N-type semiconductor material used in the manufacture of flexible thermoelectric generation elements, flexible thermoelectric generation elements, and manufacturing methods thereof

The aqueous dispersion of Ni-ETT fine particles with a solvent switch to dimethylformamide enables a stable and high-performance thermoelectric thin film, addressing the limitations of conventional methods and enabling flexible power generation elements for diverse heat sources.

JP7578970B2Active Publication Date: 2024-11-07JOSHO GAKUEN EDUCATIONAL FOUND
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020181877
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-29
Publication Date
2024-11-07
Estimated Expiration
2040-10-29

AI Technical Summary

Technical Problem

Conventional methods for producing Ni-ETT dispersions result in large particle sizes and require organic solvents, leading to low environmental friendliness and insufficient thermoelectric power generation performance.

Method used

Aqueous dispersion of Ni-ETT fine particles with a particle size of 300 nm or less is achieved using dimethylformamide as a solvent, allowing for a coating process that forms a stable and high-performance thermoelectric thin film, which is then applied to a flexible substrate.

Benefits of technology

The method produces a flexible thermoelectric power generation element with superior performance and stability, capable of generating electricity from waste heat at temperatures below 200°C, suitable for various heat sources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578970000001
    Figure 0007578970000001
Patent Text Reader

Abstract

To provide: a poly(Ni-1,1,2,2-ethentetrathiolate) fine particle aqueous dispersion with a small particle size and a manufacturing technique thereof; a thermoelectric power generation thin film with n-type thermoelectric power generation performance and a manufacturing technique thereof; and an n-type flexible thermoelectric power generation element which includes the thermoelectric power generation thin film as a component, which has excellent n-type thermoelectric power generation performance and which is stable in the atmosphere and also excellent in flexibility, and a manufacturing technique thereof.SOLUTION: There are provided: a poly(Ni-1,1,2,2-ethentetrathiolate) fine particle aqueous dispersion with an average particle size of 300 nm or less; an n-type thermoelectric power generation thin film which contains poly(Ni-1,1,2,2-ethentetrathiolate) particles with an average particle size of 300 nm or less and has a thickness of 1-50 μm and a power factor of 25 μWm-1K-2 or more; a flexible thermoelectric power generation element comprising the thermoelectric power generation thin film and a flexible insulating substrate; and manufacturing methods of the aqueous dispersion, the thermoelectric power generation thin film and the flexible thermoelectric power generation element.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an n-type semiconductor material used for producing a flexible thermoelectric generating element, a flexible thermoelectric generating element, and a method for producing the same. More specifically, the present invention relates to an aqueous dispersion of Ni-ETT microparticles in which microparticles of polynickel 1,1,2,2-ethenetetrathiolate (alkali metal salt: hereinafter referred to as "Ni-ETT"), an organic compound containing nickel and sulfur, are dispersed, an n-type thermoelectric generating thin film made of Ni-ETT microparticles produced from the aqueous dispersion, and a flexible thermoelectric generating element having the thermoelectric generating thin film as a constituent element, and further relates to methods for producing the aqueous dispersion, the thermoelectric generating thin film, and the flexible thermoelectric generating element. [Background technology]

[0002] Approximately two-thirds of the energy consumed in Japan is wasted as waste heat (unused heat), and there is a desire to utilize it effectively. In particular, waste heat below 200°C, which accounts for approximately 70% of the unused heat, is discharged thinly and widely and is emitted from heat sources of various shapes, making it difficult to utilize effectively. Therefore, there are hopes for the application of thermoelectric generation elements that are lightweight, can be attached to various heat sources, and can generate electricity and make effective use of unused heat of about 200°C or less emitted from the heat source. In particular, there is a need for the development of flexible thermoelectric generation elements that are flexible enough to be adapted to the shapes of heat sources of various shapes.

[0003] The manufacture of thermoelectric generation elements requires p-type and n-type semiconductor materials, and a method for manufacturing thermoelectric generation elements by coating these semiconductor materials onto a substrate is also known. In addition, for the manufacture of lightweight and flexible thermoelectric generation elements, semiconductor materials made of organic materials are desired.

[0004] As organic p-type semiconductor materials, poly(3,4-ethylenedioxythiophene):poly(4-styrenesulfonate) (PEDOT:PSS) and its derivatives are known to exhibit excellent performance. On the other hand, most of the conventionally known organic n-type semiconductor materials have low thermoelectric power generation performance, and when doped, they become unstable in the air and their thermoelectric power generation performance decreases over time, so they are not semiconductor materials suitable for use in the manufacture of thermoelectric generation elements by coating methods.

[0005] Ni-ETT has been reported as an organic n-type thermoelectric material that is excellent in thermoelectric generation performance and stable in the air (Non-Patent Documents 1, 2, 3), and Ni-ETT is considered to be a promising organic n-type thermoelectric material. As a method for producing a thermoelectric generation element using Ni-ETT, a method for producing a composite material film containing Ni-ETT by a coating method is also known.

[0006] However, Ni-ETT is insoluble in solvents, and there was a technical problem in applying it to the production of films by coating. Therefore, a method has been disclosed in which dodecyltrimethylammonium salt or polyvinylidene fluoride (PVDF) is used as a surfactant to disperse Ni-ETT particles in a solvent and apply it to the production of the composite material film (Non-Patent Document 1, etc.). However, the composite material film obtained by this method had low thermoelectric power generation performance. Also, a method has been disclosed in which Ni-ETT is synthesized in methanol, an insulating polymer and dimethyl sulfoxide (DMSO) are added, and the mixture is mechanically pulverized using a ball mill to obtain a dispersion of Ni-ETT, which is then used to produce a film by applying a coating method (Non-Patent Document 2). [Prior art documents] [Non-patent literature]

[0007] [Non-Patent Document 1] N. Toshima, et al., Chemistry Letters, Vol.44, No.9, pp1185-1187(2015) [Non-Patent Document 2] SKYee,et al.,Adv.Funct.Mater.2018,28,1801620 [Non-Patent Document 3] D. Zhu,et al.,Adv.Mater.2016,28,3351 Summary of the Invention [Problem to be solved by the invention]

[0008] However, the above-mentioned method for producing a dispersion of Ni-ETT has problems in that the particle size of the dispersed Ni-ETT particles is large (the average particle size is larger than about 650 nm) and that it is necessary to use an organic solvent such as DMSO, which makes it less environmentally friendly. Furthermore, due to the large particle size of the Ni-ETT particles, the thermoelectric power generation performance of the coating film produced from the dispersion by a coating method cannot be said to be sufficient.

[0009] The present invention aims to solve the above problems of the prior art, and specifically, A Ni-ETT microparticle aqueous dispersion in which the particle size of Ni-ETT particles is smaller than that of Ni-ETT particle dispersions obtained by conventional techniques, which contains substantially no organic solvents, and is therefore environmentally friendly; and a manufacturing technique therefor; A thermoelectric generating thin film obtained by coating the aqueous dispersion of Ni-ETT fine particles, which has excellent n-type thermoelectric generating performance that cannot be obtained with conventional thermoelectric generating thin films using Ni-ETT and is stable in the atmosphere, and a manufacturing technology therefor; The objective of the present invention is to provide an n-type flexible thermoelectric generating element that uses the above-mentioned thermoelectric generating thin film as a component, has excellent n-type thermoelectric generating performance, is stable in the air, and has excellent flexibility, as well as a manufacturing technology for the same. [Means for solving the problem]

[0010] As a result of extensive investigations aimed at solving the above problems, the present inventors have found that by using dimethylformamide (DMF) as the solvent in place of methanol, which has been used as the solvent in conventional techniques in the synthesis of Ni-ETT, it is possible to obtain an aqueous dispersion in which Ni-ETT particles having a smaller particle size than those obtained by conventional techniques are uniformly dispersed, without the need for a micronization step such as mechanical grinding, or the use of an organic solvent such as DMSO. The present inventors have also found that when a coating liquid in which ethylene glycol has been added to the above-mentioned aqueous dispersion prepared using DMF as a solvent is applied to a substrate to form a film, an n-type thermoelectric generating thin film that is stable in the air and has high thermoelectric generating performance that has not been obtained by conventional techniques can be obtained, and that a flexible thermoelectric generating element that has high thermoelectric generating performance and is stable in the air can be obtained by using this thermoelectric generating thin film as a component. That is, the above-mentioned object of the present invention can be achieved by the invention having the following configuration.

[0011] The first aspect of the present invention is an aqueous dispersion of Ni-ETT fine particles obtained by dispersing Ni-ETT particles having an average particle size of 300 nm or less in water or a dispersion medium mainly composed of water. The second aspect of the present invention is a preferred embodiment of the first aspect of the present invention, which is an aqueous dispersion of Ni-ETT fine particles in which the average particle size of the Ni-ETT particles is 200 nm or less.

[0012] In conventional Ni-ETT particle dispersions disclosed in Non-Patent Document 2 and the like, the average particle size of the Ni-ETT particles is at most about 650 nm, and no dispersions capable of dispersing Ni-ETT fine particles with a smaller average particle size have been obtained. The first and second aqueous dispersions of the present invention disperse Ni-ETT fine particles with an average particle size far smaller than 650 nm, and in particular, the second aqueous dispersion of the present invention has an average particle size of about one-fourth or less that of the conventional technology, and is suitable for use in the manufacture of thermoelectric generating thin films and flexible thermoelectric generating elements.

[0013] The third aspect of the present invention is a Ni-ETT electrode comprising particles having an average particle diameter of 300 nm or less, a thickness of 1 to 50 μm, and a power factor of 25 μWm-1 K -2 This is a thermoelectric generating thin film having the above n-type thermoelectric generating performance. The fourth aspect of the present invention is a preferred embodiment of the third aspect of the present invention, which comprises Ni-ETT particles having an average particle size of 200 nm or less, a thickness of 1 to 50 μm, and a power factor of 30 μWm -1 K -2 This is a thermoelectric generating thin film having the above n-type thermoelectric generating performance.

[0014] Conventionally, no thermoelectric generating thin film containing Ni-ETT particles has been known to exhibit excellent thermoelectric generating performance. The thermoelectric generating thin film disclosed in Non-Patent Document 2 can be cited as an example of the most excellent thermoelectric generating performance among conventional techniques, but even this thermoelectric generating thin film has a power factor of 23 μWm -1 K -2 The third and fourth thermoelectric generating thin films of the present invention have superior thermoelectric generating performance (larger power factor) than these conventional techniques, and in particular, the fourth thermoelectric generating thin film of the present invention has a power factor 1.3 times or more that of the conventional techniques.

[0015] A fifth aspect of the present invention is a flexible thermoelectric generating element comprising the thermoelectric generating thin film of the third or fourth aspect of the present invention and a flexible insulating substrate, the thermoelectric generating thin film being formed on the substrate. Since this thermoelectric generating element has the thermoelectric generating thin film of the third or fourth aspect of the present invention as a constituent element, it exhibits superior thermoelectric generating properties compared to the prior art, and since it uses a flexible insulating substrate, it is flexible and has excellent shape adaptability to heat sources of various shapes.

[0016] The sixth aspect of the present invention is a method for producing an aqueous dispersion of Ni-ETT microparticles, which comprises the steps of reacting 1,3,4,6-tetrathiapentalene-2,5-dione and a nickel(II)-containing compound in the presence of an alkali metal alkoxide in DMF or a solvent mainly composed of DMF, oxidizing the reaction product, and dispersing the oxidized reaction product in water or a dispersion medium mainly composed of water. The seventh aspect of the present invention is a preferred embodiment of the sixth aspect of the present invention, in which the nickel(II)-containing compound is nickel(II) acetate tetrahydrate. These manufacturing methods can provide an aqueous dispersion of Ni-ETT microparticles having a smaller average particle size than that of aqueous dispersions of Ni-ETT particles obtained by conventional methods, without requiring a mechanical pulverization step. In addition, since no organic solvent such as DMSO is used, an aqueous dispersion that is environmentally friendly and does not contain organic solvents that cause environmental problems can be obtained.

[0017] The eighth aspect of the present invention is a method for producing a thermoelectric generating thin film containing Ni-ETT particles, which comprises coating a dispersion obtained by adding ethylene glycol to the aqueous dispersion of Ni-ETT fine particles according to the first or second aspect of the present invention on a substrate, and then drying and removing the dispersion medium to form a film. This method, which is characterized by adding ethylene glycol, makes it possible to obtain a thermoelectric generating thin film having a thickness of 1 to 50 μm, which has high thermoelectric generating performance and is stable even in the air.

[0018] The ninth aspect of the present invention is a preferred embodiment of the eighth aspect of the present invention, which is a method for producing a thermoelectric generating thin film containing Ni-ETT particles, characterized in that when the dispersion medium is dried and removed to form a film, an annealing step is included in which a thermal history greater than that required for removing ethylene glycol is applied. This method including an annealing step makes it possible to obtain a thermoelectric generating thin film having a thickness of 1 to 50 μm, which has a much higher thermoelectric generating performance than thermoelectric generating thin films containing Ni-ETT particles obtained by conventional techniques, and which is stable even in the atmosphere.

[0019] A tenth aspect of the present invention is a method for producing a flexible thermoelectric generating element, comprising the step of forming a thermoelectric generating thin film on a flexible insulating substrate by the eighth or ninth method for producing a thermoelectric generating thin film of the present invention. Effect of the Invention

[0020] The aqueous dispersion of Ni-ETT microparticles of the present invention is a dispersion of Ni-ETT microparticles having a small average particle size that could not be obtained by conventional techniques, and since it uses water or a solvent mainly composed of water as a dispersion medium without using an organic solvent such as DMSO, it is environmentally friendly and can be suitably used for producing n-type thermoelectric generating thin films, and further for producing thermoelectric generating elements using the thin films. This aqueous dispersion of Ni-ETT fine particles could not be produced by conventional techniques, but can be produced by the method for producing an aqueous dispersion of Ni-ETT fine particles of the present invention. The thermoelectric generating thin film of the present invention has excellent thermoelectric generating performance not obtainable by conventional techniques, is stable in the atmosphere, and can be suitably used for manufacturing flexible thermoelectric generating elements. This thermoelectric generating thin film can be manufactured by the manufacturing method of the thermoelectric generating thin film of the present invention, which is characterized by using a dispersion liquid obtained by adding ethylene glycol to the above-mentioned aqueous dispersion liquid of Ni-ETT fine particles and further including an annealing step. The flexible thermoelectric generation element of the present invention is stable in the atmosphere, has excellent thermoelectric generating properties not obtainable by conventional techniques, and is lightweight and flexible, so that it can be applied to heat sources of various shapes to generate power from unused heat of about 200° C. or less, and is suitable for effective use of exhaust heat. This flexible thermoelectric generation element can be manufactured by the manufacturing method for a flexible thermoelectric generation element of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, the embodiments for carrying out the present invention will be described in more detail, but the scope of the present invention is not limited to the following embodiments.

[0022] 1. Aqueous dispersion of Ni-ETT fine particles and its manufacturing method The first aspect of the present invention, an aqueous dispersion of Ni-ETT microparticles, is a dispersion in which Ni-ETT microparticles are uniformly dispersed in an aqueous dispersion medium, and is characterized in that the average particle diameter of Ni-ETT is 300 nm or less, preferably 200 nm or less, and is smaller than that of Ni-ETT particle dispersions obtained by conventional technology. Since the Ni-ETT microparticle aqueous dispersion of the present invention is composed of microparticles with a small average particle size, it is easy to form a film by a coating method, and it is also easy to improve the thermoelectric power generation performance when the film is formed after removing the dispersion medium.

[0023] The average particle size of Ni-ETT is a value measured by a dynamic light scattering (DLS) measuring device.

[0024] The molecular weight of Ni-ETT is not particularly limited as long as it is within a range in which the average particle size can be made 300 nm or less by the method for producing an aqueous dispersion of Ni-ETT fine particles described below, the Ni-ETT fine particles can be uniformly dispersed in the aqueous dispersion, and the aqueous dispersion is processed as described below to produce a thermoelectric generating thin film that exhibits excellent thermoelectric generating performance.

[0025] The dispersion medium for dispersing the Ni-ETT microparticles is water or a dispersion medium mainly composed of water. A dispersion medium mainly composed of water refers to a solution (homogeneous mixture) of water and a substance compatible with water, in which the component with the largest mass in the liquid is water. The proportion of water in the mixture is preferably 60 mass% or more, and more preferably 80 mass% or more. The water-compatible substance is preferably a liquid that is compatible with water, such as a lower alcohol, but may also be a solid or gas that dissolves in water. In addition to Ni-ETT, the dispersion medium may contain a small amount of a substance that is not compatible with water, provided that the purpose of the present invention is not impaired.

[0026] The content of the Ni-ETT fine particles in the aqueous dispersion of Ni-ETT fine particles is usually 0.5 to 10% by mass, and preferably in the range of 1 to 5% by mass.

[0027] (Method of manufacturing aqueous dispersion of Ni-ETT fine particles) The aqueous dispersion of Ni-ETT microparticles of the present invention can be produced by reacting 1,3,4,6-tetrathiapentalene-2,5-dione and a nickel(II)-containing compound in the presence of an alkali metal alkoxide in DMF or a solvent mainly composed of DMF, oxidizing the reaction product, and dispersing the resulting oxide in water or a dispersion medium mainly composed of water.

[0028] A solvent mainly composed of DMF is a solvent containing anhydrous DMF as the maximum mass component, but also containing other components that dissolve in DMF. The types of other components are not particularly limited as long as they dissolve in DMF and do not impair the gist of the present invention. For example, a small amount of a lower alcohol such as methanol may be mixed into DMF as long as it does not impair the gist of the present invention. As a solvent mainly containing DMF, a solvent containing 80% by mass or more of anhydrous DMF is preferably used.

[0029] As the nickel(II)-containing compound, a nickel(II) organic acid salt or a hydrate thereof that is soluble in DMF is preferably used, among which a hydrate of a nickel(II) organic carboxylate is preferred, and nickel(II) acetate tetrahydrate is particularly preferred.

[0030] Examples of the alkali metal of the alkali metal alkoxide include sodium and potassium. Among these alkali metals, sodium is preferred from the viewpoint of obtaining excellent thermoelectric generating properties (high power factor) when the aqueous dispersion of Ni-ETT fine particles is processed as described below to produce a thermoelectric generating thin film. Also, the smaller the carbon number of the alkoxide, the more preferred. Therefore, sodium methoxide is preferred as the alkali metal alkoxide.

[0031] The ratio of the amounts of 1,3,4,6-tetrathiapentalene-2,5-dione and the nickel(II)-containing compound used in the reaction (added to the reaction system) is appropriately adjusted taking into consideration various reaction conditions. Since these react in equal equivalent amounts, a ratio close to equal equivalent is usually adopted. The alkali metal alkoxide is usually used in an amount of 1 to 10 times by mole, and preferably 3 to 7 times by mole, relative to 1,3,4,6-tetrathiapentalene-2,5-dione or the nickel(II)-containing compound.

[0032] The reaction of 1,3,4,6-tetrathiapentalene-2,5-dione with the nickel(II)-containing compound is preferably carried out in an oxygen-free atmosphere, such as a nitrogen atmosphere, to prevent oxidation of the reaction product during the reaction.

[0033] The reaction between 1,3,4,6-tetrathiapentalene-2,5-dione and the nickel(II)-containing compound is carried out usually at a temperature in the range of 0 to 100° C., preferably at a temperature in the range of 20 to 80° C., with stirring.

[0034] After the reaction of 1,3,4,6-tetrathiapentalene-2,5-dione with the nickel(II)-containing compound, the reaction product is oxidized to impart electrical conductivity. The oxidation can be carried out by adding iodine, for example, by adding iodine dissolved in methanol to the reaction product of the reaction. This oxidation is also carried out while stirring, usually at a temperature in the range of 0 to 100°C, preferably at a temperature in the range of 20 to 80°C. After the reaction, the reaction system may be neutralized by adding an acid or the like before the oxidation is carried out.

[0035] The oxidation produces a dispersion in which product particles (presumably Ni-ETT microparticles) insoluble in the solvent are dispersed in the solvent, and the product particles are usually purified by separating them from the dispersion by centrifugation or by washing the product particles with methanol, water, DMSO, etc., to produce a black solid consisting of the product particles. This black solid is added to water or a dispersion medium mainly composed of water, and the product particles are dispersed by ultrasonic treatment, etc., to produce the Ni-ETT microparticle aqueous dispersion of the present invention.

[0036] The method for producing an aqueous dispersion of Ni-ETT microparticles of the present invention is characterized in that, in the synthesis of Ni-ETT by the reaction of 1,3,4,6-tetrathiapentalene-2,5-dione with a nickel (II)-containing compound, a solvent mainly composed of DMF is used as the reaction solvent instead of the methanol used in the above-mentioned conventional technology. By using a solvent mainly composed of DMF as the reaction solvent, Ni-ETT microparticles having a smaller particle size than those of the conventional technology can be obtained without the need for a microparticulation step such as mechanical grinding. That is, in the conventional technology, Ni-ETT produced by the reaction must be mechanically pulverized with an insulating polymer and an organic solvent such as DMSO using a ball mill or the like, and the average particle size of the resulting particles is about 650 nm or more. On the other hand, according to the present invention, by using a solvent mainly composed of DMF as a reaction solvent, it is possible to produce a material (aqueous dispersion) in which fine particles with an average particle size of 300 nm or less, preferably 200 nm or less, are uniformly dispersed in water without relying on mechanical means such as mechanical pulverization using a ball mill or the like. As a result, this leads to improved performance (improved thermoelectric generation performance) of thermoelectric generating thin films and thermoelectric generating elements produced using the Ni-ETT fine particle aqueous dispersion.

[0037] In addition, while the conventional techniques require the use of organic solvents such as DMSO as described above, the production method of the present invention uses an aqueous solvent and does not require the use of organic solvents that have an adverse effect on the environment. In other words, the production method of the present invention is environmentally friendly, and the aqueous dispersion of Ni-ETT microparticles produced is also environmentally friendly.

[0038] 2. Thermoelectric generating thin film and its manufacturing method The thermoelectric generating thin film of the present invention is produced by a coating method in which the aqueous dispersion of Ni-ETT fine particles of the present invention is coated on a substrate, and then the dispersion medium is dried and removed to form a film. The method for producing a thermoelectric generating thin film of the present invention is characterized in that a dispersion obtained by adding ethylene glycol to the aqueous dispersion of Ni-ETT fine particles is used as the coating liquid to be applied. Furthermore, by adding ethylene glycol to the coating solution, the thermoelectric generating performance of the thermoelectric generating thin film was improved, and the highest thermoelectric generating performance ever achieved for an n-type thermoelectric generating thin film that is stable in air was obtained, which was not possible with conventional technology.

[0039] Ethylene glycol is also used as an additive in the production of coating films of PEDOT:PSS, a p-type material, but this invention has found for the first time that the addition of ethylene glycol is also effective in the production of coating films of Ni-ETT (n-type thermoelectric generating thin films), which have a completely different structure and properties, and that a thermoelectric generating thin film with high thermoelectric generating performance can be obtained. It is believed that the thermoelectric generating performance is improved by the high dispersion of Ni-ETT fine particles by ethylene glycol.

[0040] The amount of ethylene glycol added to the coating liquid is not particularly limited as long as it is within a range that does not impair the gist of the present invention and can improve thermoelectric power generation performance, but it is usually added in a mass ratio of 1 / 100 to 1 / 1 relative to the aqueous dispersion of Ni-ETT microparticles. If the amount of ethylene glycol is too small, the improvement in thermoelectric power generation performance may be insufficient.

[0041] In the method for producing a thermoelectric generating thin film of the present invention, a dispersion obtained by adding ethylene glycol to an aqueous dispersion of Ni-ETT fine particles is applied onto a substrate as a coating liquid, and the dispersion medium and ethylene glycol in the dispersion film are then dried and removed to produce a thermoelectric generating thin film. The drying is preferably carried out under heating to a temperature equal to or higher than the boiling point of ethylene glycol or under reduced pressure for a period of time required for the ethylene glycol to volatilize and remove it from the film. However, if this drying step is replaced by an annealing step in which a thermal history greater than the heating temperature and time (thermal history) required for removing ethylene glycol is applied to the film, a thermoelectric generating thin film with further improved thermoelectric generating performance can be obtained, which is more preferable. Annealing is thought to cause changes in the spatial arrangement between Ni-ETT particles, an increase or modification of the contact interface, etc., and as a result, further improvement in thermoelectric generating performance.

[0042] In the method for producing a thermoelectric generating thin film of the present invention, the material or shape of the substrate to which the dispersion is applied is not particularly limited as long as the substrate is one that allows the dispersion to be applied, dried, and optionally annealed. However, if an organic resin film having flexibility and excellent mechanical strength is used as the substrate, the flexible thermoelectric generating element of the present invention can be produced simply by drying the applied dispersion and optionally annealing it, which is preferable. On the other hand, the thermoelectric generating thin film of the present invention may be produced by applying the dispersion to another substrate, such as a glass plate or a stainless steel belt, drying, and optionally annealing the substrate, and then the produced film may be transferred to the organic resin film or the like to produce the flexible thermoelectric generating element of the present invention.

[0043] The thickness of the thermoelectric generating thin film of the present invention is usually 1 to 50 μm. The thermoelectric generating thin film of the present invention not only has high thermoelectric generating performance, but also has excellent stability of thermoelectric generating performance in the atmosphere. Conventionally, n-type materials that can be used for manufacturing flexible thermoelectric generating elements and can be obtained by a coating method, and that are stable and have high performance in the atmosphere, were not known. However, the present invention has made it possible to obtain, for the first time, an n-type thermoelectric generating thin film that is stable in the atmosphere and has the highest thermoelectric generating performance.

[0044] 3. Flexible thermoelectric generation element and its manufacturing method The flexible thermoelectric generating element of the present invention is composed of a flexible insulating substrate and the thermoelectric generating thin film of the present invention coated thereon, and can be manufactured by forming the thermoelectric generating thin film of the present invention on the insulating substrate. As the flexible insulating substrate, an organic resin film having flexibility and excellent mechanical strength is preferably used.

[0045] Examples of materials for resin films having flexibility and excellent mechanical strength include polyester resins such as polyethylene terephthalate and high-strength resins such as polyimide, but other resins may be used as long as they satisfy the gist of the present invention, that is, have flexibility and mechanical strength to be attached to heat sources of various shapes, and are not limited to the exemplified resins. The thickness of the film may be within a range that does not impair flexibility or mechanical strength, and a film in the range of 0.01 to 1 mm is usually used as the substrate.

[0046] A thermoelectric generating thin film can be formed on a flexible insulating substrate by applying a coating liquid prepared by adding ethylene glycol to the aqueous dispersion of Ni-ETT microparticles of the present invention to the substrate surface, drying the liquid to remove the dispersion medium, and forming a film. The flexible thermoelectric generating element of the present invention thus obtained has high thermoelectric generating performance and is stable in the atmosphere because it has the thermoelectric generating thin film of the present invention as its component. In addition, since the component is a flexible substrate, it has excellent flexibility and can be attached to heat sources of various shapes to generate electricity by effectively utilizing the exhaust heat from the heat source. EXAMPLES

[0047] The following describes experimental examples in which an aqueous dispersion of Ni-ETT fine particles was prepared based on the manufacturing method of the present invention, an n-type thermoelectric power generating thin film was prepared, and comparative experimental examples conducted for comparison with the examples of the present invention. The compounds and solvents used in the experimental examples and comparative experimental examples were all reagents. The average particle size and thermoelectric power generation performance in the experimental examples and comparative experimental examples were measured by the methods described below.

[0048] (Measurement of average particle size) Measurements were performed using a dynamic light scattering (DLS) measuring device, Malvern Zeta Sizer Nano Series Nano-ZS (manufactured by Malvern Panalytical). (Measurement of thermoelectric power generation performance) Using a thermoelectric property evaluation device ZEM-3L (manufactured by Advance Riko Co., Ltd.), the electrical conductivity σ, Seebeck coefficient S, and power factor PF (=S 2 σ) was measured.

[0049] Experiment 1: Preparation of aqueous dispersion of Ni-ETT microparticles 0.25mL of a 5mol / L solution of sodium methoxide in methanol (containing 1.25mmol of sodium methoxide) was added to a solution of 1,3,4,6-tetrathiapentalene-2,5-dione (50mg:0.24mmol) and nickel(II) acetate tetrahydrate (60mg:0.25mmol) in anhydrous DMF (2.5mL) under a nitrogen atmosphere at 60°C and stirred. After stirring for 24 hours, a mixture of acetic acid (0.1mL) and methanol (1.0mL) was added to neutralize the reaction system.

[0050] Then, iodine (30 mg: 0.12 mmol) dissolved in methanol (0.5 mL) was added to oxidize the produced Ni-ETT. After stirring for 24 hours, the resulting reaction mixture was transferred to a centrifuge tube and centrifuged at 2900 rpm. The reaction mixture was purified by repeatedly removing components dissolved in methanol, water, and DMSO by centrifugation and removing the supernatant by decantation or pipette aspiration, etc., to obtain a black solid. Water was added to the resulting black solid, and it was dispersed in water by ultrasonic treatment for 20 minutes, resulting in a dispersion in which Ni-ETT fine particles were uniformly dispersed in water at a concentration of 30 mg / mL (Ni-ETT fine particle aqueous dispersion).

[0051] (Measurement of particle size of Ni-ETT particles) The average particle size of the dispersed Ni-ETT fine particles in the aqueous dispersion of Ni-ETT fine particles obtained in Experiment 1 was measured and found to be 190 nm. As described above, the average particle size of Ni-ETT particles obtained by conventional technology is approximately 650 nm at the smallest. However, Experiment 1 (the method for producing an aqueous dispersion of Ni-ETT microparticles of the present invention) demonstrated that an aqueous dispersion containing dispersed Ni-ETT microparticles with an average particle size approximately 1 / 4 smaller than that of the conventional technology can be obtained without mechanical grinding, etc.

[0052] Comparative experiment 1 Except for using methanol as a solvent instead of anhydrous DMF, the reaction of sodium methoxide, 1,3,4,6-tetrathiapentalene-2,5-dione, and nickel(II) acetate tetrahydrate was carried out in the same manner as in Experiment 1 to synthesize Ni-ETT. However, a large amount of solid precipitated during the reaction, and it was not possible to prepare an aqueous dispersion. Therefore, it was not possible to measure the thermoelectric power generation performance.

[0053] Experiment 2: Preparation of n-type thermoelectric thin film using Ni-ETT aqueous dispersion A 1.5 cm x 1.5 cm glass substrate was thoroughly washed with water, acetone, and 2-propanol. Ethylene glycol (EG) was added to the Ni-ETT aqueous dispersion obtained in Experiment 1 in a volume ratio of 10:1, and the resulting mixture was ultrasonically treated for 20 minutes. 50 μL of the thus obtained Ni-ETT aqueous dispersion containing EG was dropped onto the glass substrate and spread to form a film of the dispersion. When the glass substrate on which the film of the dispersion liquid was formed was heated in air at 70°C for 30 minutes, the dispersion medium was removed and a black film was obtained. The black film obtained is considered to exhibit thermoelectric power generation performance, and when this black film was further annealed in air at 210°C for 30 minutes, a thin film with a thickness of 5.3 μm was obtained that exhibited excellent thermoelectric power generation performance as described below.

[0054] (Measurement of thermoelectric generation performance of n-type thermoelectric generating thin film) The thermoelectric power generation performance of the thin film with a thickness of 5.3 μm obtained in the above experiment was measured, and the results shown in Table 1 were obtained. The thin film obtained was an n-type thermoelectric power generation thin film, and the power factor (PF) was 33 μWm -1 K -2 This power factor (thermoelectric power generation performance) is about 1.5 times higher than the highest power factor known for an n-type thermoelectric power generation thin film of the prior art (described in Non-Patent Document 2). In addition, the thin film obtained in the above experiment was stored in air at room temperature for 13 days, but no significant change in thermoelectric power generation performance was observed during storage, confirming that the obtained thin film was stable in air.

[0055] Comparative experiment 2 An n-type thermoelectric thin film was prepared in the same manner as in Experiment 2, except that ethylene glycol (EG) was not added to the Ni-ETT aqueous dispersion obtained in Experiment 1. The thermoelectric power generation performance was measured in the same manner, and the power factor (PF) was 10 μWm -1 K -2 (The measurement results are shown in Table 1.)

[0056] [Table 1] [Industrial Applicability]

[0057] Flexible thermoelectric generation elements are capable of generating electricity from heat sources of about 200°C or less, and are therefore expected to be used as power sources that generate electricity by effectively utilizing the exhaust heat from various heat sources. For example, they are expected to be used as power sources for wireless sensors, which are expected to be used in huge numbers in the IoT society. Using flexible thermoelectric generation elements as a power source offers great advantages in terms of convenience, such as the elimination of the need for wiring from walls and the need for replacement. In addition, flexible thermoelectric generation elements can be installed as power generators in human clothing, buildings with relatively low-temperature heat sources, as well as in the exhaust heat of automobiles, factory piping, and animal bodies, and are expected to be used as a simple source of small electricity.

Claims

1. The polynickel 1,1,2,2-ethenetetrathiolate fine particle aqueous dispersion is obtained by dispersing particles of polynickel 1,1,2,2-ethenetetrathiolate having an average particle size of 300 nm or less in water or a dispersion medium mainly composed of water and mixed with ethylene glycol.

2. The aqueous dispersion of polynickel 1,1,2,2-ethenetetrathiolate fine particles is obtained by dispersing particles of polynickel 1,1,2,2-ethenetetrathiolate having an average particle size of 200 nm or less in water or a dispersion medium mainly composed of water and mixed with ethylene glycol.

3. The electrode contains particles of polynickel 1,1,2,2-ethenetetrathiolate having an average particle size of 300 nm or less, has a thickness of 1 to 50 μm, and has a power factor of 25 μWm -1 K -2 The thermoelectric generating thin film has the above n-type thermoelectric generating performance.

4. The electrode contains particles of polynickel 1,1,2,2-ethenetetrathiolate having an average particle size of 200 nm or less, has a thickness of 1 to 50 μm, and has a power factor of 30 μWm -1 K -2 The thermoelectric generating thin film has the above n-type thermoelectric generating performance.

5. 5. A flexible thermoelectric generating element comprising the thermoelectric generating thin film according to claim 3 or 4 and a flexible insulating substrate, the thermoelectric generating thin film being formed on the substrate.

6. A method for producing an aqueous dispersion of polynickel 1,1,2,2-ethenetetrathiolate microparticles, comprising the steps of: reacting 1,3,4,6-tetrathiapentalene-2,5-dione and a nickel(II)-containing compound in DMF or a solvent mainly composed of DMF in the presence of an alkali metal alkoxide; oxidizing a product of the reaction; and dispersing the oxidized reaction product in water or a dispersion medium mainly composed of water.

7. The method for producing an aqueous dispersion of polynickel 1,1,2,2-ethenetetrathiolate microparticles according to claim 6, wherein the compound containing nickel (II) is nickel (II) acetate tetrahydrate.

8. A method for producing a thermoelectric generating thin film containing particles of polynickel 1,1,2,2-ethene tetrathiolate, characterized in that an aqueous dispersion of polynickel 1,1,2,2-ethene tetrathiolate microparticles according to claim 1 or claim 2 is applied onto a substrate, and then the dispersion medium is dried and removed to form a film.

9. The method for producing a thermoelectric generating thin film containing particles of polynickel 1,1,2,2-ethenetetrathiolate according to claim 8, characterized in that, when the dispersion medium is dried and removed to form a film, an annealing step is performed to apply a thermal history larger than the thermal history required for removing ethylene glycol.

10. A method for producing a flexible thermoelectric generating element, comprising the step of forming a thermoelectric generating thin film on a flexible insulating substrate by the method for producing a thermoelectric generating thin film according to claim 8 or 9.

Citation Information

Patent Citations

  • Production method of surface modified carbon nanotube and dispersion liquid of the same

    JP2017137232A

  • Optical sensor, method for manufacturing and driving optical sensor, and method for measuring light intensity

    WO2004013915A1

  • Carbon NANO tube field effect transistor

    WO2006103872A1

  • Method for manufacturing film for thermoelectric conversion element