "45°" means ±45°.

[0010] A. Laminate 1 is a schematic cross-sectional view showing an outline of the structure of a laminate according to one embodiment of the present invention. The laminate 100 has, in this order, a surface protective film 30, a polarizing plate 10, a retardation layer 20, a pressure-sensitive adhesive layer 40, and a release film (separator) 50. The retardation layer-attached polarizing plate obtained from the laminate 100 is typically arranged so that the polarizing plate 10 is closer to the viewing side than the retardation layer 20.

[0011] The surface protective film 30 includes a substrate 31 and an adhesive layer 32 formed on one side of the substrate 31, and is peelably attached to the polarizing plate 10. The retardation layer 20 has a laminated structure including a first retardation layer 21 and a second retardation layer 22. In the illustrated example, the polarizing plate 10 includes a polarizer 11 and a protective layer 12 arranged on the viewing side (the side on which the retardation layer 20 is not arranged) of the polarizer 11, and no protective layer is arranged between the polarizer 11 and the retardation layer 20. According to such a form, for example, the thickness of the retardation layer-attached polarizing plate and the thickness of the polarizing plate described later can be satisfactorily achieved. The release film 50 is peelably attached to the adhesive layer 40, and can protect the adhesive layer 40. By using the release film 50, for example, the laminate 100 can be formed into a roll.

[0012] Although not shown, a protective layer may be further included on the other side of the polarizer 11 (between the polarizer 11 and the retardation layer 20). Unlike the illustrated example, the retardation layer 20 may be a single layer or may have a laminated structure of three or more layers.

[0013] Although not shown, the laminate may further have other functional layers. The type, characteristics, number, combination, arrangement, etc. of the functional layers that the laminate may have can be appropriately set according to the purpose. For example, the laminate may further have a conductive layer or a conductive layer-attached isotropic substrate. The conductive layer or the conductive layer-attached isotropic substrate is typically arranged between the retardation layer 20 and the adhesive layer 40. Note that a laminate (polarizing plate with retardation layer) having a conductive layer or a conductive layer-attached isotropic substrate is applied to, for example, an image display device in which a touch sensor is incorporated inside the image display panel. As another example, the laminate may further have other retardation layers. The optical characteristics (e.g., refractive index characteristics, in-plane retardation, Nz coefficient, photoelastic coefficient), thickness, arrangement, etc. of the other retardation layers can be appropriately set according to the purpose. As a specific example, the polarizing plate 10 may be provided on the viewing side of the polarizer 11 with other retardation layers (typically, a layer that imparts an (elliptical) polarization function, a layer that imparts an ultra-high retardation) that improve visibility when viewed through polarized sunglasses. By having such layers, excellent visibility can be achieved even when the display screen is viewed through polarized lenses such as polarized sunglasses. Therefore, the obtained polarizing plate with a retardation layer can be suitably applied to image display devices that can be used outdoors.

[0014] Each member constituting the laminate may be laminated via any suitable adhesive layer (not shown). Specific examples of the adhesive layer include an adhesive layer and a pressure-sensitive adhesive layer. For example, the retardation layer 20 is bonded to the polarizing plate 10 via an adhesive layer (preferably using an active energy ray curable adhesive). When the retardation layer 20 has a laminated structure of two or more layers as in the illustrated example, each retardation layer is bonded via an adhesive layer (preferably using an active energy ray curable adhesive).

[0015] The thickness of the laminated portion from the polarizing plate 10 to the adhesive layer 40 (sometimes simply referred to as the "thickness of the retardation layer-attached polarizing plate") is 70 μm or less, preferably 60 μm or less, and more preferably 50 μm or less. On the other hand, the thickness of the retardation layer-attached polarizing plate is, for example, 25 μm or more. The thickness of the retardation layer-attached polarizing plate includes the thickness of the adhesive layer.

[0016] A-1. Polarizing plate The polarizing plate includes a polarizer and a protective layer. The thickness of the polarizing plate depends on the number of protective layers included, but is preferably 20 μm or more, more preferably 25 μm or more. On the other hand, the thickness of the polarizing plate is preferably 40 μm or less, more preferably 36 μm or less, and even more preferably 33 μm or less. Note that the thickness of the polarizing plate does not include the thickness of an adhesive layer (for example, an adhesive layer) used when laminating the polarizer and the protective layer.

[0017] The polarizer is typically a resin film containing a dichroic substance (e.g., iodine). Examples of the resin film include hydrophilic polymer films such as polyvinyl alcohol (PVA) films, partially formalized PVA films, and partially saponified ethylene-vinyl acetate copolymer films.

[0018] The thickness of the polarizer is preferably 15 μm or less, more preferably 12 μm or less, further preferably 10 μm or less, and particularly preferably 8 μm or less, while the thickness of the polarizer is preferably 1 μm or more.

[0019] The polarizer preferably exhibits absorption dichroism at any wavelength of 380 nm to 780 nm. The single transmittance of the polarizer is, for example, 41.5% to 46.0%, preferably 42.0% to 46.0%, and more preferably 44.5% to 46.0%. The degree of polarization of the polarizer is preferably 97.0% or more, more preferably 99.0% or more, and even more preferably 99.9% or more.

[0020] The protective layer may be formed of any suitable film that can be used as a protective layer for a polarizer. Specific examples of materials that are the main components of the film include cellulose-based resins such as triacetyl cellulose (TAC), polyester-based, polyvinyl alcohol-based, polycarbonate-based, polyamide-based, polyimide-based, polyethersulfone-based, polysulfone-based, polystyrene-based, cycloolefin-based such as polynorbornene, polyolefin-based, (meth)acrylic, acetate-based, and other resins.

[0021] The retardation layer-attached polarizing plate obtained by the embodiment of the present invention is typically disposed on the viewing side of an image display device, and the protective layer 12 is disposed on the viewing side. Therefore, the protective layer 12 may be subjected to surface treatment such as hard coat (HC) treatment, anti-reflection treatment, anti-sticking treatment, and anti-glare treatment, as necessary.

[0022] The thickness of the protective layer 12 is preferably 5 μm to 80 μm, more preferably 10 μm to 40 μm, and further preferably 10 μm to 30 μm. When the above-mentioned surface treatment is performed, the thickness of the protective layer 12 includes the thickness of the surface treatment layer.

[0023] In one embodiment, the protective layer (not shown) disposed between the polarizer 11 and the retardation layer 20 is preferably optically isotropic. In this specification, "optically isotropic" means that the in-plane retardation Re(550) is 0 nm to 10 nm, and the retardation Rth(550) in the thickness direction is -10 nm to +10 nm. The thickness of the protective layer disposed between the polarizer 11 and the retardation layer 20 is preferably 5 μm to 80 μm, more preferably 10 μm to 40 μm, and further preferably 10 μm to 30 μm.

[0024] The polarizing plate may be produced by any suitable method. Specifically, the polarizing plate may include a polarizer produced from a single-layer resin film, or may include a polarizer obtained by using a laminate of two or more layers.

[0025] The method for producing a polarizer from the above-mentioned single-layer resin film typically includes subjecting the resin film to a dyeing treatment using a dichroic substance such as iodine or a dichroic dye, and a stretching treatment. As the resin film, as described above, for example, a hydrophilic polymer film such as a polyvinyl alcohol (PVA)-based film, a partially formalized PVA-based film, or an ethylene-vinyl acetate copolymer-based partially saponified film is used. The method may further include an insolubilization treatment, a swelling treatment, a crosslinking treatment, or the like. A polarizing plate can be obtained by laminating a protective layer on at least one side of the obtained polarizer. Such a production method is well known and commonly used in the art, and therefore a detailed description thereof will be omitted.

[0026] Specific examples of polarizers obtained using the laminate of two or more layers include a laminate of a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, or a polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate. A polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate can be produced by, for example, applying a PVA-based resin solution to the resin substrate and drying the resin substrate to form a PVA-based resin layer on the resin substrate to obtain a laminate of the resin substrate and the PVA-based resin layer; and stretching and dyeing the laminate to make the PVA-based resin layer into a polarizer. In this embodiment, a polyvinyl alcohol-based resin layer containing a halide and a polyvinyl alcohol-based resin is preferably formed on one side of the resin substrate. The stretching typically includes immersing the laminate in an aqueous boric acid solution to stretch it. Furthermore, the stretching may further include, as necessary, stretching the laminate in air at a high temperature (for example, 95°C or higher) before stretching in the aqueous boric acid solution. In addition, in this embodiment, the laminate is preferably subjected to a drying shrinkage treatment in which the laminate is heated while being transported in the longitudinal direction to shrink the laminate by 2% or more in the width direction. Typically, the manufacturing method of this embodiment includes subjecting the laminate to an air-assisted stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment in this order. By introducing the auxiliary stretching, even when PVA is applied onto a thermoplastic resin, it is possible to increase the crystallinity of the PVA, and to achieve high optical properties. In addition, by simultaneously increasing the orientation of the PVA in advance, problems such as a decrease in the orientation of the PVA or dissolution when immersed in water in the subsequent dyeing and stretching steps can be prevented, and high optical properties can be achieved. Furthermore, when the PVA-based resin layer is immersed in a liquid, the orientation of the polyvinyl alcohol molecules can be disturbed and the orientation can be reduced, compared to when the PVA-based resin layer does not contain a halide. This can improve the optical properties of a polarizer obtained by immersing the laminate in a liquid through a treatment process such as a dyeing treatment and an underwater stretching treatment. Furthermore, the optical properties can be improved by shrinking the laminate in the width direction through a drying shrinkage treatment.The obtained resin substrate / polarizer laminate may be used as it is (i.e., the resin substrate may be used as a protective layer for the polarizer), or any suitable protective layer may be laminated on the peeled surface of the resin substrate / polarizer laminate after peeling the resin substrate from the resin substrate / polarizer laminate, or on the surface opposite to the peeled surface, depending on the purpose. Details of the method for producing such a polarizer are described in, for example, JP2012-73580A and JP6470455A. The entire disclosures of these publications are incorporated herein by reference.

[0027] A-2. Retardation layer The thickness of the retardation layer depends on its structure (whether it is a single layer or has a laminated structure), but is preferably 10 μm or less, more preferably 8 μm or less, and even more preferably 5 μm or less. On the other hand, the thickness of the retardation layer is, for example, 1 μm or more. In addition, when the retardation layer has a laminated structure, the "thickness of the retardation layer" means the total thickness of each retardation layer. Specifically, the "thickness of the retardation layer" does not include the thickness of an adhesive layer (for example, an adhesive layer).

[0028] As the retardation layer, a liquid crystal compound alignment solidified layer (liquid crystal alignment solidified layer) is preferably used. By using a liquid crystal compound, the difference between nx and ny of the obtained retardation layer can be significantly increased compared to non-liquid crystal materials, so that the thickness of the retardation layer for obtaining a desired in-plane retardation can be significantly reduced. Therefore, a polarizing plate with a retardation layer can be significantly thinned. In this specification, the "alignment solidified layer" refers to a layer in which a liquid crystal compound is aligned in a predetermined direction within the layer and the alignment state is fixed. The "alignment solidified layer" is a concept that includes an alignment hardened layer obtained by hardening a liquid crystal monomer as described later. In the retardation layer, typically, rod-shaped liquid crystal compounds are aligned in the slow axis direction of the retardation layer (homogeneous alignment).

[0029] The liquid crystal alignment solidified layer can be formed by performing an alignment treatment on the surface of a predetermined substrate, applying a coating liquid containing a liquid crystal compound to the surface to align the liquid crystal compound in a direction corresponding to the alignment treatment, and fixing the alignment state. Any appropriate alignment treatment can be adopted as the alignment treatment. Specifically, mechanical alignment treatment, physical alignment treatment, and chemical alignment treatment can be mentioned. Specific examples of mechanical alignment treatment include rubbing treatment and stretching treatment. Specific examples of physical alignment treatment include magnetic field alignment treatment and electric field alignment treatment. Specific examples of chemical alignment treatment include oblique deposition method and photoalignment treatment. As the treatment conditions of various alignment treatments, any appropriate conditions can be adopted depending on the purpose.

[0030] The alignment of the liquid crystal compound is performed by treating the liquid crystal compound at a temperature at which the liquid crystal compound exhibits a liquid crystal phase according to the type of liquid crystal compound. By performing such temperature treatment, the liquid crystal compound takes on a liquid crystal state and is aligned according to the alignment treatment direction of the substrate surface.

[0031] In one embodiment, the alignment state is fixed by cooling the liquid crystal compound aligned as described above. When the liquid crystal compound is a polymerizable monomer or a crosslinkable monomer, the alignment state is fixed by subjecting the liquid crystal compound aligned as described above to a polymerization treatment or a crosslinking treatment.

[0032] Specific examples of the liquid crystal compound and details of the method for forming the alignment solidified layer are described in JP-A-2006-163343, the disclosure of which is incorporated herein by reference.

[0033] As described above, the retardation layer 20 may be a single layer, or may have a laminated structure of two or more layers.

[0034] Unlike the illustrated example, in one embodiment in which the retardation layer 20 is a single layer, the retardation layer 20 can function as a λ / 4 plate. Specifically, the Re(550) of the retardation layer is preferably 100 nm to 180 nm, more preferably 110 nm to 170 nm, and further preferably 110 nm to 160 nm. The thickness of the retardation layer can be adjusted so as to obtain a desired in-plane retardation of the λ / 4 plate. When the retardation layer is the above-mentioned liquid crystal alignment solidified layer, the thickness is, for example, 1.0 μm to 2.5 μm. In this embodiment, the angle between the slow axis of the retardation layer and the absorption axis of the polarizer is preferably 40° to 50°, more preferably 42° to 48°, and further preferably 44° to 46°. In this embodiment, the retardation layer preferably exhibits an inverse dispersion wavelength characteristic in which the retardation value increases according to the wavelength of the measurement light. In this embodiment, the laminate may further include a layer (another retardation layer, not shown) that is disposed between the retardation layer 20 and the pressure-sensitive adhesive layer 40 and exhibits refractive index characteristics of nz>nx=ny.

[0035] In another embodiment in which the retardation layer 20 is a single layer, the retardation layer 20 can function as a λ / 2 plate. Specifically, the Re(550) of the retardation layer is preferably 200 nm to 300 nm, more preferably 230 nm to 290 nm, and further preferably 230 nm to 280 nm. The thickness of the retardation layer can be adjusted so as to obtain a desired in-plane retardation of the λ / 2 plate. When the retardation layer is the above-mentioned liquid crystal alignment solidified layer, the thickness is, for example, 2.0 μm to 4.0 μm. In this embodiment, the angle between the slow axis of the retardation layer and the absorption axis of the polarizer is preferably 10° to 20°, more preferably 12° to 18°, and further preferably 12° to 16°.

[0036] As shown in Fig. 1, when the retardation layer 20 has a laminated structure, the retardation layer 20 has, for example, a two-layer laminated structure in which a first retardation layer (H layer) 21 and a second retardation layer (Q layer) 22 are arranged in order from the polarizer side. The H layer can typically function as a λ / 2 plate, and the Q layer can typically function as a λ / 4 plate. Specifically, Re(550) of the H layer is preferably 200 nm to 300 nm, more preferably 220 nm to 290 nm, and even more preferably 230 nm to 280 nm; Re(550) of the Q layer is preferably 100 nm to 180 nm, more preferably 110 nm to 170 nm, and even more preferably 110 nm to 150 nm. The thickness of the H layer can be adjusted so as to obtain a desired in-plane retardation of the λ / 2 plate. When the H layer is the above-described liquid crystal alignment solidified layer, its thickness is, for example, 2.0 μm to 4.0 μm. The thickness of the Q layer can be adjusted so as to obtain a desired in-plane retardation of the λ / 4 plate. When the Q layer is the above-described liquid crystal alignment solidified layer, its thickness is, for example, 1.0 μm to 2.5 μm. In the present embodiment, the angle formed by the slow axis of the H layer and the absorption axis of the polarizer is preferably 10° to 20°, more preferably 12° to 18°, and even more preferably 12° to 16°; the angle formed by the slow axis of the Q layer and the absorption axis of the polarizer is preferably 70° to 80°, more preferably 72° to 78°, and even more preferably 72° to 76°. When the retardation layer 20 has a laminated structure, each layer (for example, the H layer and the Q layer) may exhibit an inverse dispersion wavelength characteristic in which the retardation value increases according to the wavelength of the measurement light, a positive wavelength dispersion characteristic in which the retardation value decreases according to the wavelength of the measurement light, or a flat wavelength dispersion characteristic in which the retardation value hardly changes depending on the wavelength of the measurement light.

[0037] The retardation layer 20 (each layer when it has a laminated structure) typically exhibits a refractive index characteristic showing a relationship of nx > ny = nz. Note that "ny = nz" includes not only the case where ny and nz are exactly equal but also the case where they are substantially equal. Therefore, within a range that does not impair the effects of the present invention, ny > nz or ny < nz may occur. The Nz coefficient of the retardation layer is preferably 0.9 to 1.5, and more preferably 0.9 to 1.3.

[0038] As described above, the retardation layer is preferably a liquid crystal alignment solidified layer. The liquid crystal compound may be, for example, a liquid crystal compound (nematic liquid crystal) whose liquid crystal phase is a nematic phase. For example, a liquid crystal polymer or a liquid crystal monomer may be used as such a liquid crystal compound. The liquid crystal compound may exhibit liquid crystallinity by either lyotropic or thermotropic mechanism. The liquid crystal polymer and the liquid crystal monomer may be used alone or in combination.

[0039] When the liquid crystal compound is a liquid crystal monomer, the liquid crystal monomer is preferably a polymerizable monomer and a crosslinkable monomer. This is because the liquid crystal monomer can be polymerized or crosslinked (i.e., cured) to fix the alignment state of the liquid crystal monomer. After the liquid crystal monomer is aligned, for example, the liquid crystal monomers can be polymerized or crosslinked with each other to fix the alignment state. Here, a polymer is formed by polymerization, and a three-dimensional network structure is formed by crosslinking, but these are non-liquid crystals. Therefore, the formed retardation layer does not undergo transition to a liquid crystal phase, a glass phase, or a crystalline phase due to temperature changes specific to liquid crystal compounds, for example. As a result, the retardation layer becomes a retardation layer that is not affected by temperature changes and has extremely excellent stability.

[0040] The temperature range in which the liquid crystal monomer exhibits liquid crystallinity varies depending on the type of the liquid crystal monomer. Specifically, the temperature range is preferably 40°C to 120°C, more preferably 50°C to 100°C, and most preferably 60°C to 90°C.

[0041] Any suitable liquid crystal monomer can be used as the liquid crystal monomer. For example, the polymerizable mesogen compounds described in JP-A-2002-533742 (WO00 / 37585), EP358208 (US5211877), EP66137 (US4388453), WO93 / 22397, EP0261712, DE19504224, DE4408171, and GB2280445 can be used. Specific examples of such polymerizable mesogen compounds include BASF's product name LC242, Merck's product name E7, and Wacker-Chem's product name LC-Sillicon-CC3767. As the liquid crystal monomer, a nematic liquid crystal monomer is preferable.

[0042] A-3. Surface protection film The substrate of the surface protection film may be formed of any suitable material. Specific examples of the forming material include polyester-based polymers such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), and polybutylene terephthalate (PBT); cellulose-based polymers such as diacetyl cellulose and triacetyl cellulose; polycarbonate-based polymers; (meth)acrylic polymers such as polymethyl methacrylate; and cycloolefin-based polymers such as polynorbornene. These may be used alone or in combination of two or more.

[0043] The thickness of the substrate of the surface protection film is, for example, 10 μm or more and 100 μm or less, preferably 15 μm or more and 90 μm or less, and more preferably 25 μm or more and 80 μm or less.

[0044] Any suitable structure may be adopted for the adhesive layer of the surface protection film. Specific examples include acrylic adhesives, rubber adhesives, silicone adhesives, polyester adhesives, urethane adhesives, epoxy adhesives, and polyether adhesives. By adjusting the type, number, combination, and compounding ratio of monomers forming the base resin of the adhesive, as well as the compounding amount of the crosslinking agent, reaction temperature, reaction time, and the like, an adhesive having desired properties according to the purpose can be prepared. The base resin of the adhesive may be used alone or in combination of two or more kinds. The base resin is preferably an acrylic resin (specifically, the adhesive layer is preferably composed of an acrylic adhesive). The thickness of the adhesive layer is, for example, 5 μm to 15 μm. The storage modulus of the adhesive layer at 25° C. is, for example, 1.0×10 5 Pa~1.0×10 7 It is Pa.

[0045] The thickness of the surface protective film is, for example, 40 μm or more, preferably 50 μm or more, more preferably 60 μm or more, and even more preferably 70 μm or more. In one embodiment, the thickness of the surface protective film is greater than the thickness of the retardation layer-attached polarizing plate. Such a surface protective film can adequately protect a thin retardation layer-attached polarizing plate from external stress. Specifically, the retardation layer-attached polarizing plate obtained can be prevented from having defects in appearance such as dents due to external stress. In addition, the workability when peeling off the release film from the laminate described later can be further improved. On the other hand, the thickness of the surface protective film is preferably 100 μm or less.

[0046] A-4.Adhesive layer The thickness of the adhesive layer 40 is preferably 10 μm to 20 μm. Details of the adhesive constituting the adhesive layer 40 are the same as those of the adhesive layer contained in the above-mentioned surface protection film.

[0047] A-5. Release film The release film may be made of any suitable plastic film. Specific examples of the plastic film include polyethylene terephthalate (PET) film, polyethylene film, and polypropylene film. The release film may function as a separator. Specifically, a plastic film whose surface is coated with a release agent is preferably used as the release film. Specific examples of the release agent include silicone-based release agents, fluorine-based release agents, and long-chain alkyl acrylate-based release agents.

[0048] The thickness of the release film is 40 μm or more, preferably 45 μm or more. Such a release film can protect a thin retardation layer-attached polarizing plate (particularly, the pressure-sensitive adhesive layer 40) from external stress. Specifically, the resulting retardation layer-attached polarizing plate can be prevented from having defects in appearance such as dents caused by external stress. On the other hand, the thickness of the release film is preferably 80 μm or less.

[0049] A-6.Relationship between peeling forces The peeling force Fp of the surface protective film 30 to the polarizing plate 10 is greater than the peeling force Fr of the release film 50 to the adhesive layer 40. Fr is 0.04 N / 25 mm or less, preferably 0.03 N / 25 mm or less, and more preferably 0.02 N / 25 mm or less. According to such a peeling force relationship, the workability in the manufacturing process of the image display panel described later can be significantly improved. Such an effect can be obtained remarkably when the thickness of the release film is thick. Specifically, a thin retardation layer-attached polarizing plate tends to have low stiffness, and the peelability of a thick (for example, 40 μm or more) release film attached to the thin retardation layer-attached polarizing plate tends to be low. As a result, the workability in the manufacturing process of the image display panel decreases, which may be a factor in reducing the yield. By satisfying the above peeling force relationship, even when a thick release film is attached to a thin retardation layer-attached polarizing plate, the peelability can be excellent. In addition, Fp is 0.1 N / 25 mm or less, preferably 0.07 N / 25 mm or less, and more preferably 0.05 N / 25 mm or less. With such a peeling force, the workability in the manufacturing process of the image display panel can be significantly improved. Specifically, the peeling property of the surface protection film can be excellent.

[0050] The Fr is preferably 0.005 N / 25 mm or more, and preferably 0.01 N / 25 mm or more. The Fp is preferably 0.02 N / 25 mm or more, and preferably 0.03 N / 25 mm or more. Fr can be adjusted, for example, by appropriately selecting the configuration of the pressure-sensitive adhesive layer 40 and the type of the release film 50. Fp can be adjusted, for example, by appropriately selecting the type of the surface protection film 30.

[0051] A-7. Preparation of laminate The laminate 100 can be obtained, for example, by laminating a polarizing plate 10 and a retardation layer 20 to prepare a laminate precursor, and then laminating a surface protective film 30 and a release film 50 on the obtained laminate precursor.

[0052] The polarizing plate 10 and the retardation layer 20 are laminated, for example, while they are being transported by rolls (so-called roll-to-roll). The lamination is typically performed by transferring a liquid crystal alignment solidified layer formed on a substrate. As in the illustrated example, when the retardation layer has a laminated structure, each retardation layer may be laminated (transferred) sequentially onto the polarizing plate, or a laminate of retardation layers may be laminated (transferred) onto the polarizing plate.

[0053] The transfer is performed, for example, by using an active energy ray curable adhesive. The thickness of the active energy ray curable adhesive after curing (thickness of the adhesive layer) is, for example, 0.2 μm to 3.0 μm, preferably 0.4 μm to 2.0 μm, and more preferably 0.6 μm to 1.5 μm. For example, the laminate precursor obtained by laminating the polarizing plate 10 and the retardation layer 20 may be warped due to the adhesive used for laminating the polarizing plate and the retardation layer (specifically, shrinkage during curing of the active energy ray curable adhesive).

[0054] Fig. 2 is a cross-sectional view showing an example of a warped state of a laminate precursor. In Fig. 2, hatching is omitted from the cross section of the laminate precursor to make the drawing easier to see. In the example shown in Fig. 2, a convex warp occurs in the laminate precursor 90 on the polarizing plate 10 side. The warp tends to occur along the absorption axis direction of the polarizing plate 10 (polarizer 11).

[0055] The lamination of the polarizing plate 10 and the retardation layer 20 was performed with a water vapor amount of 10.2 g / m 3 It is preferable that lamination is performed under the following conditions: The amount of water vapor during lamination is more preferably 6.0 g / m 3 ~10.0g / m 3 and more preferably 8.0 g / m 3 ~9.5g / m 3By performing lamination under an environment in which the amount of water vapor is in such a range, for example, the effect of the humidification treatment described below becomes remarkable. Such an amount of water vapor in lamination can be realized, for example, by changing the relative humidity according to the temperature in the range of 18°C ​​to 25°C. For example, when the temperature is 18°C, the amount of water vapor can be realized by setting the relative humidity to 65% RH or less; for example, when the temperature is 20°C, the amount of water vapor can be realized by setting the relative humidity to 55% RH or less; and for example, when the temperature is 23°C, the amount of water vapor can be realized by setting the relative humidity to 45% RH or less. The lower limit of the relative humidity can be, for example, 30% RH.

[0056] As described above, when the laminate further has other functional layers (for example, a conductive layer, other retardation layers), the functional layers can be laminated or formed at predetermined positions by any appropriate method.

[0057] A surface protective film 30 and a release film 50 are laminated on a laminate precursor including at least a polarizing plate 10 and a retardation layer 20. Here, the surface protective film 30 is arranged so that the adhesive layer 32 faces the laminate precursor. The release film 50 is laminated on the laminate precursor via the adhesive layer 40. The laminate thus obtained may have warpage (for example, a convex warpage on the release film 50 side). The warpage of the laminate may affect the workability in the manufacturing process of the image display panel (for example, the workability when peeling off the release film from the laminate described later). The warpage of the laminate is preferably 7% or less, more preferably 5% or less, and even more preferably 3% or less. A method for measuring the warpage (%) will be described later.

[0058] B. Manufacturing method of image display panel Typically, the laminate is used for manufacturing an image display panel. Figures 3A to 3E are diagrams showing an example of a manufacturing process for an image display panel according to one embodiment. In Figures 3A to 3E, the laminated structure of the polarizing plate 10, the retardation layer 20, and the adhesive layer 40 is simply shown as a retardation layer-attached polarizing plate 110.

[0059] FIG. 3A shows a state in which the release film 50 is peeled off from the laminate 100. After the release tape T1 is attached to the bottom surface (release film 50) of the laminate 100 adsorbed to the adsorption plate A, the release tape T1 is pulled in a direction of 180° from the end of the release film 50 (in the direction of the arrow), thereby peeling the release film 50 off from the laminate 100. As described above, the peeling force Fp of the surface protective film 30 against the polarizing plate 10 is greater than the peeling force Fr of the release film 50 against the adhesive layer 40, and Fr is 0.04 N / 25 mm or less. By satisfying such a relationship, the release property of the release film 50 can be excellent. Specifically, when the release film 50 is peeled off from the laminate 100, the retardation layer-attached polarizing plate 110 can be prevented from peeling off from the surface protective film 30.

[0060] Figure 3B shows the state in which the laminate 100 from which the release film 50 has been peeled off is attached to the surface of an image display panel (e.g., an organic EL panel) main body 70 that is adsorbed to an adsorption plate B, and Figure 3C shows the state in which the adsorption plate A has been removed from the laminate 100 after the laminate 100 has been attached to the image display panel main body 70.

[0061] FIG. 3D shows a state in which the surface protective film 30 is peeled off from the laminate 100. After the peeling tape T2 is attached to the top surface (surface protective film 30) of the laminate 100 bonded to the surface of the image display panel main body 70, the peeling tape T2 is pulled in a direction of 180° from the end of the surface protective film 30 (in the direction of the arrow), to peel off the surface protective film 30 from the laminate 100. As described above, Fp is 0.1 N / 25 mm or less. By satisfying such a relationship, the peeling property of the surface protective film 30 can be excellent. Specifically, when the surface protective film 30 is peeled off from the laminate 100, it is possible to prevent the surface protective film 30 from peeling off from the laminate 100 and the image display panel main body 70 from falling off from the adsorption plate B. In this way, the image display panel 80 shown in FIG. 3E is obtained. Specifically, the image display panel 80 in which the retardation layer-attached polarizing plate 110 is bonded to the image display panel main body 70 is obtained. EXAMPLES

[0062] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The thicknesses are values ​​measured by the following measuring method. In addition, unless otherwise specified, "parts" and "%" in the examples and comparative examples are based on weight. <Thickness> The thickness of 10 μm or less was measured using a scanning electron microscope (manufactured by JEOL, product name "JSM-7100F"), and the thickness of more than 10 μm was measured using a digital micrometer (manufactured by Anritsu, product name "KC-351C").

[0063] [Example 1] (Preparation of polarizing plate) As a thermoplastic resin substrate, a long amorphous isophthalic copolymerized polyethylene terephthalate film (thickness: 100 μm) having a Tg of about 75° C. was used, and one side of this resin substrate was subjected to a corona treatment. A PVA aqueous solution (coating solution) was prepared by adding 13 parts by weight of potassium iodide to 100 parts by weight of a PVA-based resin made by mixing polyvinyl alcohol (polymerization degree 4200, saponification degree 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., product name "GOHSEFFIMER") in a ratio of 9:1, and dissolving the mixture in water. The above PVA aqueous solution was applied to the corona-treated surface of a resin substrate and dried at 60° C. to form a PVA-based resin layer with a thickness of 13 μm, thereby producing a laminate. The obtained laminate was uniaxially stretched 2.4 times in the machine direction (longitudinal direction) in an oven at 130° C. (auxiliary air stretching treatment). Next, the laminate was immersed in an insolubilizing bath (a boric acid aqueous solution obtained by mixing 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (insolubilizing treatment). Next, the film was immersed in a dye bath (an aqueous iodine solution obtained by mixing iodine and potassium iodide in a weight ratio of 1:7 with 100 parts by weight of water) at a liquid temperature of 30°C for 60 seconds while adjusting the concentration so that the single transmittance (Ts) of the finally obtained polarizer would be the desired value (dyeing treatment). Next, the piece was immersed in a crosslinking bath (a boric acid aqueous solution obtained by mixing 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with respect to 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (crosslinking treatment). Thereafter, the laminate was immersed in an aqueous boric acid solution (boric acid concentration: 4% by weight, potassium iodide concentration: 5% by weight) at a liquid temperature of 70°C and uniaxially stretched in the longitudinal direction (longitudinal direction) between rolls with different peripheral speeds to a total stretch ratio of 5.5 times (underwater stretching treatment). Thereafter, the laminate was immersed in a cleaning bath (an aqueous solution obtained by mixing 4 parts by weight of potassium iodide with 100 parts by weight of water) at a liquid temperature of 20° C. (cleaning treatment). Thereafter, the film was dried in an oven maintained at about 90° C. while being brought into contact with a SUS heated roll whose surface temperature was maintained at about 75° C. (drying shrinkage treatment). In this manner, a polarizer having a thickness of about 5 μm was formed on the resin substrate, and a laminate having a resin substrate / polarizer structure was obtained.

[0064] An acrylic film (thickness: 20 μm) was attached as a protective layer to the polarizer side of the obtained laminate via a UV-curable adhesive. The resin substrate was then peeled off from the polarizer to obtain a polarizing plate having an acrylic film (protective layer) / polarizer structure.

[0065] (Preparation of Retardation Layer) A liquid crystal composition (coating liquid) was prepared by dissolving 10 g of a polymerizable liquid crystal exhibiting a nematic liquid crystal phase (manufactured by BASF: product name "Paliocolor LC242", represented by the following formula) and 3 g of a photopolymerization initiator for the polymerizable liquid crystal compound (manufactured by BASF: product name "Irgacure 907") in 40 g of toluene. [ka]

[0066] The surface of a polyethylene terephthalate (PET) film (thickness 38 μm) was rubbed with a rubbing cloth and subjected to an alignment treatment. The direction of the alignment treatment was set to be 15° from the viewing side with respect to the direction of the absorption axis of the polarizer when it was attached to the polarizing plate. The above liquid crystal coating liquid was applied to this alignment-treated surface with a bar coater, and the liquid crystal compound was aligned by heating and drying at 90°C for 2 minutes. The liquid crystal layer thus formed was then irradiated with 1 mJ / cm using a metal halide lamp. 2 The liquid crystal layer was cured by irradiating the liquid crystal with light, forming a liquid crystal alignment layer A (H layer) on the PET film. The liquid crystal alignment layer A had a thickness of 2.5 μm and an in-plane retardation Re(550) of 270 nm. Furthermore, the liquid crystal alignment layer A showed a refractive index characteristic of nx>ny=nz.

[0067] A liquid crystal alignment layer B (Q layer) was formed on a PET film in the same manner as above, except that the coating thickness was changed and the orientation treatment direction was set to a 75° direction from the viewing side with respect to the absorption axis direction of the polarizer. The thickness of the liquid crystal alignment layer B was 1.5 μm, and the in-plane retardation Re (550) was 140 nm. Furthermore, the liquid crystal alignment layer B showed a refractive index characteristic of nx>ny=nz.

[0068] (Preparation of Laminate) The obtained liquid crystal alignment solidified layer A (H layer) and liquid crystal alignment solidified layer B (Q layer) were transferred in this order onto the polarizer side of the obtained polarizing plate. At this time, the transfer (lamination) was performed so that the angle between the absorption axis of the polarizer and the slow axis of the alignment solidified layer A was 15°, and the angle between the absorption axis of the polarizer and the slow axis of the alignment solidified layer B was 75°. The liquid crystal alignment solidified layer A (H layer) was transferred via an ultraviolet curing adhesive (thickness 0.5 μm). The liquid crystal alignment solidified layer B (Q layer) was transferred via an ultraviolet curing adhesive (thickness 1.5 μm). In this way, a laminate precursor was obtained. The transfer was performed while transporting with a roll. Furthermore, the transfer was performed at a water vapor content of 9.3 g / m 3 The experiment was carried out under the following conditions: 23°C and 45% RH.

[0069] A 90 μm thick surface protection film (manufactured by Fujimori Kogyo Co., Ltd., "PPF-911", substrate (PET) thickness 75 μm, adhesive layer thickness 15 μm) was attached to the protective layer side of the polarizing plate of the obtained laminate precursor while being transported by rolls. Furthermore, a 50 μm thick release film (manufactured by Mitsubishi Chemical Corporation, "MHE50", PET film) was attached to the liquid crystal alignment solidified layer B (Q layer) side of the laminate precursor while being transported by rolls via an acrylic adhesive layer (thickness 15 μm) to obtain a laminate. The thickness of the laminated portion from the polarizing plate to the pressure-sensitive adhesive layer of the obtained laminate (thickness of the retardation layer-attached polarizing plate) was 46 μm.

[0070] [Example 2] A laminate was obtained in the same manner as in Example 1, except that a 48 μm thick surface protection film (manufactured by Nitto Denko Corporation, "RP109F", substrate (PET) thickness 38 μm, adhesive layer thickness 10 μm) was attached to the protective layer side of the polarizing plate of the laminate precursor.

[0071] [Example 3] A laminate was obtained in the same manner as in Example 1, except that the tension applied to the surface protective film when bonding the surface protective film was changed.

[0072] [Comparative Example 1] A laminate was obtained in the same manner as in Example 1, except that a release film having a thickness of 38 μm ("MHE38", a PET film, manufactured by Mitsubishi Chemical Corporation) was attached to the liquid crystal alignment solidified layer B (Q layer) side of the laminate precursor.

[0073] [Comparative Example 2] A laminate was obtained in the same manner as in Example 1, except that a release film having a thickness of 50 μm ("MRF50", a PET film, manufactured by Mitsubishi Chemical Corporation) was attached to the liquid crystal alignment solidified layer B (Q layer) side of the laminate precursor.

[0074] [Comparative Example 3] A laminate was obtained in the same manner as in Example 1, except that a 48 μm thick surface protection film (manufactured by Nitto Denko Corporation, "RP1010M", substrate (PET) thickness 38 μm, adhesive layer thickness 10 μm) was attached to the protective layer side of the polarizing plate of the laminate precursor.

[0075] <Evaluation> 1. Peeling force The obtained laminate was cut into a sample with a width of 25 mm and a length of 50 mm, and left in an environment of 23°C x 50% RH for 30 minutes or more, and then the peel force (N / 25 mm) was measured when peeled in the length direction at a peel speed of 300 mm / min and a peel angle of 180° using a universal tensile tester. Specifically, the peel force Fr of the release film to the adhesive layer and the peel force Fp of the surface protection film to the polarizing plate were measured. The measurements were performed in an environment of 23°C x 50% RH. 2. Warping A test piece measuring 171 mm x 127 mm was cut out from the obtained laminate. At this time, the absorption axis direction of the polarizer was cut out in the direction of the long side. The cut out test piece was placed on a flat surface with the release film side facing the flat surface, and the height of the highest part from the flat surface was measured to determine the amount of warping. Here, when the warping was convex toward the surface on which it was placed, it was designated as "negative (-)", and when it was convex toward the opposite side to the surface on which it was placed, it was designated as "positive (+)". The values ​​shown in Table 1 were calculated by warping amount (mm) / long side (171 mm) x 100. 3. Peel test The resulting laminate was cut into a sheet of 171 mm×127 mm size, so that the absorption axis direction of the polarizer was at an angle of 45° to the long side. As shown in FIG. 3, the release film and the surface protective film were peeled off from the obtained laminate in a sheet form, and the retardation layer-attached polarizing plate was attached to the organic EL panel body, and the occurrence of peeling failure was confirmed.

[0076] [Table 1]

[0077] It can be seen that even when negative warpage (for example, 1% or more) occurs in the laminate, each Example can have excellent peelability. In the laminate of Comparative Example 1, many dents were found in the adhesive layer (glue) disposed between the retardation layer and the release film. In Comparative Example 2, when the release film was peeled off, the release film did not peel off from the adhesive layer, and peeling occurred between the surface protection film and the polarizing plate. In Comparative Example 3, when the surface protection film was peeled off, the surface protection film did not peel off from the polarizing plate, and the organic EL panel body fell off from the adsorption plate. [Industrial Applicability]

[0078] The retardation layer-attached polarizing plate obtained from the laminate according to one embodiment of the present invention is used as a retardation layer-attached polarizing plate for an image display device, and can be particularly suitably used for a curved, bent, foldable, or rollable image display device. Representative examples of the image display device include a liquid crystal display device, an organic EL display device, and an inorganic EL display device. [Explanation of symbols]

[0079] 10 Polarizing plate 11 Polarizer 12 Protective layer 20 Retardation layer 21 First retardation layer (H layer) 22 Second retardation layer (Q layer) 30 Surface protection film 40 Adhesive layer 50 Release film 70 Image display panel body 80 Image display panel 90 Laminate precursor 100 Laminate 110 Polarizing plate with retardation layer

Claims

1. A laminate having, in this order, a surface protective film, a polarizing plate including a polarizer and a protective layer, a retardation layer, a pressure-sensitive adhesive layer, and a release film, The thickness of the polarizing plate is 40 μm or less, The thickness of the laminated portion from the polarizing plate to the pressure-sensitive adhesive layer is 25 μm or more and 70 μm or less, The thickness of the release film is 50 μm or more and 80 μm or less, a peel strength Fr of the release film to the pressure-sensitive adhesive layer is 0.005 N / 25 mm or more and 0.04 N / 25 mm or less; A peel force Fp of the surface protective film with respect to the polarizing plate is greater than the peel force Fr and is 0.05 N / 25 mm or less. Laminate.

2. The laminate according to claim 1 , wherein the surface protective film has a thickness of 60 μm or more.

3. The laminate according to claim 1 , wherein the thickness of the surface protection film is greater than the thickness of the laminated portion.

4. The laminate according to claim 1 , wherein the polarizing plate has a protective layer disposed only on a side of the polarizer on which the retardation layer is not disposed.

5. The laminate according to claim 1 , wherein the polarizer has a thickness of 8 μm or less.

6. The laminate according to claim 1 , wherein the retardation layer is a layer in which a liquid crystal compound is aligned and solidified.

7. 7. The laminate according to claim 1, having a warpage of 5% or less.

8. Providing a laminate according to any one of claims 1 to 7; bonding the laminate, in which the release film has been peeled off from the pressure-sensitive adhesive layer, to an image display panel body; and Peeling off the surface protective film from the polarizing plate; A method for manufacturing an image display panel comprising the steps of:

Citation Information

Patent Citations

  • Display module

    CN113345943A

  • Optical laminate and image display device

    JP2018120119A

  • Retardation film and optical device using the same

    JP3325560B2

  • Birefringent artificial dielectric structures

    US4712881A

  • Film layered body

    WO2021029191A1