Manufacturing method of piezoelectric ceramics, piezoelectric ceramics, piezoelectric element, ultrasonic motor, optical device, dust removal device, imaging device, ultrasonic probe, ultrasonic diagnostic device, and electronic device
The described manufacturing process for lead-free piezoelectric ceramics with titanium and barium components addresses performance fluctuations by ensuring low surface roughness and high electromechanical coupling, enhancing drive efficiency and reducing power consumption.
Patent Information
- Application Number
- JP2020074641
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-04-20
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2040-04-20
AI Technical Summary
Conventional lead-free piezoelectric materials exhibit significant fluctuations in piezoelectric performance and mechanical quality factor within the operating temperature range, and heat treatment to improve properties results in surface roughness, affecting drive efficiency and power consumption.
A manufacturing method involving sintering, polishing, and annealing at specific temperatures to produce piezoelectric ceramics with titanium and barium as main components, achieving low surface roughness and high electromechanical coupling coefficient, while avoiding lead content.
The method results in piezoelectric ceramics with stable piezoelectric constants and mechanical quality factors, reducing temperature dependence and improving drive efficiency and power consumption.
Smart Images

Figure 0007575884000006 
Figure 0007575884000007 
Figure 0007575884000008
Abstract
Description
[Technical field]
[0001] The present invention relates to piezoelectric ceramics and a manufacturing method thereof, and also to a piezoelectric element, an ultrasonic motor, an optical device, a dust removal device, an imaging device, an ultrasonic probe, an ultrasonic diagnostic device, and an electronic device, each using the piezoelectric ceramics. [Background technology]
[0002] Lead-containing lead zirconate titanate is a typical piezoelectric material and is used in a variety of piezoelectric devices such as actuators, oscillators, sensors, and filters. However, lead components in discarded piezoelectric materials can leach into soil and cause harm to ecosystems. Therefore, research and development of lead-free piezoelectric materials is being actively conducted to eliminate lead in piezoelectric devices.
[0003] When using piezoelectric elements in products such as home appliances, it is required that the electromechanical coupling coefficient is large and that fluctuations are small within the operating temperature range of the product. If the electromechanical coupling coefficient is small, the efficiency of conversion from electrical energy to mechanical energy is low, and power consumption increases. Furthermore, if the electromechanical coupling coefficient fluctuates significantly with temperature (for example, by more than 35%), it becomes difficult to obtain stable element performance within the operating temperature range. Since the electromechanical coupling coefficient is proportional to the piezoelectric constant, fluctuations in the electromechanical coupling coefficient also cause fluctuations in the piezoelectric constant. If the piezoelectric constant fluctuates, distortions that differ depending on the temperature will occur even if a constant voltage is input, making it necessary to change the driving method for each temperature.
[0004] Furthermore, regarding the variation of the electromechanical coupling coefficient, when the piezoelectric material undergoes a phase transition, the electromechanical coupling coefficient increases as the temperature approaches the phase transition temperature. Therefore, the phase transition of the piezoelectric material is the largest factor that varies the electromechanical coupling coefficient. Therefore, if it is desired to minimize the variation of the piezoelectric constant and electromechanical coupling coefficient within the operating temperature range of a product, a piezoelectric material that does not have a phase transition temperature within the operating temperature range is required.
[0005] On the other hand, when using piezoelectric materials in resonant devices such as ultrasonic motors, they are required to have a large mechanical quality factor, which indicates the sharpness of the resonance. If the mechanical quality factor is small, the power required for operation will be high, or the piezoelectric element will generate heat, making drive control difficult. For this reason, piezoelectric materials with a large mechanical quality factor are required.
[0006] In Patent Document 1, {[(Ba 1-x1 M1 x1 )((Ti 1-x Zr x ) 1-y1 N1 y1 )O3]-δ%[(Ba 1-y Ca y ) 1-x2 M2 x2 (Ti 1-y2 N2 y2 The paper discloses a lead-free piezoelectric material represented by a pseudo-binary solid solution of (Ba 1-x1 M1 x1 )((Ti 1-x Zr x ) 1-y1 N1 y1 )O3 is rhombohedral, (Ba 1-y Ca y ) 1-x2 M2 x2 (Ti 1-y2 N2 y2 )O3 is a tetragonal crystal. By dissolving two components with different crystal systems, the phase transition temperature between the rhombohedral and tetragonal crystals is adjusted to be near room temperature. For example, BaTi 0.8 Zr 0.2 O3-50%Ba 0.7 Ca 0.3 The phase transition temperature of TiO3 is near room temperature, and the piezoelectric constant d 33 The piezoelectric constant of the same material at 70°C was d 33 The company discloses that the d 33 Compared with the above, when the temperature increases by 50°C, the piezoelectric constant d 33 The electromechanical coupling coefficient is proportional to the piezoelectric constant, so it is expected that the electromechanical coupling coefficient will also vary by the same amount.
[0007] The piezoelectric material of Patent Document 1 exhibits a high piezoelectric constant near room temperature because the phase transition at which the piezoelectric properties are maximized occurs near room temperature, but has the problem that the piezoelectric constant and electromechanical coupling coefficient vary significantly when the temperature changes. Furthermore, as a result of extensive research by the present inventors, it has been found that there is also a problem that the mechanical quality factor at room temperature is low, at less than 500.
[0008] On the other hand, Patent Document 2 describes a method of improving the piezoelectric properties by heat-treating the piezoelectric material at a temperature of 1000°C or higher after polishing the piezoelectric material, thereby alleviating the residual stress generated during the polishing process. However, as a result of the inventor's intensive research, it was found that although a high piezoelectric constant and a high electromechanical coupling coefficient can be obtained, heat-treating the piezoelectric material at a temperature of 1000°C or higher causes grain growth on the surface of the piezoelectric material, resulting in a rough surface. If the surface becomes rough, when an adhesive is used to adhere a vibrating body that vibrates together with the piezoelectric material to the surface, the adhesive will enter the recesses of the rough surface, resulting in a thick adhesive, making it difficult for vibration to be transmitted from the piezoelectric material to the vibrating body. As a result, there is a problem that the driving efficiency is deteriorated and power consumption is increased. In addition, if the surface of the piezoelectric material is rough, when an electrode is provided on the surface of the piezoelectric material, the electrode will enter the recesses of the rough surface, resulting in an increase in the thickness of the electrode, suppressing the vibration of the piezoelectric material. In this case, there is also a problem that the driving efficiency is deteriorated and power consumption is increased. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2009-215111 A [Patent Document 2] JP 2015-035587 A Summary of the Invention [Problem to be solved by the invention]
[0010] With conventional technology, the piezoelectric performance of lead-free piezoelectric materials varies greatly within the operating temperature range of the piezoelectric material. In addition, the mechanical quality factor is small, and attempts to improve the piezoelectric performance by heat treatment at 1,000°C or higher result in a rough surface.
[0011] The present invention has been made to solve such problems, and provides a piezoelectric ceramic that is lead-free, has a small temperature dependence of the piezoelectric constant within the operating temperature range, has a high density, a high mechanical quality factor, a good piezoelectric constant, and small surface roughness, and a manufacturing method thereof.
[0012] The present invention also provides a piezoelectric element, an ultrasonic motor, an optical device, a dust removal device, an imaging device, an ultrasonic probe, an ultrasonic diagnostic device, and an electronic device that use the piezoelectric ceramic. [Means for solving the problem]
[0013] The method for producing piezoelectric ceramics of the present invention for solving the above problems is characterized by comprising the steps of sintering a molded body containing raw materials at 1000°C or higher to obtain a sintered body, polishing the sintered body, and annealing the polished sintered body at 800°C or higher but less than 1000°C.
[0014] The method for producing a piezoelectric element of the present invention is characterized in that a step of providing electrodes on the piezoelectric ceramic is carried out before the step of annealing, and the electrodes are baked in the step of annealing.
[0015] The piezoelectric ceramic of the present invention is a piezoelectric ceramic mainly composed of titanium and barium, and has an electromechanical coupling coefficient k 31 is 0.252 or more, and the surface roughness Ra of at least a part of the piezoelectric ceramic is 0.19 μm or less.
[0016] The piezoelectric element of the present invention is characterized by having electrodes and a piezoelectric ceramic. The ultrasonic motor of the present invention is characterized by having at least a vibrating body on which the piezoelectric element or the laminated piezoelectric element is disposed, and a moving body in contact with the vibrating body. The optical device of the present invention is characterized in that a drive section includes the ultrasonic motor described above. The vibration device of the present invention is characterized by having a vibrating body in which the piezoelectric element is arranged on a diaphragm. The dust removing device of the present invention is characterized in that a vibration section includes the vibration device. The imaging device of the present invention includes at least the dust removal device and an imaging element unit, and is characterized in that the diaphragm of the dust removal device is provided on the light receiving surface side of the imaging element unit. The ultrasonic probe of the present invention includes the piezoelectric element and transmits and receives waves by means of the piezoelectric element. The ultrasonic diagnostic apparatus of the present invention is characterized by having at least the ultrasonic probe and an image output unit. An electronic device according to the present invention is characterized in that it includes a piezoelectric acoustic component having the piezoelectric element described above. Effect of the Invention
[0017] According to the present invention, it is possible to provide a piezoelectric ceramic which is lead-free, has a small temperature dependence of the electromechanical coupling coefficient within the operating temperature range of the piezoelectric element, has a high density, a high mechanical quality factor, good piezoelectric properties, and has a small surface roughness. The piezoelectric ceramic of the present invention has a small load on the environment because it does not use lead. [Brief description of the drawings]
[0018] [Figure 1] 1 is a schematic diagram showing an embodiment of a configuration of a piezoelectric element of the present invention. [Diagram 2] 1 is a schematic diagram showing an embodiment of a configuration of an ultrasonic motor of the present invention. [Diagram 3] 1 is a schematic diagram illustrating an embodiment of an optical device according to the present invention. [Figure 4] 1 is a schematic diagram illustrating an embodiment of an optical device according to the present invention. [Diagram 5]1 is a schematic diagram showing an embodiment in which a vibration device of the present invention is used as a dust removing device. [Figure 6] 3 is a schematic diagram illustrating a configuration of a piezoelectric element in the dust removing device of the present invention. [Figure 7] 2A to 2C are schematic diagrams illustrating the vibration principle of the dust removing device of the present invention. [Figure 8] 1 is a schematic diagram illustrating an embodiment of an imaging device of the present invention. [Figure 9] 1 is a schematic diagram illustrating an embodiment of an imaging device of the present invention. [Figure 10] 1 is a schematic diagram illustrating an embodiment of an ultrasonic probe according to the present invention. [Figure 11] 1 is a schematic diagram showing an embodiment of an ultrasonic diagnostic apparatus according to the present invention. [Figure 12] 1 is a schematic diagram illustrating an embodiment of an electronic device of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, an embodiment of the present invention will be described. The present invention provides a lead-free piezoelectric ceramic having a high mechanical quality factor, a small temperature dependency of the electromechanical coupling coefficient in the operating temperature range (for example, a range of 0°C to 60°C), a high density, a high electromechanical coupling coefficient, and a small surface roughness, and a method for producing the same. The piezoelectric ceramic of the present invention can be used in various applications such as memories and sensors by utilizing its ferroelectric properties.
[0020] The method for producing piezoelectric ceramics of the present invention includes the steps of sintering a molded body containing raw materials at 1000°C or higher to obtain a sintered body, polishing the sintered body, and annealing the polished sintered body at 800°C or higher but less than 1000°C.
[0021] A specific method for producing the piezoelectric ceramic of the present invention will now be described. (Raw material powder) The raw materials used in the method for producing the piezoelectric ceramic of the present invention are solid powders of oxides, carbonates, nitrates, oxalates, etc., containing the constituent elements that make up the piezoelectric ceramic, or mixed powders of these. It is more preferable that the lead (Pb) content in the raw materials is less than 1000 ppm, since this reduces the burden on the environment.
[0022] Preferred elements constituting the raw materials include, for example, Li, Na, Mg, Al, Si, K, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Zn, Ge, Sr, Y, Zr, Nb, Mo, Sn, Sb, Ba, Hf, Ta, Bi, La, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, and Yb.
[0023] The raw materials may be heat-treated for the purpose of homogenization, or may be crushed after heat treatment. It is preferable to perform the heat treatment for homogenizing the raw materials at a temperature in the range of 800° C. to 1300° C., since the raw materials are easily crushed after the heat treatment.
[0024] (granulation) The raw materials used in the manufacturing method of the piezoelectric ceramic of the present invention may be granulated, and the granulation method is not particularly limited. Examples of binders that can be used in granulation include PVA (polyvinyl alcohol), PVB (polyvinyl butyral), and acrylic resins. The amount of binder added to the mixed powder is preferably 1 to 10 parts by weight, and more preferably 2 to 5 parts by weight from the viewpoint of increasing the density of the molded body. The most preferable granulation method is the spray drying method from the viewpoint of making the particle size of the granulated powder more uniform.
[0025] (molded body) The molded body used in the method for producing the piezoelectric ceramic of the present invention is a molded body obtained by solidifying the raw material powder into a desired shape, and the method for producing the molded body is not particularly limited. The molded body is a solid body produced from the raw material powder, granulated powder (binder), or slurry. The molded body can be produced by uniaxial pressing, cold isostatic pressing, warm isostatic pressing, casting molding, extrusion molding, or the like. The raw material in a slurry state can also be dried in a sheet shape using a doctor blade method, and the sheets can be stacked to form the desired shape.
[0026] (Firing) The sintering method in the method for producing the piezoelectric ceramic of the present invention includes a step of sintering a molded body containing the above-mentioned raw materials at 1000° C. or higher to obtain a sintered body. Examples of the sintering method include sintering in an electric furnace, sintering in a gas furnace, resistance heating, microwave sintering, millimeter wave sintering, and HIP (hot isostatic pressing). Sintering in an electric furnace or gas may be performed in a continuous furnace or a batch furnace.
[0027] By sintering at 1000°C or higher, the compounds contained in the raw materials react with each other and grow into crystals sufficiently. Examples of sintered bodies obtained by firing include sintered bodies mainly composed of titanium and barium, sintered bodies mainly composed of niobium and at least one selected from lithium, potassium, and sodium, sintered bodies mainly composed of bismuth and titanium, sintered bodies mainly composed of bismuth, iron, and cobalt, sintered bodies mainly composed of bismuth, titanium, and sodium, and sintered bodies mainly composed of a combination of these.
[0028] A preferred sintering temperature, from the viewpoint of setting the grain size of the sintered body in the range of 3 μm to 30 μm when the raw material is mainly composed of barium titanate, is 1100° C. to 1550° C., more preferably 1100° C. to 1380° C. Piezoelectric ceramics obtained from sintered bodies sintered in the above temperature range have the advantage of having high density.
[0029] Furthermore, in order to reproducibly and stably obtain the characteristics of the piezoelectric ceramics obtained by the sintering process, it is advisable to carry out the sintering process for 2 hours or more and 24 hours or less at a constant sintering temperature within the above range.
[0030] (polishing) The method for producing a piezoelectric ceramic according to the present invention includes a step of polishing the sintered body obtained by sintering as described above. Here, polishing refers to a step of polishing a part or the whole surface of the sintered body and adjusting the polished surface to a desired roughness.
[0031] Roughness is the arithmetic mean roughness Ra, which is the average value of the surface unevenness as a reference line, and is expressed in micrometers (μm) as the average value of the distance from the reference line in that section. The method for measuring surface roughness is based on the Japanese Industrial Standards (JIS B 0601:2013), and uses a stylus-type surface step gauge to divide the measurement distance L into n parts, and the height of the i-th part is expressed as y. i Then, the roughness Ra can be calculated by the following formula (1): It is preferable that the tip of the needle is as small as possible. For example, it is good to use a needle with a tip curvature radius of 1 μm.
number
[0032] Before or after the step of polishing the sintered body, a deburring step by barrel polishing or blast polishing, or a step of machining the sintered body to the desired dimensions using a lathe, a grinder, or a cutter may be added.
[0033] Polishing processes include mechanical polishing, chemical polishing, and CMP polishing, and the desired surface roughness can be achieved by combining these.
[0034] Mechanical polishing refers to polishing using a machine, and when performing mechanical polishing, a polishing machine, lapping machine, polishing machine, or buffing machine can be selected and used. If the surface roughness can be adjusted, for example, a process using a precision grinding machine with a very fine grinding wheel can also be used as the polishing process.
[0035] Chemical polishing is a polishing method in which metal is immersed in a polishing solution and the surface of the metal is corroded by a chemical reaction using the power of acid or alkali. For example, a rotary polishing method is used in which a polishing pad is attached to a disk-shaped surface plate, and a liquid abrasive containing chemical components and fine particles is dripped onto the pad and polished while rotating.
[0036] CMP polishing is a technique that combines mechanical polishing and chemical polishing. It not only uses the mechanical action of abrasive grains to scrape the metal surface, but also creates a chemical reaction between the abrasive grains and the metal, and between the abrasive and grinding fluids, resulting in a planarization of the surface through physical polishing and chemical reactions.
[0037] To omit the polishing process, it is possible to mold the sintered body into the desired shape after sintering, but the surface of the sintered body immediately after sintering will have large surface roughness due to the growth of crystal grains. Therefore, a polishing process is required to make at least a part of the surface have the desired roughness Ra (for example, a roughness Ra of 0.19 μm or less).
[0038] (Annealing treatment) The method for producing a piezoelectric ceramic of the present invention includes a step of annealing the polished sintered body at a temperature of 800°C or higher and lower than 1000°C.
[0039] It is believed that crystal defects occur on the surface of the sintered body that has undergone the above-mentioned polishing process. Therefore, by annealing at 800°C or more and less than 1000°C, the crystal defects are repaired, and the electromechanical coupling coefficient of the piezoelectric ceramic becomes good. When annealing at 1000°C or more, the crystal grains grow and become larger in size, and even if the surface roughness Ra is adjusted in the above-mentioned polishing process, the surface roughness Ra becomes larger by the annealing process. As a result, the surface roughness Ra of both the unpolished and polished surfaces becomes large, so that the thickness of any adhesive or electrode applied to any surface becomes large, and the efficiency of vibration of the piezoelectric ceramic becomes poor. In addition, if the annealing temperature is less than 800°C, a good electromechanical coupling coefficient cannot be obtained.
[0040] If the annealing temperature is 900° C. or higher and lower than 1000° C., and further 950° C. or higher and lower than 1000° C., crystal defects on the polished surface are further repaired, and the electromechanical coupling coefficient is further improved, which is more preferable.
[0041] The method for the annealing treatment is not particularly limited, and like the method for obtaining a sintered body by sintering, sintering in an electric furnace, sintering in a gas furnace, resistance heating method, microwave sintering method, millimeter wave sintering method, HIP (hot isostatic pressing), etc. can be used, and either a continuous furnace or a batch furnace can be used. The annealing treatment is preferably performed in air, since crystal defects are easily repaired.
[0042] In the method for producing a piezoelectric ceramic of the present invention, the temperature is preferably maintained for at least 6 minutes and less than 10 hours in the annealing step. In the annealing treatment, the temperature is preferably maintained for 6 minutes or more and less than 10 hours, since defects in the crystal grains are repaired and the electromechanical coupling coefficient is improved.The temperature is preferably maintained for 2 hours or more and less than 5 hours, since defects in the crystal grains are repaired efficiently and sufficiently, and the electromechanical coupling coefficient is further improved.
[0043] Next, a specific method for producing the piezoelectric element of the present invention will be described. In the method for producing a piezoelectric element of the present invention, in the method for producing a piezoelectric ceramic, a step of providing electrodes on the piezoelectric ceramic is preferably carried out before the annealing treatment step, and the electrodes are baked in the annealing treatment step.
[0044] The material of the electrode to be used is not particularly limited as long as it can be baked at a temperature range of 800°C or more and less than 1000°C, and may be any material that is normally used for piezoelectric elements. For example, metals such as Ti, Pt, Ta, Ir, Au, Fe, Cr, Ni, Pd, Ag, Cu, Sn, In, Sr, Al, and their compounds can be mentioned. An electrode paste containing water or organic matter in the electrode material is applied to the polished sintered body, and then baked by annealing. Here, when Sn, In, Sr, Al, etc. are selected as electrode materials for baking by annealing, the melting point is low, so it is necessary to increase the melting point by mixing with other metals. In addition, the atmosphere when baking by annealing is preferably air, but when Al, Fe, Ni, Cu, etc. are selected as electrode materials, they are easily oxidized, so it is preferable to perform the annealing under an atmosphere such as nitrogen. As a result, the crystal defects on the polished surface of the sintered body are repaired by the annealing treatment, improving the electromechanical coupling coefficient, and the electrodes are baked at the same time, reducing the number of steps required to manufacture the piezoelectric element and reducing manufacturing costs. Ag is a common electrode material that can be baked at a temperature range of 800°C to 1000°C. For example, in the case of Ag electrodes, Pd may be mixed in to adjust the melting point as necessary. The thickness of the electrode is preferably 5 nm to 10 μm, and is more preferably 5 μm or less, since it does not inhibit the vibration of the piezoelectric element.
[0045] After the annealing process, the electrodes may be baked, in which case the annealing process is essentially performed twice, but the effect of improving the electromechanical coupling coefficient can be similarly obtained. When forming the electrodes after the annealing process, the means for forming the electrodes is not particularly limited, and they may be formed by a sputtering method, a vapor deposition method, a plating method, or the like.
[0046] The piezoelectric ceramics used in the method for producing a piezoelectric element of the present invention preferably contain titanium and barium as their main components. Barium titanate, a compound of titanium and barium, is widely used in capacitors, and is a low-cost raw material with little quality variation, so titanium and barium are preferably used as the main components.
[0047] The piezoelectric ceramic of the present invention is a piezoelectric ceramic mainly composed of titanium and barium, and has an electromechanical coupling coefficient k 31 is 0.252 or more, and the surface roughness Ra of at least a part of the piezoelectric ceramic is 0.19 μm or less.
[0048] The piezoelectric ceramic of the present invention is mainly composed of titanium and barium. Piezoelectric ceramics mainly composed of titanium and barium have a high electromechanical coupling coefficient, which is preferable because it consumes less power when vibrating the piezoelectric ceramic. In addition, according to the following formula (2), it has a high piezoelectric constant d 31 This increases the vibration of the piezoelectric element, which is preferable.
number
[0049] k 31 If k is 0.252 or more, the power consumption during operation is small. 31 When the ratio is 0.270 or more, a sufficient vibration displacement amount can be obtained even if the driving voltage is lowered, so that the loss in the driving circuit caused by the magnitude of the driving voltage is reduced and the power consumption is further reduced, which is more preferable.
[0050] The piezoelectric ceramic of the present invention has a surface roughness Ra of 0.19 μm or less on at least a portion thereof. For piezoelectric ceramics, if the surface roughness Ra exceeds 0.19 μm, when attempting to glue a vibrating body or other object that vibrates together with the surface, the adhesive will seep into the recesses in the rough surface, making the adhesive thicker and making it difficult for vibrations to be transmitted from the piezoelectric ceramic to the vibrating body. Furthermore, if an electrode is placed on the surface of the piezoelectric ceramic with a rough surface, the thickness of the electrode will increase for the same reason as with the adhesive, suppressing the vibration of the piezoelectric ceramic and reducing drive efficiency.
[0051] A surface roughness Ra of 0.15 μm or less is preferable because the unevenness of the electrodes is small, resulting in a uniform distribution of the voltage applied to the piezoelectric ceramic and a larger electromechanical coupling coefficient. A surface roughness Ra of 0.10 μm or less is even more preferable because an even larger electromechanical coupling coefficient can be obtained.
[0052] The piezoelectric ceramic of the present invention is a piezoelectric ceramic containing an oxide including Ba, Ca, Ti, and Zr, and Mn, wherein x, which is a molar ratio of Ca to the sum of Ba and Ca, is 0.02≦x≦0.30, y, which is a molar ratio of Zr to the sum of Ti and Zr, is 0.020≦y≦0.095, and x and y have a relationship of y≦x, a, which is a molar ratio of the sum of Ba and Ca to the sum of Ti and Zr, is 1.00≦a≦1.01, and the content of Mn relative to 100 parts by weight of the oxide is preferably 0.02 parts by weight or more and 0.40 parts by weight or less in terms of metal.
[0053] The piezoelectric ceramic of the present invention preferably contains an oxide containing Ba, Ca, Ti, and Zr, and Mn.
[0054] The raw materials for producing the piezoelectric ceramic of the present invention are composed of metal compounds such as Ba compounds, Ca compounds, Ti compounds, Zr compounds, and Mn compounds.
[0055] Usable Ba compounds include barium oxide, barium carbonate, barium oxalate, barium acetate, barium nitrate, barium titanate, barium zirconate, and barium titanate zirconate.
[0056] Examples of Ca compounds that can be used include calcium oxide, calcium carbonate, calcium oxalate, calcium acetate, calcium titanate, and calcium zirconate.
[0057] Usable Ti compounds include titanium oxide, barium titanate, barium titanate zirconate, and calcium titanate.
[0058] Usable Zr compounds include zirconium oxide, barium zirconate, barium zirconate titanate, calcium zirconate, and the like.
[0059] Usable Mn compounds include manganese carbonate, manganese monoxide, manganese dioxide, trimanganese tetroxide, and manganese acetate.
[0060] Here, the Mn content "converted to metal" refers to the following. The contents of each metal, Ba, Ca, Ti, Zr, and Mn, are measured from the piezoelectric ceramic by X-ray fluorescence analysis (XRF), ICP atomic emission spectrometry, atomic absorption spectrometry, etc. From the contents, the elements constituting the metal oxide represented by the following general formula (3) are converted to oxides, and the value is calculated as the ratio of the weight of Mn to the total weight of 100. (Ba 1-x , Ca x ) a (Ti 1-y ,Zr y )O3(3)
[0061] From the viewpoint of insulation, the piezoelectric ceramic of the present invention preferably has a perovskite metal oxide as the main phase. The perovskite metal oxide refers to a metal oxide having a perovskite structure (also called "perovskite structure") as described in the Iwanami Physics and Chemistry Dictionary, 5th Edition (Iwanami Shoten, published February 20, 1998). The metal oxide having a perovskite structure is expressed by the chemical formula ABO3, as in the above general formula (3). In the perovskite metal oxide, the elements A and B each occupy specific positions of the unit lattice called the A site and the B site in the form of an ion. For example, in the case of a cubic unit lattice, the element A is located at the vertex of the cube, and the element B is located at the body center. The element O occupies the face center position of the cube as an oxygen anion.
[0062] Whether or not the perovskite metal oxide is the main phase can be determined by, for example, whether or not the maximum diffraction intensity derived from the perovskite metal oxide is 100 times or more the maximum diffraction intensity derived from the impurity phase in X-ray diffraction. If the piezoelectric ceramic is composed only of the perovskite metal oxide, the insulation is the highest, and therefore it is preferable. The "main phase" is when, when the powder X-ray diffraction of the piezoelectric ceramic is performed, the peak with the strongest diffraction intensity is due to the perovskite structure. More preferably, it is a "single phase" in which the crystals of the perovskite structure occupy almost all of the phase.
[0063] The metal oxide represented by the general formula (3) means that the metal elements located at the A site are Ba and Ca, and the metal elements located at the B site are Ti and Zr. However, some of Ba and Ca may be located at the B site. Similarly, some of Ti and Zr may be located at the A site.
[0064] In the general formula (3), the molar ratio of the B site element to the O element is 1:3, but the ratio of the amounts of the elements may vary slightly (for example, 1.00:2.94 to 1.00:3.06).
[0065] In the piezoelectric ceramic of the present invention, it is preferable that the range of x is 0.02≦x≦0.30, the range of y is 0.020≦y≦0.095, and y and x are y≦x. In addition, it is preferable that the molar ratio a of the sum of the Ba and Ca to the sum of the Ti and Zr is 1.00≦a≦1.01, since a good electromechanical coupling coefficient can be obtained in the operating temperature range.
[0066] The range of x in the piezoelectric ceramic of the present invention is preferably 0.02≦x≦0.30. When x is less than 0.02, the orthorhombic to tetragonal phase transition temperature (hereinafter T ot ) becomes higher than 0° C., and as a result, the temperature dependence of the electromechanical coupling coefficient and the piezoelectric constant becomes large within the operating temperature range.
[0067] Near the phase transition temperature, the electromechanical coupling coefficient reaches a maximum, showing a maximum value or an inflection point. Therefore, if a phase transition exists within the operating temperature range of the device, the performance of the device will vary extremely with temperature, making it difficult to control the device. Thus, it is desirable that the phase transition, which is the largest factor causing fluctuations in the electromechanical coupling coefficient, does not exist within the operating temperature range. The farther the phase transition temperature is from the operating temperature range, the lower the temperature dependence of the electromechanical coupling coefficient within the operating temperature range, which is preferable.
[0068] On the other hand, when x is greater than 0.30, it becomes difficult for Ca to solidify, and an impurity phase of CaTiO3 is generated, resulting in a decrease in the electromechanical coupling coefficient and piezoelectric constant. Also, from the perspective of obtaining more preferable electromechanical coupling coefficients and piezoelectric constants, x≦0.26 is preferable, and more preferably x≦0.17.
[0069] For the piezoelectric ceramics of the present invention, it is preferable that 0.020≦y≦0.095. When y is 0.020 or more, the dielectric constant at room temperature can be increased to further improve the electromechanical coupling coefficient. Furthermore, when the amount of Zr, y, is greater than 0.020, good electromechanical coupling coefficients and piezoelectric constants can be obtained. Therefore, the range of y is preferably y≧0.020. From the perspective of obtaining a more preferable electromechanical coupling coefficient, y≧0.050. When y is greater than 0.095, the Curie temperature (hereinafter T C ) may be less than 100°C, which is not preferable. To obtain good electromechanical coupling coefficients and piezoelectric constants and set T C to 100°C or more, the range of y is more preferably 0.020<y≦0.095.
[0070] The range of a, which is the molar ratio of the sum of Ba and Ca to the sum of Ti and Zr {a=(Ba + Ca) / (Zr + Ti)}, is preferably 1.00≦a≦1.01. When a is less than 1.00, abnormal grain growth occurs during firing. Furthermore, the average grain size becomes larger than 50μm, and the mechanical strength of the material decreases. When a is greater than 1.01, a high-density piezoelectric ceramic cannot be obtained. When the density of the piezoelectric ceramic is low, the electromechanical coupling coefficient decreases.
[0071] In the present invention, the density of an insufficiently sintered sample is at least 5% lower than that of a sufficiently sintered high-density sample. In order to obtain a piezoelectric ceramic having high density and mechanical strength, the range of a is preferably 1.00≦a≦1.01.
[0072] The piezoelectric ceramic of the present invention preferably contains 0.02 parts by weight or more and 0.40 parts by weight or less of Mn, calculated as metal, per 100 parts by weight of the perovskite metal oxide represented by the general formula (3). When Mn is contained in the above range, the mechanical quality factor increases. However, when the Mn content is less than 0.02 parts by weight, the effect of increasing the mechanical quality factor cannot be obtained. On the other hand, when the Mn content is more than 0.40 parts by weight, the insulation resistance of the piezoelectric ceramic decreases. When the insulation resistance is low, the dielectric loss tangent at room temperature measured by applying an AC electric field with a frequency of 1 kHz and an electric field strength of 10 V / cm using an impedance analyzer exceeds 0.01. Or the resistivity is 1 GΩcm or less.
[0073] Mn is not limited to metallic Mn, and may be contained in the piezoelectric ceramic as a Mn component, regardless of the form of inclusion. For example, Mn may be dissolved in the B site or may be contained in the grain boundary. Alternatively, Mn may be contained in the piezoelectric ceramic in the form of metal, ion, oxide, metal salt, complex, etc. More preferably, Mn is present from the viewpoint of insulation and sinterability.
[0074] The piezoelectric ceramic of the present invention preferably has a mechanical quality factor Qm of 1000 or more. When the mechanical quality factor of a piezoelectric ceramic is 1000 or more, the power required to operate it is low, and heat generation in the piezoelectric ceramic can be suppressed.
[0075] The piezoelectric ceramic of the present invention preferably contains 0.042 to 0.850 parts by weight of Bi, calculated as metal, per 100 parts by weight of the perovskite metal oxide represented by the general formula (3). If the Bi content is less than 0.042 parts by weight, the effect of lowering the phase transition temperature and improving the mechanical quality factor cannot be obtained. If the Bi content is more than 0.850 parts by weight, the electromechanical coupling factor decreases by more than 30% compared to when no Bi is contained.
[0076] In the piezoelectric ceramic of the present invention, Bi may be present at the grain boundaries, or may be dissolved in the perovskite structure of (Ba,Ca)(Ti,Zr)O3.
[0077] When Bi is present at grain boundaries, friction between crystal grains is reduced and the mechanical quality factor is increased. When Bi is dissolved in the perovskite structure of (Ba,Ca)(Ti,Zr)O3, T ot and T to Since the temperature is lowered, the temperature dependency of the piezoelectric constant within the operating temperature range is reduced, and the mechanical quality factor can be improved.
[0078] For the purpose of facilitating the production of the piezoelectric ceramic of the present invention or adjusting the physical properties of the piezoelectric ceramic of the present invention, up to 1 mol % of Ba and Ca may be replaced with a divalent metal element, such as Sr, and up to 1 mol % of Ti and Zr may be replaced with a tetravalent metal element, such as Hf.
[0079] The piezoelectric ceramic of the present invention has the electromechanical coupling coefficient k 31 It is preferable that the fluctuation rate of is 35% or less.
[0080] When piezoelectric ceramics are used indoors, the temperature of the piezoelectric ceramics, including the heat generated during operation, is mainly in the range of 0°C to 60°C. In this temperature range, the electromechanical coupling coefficient k 31 When the rate of change is 35% or less, the variation in piezoelectric performance with respect to temperature is small, and there is no need to change the method of controlling the piezoelectric ceramic in accordance with temperature changes.
[0081] The average equivalent circle diameter of the piezoelectric ceramic of the present invention is preferably 1 μm or more and 10 μm or less. By setting the average equivalent circular diameter of the piezoelectric ceramic of the present invention to 10 μm or less, chipping during cutting and polishing processes is reduced.
[0082] The term "particle size" in the present invention refers to the "projected area circle equivalent diameter" generally referred to in microscopic observation, and refers to the diameter of a perfect circle having the same area as the projected area of a crystal grain. In the present invention, the method for measuring the particle size is not particularly limited. For example, the particle size can be obtained by image processing of a photographic image obtained by photographing the surface of a piezoelectric ceramic with a polarizing microscope or a scanning electron microscope. Since the optimal magnification differs depending on the particle size of interest, an optical microscope and an electron microscope may be used separately. The circle equivalent diameter may also be obtained from an image of a polished surface or cross section of the material, rather than from the surface.
[0083] The relative density of the piezoelectric ceramic of the present invention is preferably 93% or more and 100% or less. The density of the sintered body can be measured, for example, by the Archimedes method. In the present invention, the theoretical density (ρ calc. ) versus measured density (ρ meas. ), i.e., the relative density (ρ calc. / ρ meas. ) of 93% or more can be said to be sufficiently high for use as a piezoelectric ceramic.
[0084] The thickness of the piezoelectric ceramic of the present invention is preferably 10 μm or more, and more preferably 50 μm or more. By making the thickness of the piezoelectric ceramic 10 μm or more, the polishing process becomes easy and the desired roughness Ra can be obtained. By making the thickness of the piezoelectric ceramic 50 μm or more, it becomes difficult to break during processing such as polishing.
[0085] The piezoelectric element of the present invention is characterized by having a plurality of electrodes and a piezoelectric ceramic. A piezoelectric element using the piezoelectric ceramic of the present invention will be described below. Fig. 1 is a schematic diagram showing one embodiment of the configuration of the piezoelectric element of the present invention. In Fig. 1, the multiple electrodes include a first electrode 1 provided on a first surface of the piezoelectric ceramic 2, and a second electrode 3 split into two provided on the surface of the piezoelectric ceramic 2 opposite to the surface on which the first electrode 1 is provided. The piezoelectric element of the present invention is a piezoelectric element having multiple electrodes and a piezoelectric ceramic, and is characterized in that the piezoelectric ceramic 2 is the piezoelectric ceramic of the present invention.
[0086] The piezoelectric ceramic according to the present invention can be used to evaluate the electromechanical coupling coefficient and mechanical quality coefficient by forming a piezoelectric element having a plurality of electrodes. The first electrode and the second electrode are each made of a conductive layer having a thickness of about 5 nm to 10 μm.
[0087] The first electrode and the second electrode may be made of one material or a laminate of two or more materials, and the first electrode and the second electrode may be made of different materials.
[0088] The method of polarization of the piezoelectric element is not particularly limited. The polarization process may be performed in air or in silicone oil. The temperature during polarization is preferably 60°C to 150°C, but the optimal conditions vary slightly depending on the composition of the piezoelectric ceramics that constitute the element. The electric field applied for polarization process is preferably 600V / mm to 2.0kV / mm.
[0089] The electromechanical coupling coefficient and mechanical quality coefficient of the piezoelectric element can be calculated based on the measurement results of the resonance frequency and anti-resonance frequency obtained by using a commercially available impedance analyzer, in accordance with the Japan Electronics and Information Technology Industries Association standard (JEITA EM-4501). Hereinafter, this method will be referred to as the resonance-anti-resonance method.
[0090] In addition, the raw material for adjusting the ratio of a to the sum of the moles of Ti and Zr {a=(Ba+Ca) / (Zr+Ti)} to the sum of the moles of Ba and Ca in the piezoelectric ceramic according to the present invention is not particularly limited. The effect is the same whether a Ba compound, a Ca compound, a Ti compound, or a Zr compound is used as the raw material.
[0091] The piezoelectric element according to the present invention also includes a laminated piezoelectric element in which a number of sheets of the piezoelectric ceramic of the present invention are laminated, or a number of piezoelectric elements are laminated to form a rod-like shape and the displacement in the thickness direction is utilized.
[0092] Next, an ultrasonic motor using the piezoelectric element of the present invention will be described. (Ultrasonic motor) The ultrasonic motor according to the present invention is characterized by having at least a vibrating body on which the piezoelectric element is arranged, and a moving body in contact with the vibrating body. FIG. 2 is a schematic diagram showing one embodiment of the configuration of the ultrasonic motor according to the present invention. FIG. 2 shows an ultrasonic motor in which the piezoelectric element of the present invention is made of a single plate. The ultrasonic motor has a vibrator 201, a rotor 202 that is in contact with the sliding surface of the vibrator 201 by the pressure of a pressure spring (not shown), and an output shaft 203 that is integrally provided with the rotor 202. The vibrator 201 is composed of a metal elastic ring 2011, the piezoelectric element 2012 of the present invention, and an organic adhesive 2013 (epoxy-based, cyanoacrylate-based, etc.) that bonds the piezoelectric element 2012 to the elastic ring 2011. The piezoelectric element 2012 of the present invention is composed of a piezoelectric ceramic sandwiched between a first electrode and a second electrode (not shown). When a two-phase alternating voltage with a phase difference of an odd multiple of π / 2 is applied to the piezoelectric element of the present invention, a flexural traveling wave is generated in the vibrator 201, and each point on the sliding surface of the vibrator 201 moves elliptically. When the rotor 202 is pressed against the sliding surface of the vibrator 201, the rotor 202 receives a frictional force from the vibrator 201 and rotates in the opposite direction to the flexural traveling wave. The driven body (not shown) is connected to the output shaft 203 and is driven by the rotational force of the rotor 202. When a voltage is applied to the piezoelectric ceramic, the piezoelectric ceramic expands and contracts due to the piezoelectric transverse effect. The conversion efficiency from this electrical energy to mechanical energy depends on the magnitude of the electromechanical coupling coefficient. When an elastic body such as a metal is bonded to the piezoelectric element by an adhesive or the like, the elastic body is bent by the expansion and contraction of the piezoelectric ceramic via the adhesive. The ultrasonic motor of the type described here utilizes this principle.
[0093] (optical equipment) Next, an optical device according to the present invention will be described. The optical device according to the present invention is characterized in that a drive unit thereof includes the ultrasonic motor described above.
[0094] Figures 3(a) and 3(b) are cross-sectional views of the main parts of an interchangeable lens barrel for a single-lens reflex camera, which is an example of a preferred embodiment of the optical device of the present invention. Also, Figure 4 is an exploded perspective view of an interchangeable lens barrel for a single-lens reflex camera, which is an example of a preferred embodiment of the optical device of the present invention. A fixed barrel 712, a linear guide barrel 713, and a front group barrel 714 are fixed to a detachable mount 711 for the camera. These are fixed members of the interchangeable lens barrel.
[0095] A linear guide groove 713a in the optical axis direction for the focus lens 702 is formed in the linear guide barrel 713. Cam rollers 717a, 717b protruding radially outward are fixed to a rear group barrel 716 holding the focus lens 702 by shaft screws 718, and the cam roller 717a fits into the linear guide groove 713a.
[0096] A cam ring 715 is rotatably fitted on the inner periphery of the linear guide barrel 713. The relative movement between the linear guide barrel 713 and the cam ring 715 in the optical axis direction is restricted by a roller 719 fixed to the cam ring 715 fitting into a circumferential groove 713b of the linear guide barrel 713. A cam groove 715a for the focus lens 702 is formed in this cam ring 715, and the above-mentioned cam roller 717b is fitted into the cam groove 715a at the same time.
[0097] A rotation transmission ring 720 is disposed on the outer periphery of the fixed barrel 712, and is held by a ball race 727 so as to be rotatable at a fixed position relative to the fixed barrel 712. In the rotation transmission ring 720, rollers 722 are rotatably held on shafts 720f extending radially from the rotation transmission ring 720, and large diameter portions 722a of the rollers 722 are in contact with a mount side end face 724b of the manual focus ring 724. In addition, small diameter portions 722b of the rollers 722 are in contact with a joining member 729. Six rollers 722 are disposed at equal intervals on the outer periphery of the rotation transmission ring 720, and each roller is configured as described above.
[0098] A low-friction sheet (washer member) 733 is disposed on the inner diameter portion of the manual focus ring 724, and this low-friction sheet is sandwiched between a mount side end face 712a of the fixed barrel 712 and a front end face 724a of the manual focus ring 724. The outer diameter surface of the low-friction sheet 733 is ring-shaped and radially fits into an inner diameter 724c of the manual focus ring 724, which in turn radially fits into an outer diameter portion 712b of the fixed barrel 712. The low-friction sheet 733 serves to reduce friction in a rotating ring mechanism in which the manual focus ring 724 rotates relatively to the fixed barrel 712 around the optical axis.
[0099] The large diameter portion 722a of the roller 722 and the mount side end surface 724b of the manual focus ring are in contact with each other under a pressure applied thereto by the force of the wave washer 726 pressing the ultrasonic motor 725 toward the front of the lens. Similarly, the small diameter portion 722b of the roller 722 and the joining member 729 are in contact with each other under a moderate pressure applied thereto by the force of the wave washer 726 pressing the ultrasonic motor 725 toward the front of the lens. The movement of the wave washer 726 toward the mount direction is restricted by a washer 732 bayonet-coupled to the fixed barrel 712, and the spring force (biasing force) generated by the wave washer 726 is transmitted to the ultrasonic motor 725 and further to the roller 722, and also serves as a pressing force of the manual focus ring 724 against the mount side end surface 712a of the fixed barrel 712. In other words, the manual focus ring 724 is assembled in a state where it is pressed against the mount side end surface 712 a of the fixed barrel 712 via the low friction sheet 733 .
[0100] Therefore, when the ultrasonic motor 725 is driven to rotate relative to the fixed cylinder 712 by a control unit (not shown), the joining member 729 is in frictional contact with the small diameter portion 722b of the roller 722, so that the roller 722 rotates around the center of the shaft 720f. When the roller 722 rotates around the shaft 720f, the rotation transmission ring 720 rotates around the optical axis (autofocus operation).
[0101] Furthermore, when a rotational force about the optical axis is applied to the manual focus ring 724 from a manual operation input unit (not shown), the mount side end face 724b of the manual focus ring 724 is in pressure contact with the large diameter portion 722a of the roller 722, so that the roller 722 rotates about the axis 720f due to frictional force. When the large diameter portion 722a of the roller 722 rotates about the axis 720f, the rotation transmission ring 720 rotates about the optical axis. At this time, the ultrasonic motor 725 does not rotate due to the frictional holding force between the rotor 725c and the stator 725b (manual focus operation).
[0102] Two focus keys 728 are attached to the rotation transmission ring 720 at positions facing each other, and the focus keys 728 fit into notches 715b provided at the tip of the cam ring 715. Therefore, when an autofocus operation or a manual focus operation is performed and the rotation transmission ring 720 is rotated around the optical axis, the rotational force is transmitted to the cam ring 715 via the focus keys 728. When the cam ring is rotated around the optical axis, the rear group barrel 716, whose rotation is restricted by the cam rollers 717a and the linear guide grooves 713a, advances and retreats along the cam grooves 715a of the cam ring 715 by the cam rollers 717b. This drives the focus lens 702 and performs the focus operation.
[0103] Here, we have described an interchangeable lens barrel for a single-lens reflex camera as the optical device of the present invention, but the present invention can be applied to optical devices that have an ultrasonic motor in the drive section, regardless of the type of camera, such as compact cameras, electronic still cameras, and camera-equipped portable information terminals.
[0104] (Vibration device and dust removal device) 2. Description of the Related Art Vibration devices that are used for transporting, removing, and the like of particles, powder, and droplets are widely used in electronic devices and the like.
[0105] A dust removing device using the piezoelectric element of the present invention will be described below as an example of the vibration device of the present invention.
[0106] The dust removing device according to the present invention is characterized in that it has a vibrating body in which the piezoelectric element or the laminated piezoelectric element is arranged on a vibrating plate, that is, the vibrating section is provided with a vibrating device.
[0107] 5(a) and 5(b) are schematic diagrams showing one embodiment of a dust removal device of the present invention. Dust removal device 310 is composed of a plate-shaped piezoelectric element 330 and a vibration plate 320. The material of vibration plate 320 is not limited, but when dust removal device 310 is used in an optical device, a light-transmitting material or a light-reflective material can be used for vibration plate 320.
[0108] Fig. 6 is a schematic diagram showing the configuration of the piezoelectric element 330 in Fig. 5. Fig. 6(a) and Fig. 6(c) show the configuration of the front and back surfaces of the piezoelectric element 330, and Fig. 6(b) shows the configuration of the side surface. As shown in Fig. 5(a), the piezoelectric element 330 is composed of a piezoelectric ceramic 331, a first electrode 332, and a second electrode 333, and the first electrode 332 and the second electrode 333 are arranged to face the plate surface of the piezoelectric ceramic 331.
[0109] In FIG. 6(c), the surface on which the first electrode 332 protruding in front of the piezoelectric element 330 is disposed is referred to as the first electrode surface 336, and in FIG. 6(a), the surface on which the second electrode 333 protruding in front of the piezoelectric element 330 is disposed is referred to as the second electrode surface 337.
[0110] Here, the electrode surface in the present invention refers to the surface of the piezoelectric element on which the electrode is disposed. For example, the first electrode 332 may wrap around to the second electrode surface 337 as shown in FIG.
[0111] As shown in Figures 5(a) and 5(b), the piezoelectric element 330 and the diaphragm 320 are fixed to the plate surface of the diaphragm 320 by a first electrode surface 336 of the piezoelectric element 330. Then, by driving the piezoelectric element 330, stress is generated between the piezoelectric element 330 and the diaphragm 320, and out-of-plane vibration is generated in the diaphragm. The dust removal device 310 of the present invention is a device that removes foreign matter such as dust attached to the surface of the diaphragm 320 by the out-of-plane vibration of the diaphragm 320. The out-of-plane vibration means an elastic vibration that displaces the diaphragm in the optical axis direction, that is, in the thickness direction of the diaphragm.
[0112] FIG. 7 is a schematic diagram showing the vibration principle of the dust removal device 310 of the present invention. FIG. 7(a) shows a state in which an alternating voltage of the same phase is applied to a pair of left and right piezoelectric elements 330 to generate out-of-plane vibration in the vibration plate 320. The polarization direction of the piezoelectric ceramics constituting the pair of left and right piezoelectric elements 330 is the same as the thickness direction of the piezoelectric elements 330, and the dust removal device 310 is driven in a seventh vibration mode. FIG. 7(b) shows a state in which an alternating voltage of an opposite phase, which is 180° out of phase, is applied to the pair of left and right piezoelectric elements 330 to generate out-of-plane vibration in the vibration plate 320. The dust removal device 310 is driven in a sixth vibration mode. The dust removal device 310 of the present invention is a device that can effectively remove dust attached to the surface of the vibration plate by using at least two vibration modes appropriately.
[0113] (Imaging device) Next, the imaging device of the present invention will be described. The imaging device of the present invention is an imaging device having at least the dust removal device and an imaging element unit, and is characterized in that the vibration plate of the dust removal device is provided on the light receiving surface side of the imaging element unit. Figures 8 and 9 are diagrams showing a digital single-lens reflex camera that is an example of a preferred embodiment of the imaging device of the present invention.
[0114] Fig. 8 is a front perspective view of camera body 601 as viewed from the subject side with the photographing lens unit removed. Fig. 9 is an exploded perspective view showing a schematic configuration inside the camera for explaining the peripheral structure of the dust removal device and imaging unit 400 of the present invention.
[0115] A mirror box 605 to which a photographing light beam that has passed through a photographing lens is provided within the camera body 601, and a main mirror (quick return mirror) 606 is disposed within the mirror box 605. The main mirror 606 can be held at an angle of 45° with respect to the photographing optical axis in order to guide the photographing light beam in the direction of a pentagonal roof mirror (not shown), or held at a position retracted from the photographing light beam in order to guide it in the direction of an image sensor (not shown).
[0116] A mirror box 605 and a shutter unit 200 are arranged, in that order from the subject side, on the subject side of the main body chassis 300, which forms the framework of the camera body. In addition, an imaging unit 400 is arranged on the photographer side of the main body chassis 300. The imaging unit 400 is installed such that the imaging surface of the imaging element is spaced a predetermined distance from and adjusted to be parallel to the attachment surface of a mount section 602, which serves as a reference for attaching a photographing lens unit.
[0117] Here, a digital single-lens reflex camera has been described as the imaging device of the present invention, but the imaging device may also be a camera with an interchangeable lens unit, such as a mirrorless digital single-lens camera that does not have a mirror box 605. The imaging device may also be applied to video cameras with interchangeable lens units, copiers, facsimiles, scanners, and other imaging devices or electronic and electrical devices equipped with imaging devices, particularly devices that require the removal of dust adhering to the surfaces of optical components.
[0118] (Ultrasound probe) Next, the ultrasonic probe of the present invention will be described. The ultrasonic probe of the present invention is characterized in that it has the piezoelectric element and transmits and receives waves by the piezoelectric element.
[0119] FIG. 10 is a schematic cross-sectional view showing one embodiment of an ultrasonic probe of the present invention. The ultrasonic probe 1100 in Fig. 10 is composed of a piezoelectric element 1101, a backing material 1102, an acoustic matching layer 1103, and an acoustic lens 1104. As shown in Fig. 10, a plurality of piezoelectric elements 1101 are arranged and bonded on the backing material 1102, and an acoustic matching layer 1103 for matching acoustic impedance is provided on the opposite surface, which is the transmitting / receiving surface.
[0120] Acoustic matching layer 1103 may be a single layer or multiple layers, and preferably is two or more layers. Materials that can be used for acoustic matching layer 1103 include, for example, carbon, aluminum, aluminum alloy (e.g., AL-Mg alloy), magnesium alloy, Macol glass, glass, fused quartz, copper graphite, polyethylene, polypropylene, polycarbonate, ABC resin, polyphenylene ether, ABS resin, AAS resin, AES resin, nylon, polyamideimide, polyethylene terephthalate, polycarbonate, epoxy resin, urethane resin, etc.
[0121] In addition, the backing material 1102 can be made of thermoplastic resins such as natural rubber, ferrite rubber, epoxy resin, vinyl chloride, polyvinyl butyral, ABS resin, polyurethane, polyvinyl alcohol, polyethylene, polypropylene, polyacetal, polyethylene terephthalate, fluororesin, polyethylene glycol, and polyethylene terephthalate, or these mixed with metal powder, or a super-hard material such as tungsten carbide.
[0122] Piezoelectric element 1101 may be one unit or divided into multiple pieces. Fig. 10 shows an example in which it is divided. A flexible cable (not shown) is connected to the electrodes of each piezoelectric element, allowing signals transmitted and received by the piezoelectric element to be input and output. Acoustic lens 1104 is bonded to acoustic matching layer 1103. Acoustic lens 1104 is a member for converging ultrasonic waves transmitted from piezoelectric element 1101 toward the subject, and has an arc shape in the example of Fig. 10. Note that, as a material for acoustic lens 1104, rubber mainly composed of silicone resin (rubber), for example, is generally used.
[0123] When using this ultrasonic probe 1100, an alternating voltage is applied to the piezoelectric element 1101 through a flexible cable, and the piezoelectric element is vibrated by the piezoelectric effect, causing the piezoelectric element 1101 to transmit ultrasonic waves. At this time, if the acoustic impedance of the subject on which the ultrasonic waves are applied is small, or if the ultrasonic waves are applied to the subject through water or air, the presence of the acoustic matching layer 1103 makes it possible to suppress reflected waves caused by large changes in acoustic impedance, and the ultrasonic waves can be efficiently irradiated to the subject. Then, at the time of reception, the piezoelectric element 1101 vibrates due to the ultrasonic waves reflected from inside the subject, and this vibration is electrically converted by the piezoelectric effect to obtain a received signal. At the time of transmission and reception, conversion between electrical energy and mechanical energy is performed, and the conversion efficiency at this time depends on the magnitude of the electromechanical coupling coefficient.
[0124] (Ultrasound diagnostic equipment) Next, the ultrasonic diagnostic device of the present invention will be described. The ultrasonic diagnostic device of the present invention is characterized by having at least the ultrasonic probe and an image output unit. FIG. 11 is a schematic diagram showing one embodiment of the ultrasonic diagnostic device of the present invention. The ultrasonic diagnostic device 1110 of FIG. 11 is composed of an ultrasonic probe 1100, a cable 1111, a drive control unit 1113, and an image output unit. The flexible cable of the ultrasonic probe 1100 and the drive control unit 1113 are connected by the cable 1111, and an alternating voltage is applied from the drive control unit 1113 to the piezoelectric element 1101 of the ultrasonic probe 1100 via the cable 1111. When ultrasonic waves are irradiated from the ultrasonic probe 1100 into the subject, the ultrasonic waves reflected from inside the subject are converted into electrical signals again by the ultrasonic probe, and input to the image processing unit 1114 through the cable 1111. The image processing unit 1114 creates image data by performing calculations based on the delay time and the change in signal intensity relative to the alternating voltage output from the drive control unit 1113. The created image data is output to the image output unit 1112.
[0125] (electronic equipment) Next, the electronic device of the present invention will be described. The electronic device of the present invention is characterized by being equipped with a piezoelectric acoustic component having the piezoelectric element or the laminated piezoelectric element. The piezoelectric acoustic component includes a speaker, a buzzer, a microphone, and a surface acoustic wave (SAW) element.
[0126] 12 is an overall perspective view seen from the front of a digital camera body 931, which is an example of a preferred embodiment of an electronic device of the present invention. On the front of body 931, optical device 901, microphone 914, strobe light emission unit 909, and fill light unit 916 are arranged. Microphone 914 is shown by a dashed line as it is built into the body. A hole is provided in front of microphone 914 to pick up sound from the outside.
[0127] A power button 933, a speaker 912, a zoom lever 932, and a release button 908 for performing a focusing operation are arranged on the top surface of the main body 931. The speaker 912 is incorporated inside the main body 931 and is indicated by a dashed line. A hole is provided in front of the speaker 912 to transmit sound to the outside.
[0128] The piezoelectric acoustic component of the present invention is used in at least one of the microphone 914, the speaker 912, and the surface acoustic wave element.
[0129] Here, a digital camera has been described as an example of the electronic device of the present invention, but the electronic device of the present invention can also be applied to electronic devices having various piezoelectric acoustic components, such as audio playback devices, audio recording devices, mobile phones, and information terminals.
[0130] As described above, the piezoelectric element of the present invention is suitable for use in ultrasonic motors, optical instruments, vibration devices, dust removal devices, imaging devices, ultrasonic probes, ultrasonic diagnostic devices and electronic devices.
[0131] By using the piezoelectric element of the present invention, it is possible to provide an ultrasonic motor having driving efficiency equal to or higher than that of a piezoelectric element containing lead.
[0132] By using the ultrasonic motor of the present invention, it is possible to provide an optical device having an operating speed and operating efficiency equal to or greater than that of a piezoelectric element containing lead.
[0133] By using the piezoelectric element of the present invention, it is possible to provide a vibration device having vibration capabilities equal to or greater than those of a piezoelectric element containing lead.
[0134] By using the vibration device of the present invention, it is possible to provide a dust removal device having dust removal efficiency equal to or greater than that of a device using a piezoelectric element containing lead.
[0135] By using the dust removing device of the present invention, it is possible to provide an imaging device having a dust removing function equal to or better than that of a device using a piezoelectric element containing lead.
[0136] By using the piezoelectric element of the present invention, it is possible to provide an ultrasonic probe having transmission and reception performance equal to or better than that of a piezoelectric element containing lead.
[0137] By using the ultrasonic probe of the present invention, it is possible to provide an ultrasonic diagnostic apparatus having driving efficiency equal to or higher than that of a piezoelectric element containing lead.
[0138] By using a piezoelectric acoustic component including a piezoelectric element of the present invention, it is possible to provide electronic equipment that has sound generation properties equal to or greater than those achieved by using a piezoelectric element containing lead.
[0139] In addition to the above-mentioned devices, the piezoelectric ceramics and piezoelectric element of the present invention can be used in devices such as motors, liquid discharge heads, liquid discharge apparatuses, piezoelectric actuators, piezoelectric sensors, and ferroelectric memories. EXAMPLES
[0140] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples. The piezoelectric ceramic and piezoelectric element of the present invention were produced by the method described below.
[0141] Example 1 The raw powders were barium titanate (BaTiO3, Ba / Ti=0.9985) with an average particle size of 100 nm, calcium titanate (CaTiO3, Ca / Ti=0.9978), calcium zirconate (CaZrO3, Ca / Zr=0.999), bismuth oxide (Bi2O3), trimanganese tetroxide (Mn3O4), and barium carbonate was used to adjust the ratio a of the sum of the moles of Ti and Zr to the sum of the moles of Ba and Ca. These raw powders were mixed together with the composition formula (Ba 0.86 , Ca 0.14 ) 1.002 (Ti 0.93 ,Zr 0.07)O3 ratio. Mn was added to 100 parts by weight of this metal oxide so that the content was 0.16 parts by weight in terms of metal. Furthermore, Bi was added to this metal oxide to which Mn had been added so that the content was 0.17 parts by weight in terms of metal, and mixed by dry mixing for 24 hours using a ball mill. To granulate the resulting mixed powder, 3 parts by weight of PVA binder was attached to the surface of the mixed powder using a spray dryer device.
[0142] Next, the obtained granulated powder was filled into a metal mold, and a molding pressure of 200 MPa was applied using a press molding machine to produce a disk-shaped molded body. This molded body may be further pressed using a cold isostatic pressing machine.
[0143] The obtained molded body was placed in an electric furnace and held at a maximum temperature of 1300°C for 5 hours, and then sintered in air for a total of 24 hours to obtain a disk-shaped sintered body.
[0144] The average equivalent circular diameter and relative density of the crystal grains constituting the obtained sintered body were evaluated. As a result, the average equivalent circular diameter was 8 μm and the relative density was 98%. A polarizing microscope was mainly used to observe the crystal grains. A scanning electron microscope (SEM) was used to identify the grain size of small crystal grains. The average equivalent circular diameter was calculated from the observation results. The relative density was evaluated using the theoretical density calculated from the lattice constant obtained from X-ray diffraction and the weighed composition, and the actual density measured by the Archimedes method.
[0145] Next, both sides of the obtained disk-shaped sintered body were polished using a polishing machine while changing the grit size of the abrasive grains so that the thickness became 0.5 mm, and finally, chemical polishing was performed as a finishing polishing.
[0146] The roughness Ra of the polished surface of the sintered body was then measured. The roughness Ra was measured using a stylus-type surface step gauge with a tip curvature radius of 1 μm. The measurement conditions for roughness Ra were a stylus scanning speed of 5 μm per second, a scanning distance of 200 μm, and a sampling rate of 200 Sa per second. The resulting roughness Ra was 0.03 μm.
[0147] Next, the crystal structure of the polished sintered body was analyzed by X-ray diffraction, and only peaks corresponding to the perovskite structure were observed.
[0148] Next, the composition of the sintered body was evaluated by ICP emission spectroscopy.The results showed that the weighed composition of Ba, Ca, Ti, Zr, Mn, and Bi was consistent with the composition after sintering.
[0149] Next, the polished sintered body was placed in an electric furnace and annealed in air at a maximum temperature of 990°C for 120 minutes to obtain the piezoelectric ceramic of the present invention. The surface roughness Ra of the polished surface of the obtained piezoelectric ceramic was measured. The roughness Ra was measured using a stylus-type surface step gauge with a tip radius of curvature of 1 μm. The measurement conditions for roughness Ra were a stylus scanning speed of 5 μm per second, a scanning distance of 200 μm, and a sampling rate of 200 Sa per second. As a result, the surface roughness Ra after annealing was 0.03 μm, which was the same as the surface roughness Ra before annealing.
[0150] Next, gold electrodes with a thickness of 400 nm were formed on the front and back of the piezoelectric ceramic by DC sputtering. A 30 nm titanium film was formed between the electrode and the ceramic as an adhesive layer. The ceramic with the electrode was cut to produce a rectangular piezoelectric element of the present invention with a size of 10 mm x 2.5 mm x 0.5 mm. The obtained piezoelectric element was subjected to polarization treatment by setting the surface of a hot plate to 60°C to 100°C and applying an electric field of 1 kV / mm on the hot plate for 30 minutes.
[0151] Next, as the static characteristics of the piezoelectric element having the piezoelectric ceramic of the present invention, the electromechanical coupling coefficient k 31 The mechanical quality factor Qm was evaluated by a resonance-antiresonance method at room temperature (25° C.) using an impedance analyzer (4294A manufactured by Agilent Technologies).
[0152] The electromechanical coupling coefficient was measured in 5°C increments while changing the temperature of the sample from 60°C to 0°C at a rate of 0.5°C per minute. The electromechanical coupling coefficient k 31 The fluctuation rate of was derived according to the following equation (4).
number
[0153] Next, the power consumption of the rectangular piezoelectric element was evaluated. The power consumption was measured with a power meter when an alternating voltage was applied and the magnitude and frequency of the alternating voltage were changed so that the displacement was 1.0 μm. The displacement was measured with a laser Doppler vibrometer. The power consumption in this case was 16 mW.
[0154] (Examples 2 to 8) Piezoelectric ceramics and piezoelectric elements according to the present invention of Examples 2 to 8 were obtained in the same manner as in Example 1, except for the maximum temperature and the time for which the maximum temperature was maintained in the polishing step and the annealing step.
[0155] In the polishing process, both sides were polished using a polishing machine while changing the grit size so that the thickness was 0.5 mm, and finally, the polishing was finished using a polishing machine with a grit size of 4000. The specific values for the maximum temperature and the holding time at the maximum temperature in the annealing process are shown in Table 1.
[0156] Next, in the same process as in Example 1, the crystal structure of the piezoelectric ceramic constituting the piezoelectric element of the present invention, the surface roughness Ra before and after the annealing treatment, and the electromechanical coupling coefficient k 31 , k in each temperature range 31 The fluctuation rate of the temperature, the mechanical quality factor Qm, and the power consumption were evaluated. The results are shown in Table 2.
[0157] (Examples 9 to 11) The piezoelectric ceramics and piezoelectric elements of the present invention of Examples 9 to 11 were obtained in the same manner as in Example 1, except for the polishing step, the annealing treatment step, and the method of forming the electrodes.
[0158] In the polishing process of Examples 9 to 11, both sides were polished using a polishing machine while changing the grit size of the abrasive grains until the thickness reached 0.5 mm, and finally, the polishing was finished using a polishing machine with abrasive grains of No. 4000.
[0159] In addition, in Examples 9 to 11, a paste of Ag electrodes, instead of gold electrodes, was applied to both sides of the piezoelectric ceramic by screen printing, and the piezoelectric element having the piezoelectric ceramic of the present invention was obtained by placing the piezoelectric element in an electric furnace and performing an annealing process in an air atmosphere. However, in Examples 9 and 10, the annealing process was not performed before applying the Ag electrode paste, whereas in Example 11, the annealing process was performed before applying the Ag electrode paste, so that the annealing process was essentially performed twice.
[0160] The annealing temperature and holding time in the annealing process, and the temperature and time in baking the electrodes are shown in Table 1. The surface roughness Ra after the annealing process was measured on the polished surface on which the electrodes were not applied. The surface roughness Ra was measured under the same conditions as in Example 1.
[0161] Next, in the same process as in Example 1, the crystal structure of the piezoelectric ceramic constituting the piezoelectric element of the present invention, the surface roughness Ra before and after the annealing treatment, and the electromechanical coupling coefficient k 31 , k in each temperature range 31 The fluctuation rate of the temperature, the mechanical quality factor Qm, and the power consumption were evaluated. The results are shown in Table 2.
[0162] Example 12 The raw material powders used were barium titanate (BaTiO3, Ba / Ti = 0.9985) with an average particle size of 100 nm, calcium titanate (CaTiO3, Ca / Ti = 0.9978), and trimanganese tetroxide (Mn3O4), and barium carbonate was used to adjust the ratio a of the sum of the moles of Ti and Zr to the sum of the moles of Ba and Ca.
[0163] These raw powders were treated with a composition formula (Ba 0.96 , Ca 0.04 ) 1.005 The mixture was weighed out so that the ratio of TiO3 to Mn was 0.10 parts by weight per 100 parts by weight of the metal oxide. The metal oxide to which Mn was added was then mixed by dry mixing for 24 hours using a ball mill. To granulate the resulting mixed powder, 3 parts by weight of PVA binder was attached to the surface of the mixed powder using a spray dryer.
[0164] Next, the obtained granulated powder was filled into a metal mold, and a molding pressure of 200 MPa was applied using a press molding machine to produce a disk-shaped molded body. This molded body may be further pressed using a cold isostatic pressing machine.
[0165] The obtained molded body was placed in an electric furnace, held at a maximum temperature of 1200°C for 5 hours, and sintered in air for a total of 24 hours to obtain a sintered body.
[0166] The average equivalent circular diameter and relative density of the crystal grains constituting the obtained sintered body were then evaluated. As a result, the average equivalent circular diameter was 10 μm and the relative density was 96%. A polarizing microscope was mainly used to observe the crystal grains. A scanning electron microscope (SEM) was used to identify the grain size of small crystal grains. The average equivalent circular diameter was calculated from the observation results. The relative density was evaluated using the theoretical density calculated from the lattice constant obtained from X-ray diffraction and the weighed composition, and the actual density measured using the Archimedes method.
[0167] Next, both sides of the obtained disk-shaped sintered body were polished using a polishing machine while changing the grit size of the abrasive grains so that the thickness became 0.5 mm, and finally, the polishing was finished using a polishing machine with abrasive grains of No. 2000.
[0168] The surface roughness Ra of the polished surface of the sintered body was then measured. A stylus with a tip curvature radius of 1 μm was used for the stylus-type surface step measurement system. The surface roughness Ra measurement conditions were a stylus scanning speed of 5 μm per second, a scanning distance of 200 μm, and a sampling rate of 200 Sa per second. The resulting surface roughness Ra was 0.19 μm.
[0169] Next, the crystal structure of the polished sintered body was analyzed by X-ray diffraction, and only peaks corresponding to the perovskite structure were observed.
[0170] Next, the composition of the sintered body was evaluated by ICP emission spectroscopy.The results showed that the weighed composition of Ba, Ca, Ti, and Mn was consistent with the composition after sintering.
[0171] Next, the polished sintered body was placed in an electric furnace and annealed in air at a maximum temperature of 990°C for 120 minutes to obtain the piezoelectric ceramic of the present invention. The surface roughness Ra of the polished surface of the obtained piezoelectric ceramic was measured. The roughness Ra was measured using a stylus-type surface step gauge with a stylus having a tip radius of curvature of 1 μm. The measurement conditions for the surface roughness Ra were a stylus scanning speed of 5 μm per second, a scanning distance of 200 μm, and a sampling rate of 200 Sa per second. As a result, the surface roughness Ra after the annealing treatment was 0.19 μm, which was the same as the surface roughness Ra before the annealing treatment.
[0172] Next, gold electrodes with a thickness of 400 nm were formed on the front and back of the piezoelectric ceramic by DC sputtering. A 30 nm titanium film was formed between the electrode and the ceramic as an adhesive layer. The ceramic with the electrode was cut to produce a rectangular piezoelectric element of the present invention with a size of 10 mm x 2.5 mm x 0.5 mm. The obtained piezoelectric element was subjected to polarization treatment by setting the surface of a hot plate to 60°C to 100°C and applying an electric field of 1 kV / mm on the hot plate for 30 minutes.
[0173] Next, in the same process as in Example 1, the crystal structure of the piezoelectric ceramic constituting the piezoelectric element of the present invention, the surface roughness Ra before and after the annealing treatment, and the electromechanical coupling coefficient k 31 , k in each temperature range 31 The fluctuation rate of the temperature, the mechanical quality factor Qm, and the power consumption were evaluated. The results are shown in Table 2.
[0174] (Example 13) The raw material powders used were barium titanate (BaTiO3, Ba / Ti=0.9985) with an average particle size of 100 nm, calcium titanate (CaTiO3, Ca / Ti=0.9978), calcium zirconate (CaZrO3, Ca / Zr=0.999), and trimanganese tetroxide (Mn3O4), as well as barium carbonate to adjust the ratio a of the sum of the moles of Ti and Zr to the sum of the moles of Ba and Ca.
[0175] These raw powders were treated with a composition formula (Ba 0.86 , Ca 0.14 ) 1.0026 (Ti 0.94 ,Zr 0.06 )O3 ratio. Mn was added so that the content was 0.10 parts by weight in terms of metal per 100 parts by weight of this metal oxide. Furthermore, this metal oxide to which Mn was added was mixed by dry mixing for 24 hours using a ball mill. In order to granulate the obtained mixed powder, 3 parts by weight of PVA binder was attached to the surface of the mixed powder using a spray dryer device.
[0176] Next, the obtained granulated powder was filled into a metal mold, and a molding pressure of 200 MPa was applied using a press molding machine to produce a disk-shaped molded body. This molded body may be further pressed using a cold isostatic pressing machine.
[0177] The obtained molded body was placed in an electric furnace, held at a maximum temperature of 1340°C for 5 hours, and sintered in air for a total of 24 hours to obtain a sintered body.
[0178] The average equivalent circular diameter and relative density of the crystal grains constituting the obtained sintered body were then evaluated. As a result, the average equivalent circular diameter was 10 μm and the relative density was 96%. A polarizing microscope was mainly used to observe the crystal grains. A scanning electron microscope (SEM) was used to identify the grain size of small crystal grains. The average equivalent circular diameter was calculated from the observation results. The relative density was evaluated using the theoretical density calculated from the lattice constant obtained from X-ray diffraction and the weighed composition, and the actual density measured using the Archimedes method.
[0179] Next, both sides of the obtained disk-shaped sintered body were polished using a polishing machine while changing the grit size of the abrasive grains so that the thickness became 0.5 mm, and finally, the polishing was finished using a polishing machine with abrasive grains of No. 2000.
[0180] The surface roughness Ra of the polished surface of the sintered body was then measured. The roughness Ra was measured using a stylus-type surface step gauge with a tip radius of curvature of 1 μm. The surface roughness Ra was measured under the following conditions: needle scanning speed 5 μm per second, scanning distance 200 μm, and sampling rate 200 Sa per second. The resulting surface roughness Ra was 0.19 μm.
[0181] Next, the crystal structure of the polished sintered body was analyzed by X-ray diffraction, and only peaks corresponding to the perovskite structure were observed.
[0182] Next, the composition of the sintered body was evaluated by ICP emission spectroscopy.The results showed that the weighed composition of Ba, Ca, Ti, Zr, and Mn was consistent with the composition after sintering.
[0183] Next, the polished sintered body was placed in an electric furnace and annealed in air at a maximum temperature of 990°C for 120 minutes to obtain the piezoelectric ceramic of the present invention. The surface roughness Ra of the polished surface of the obtained piezoelectric ceramic was measured. The roughness Ra was measured using a stylus-type surface step gauge with a tip curvature radius of 1 μm. The measurement conditions for the surface roughness Ra were a stylus scanning speed of 5 μm per second, a scanning distance of 200 μm, and a sampling rate of 200 Sa per second. As a result, the surface roughness Ra after the annealing treatment was 0.19 μm, which was the same as the surface roughness Ra before the annealing treatment process.
[0184] Next, gold electrodes with a thickness of 400 nm were formed on the front and back of the piezoelectric ceramic by DC sputtering. A 30 nm titanium film was formed between the electrode and the ceramic as an adhesive layer. The ceramic with the electrode was cut to produce a rectangular piezoelectric element of the present invention with a size of 10 mm x 2.5 mm x 0.5 mm. The obtained piezoelectric element was subjected to polarization treatment by setting the surface of a hot plate to 60°C to 100°C and applying an electric field of 1 kV / mm on the hot plate for 30 minutes.
[0185] Next, in the same process as in Example 1, the crystal structure of the piezoelectric ceramic constituting the piezoelectric element of the present invention, the surface roughness Ra before and after the annealing treatment, and the electromechanical coupling coefficient k 31 , k in each temperature range 31 The fluctuation rate of the temperature, the mechanical quality factor Qm, and the power consumption were evaluated. The results are shown in Table 2.
[0186] Comparative Example 1 The raw powders were barium titanate (BaTiO3, Ba / Ti=0.9985) with an average particle size of 100 nm, calcium titanate (CaTiO3, Ca / Ti=0.9978), calcium zirconate (CaZrO3, Ca / Zr=0.999), bismuth oxide (Bi2O3), trimanganese tetroxide (Mn3O4), and barium carbonate was used to adjust the ratio a of the sum of the moles of Ti and Zr to the sum of the moles of Ba and Ca. These raw powders were mixed together with the composition formula (Ba 0.86, Ca 0.14 ) 1.002 (Ti 0.93 ,Zr 0.07 )O3 ratio. Mn was added to 100 parts by weight of this metal oxide so that the content was 0.16 parts by weight in terms of metal. Furthermore, Bi was added to this metal oxide to which Mn had been added so that the content was 0.17 parts by weight in terms of metal, and mixed by dry mixing for 24 hours using a ball mill. To granulate the resulting mixed powder, 3 parts by weight of PVA binder was attached to the surface of the mixed powder using a spray dryer device.
[0187] Next, the obtained granulated powder was filled into a metal mold, and a molding pressure of 200 MPa was applied using a press molding machine to produce a disk-shaped molded body. This molded body may be further pressed using a cold isostatic pressing machine.
[0188] The obtained molded body was placed in an electric furnace, held at a maximum temperature of 1300°C for 5 hours, and sintered in air for a total of 24 hours to obtain a sintered body.
[0189] The average equivalent circular diameter and relative density of the crystal grains constituting the obtained sintered body were then evaluated. As a result, the average equivalent circular diameter was 7 μm and the relative density was 96%. A polarizing microscope was mainly used to observe the crystal grains. A scanning electron microscope (SEM) was used to identify the grain size of small crystal grains. The average equivalent circular diameter was calculated from the observation results. The relative density was evaluated using the theoretical density calculated from the lattice constant obtained from X-ray diffraction and the weighed composition, and the actual density measured using the Archimedes method.
[0190] Next, both sides of the obtained disk-shaped sintered body were polished using a polishing machine while changing the grit size of the abrasive grains until the thickness became 0.5 mm, and finally, the polishing was finished using a polishing machine with abrasive grains of No. 2000 to obtain the piezoelectric ceramic of Comparative Example 1.
[0191] The surface roughness Ra of the polished surface of the piezoelectric ceramic was then measured. A stylus-type surface step gauge was used to measure the roughness Ra, with a needle having a tip with a radius of curvature of 1 μm. The conditions for measuring the surface roughness Ra were a needle scanning speed of 5 μm per second, a scanning distance of 200 μm, and a sampling rate of 200 Sa per second. The resulting surface roughness Ra was 0.13 μm.
[0192] Next, the crystal structure of the polished sintered body was analyzed by X-ray diffraction, and only peaks corresponding to the perovskite structure were observed.
[0193] Next, the composition of the sintered body was evaluated by ICP emission spectroscopy.The results showed that the weighed composition of Ba, Ca, Ti, Zr, Mn, and Bi was consistent with the composition after sintering.
[0194] Next, gold electrodes with a thickness of 400 nm were formed on the front and back of the piezoelectric ceramic by DC sputtering. A 30 nm titanium film was formed between the electrode and the ceramic as an adhesive layer. The ceramic with the electrode was cut to produce a rectangular piezoelectric element of Comparative Example 1 with a size of 10 mm x 2.5 mm x 0.5 mm. The obtained piezoelectric element was subjected to polarization treatment by setting the surface of a hot plate to 60°C to 100°C and applying an electric field of 1 kV / mm on the hot plate for 30 minutes.
[0195] Next, in the same process as in Example 1, the crystal structure of the piezoelectric ceramic of Comparative Example 1 constituting the piezoelectric element, the surface roughness Ra after the polishing process, and the electromechanical coupling coefficient k 31 , k in each temperature range 31 The fluctuation rate of the temperature, the mechanical quality factor Qm, and the power consumption were evaluated. The results are shown in Table 2.
[0196] Comparative Example 2 A piezoelectric ceramic and a piezoelectric element of Comparative Example 2 were obtained in the same manner as in Comparative Example 1, except that an annealing treatment step was performed after the polishing step.
[0197] After the polishing process, the polished sintered body was placed in an electric furnace and annealed in air at a maximum temperature of 1000°C for 600 minutes to obtain a piezoelectric ceramic of Comparative Example 2. The surface roughness Ra of the polished surface of the obtained piezoelectric ceramic was measured. The roughness Ra was measured using a stylus-type surface step gauge with a tip curvature radius of 1 μm. The measurement conditions for the surface roughness Ra were a stylus scanning speed of 5 μm per second, a scanning distance of 200 μm, and a sampling rate of 200 Sa per second. As a result, the surface roughness Ra after the annealing treatment was 0.20 μm, which was larger than the surface roughness Ra before the annealing treatment. It is believed that the annealing treatment was performed at 1000°C in Comparative Example 2, so that the crystal grains on the polished surface grew, causing the surface roughness Ra to increase.
[0198] In the polishing process, both sides were polished using a polishing machine while changing the grit size so that the thickness was 0.5 mm, and finally, the polishing was finished using a polishing machine with a grit size of 4000. The specific values for the maximum temperature and the holding time at the maximum temperature in the annealing process are shown in Table 1.
[0199] Next, in the same process as in Example 1, the crystal structure of the piezoelectric ceramic constituting the piezoelectric element of the present invention, the surface roughness Ra before and after the annealing treatment, and the electromechanical coupling coefficient k 31 , k in each temperature range 31 The fluctuation rate of the temperature, the mechanical quality factor Qm, and the power consumption were evaluated. The results are shown in Table 2.
[0200] [Table 1]
[0201] [Table 2]
[0202] Example 14 An ultrasonic motor shown in Fig. 2 was fabricated using the piezoelectric element of Example 1. In the fabricated ultrasonic motor, rotation of the motor in response to application of an alternating voltage was confirmed.
[0203] Example 15 The ultrasonic motor of Example 14 was used to fabricate the optical device shown in Fig. 3. In the fabricated optical device, autofocus operation in response to application of an alternating voltage was confirmed.
[0204] Example 16 A dust removal device shown in Fig. 5 was produced using the piezoelectric element of Example 1. When plastic beads were scattered in the produced dust removal device and an alternating voltage was applied, a good dust removal rate was confirmed.
[0205] (Example 17) The imaging device shown in Fig. 8 was fabricated using the dust removal device of Example 16. When the fabricated imaging device was operated, dust on the surface of the imaging unit was successfully removed, and an image without dust defects was obtained.
[0206] (Example 18) An ultrasonic probe shown in Fig. 10 was fabricated using the piezoelectric element of Example 1. In the fabricated ultrasonic probe, ultrasonic waves were transmitted by application of an alternating voltage, and a received signal due to reflection from inside the subject was confirmed.
[0207] (Example 19) An ultrasonic diagnostic apparatus shown in Fig. 11 was fabricated using the ultrasonic probe of Example 18. When the fabricated ultrasonic diagnostic apparatus was operated, a clear image of the inside of the subject was output.
[0208] (Example 20) An electronic device shown in Fig. 12 was fabricated using the piezoelectric element of Example 1. In the fabricated electronic device, speaker operation in response to application of an alternating voltage was confirmed. [Industrial Applicability]
[0209] The piezoelectric ceramic of the present invention has a high piezoelectricity due to its large electromechanical coupling coefficient. In addition, since it does not contain lead, it has a low environmental impact. Therefore, the piezoelectric ceramic of the present invention can be used without problems in many devices that use piezoelectric ceramics, such as ultrasonic motors, dust removal devices, and ultrasonic probes. [Explanation of symbols]
[0210] 1. First electrode 2 Piezoelectric ceramics section 3 Second electrode 201 Transducer 202 Rotor 203 Output shaft 2011 Elastic Ring 2012 Piezoelectric element 2013 Organic adhesives 310 Dust removal equipment 320 diaphragm 330 Piezoelectric element 331 Piezoelectric Ceramics 332 First electrode 333 Second Electrode 336 First electrode surface 337 Second electrode surface 601 Camera body 602 Mounting section 605 Mirror Box 606 Main Mirror 200 Shutter unit 300 Main Chassis 400 Imaging unit 701 Front lens 702 Rear lens (focus lens) 711 Detachable Mount 712 Fixed tube 713 Straight guide tube 714 Front group tube 715 Cam Ring 716 Rear group tube 717 Cam Roller 718 Axle screw 719 Lola 720 Rotation Transmission Ring 722 Coro 724 Manual Focus Ring 725 Ultrasonic Motor 726 Wave washer 727 Ball Race 728 Focus Key 729 Joint materials 732 Washer 733 Low Friction Sheet 901 Optical equipment 908 Release button 909 Strobe light emitter 912 Speaker 914 Mike 916 Auxiliary Light Unit 931 Main unit 932 Zoom Lever 933 Power button 1100 Ultrasound Probe 1101 Piezoelectric element 1102 Backing layer 1103 Acoustic matching layer 1104 Acoustic Lens 1110 Ultrasound diagnostic equipment 1111 Cable 1112 Image output unit 1113 Drive control unit 1114 Image processing section
Claims
1. A method for producing a piezoelectric ceramic containing titanium and barium as its main components, comprising the steps of: A step of sintering the molded body containing the raw materials at 1000° C. or more to obtain a sintered body; polishing the sintered body; A method for producing a piezoelectric ceramic, comprising the step of annealing the polished sintered body at 950°C or higher but lower than 1000°C for 2 hours or higher but lower than 5 hours, wherein the piezoelectric ceramic is mainly composed of titanium and barium.
2. The method for producing a piezoelectric ceramic according to claim 1, a step of providing electrodes on the piezoelectric ceramic prior to the step of annealing; A method for manufacturing a piezoelectric element, comprising baking the electrodes in the annealing step.
3. A piezoelectric ceramic mainly composed of titanium and barium, Electromechanical coupling coefficient k at room temperature 31 is 0.275 or more, and wherein at least a portion of the surface of the piezoelectric ceramic has a roughness Ra of 0.19 μm or less.
4. A piezoelectric ceramic containing an oxide including Ba, Ca, Ti, and Zr, and Mn, x, which is a molar ratio of Ca to the sum of Ba and Ca, is 0.02≦x≦0.30; a molar ratio y of the Zr to the sum of the Ti and the Zr is 0.020≦y≦0.095; The y and the x have a relationship of y≦x, a, which is a molar ratio of the sum of the Ba and the Ca to the sum of the Ti and the Zr, is 1.00≦a≦1.01; 4. The piezoelectric ceramic according to claim 3, wherein the content of said Mn is 0.02 parts by weight or more and 0.40 parts by weight or less relative to 100 parts by weight of said oxide, calculated as metal.
5. The electromechanical coupling coefficient k in the temperature range of 0° C. to 60° C. 31 5. The piezoelectric ceramic according to claim 3, wherein the rate of change in the piezoelectric constant is 35% or less.
6. 6. The piezoelectric ceramic according to claim 3, wherein the mechanical quality factor Qm of the piezoelectric ceramic is 1000 or more.
7. 7. The piezoelectric ceramic according to claim 3, wherein the average equivalent circle diameter of crystal grains constituting the piezoelectric ceramic is 1 [mu]m or more and 10 [mu]m or less.
8. The piezoelectric ceramic according to any one of claims 3 to 7, wherein the relative density of the piezoelectric ceramic is 93% or more and 100% or less.
9. A piezoelectric element having a plurality of electrodes and a piezoelectric ceramic, the piezoelectric ceramic being the piezoelectric ceramic according to any one of claims 3 to 8.
10. 10. An ultrasonic motor comprising at least a vibrating body having the piezoelectric element according to claim 9 disposed thereon, and a moving body in contact with the vibrating body.
11. An optical device comprising the ultrasonic motor according to claim 10 in a drive section.
12. A vibration device comprising a vibrating body having the piezoelectric element according to claim 9 disposed on a vibration plate.
13. A dust removing device comprising a vibration section including the vibration device according to claim 12.
14. 14. An imaging device comprising at least the dust removal device according to claim 13 and an imaging element unit, wherein a diaphragm of the dust removal device is provided on a light receiving surface side of the imaging element unit.
15. 10. An ultrasonic probe comprising the piezoelectric element according to claim 9, for transmitting and receiving a signal by means of the piezoelectric element.
16. 16. An ultrasonic diagnostic apparatus comprising at least the ultrasonic probe according to claim 15 and an image output unit.
17. 10. An electronic device comprising a piezoelectric acoustic part having the piezoelectric element according to claim 9.
Citation Information
Patent Citations
Production of piezoelectric ceramics
JP1998279352A
Crystal-oriented ceramic and its manufacturing method
JP2004300019A
Non-lead-based piezoelectric material
JP2009215111A
Piezoelectric ceramic and method for producing the same
JP2011157252A