Resin composition for water-repellent lens protective film and method for protecting water-repellent lens

A resin composition for super-water-repellent lenses, using polyfunctional (meth)acrylate and a nonionic surfactant, addresses adhesion and thermal issues, ensuring uniform application and preventing axis misalignment during processing.

JP7583357B2Active Publication Date: 2024-11-14NOF CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020165949
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-30
Publication Date
2024-11-14
Estimated Expiration
2040-09-30

AI Technical Summary

Technical Problem

Existing methods for protecting super-water-repellent lenses during processing fail to maintain water repellency and cause axis misalignment due to insufficient adhesion and thermal effects during the formation of protective films.

Method used

A resin composition containing polyfunctional (meth)acrylate, photopolymerization initiator, and nonionic surfactant, curable with an LED light source near the visible light region, forming a protective film that adheres well to super-water-repellent lenses without causing thermal damage.

Benefits of technology

The composition ensures uniform application and high water repellency, prevents axis misalignment, and allows easy peeling without residue, while maintaining lens integrity during processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583357000011
    Figure 0007583357000011
  • Figure 0007583357000012
    Figure 0007583357000012
  • Figure 0007583357000001
    Figure 0007583357000001
Patent Text Reader

Abstract

To provide a resin composition for a water-repellent lens protection film that has controlled coating property and adhesion to a lens subjected to super water-repellency which can be uniformly coated to a lens having high water repellency and can be cured even with an LED light source having a peak wavelength of 395 nm.SOLUTION: A resin composition for a water-repellent lens protection film contains (A) polyfunctional (meth)acrylate having a weight average molecular weight of 200-30,000, (B) a photopolymerization initiator, and (C) a nonionic surface active agent. The resin composition for the water-repellent lens protection film can be uniformly coated to even the whole of a water-repellent lens that has water-repellency and is difficult to be coated to the surface, and a protective film formed of the resin composition for the water-repellent protection film prevents axis deviation at the time of lens circumference processing, and can be easily peeled without a residue in peeling.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition for a water-repellent lens protective film that protects the lens surface during peripheral processing of a super water-repellent lens, and also to a method for protecting a water-repellent lens in order to hold the lens in a processing device during peripheral processing of the super water-repellent lens. [Background technology]

[0002] The periphery of the eyeglass lens is processed using a processing device so that it fits the frame shape of the eyeglass frame. This processing device holds the eyeglass lens on a pair of lens chuck shafts, rotates the lens by rotating the lens chuck shafts, and processes the lens into the desired shape by pressing a processing tool such as a grindstone against the lens. At this time, a jig is attached to the eyeglass lens with double-sided tape, and the lens is held by the lens chuck shafts via the jig. In recent years, water-repellent lenses, whose lens surface is coated with water- and oil-repellent substances that make it difficult for dirt such as water and oil to adhere, have become widely used, and super water-repellent lenses with even better dirt-resistant properties have also been developed. Because the surface of these water-repellent lenses is slippery, the adhesive strength of the double-sided tape used for processing them is not sufficient, and when processed in the same way as lenses that have not been treated with water-repellent coating, the double-sided tape slips, causing the rotation angle of the lens to deviate from the rotation angle of the lens chuck axis, which is known as axial misalignment.

[0003] In order to prevent the misalignment, a protective film is provided on the lens surface to prevent slippage. In this method, a protective layer that has good adhesion to the lens surface and to the double-sided tape for fixing the jig is formed on the lens surface, and the misalignment during lens processing can be prevented. After processing, the protective film can be easily peeled off from the lens, allowing the lens to be processed while maintaining its water repellency. However, when forming this protective film, there is a problem that the heat generated during curing causes cracks in the water-repellent layer of the thermosetting protective film, causing the surface to lose its smoothness and reducing the water repellency. Also, even when using a photocurable protective film, if a mercury lamp or metal halide lamp that emits light over a wide wavelength range is used as a light source for curing, the lens absorbs the irradiated light and generates heat, which causes cracks.

[0004] Patent Document 1 discloses a method for forming a thermosetting protective film made of an organic polymer in which inorganic matter is dispersed in a colloidal state on a lens having a water-repellent function. Patent Document 2 discloses a method for forming a photocurable protective film containing a metal oxide on a lens having a water-repellent function. Patent Document 3 discloses a photocurable acrylic resin composition as a temporary fixing agent that has an appropriate peel strength required for peeling the cured product from an adherend and also has appropriate flexibility in the cured product.

[0005] However, the aforementioned literature only describes the target substrate to be coated as a lens that has been treated to be water- and oil-repellent, and there are issues with lenses that have a function known as super-water repellency, which also has excellent dirt resistance, such as poor coatability and poor adhesion to the lens, resulting in low prevention of axis misalignment. In addition, in recent years, attention has been focused on UV-LED irradiation devices with a narrow emission wavelength range (emission wavelength 365 or 380-405 nm) to prevent the thermal effect during the formation of the protective film. Among them, a light source with a peak wavelength as close as possible to visible light is preferable, and in particular, a light source with a peak wavelength of 395 nm or more makes it possible to harden the protective film without generating heat in the lens. However, the longer the wavelength of the light, the more difficult it is to harden the film, so hardening was difficult in the above-mentioned patent documents. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2010-085691 A [Patent Document 2] International Publication No. 2017 / 110472 [Patent Document 3] International Publication No. 2013 / 073364 Summary of the Invention [Problem to be solved by the invention]

[0007] Therefore, the present invention aims to provide a resin composition for a water-repellent lens protective film, which is a resin composition with adjusted coatability and adhesion to a lens that has been treated for super-water repellency, can be uniformly coated on a highly water-repellent lens, and can be cured even with an LED light source with a peak wavelength of 395 nm. This makes it possible to form a protective film on a super-water-repellent lens without causing a decrease in water repellency due to heat. Another aim is to form a protective film on a super-water-repellent lens, even if it is a super-water-repellent lens, and to process the super-water-repellent lens into a desired shape without causing axial misalignment due to edging. [Means for solving the problem]

[0008] The present invention relates to a resin composition for a water-repellent lens protective film, which contains (A) a polyfunctional (meth)acrylate having a weight average molecular weight of 200 to 30,000, (B) a photopolymerization initiator, and (C) a nonionic surfactant.

[0009] The present invention also provides a method for protecting a water-repellent lens by coating the above-mentioned resin composition for a protective film on the water-repellent lens, followed by curing to obtain a cured film as a protective layer. Effect of the Invention

[0010] The resin composition for water-repellent lens protective film of the present invention has high water repellency and can be uniformly coated on the entire surface even on water-repellent lenses that are difficult to coat on the surface, and the protective film formed by this resin composition for water-repellent lens protective film can be easily peeled off without leaving any residue when peeled off. Furthermore, since the composition can be cured with an LED ultraviolet ray irradiation device having a peak wavelength close to the visible light region, it is possible to suppress the thermal effect on the water-repellent lens during curing and form a protective film without causing defects such as cracks and distortions in the water-repellent layer. Furthermore, the resin composition for water-repellent lens protective film of the present invention not only protects the lens from scratches and contamination during transportation and processing, but also has an appropriate adhesion to the lens, making it possible to prevent axial misalignment during processing. [Brief description of the drawings]

[0011] [Figure 1] FIG. 2 is a schematic diagram illustrating a test method for evaluating the retention strength of a protective film in an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram illustrating a method for evaluating the retention strength of a protective film in an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will be described in detail below. In the present invention, "(meth)acrylate" is a generic term including both acrylate and methacrylate. In the present invention, "XX to XX" indicating a numerical range is a concept including the lower limit ("XX") and the upper limit ("XX"), unless otherwise specified. In other words, it means "not less than XX and not more than XX" precisely.

[0013] The resin composition for a water-repellent lens protective film of the present invention is a curable resin composition containing the following components (A), (B) and (C) as essential components, and optionally further containing components (D) and (E). <Component (A): Polyfunctional (meth)acrylate> The polyfunctional (meth)acrylate of component (A) is a compound having a weight average molecular weight (Mw) of 200 to 30,000 and a (meth)acryloxy group at the end, and a preferred example thereof is a compound represented by the following general formula (Formula 1). The polyfunctional (meth)acrylate of component (A) may be used alone or in combination of two or more kinds. [ka]

[0014] In the formula, a is preferably 2-10. R 1 R is a hydrocarbon group having 2 to 300 carbon atoms or a hydrocarbon group having 2 to 300 carbon atoms containing at least one selected from the group consisting of an ether oxygen (-O-) and a hydroxyl group (-OH), an isocyanurate ring or a group consisting of an isocyanurate ring and a hydrocarbon group or a hydrocarbon group having 2 to 20 carbon atoms, or a hydrocarbon group having 2 to 250 carbon atoms or a hydrocarbon group having 2 to 250 carbon atoms containing at least one selected from the group consisting of an ether oxygen (-O-) and a hydroxyl group (-OH). 2 is a hydrogen atom or a methyl group.

[0015] In addition, as the (A) polyfunctional (meth)acrylate, a polymer type can also be suitably used. Examples of the polymer type polyfunctional (meth)acrylate include a polymer obtained by reacting a (meth)acrylate having a group reactive with an epoxy group, such as (meth)acrylic acid, with a (meth)acrylate having a group reactive with an epoxy group, such as (meth)acrylic acid, with a (meth)acrylate having a group reactive with an epoxy group, such as (meth)acrylic acid, with a (meth)acrylate having a group reactive with an epoxy group, such as 2-isocyanatoethyl 2-methylpropenoate, with a (meth)acrylate having a group reactive with an epoxy group, such as (meth)acrylic acid ...

[0016] Among them, urethane (meth)acrylate compounds having a urethane bond are preferred. Urethane (meth)acrylate can be obtained by reacting a diisocyanate compound, a diol compound, and a (meth)acrylate compound. By using a compound having a urethane bond, the toughness of the cured film is improved, and the cured film is less likely to break when peeled off. In addition, the adhesion to the water-repellent lens is improved, and the effect of suppressing axial deviation during processing is enhanced.

[0017] Commercially available urethane (meth)acrylate products include, for example, UN-333 (functional groups: 2, Mw: 5,000), UN-1255 (functional groups: 2, Mw: 8,000), UN-904 (functional groups: 10, Mw: 4,900), UN-6200 (functional groups: 2, Mw: 6,500), UN-6201 (functional groups: 2, Mw: 1,600), UN-9000PEP (functional groups: 2, Mw: 5,000), UN-9200A (functional groups: 2, Mw: 15,000), UN-3320HA (functional groups: 6, Mw: 1,500), UN-6301 (functional groups: 2, Mw: 33,000), UN-954: (functional groups: 2, Mw: 33,000), and UN-1255 (functional groups: 2, Mw: 8,000). functional groups: 6, Mw: 4,500), UN-953: (functional groups: 20, Mw: 14,000 to 40,000), H-219 (functional groups: 9, Mw: 25,000 to 50,000) (all of the above are trade names, manufactured by Negami Chemical Industrial Co., Ltd.), EBECRYL230 (functional groups: 2, Mw: 5,000), EBECRYL9260 (functional groups: 3, Mw: 15,000) (all of the above are trade names, manufactured by Daicel-Allnex Corporation), UX-4101 (functional groups: 2, Mw: 6,500), UX-6101 (functional groups: 2, Mw: 6,500) (all of the above are trade names, manufactured by Nippon Kayaku Kogyo Co., Ltd.), and the like.

[0018] The weight average molecular weight of the (A) polyfunctional (meth)acrylate is 200 to 30,000, preferably 200 to 15,000. If the weight average molecular weight of the (A) polyfunctional (meth)acrylate is in the range of 200 to 30,000, the cured film is strong and does not easily break when peeled off, and the workability during peeling is good. Furthermore, if the weight average molecular weight is in the range of 200 to 15,000, in addition to the toughness of the cured film, the water resistance is improved and the cured film is not easily broken during lens edging, which makes it possible to further suppress axial deviation, which is preferable.

[0019] In this specification, the weight average molecular weight was determined in terms of polystyrene using a gel permeation chromatography apparatus HLC-8220GPC manufactured by Tosoh Corporation, a column TSKgel HZM-M manufactured by Tosoh Corporation, THF as an eluent, and an RI detector.

[0020] The content of component (A) is 20.0 to 99.5% by mass, preferably 40.0 to 99.5% by mass, based on the total solid content of the resin composition for water-repellent lens protective film. By setting the content within the above range, a strong protective film can be formed, and it is possible to achieve both prevention of axial deviation during edging and easy peelability after use.

[0021] <Component (B): Photopolymerization initiator> The resin composition for a water-repellent lens protective film of the present invention contains, as component (B), a photopolymerization initiator that generates radicals when irradiated with ultraviolet light. This resin composition for water-repellent lens protective films contains component (B), so it can be cured even when exposed to an LED ultraviolet irradiation device that emits wavelengths close to the visible light region, and the thermal effects on the water-repellent lens caused by light irradiation can be suppressed.

[0022] The component (B) is not particularly limited as long as it can polymerize the photosensitive resin, and can be appropriately selected from commonly used photopolymerization initiators, such as acylphosphine oxide-based, oxime ester-based, aromatic ketone-based, quinone-based, alkylphenone-based, imidazole-based, acridine-based, and phenylglycine-based photopolymerization initiators.

[0023] The acylphosphine oxide photopolymerization initiator has an acylphosphine oxide group (>P(=O)-C(=O)- group), and examples thereof include (2,6-dimethoxybenzoyl)-2,4,6-pentylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide ("IRGACURE-TPO" (manufactured by BASF)), ethyl-2,4,6-trimethylbenzoylphenylphosphinate, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide ("IRGACURE-819" (manufactured by BASF)), (2,5-dihydroxyphenyl)diphenylphosphine oxide, (p-hydroxyphenyl)diphenylphosphine oxide, bis(p-hydroxyphenyl)phenylphosphine oxide, and tris(p-hydroxyphenyl)phosphine oxide.

[0024] The oxime ester photopolymerization initiator is a photopolymerization initiator having an oxime ester bond, and examples thereof include 1,2-octanedione-1-[4-(phenylthio)phenyl]-2-(O-benzoyloxime) (trade name: OXE-01, manufactured by BASF), 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone-1-(O-acetyloxime) (trade name: OXE-02, manufactured by BASF), and 1-phenyl-1,2-propanedione-2-[O-(ethoxycarbonyl)oxime] (trade name: Quantacure-PDO, manufactured by Nippon Kayaku Co., Ltd.).

[0025] Examples of aromatic ketone-based photopolymerization initiators include benzophenone, N,N'-tetramethyl-4,4'-diaminobenzophenone (Michler's ketone), N,N'-tetraethyl-4,4'-diaminobenzophenone, 4-methoxy-4'-dimethylaminobenzophenone, 2,2-dimethoxy-1,2-diphenylethan-1-one ("IRGACURE-651" (BASF)), 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one ("IRGACURE-369" (BASF)), and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one ("IRGACURE-907" (BASF)).

[0026] Examples of quinone-based photopolymerization initiators include 2-ethylanthraquinone, phenanthrenequinone, 2-t-butylanthraquinone, octamethylanthraquinone, 1,2-benzanthraquinone, 2,3-benzanthraquinone, 2-phenylanthraquinone, 2,3-diphenylanthraquinone, 1-chloroanthraquinone, 2-methylanthraquinone, 1,4-naphthoquinone, 9,10-phenanthraquinone, 2-methyl-1,4-naphthoquinone, and 2,3-dimethylanthraquinone.

[0027] Examples of the alkylphenone-based photopolymerization initiator include benzoin-based compounds such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin phenyl ether, 2,2-dimethoxy-1,2-diphenylethan-1-one ("IRGACURE-651" (BASF)), 1-hydroxy-cyclohexyl-phenyl-ketone ("IRGACURE-184" (BASF)), 2-hydroxy-2-methyl-1- Examples of such phenyl-propan-1-one include "IRGACURE-1173" (BASF), 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one ("IRGACURE-2959" (BASF)), and 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one ("IRGACURE-127" (BASF)).

[0028] Examples of the imidazole-based photopolymerization initiator include 2,4,5-triarylimidazole dimers, and more specifically, 2-(o-chlorophenyl)-4,5-diphenylimidazole dimers such as 2-(2-chlorophenyl)-1-[2-(2-chlorophenyl)-4,5-diphenyl-1,3-diazol-2-yl]-4,5-diphenylimidazole, 2-(o-chlorophenyl)-4,5-di(methoxyphenyl)imidazole dimers, 2-(o-fluorophenyl)-4,5-diphenylimidazole dimers, 2-(o-methoxyphenyl)-4,5-diphenylimidazole dimers, and 2-(p-methoxyphenyl)-4,5-diphenylimidazole dimers.

[0029] Among these, from the viewpoint of curability when using a UV-LED light source, the component (B) may contain at least one compound selected from the group consisting of compounds represented by the following general formula (Formula 2).

[0030] [ka] (In the general formula (Formula 2), R 3 represents a hydroxyl group, an alkoxy group having 1 to 8 carbon atoms, or an amino group; R 4 and R 5 R each independently represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, or an aryl group having 6 to 12 carbon atoms. 4 and R 5 may be bonded to each other to form a ring structure having 3 to 16 carbon atoms. 3 ~R 5 R may have a substituent, except for a hydroxyl group or a hydrogen atom, and in the case of amino groups having a substituent, the substituents may be bonded to each other to form a ring structure having 3 to 12 carbon atoms. 6 each independently represents a hydrogen atom, a halogen atom, a hydroxyl group, an amino group, a mercapto group, or an organic group having 1 to 10 carbon atoms which may contain one or more atoms selected from an oxygen atom, a nitrogen atom, and a sulfur atom.

[0031] In the general formula (Formula 2), R 3 represents a hydroxyl group, an alkoxy group having 1 to 8 carbon atoms, or an amino group. R 3 The alkoxy group represented by may be a hydroxyl group or a methoxy group from the viewpoint of curing properties when a UV-LED is used as a light source.

[0032] In the general formula (Formula 2), R 4 and R 5 each independently represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, or an aryl group having 6 to 12 carbon atoms. R 4 and R 5The alkyl group represented by may be an alkyl group having 1 to 4 carbon atoms, or may be an alkyl group having 1 or 2 carbon atoms. Examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a tert-butyl group, an n-heptyl group, an n-hexyl group, and an n-octyl group. The alkoxy group may be an alkoxy group having 1 to 4 carbon atoms, or may be an alkoxy group having 1 or 2 carbon atoms. Examples of the alkoxy group include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, a tert-butoxy group, an n-heptyloxy group, an n-hexyloxy group, and an n-octyloxy group. The aryl group may be an aryl group having 6 to 10 carbon atoms, or may be an aryl group having 6 to 8 carbon atoms. Examples of the aryl group include a phenyl group and a naphthyl group. R 4 and R 5 may be bonded to each other to form a ring structure having 3 to 16 carbon atoms. The cyclic structure may be a cyclic structure having 4 to 10 carbon atoms, or may be a cyclic structure having 5 to 8 carbon atoms. The cyclic structure may be an alicyclic structure, and examples of the alicyclic structure include a cyclopentane structure, a cyclohexane structure, a cycloheptane structure, and a cyclooctane structure. In addition, these alicyclic structures can be represented by R 4 and R 5 may contain carbon atoms which are directly bonded together.

[0033] The content of component (B) is usually 0.05 to 20 mass %, preferably 0.1 to 10 mass %, based on the total solid content of the resin composition for water-repellent lens protective film. By setting the content within the above range, the curability of the resin composition for water-repellent lens protective film when a UV-LED is used as a light source can be improved, and a cured product can be formed in a shorter time and at a lower illuminance.

[0034] <Component (C): Nonionic surfactant> The nonionic surfactant of component (C) may be, for example, a hydrocarbon-based, silicone-based, or fluorine-based surfactant. By adding component (C), the surface tension of the blended liquid of the resin composition for water-repellent lens protective film is reduced, making it possible to uniformly coat the resin composition even on substrates that are extremely difficult to coat, such as ultrawater-repellent lenses. Component (C) can be used alone or in combination of two or more types.

[0035] Examples of the hydrocarbon surfactant include polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene oleyl ether, etc.; polyoxyethylene alkyl phenyl ethers such as polyoxyethylene n-octylphenyl ether, polyoxyethylene n-nonylphenyl ether, etc.; polyethylene glycol diesters such as polyethylene glycol dilaurate, polyethylene glycol distearate, etc.; sorbitan fatty acid esters; fatty acid modified polyesters; acrylic polymers, etc. Examples of the hydrocarbon surfactants that have acrylic polymer as the main component include Polyflow No. 75, Polyflow No. 90, Polyflow WS-314 (all of which are product names manufactured by Kyoeisha Chemical Co., Ltd.) and the like.

[0036] Commercially available silicone surfactants include, for example, Polyflow KL-100, Polyflow KL-401, Polyflow KL-402, Polyflow KL-403 (all of which are product names manufactured by Kyoeisha Chemical Co., Ltd.); KP-323, KP-341, KP-392 (all of which are product names manufactured by Shin-Etsu Chemical Co., Ltd.); SZ-1642, SZ-1677, SH192, SH193 (all of which are product names manufactured by Dow Corning Toray Co., Ltd.), and the like.

[0037] The fluorosurfactant is a fluorosurfactant nonionic surfactant consisting of a fluorine segment and a non-fluorine segment. Examples of the combination of the fluorine segment and the non-fluorine segment of the fluorosurfactant include molecular designs such as an addition polymer of a fluorinated alkyl group-containing alcohol and a monomer containing an oxyalkylene group such as ethylene oxide or propylene oxide, and a copolymer of a fluorinated alkyl group-containing ethylenically unsaturated compound and a polyoxyalkylene group-containing ethylenically unsaturated compound.

[0038] As the ethylenically unsaturated compound containing a fluorinated alkyl group, a monomer containing a (meth)acrylic ester group is suitable from the viewpoint of compatibility with the resin composition for a water-repellent lens protective film or the coating film uniformity based on such compatibility. Specifically, it is a fluoroalkyl (meth)acrylate (C1) represented by the following general formula (c1).

[0039] [ka] (In the formula, Rf is a perfluoroalkyl group having 4 to 8 carbon atoms, and R 7 is a hydrogen atom or a methyl group, and p is an integer of 1 to 6. The number of carbon atoms in the fluorinated alkyl group Rf in the fluoroalkyl (meth)acrylate (C1) is preferably 4 to 6. When the number of carbon atoms is 4 or more, the surface tension reducing ability is improved, and when the number of carbon atoms is 6 or less, the compatibility with other compounds is improved. The fluoroalkyl (meth)acrylate (C1) can be used alone or in combination of two or more.

[0040] Furthermore, from the viewpoint of reducing the amount of residual components remaining in the water-repellent lens after the protective film is peeled off, the fluorine-based nonionic surfactant preferably contains a photopolymerizable group, and the preferred form of the surfactant is a polymer having a side chain having an ethylenically unsaturated group and a side chain having a fluorinated alkyl group or a group containing an oxygen atom as part of the fluorinated alkyl group.

[0041] From the viewpoint of photoreactivity, the repeating units having an unsaturated group-containing side chain are preferably repeating units c2 to c5 represented by the following general formula: In addition, the repeating units having an unsaturated group-containing side chain in one molecule may be the same or different.

[0042] [ka] [ka] [ka] [ka] R 8 , R 9 , R 10 , R 11 is a hydrogen atom or a methyl group.

[0043] Among these nonionic surfactants, it is particularly preferable to use a fluorosurfactant. Fluorosurfactants have a high ability to reduce the surface tension of the resin composition for the water-repellent lens protective film, so they are suitable for coating ultra-water-repellent lenses with low surface energy. In addition, the protective film for this application is required to have adhesion to the ultra-water-repellent lens so as not to cause axial misalignment during processing, and to have releasability so that it can be easily peeled off after use. Since the water-repellent layer formed on the surface of the ultra-water-repellent lens is treated with a fluorine-based coating, the protective film is also formulated with a fluorosurfactant that easily interacts with this layer, thereby achieving the contradictory properties of moderate adhesion and releasability. Furthermore, the fluorosurfactant is preferably one that, when mixed in propylene glycol monomethyl ether acetate at a concentration of 0.1 parts by mass, reduces the surface tension of the mixed liquid to 26.0 mN / m or less, more preferably to 23.0 mN / m or less. By using a surfactant that can reduce the surface tension to 23.0 mN / m or less, the surface tension can be reduced efficiently, and uniform coating can be achieved with a smaller amount added.

[0044] Examples of commercially available fluorosurfactants having the above-mentioned surface tension reducing ability include Megafac F-477, Megafac F-554, Megafac F-557, Megafac R-41, Megafac RS-56, Megafac RS-72-K, Megafac RS-75-A, Megafac RS-75-NS, Megafac RS-78 (all trade names manufactured by DIC Corporation).

[0045] The content of component (C) is preferably 0.01 to 10% by mass, more preferably 0.01 to 5% by mass, based on the total solid content of the resin composition for water-repellent lens protective film. If the content is in the range of 0.01 to 10% by mass, it becomes possible to uniformly coat the resin composition for water-repellent lens protective film even on a substrate that is extremely difficult to coat, such as an ultra-water-repellent lens. Furthermore, if the content is in the range of 0.01 to 5% by mass, it becomes possible to obtain a uniform protective film without causing a decrease in the water repellency of the water-repellent lens due to residual surfactant when the protective film is peeled off.

[0046] <Component (D): Hardener> The resin composition for water-repellent lens protective film may contain a compound having a functional group capable of reacting with a (meth)acrylate compound as a curing agent. Although not particularly limited, a polyfunctional thiol compound having good curing properties in the atmosphere is preferable. The polyfunctional thiol compound is an organic compound having two or more thiol groups (-SH groups). For example, a polyfunctional thiol compound represented by the following general formula (Formula 3) can be mentioned. The polyfunctional thiol compound can be used alone or in combination of two or more kinds.

[0047] [ka] (In the formula, n is an integer of 2 to 5, b is an integer of 2 to 10, and R 12 is either a hydrocarbon group (α1) having 2 to 30 carbon atoms, a group (α2) consisting only of an ether oxygen (-O-) and a hydrocarbon group having 2 to 40 carbon atoms, an isocyanurate ring (α3), or a group (α4) consisting only of an isocyanurate ring and a hydrocarbon group.

[0048] In the above general formula (Formula 3), a compound with n=1 can be used without any major problems, but the high reactivity of the resulting polyfunctional thiol compound tends to slightly deteriorate the storage stability of the resin composition for water-repellent lens protective film containing the compound. In contrast, a compound with n=2 to 5 has excellent storage stability and good curability even in air. As the number of n increases, the reactivity of the resulting polyfunctional thiol compound decreases, and the amount of UV irradiation during curing of the resin composition for water-repellent lens protective film containing the compound tends to increase. Therefore, among the compounds represented by the above general formula (Formula 3), a compound with n=2 is most preferable. This is because the reactivity of the polyfunctional thiol compound is most suitable for achieving both storage stability and shortening the curing time during heat curing when the compound is cured. For example, examples of polyfunctional thiols include trimethylolpropane tris(3-mercaptopropionate), tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate, pentaerythritol tetrakis(3-mercaptopropionate), tetraethylene glycol bis(3-mercaptopropionate), and dipentaerythritol hexakis(3-mercaptopropionate).

[0049] The weight average molecular weight of the polyfunctional thiol compound is 200 to 2000, preferably 300 to 1800, and more preferably 350 to 1600. If the molecular weight is less than 200, there is no problem with curability, but the polyfunctional thiol compound tends to be highly volatile and have a strong odor. On the other hand, if the molecular weight is more than 2000, the solubility in the (A) polyfunctional (meth)acrylate resin may be reduced.

[0050] Strictly speaking, the properties of the resin composition for use in a water-repellent lens protective film after it has been cured are affected by the value of ((D) number of functional groups in the curing agent) / (number of (meth)acryloxy groups) (hereinafter referred to as the (D) / (A) functional group ratio) per unit weight of the resin composition for use in a water-repellent lens protective film. If the (D) / (A) functional group ratio is in the range of 0.15 to 2.0, dense crosslinks are formed, resulting in a tough cured product. More preferably, if the ratio is in the range of 0.3 to 1.5, a tough cured product will be obtained, and the UV curability will be improved, allowing curing with a smaller cumulative light dose, thereby suppressing the effects on the water-repellent lens during curing.

[0051] <(E): Diluent> The resin composition for water-repellent lens protective film of the present invention may be diluted with an organic solvent or a reactive diluent to make the reaction system uniform and facilitate coating. Examples of such organic solvents include alcohol-based solvents, aromatic hydrocarbon-based solvents, ether-based solvents, ester-based solvents, ether ester-based solvents, ketone-based solvents, and phosphate ester-based solvents. It is preferable to limit the amount of these organic solvents to less than 10,000 parts by mass per 100 parts by mass of the resin composition for water-repellent lens protective film, but since the solvent is basically volatilized at the time of forming a cured film, it does not have a significant effect on the physical properties of the cured film. As the reactive diluent, a monofunctional or polyfunctional photopolymerizable monomer having a vinyl group, an acryloyl group, a methacryloyl group, or the like can be used. Of these, (meth)acrylate compounds having an acryloyl group or a methacryloyl group are preferred, and examples thereof include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, tert-butyl (meth)acrylate, isobutyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isodecyl (meth)acrylate, n-hexyl (meth)acrylate, stearyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, cyclohexyl (meth)acrylate, and isobornyl (meth)acrylate, ethoxyethyl (meth)acrylate, methoxyethyl (meth)acrylate, and butoxy (meth)acrylate. Alkoxyalkyl (meth)acrylates such as ethyl (meth)acrylate, 2-methoxyethoxyethyl (meth)acrylate, and 2-ethoxyethoxyethyl (meth)acrylate; hydroxyalkyl (meth)acrylates such as glycidyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, and 2-hydroxypropyl (meth)acrylate; alkoxy(poly)alkylene glycol (meth)acrylates such as methoxydiethylene glycol (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, and methoxydipropylene glycol (meth)acrylate; fluorinated alkyl (meth)acrylates such as octafluoropentyl (meth)acrylate; N,N-dimethylaminoethyl (meth)acrylate; N,Dialkylaminoalkyl(meth)acrylates such as N-diethylaminoethyl(meth)acrylate, allyl(meth)acrylate, 1,3-butanediol(meth)acrylate, 1,4-butanediol(meth)acrylate, 1,6-hexanediol(meth)acrylate, 3-methylpentanediol(meth)acrylate and other glycol mono(meth)acrylates, monofunctional(meth)acrylate compounds, polyethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, hydroxypivalic acid ester neopentyl glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, 1,3-bis(hydroxypropyl) Examples of the polyfunctional (meth)acrylates include hydroxyethyl)-5,5-dimethylhydantoin di(meth)acrylate, α,ω-di(meth)acrylbisdiethylene glycol phthalate, trimethylolpropane tri(meth)acrylate, pentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol monohydroxypenta(meth)acrylate, 2-hydroxyethyl(meth)acryloyl phosphate, trimethylolpropane tri(meth)acrylate, ethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, and diacryloxyethyl phosphate.

[0052] The resin composition for water-repellent lens protective film of the present invention may contain additives such as colorants such as pigments and dyes, stabilizers, flame retardants, organic fillers, plasticizers, antioxidants, defoamers, coupling agents, rheology control agents, etc. in appropriate amounts within the range that does not impair the characteristics of the present invention. By adding these additives, it is possible to obtain a resin composition for water-repellent lens protective film and a protective film, which is its cured product, that are excellent in resin strength, adhesive strength, workability, storage stability, etc.

[0053] <Formation of protective film> The method of forming a protective film using the resin composition for water-repellent lens protective film of the present invention is not particularly limited, but examples thereof include methods such as dip coating, spray coating, and spin coating. The thickness of the protective film formed using the resin composition for water-repellent lens protective film of the present invention is not particularly limited, but it is preferably 10 μm or more from the viewpoint of preventing axial deviation during edging and preventing scratches during processing and storage. On the other hand, the thickness of the coating film is preferably 100 μm or less so that position deviation does not occur when identifying the lens center.

[0054] After coating the resin composition for water-repellent lens protective film of the present invention, the composition coated on the substrate can be irradiated with active energy rays such as ultraviolet rays to obtain a protective film. Examples of light sources used in the active energy ray irradiation step include UV-LED (ultraviolet LED), low pressure mercury lamp, high pressure mercury lamp, ultra-high pressure mercury lamp, metal halide lamp, carbon arc, xenon arc, gas laser, solid laser, and electron beam irradiation device. Among these, UV-LEDs are preferred as they consume significantly less power than conventional UV lamps and generate less heat from their light source than UV lamps. Furthermore, by using UV-LEDs with a peak illuminance of 395 nm or more, which is close to visible light, the impact of ultraviolet light exposure on the water-repellent lens can be suppressed and the occurrence of cracks in the water-repellent layer can be suppressed.

[0055] The resin composition for water-repellent lens protective film of the present invention can be uniformly applied to a water-repellent lens having a water-repellent / oil-repellent layer formed on the surface of a plastic or glass substrate to impart antifouling properties. The resin composition for water-repellent lens protective film of the present invention can form a uniform protective film even on a lens having a super water-repellent layer formed thereon, which has been developed in recent years to further improve antifouling properties. The present invention can be applied to a lens having a water-repellent layer with a contact angle to water of 90° or more, and is particularly effective for a lens having a water-repellent layer with a contact angle of 140° or more. A lens having a contact angle to water of 90° or more and 110° or less is called a normal water-repellent lens, a lens having a contact angle to water of more than 110° and 140° or less is called a highly water-repellent lens, and a lens having a contact angle to water of more than 140° is called a super water-repellent lens.

[0056] The contact angle of a water-repellent lens can be evaluated using a method called the sessile drop method. A 1 μL droplet of pure water is prepared and brought into contact with the target water-repellent lens so that it lands on the lens. The angle between the water-repellent lens and the droplet at that time is evaluated as the contact angle. EXAMPLES

[0057] (A) Component: Multifunctional (meth)acrylate A-1: Ethylene oxide modified bisphenol A dimethacrylate (Blenmer PDBE-200A, NOF Corporation: bifunctional, molecular weight 541) A-2: Urethane acrylate (Art Resin UN-2700 manufactured by Negami Chemical Industries, Ltd.: bifunctional, weight average molecular weight 2000) A-3: Urethane acrylate (Art Resin UN-352, manufactured by Negami Chemical Industries, Ltd.: bifunctional, weight average molecular weight 3000) A-4: Polyether-based urethane acrylate (Art Resin UN-6200, manufactured by Negami Chemical Industries, Ltd.: bifunctional, weight average molecular weight 8000) A-5: Polycarbonate-based urethane acrylate (Art Resin UN-9200A, manufactured by Negami Chemical Industries, Ltd.: bifunctional, weight average molecular weight 15,000) A-6: Polyether-based urethane acrylate (Art Resin UN-6305, manufactured by Negami Chemical Industries, Ltd.: bifunctional, weight average molecular weight 27,000) A'-1: Ethylene glycol dimethacrylate (Light Ester EG, Kyoeisha Chemical Co., Ltd.: bifunctional, molecular weight 198) A'-2: Urethane acrylate (Shiko UV-3700B, manufactured by Nippon Synthetic Chemical Industry Co., Ltd.: bifunctional, weight average molecular weight 38,000)

[0058] Component (B): Photopolymerization initiator B-1: 2,2-dimethoxy-2-phenylacetophenone (OMNIRAD651, manufactured by IGM) B-2: 2-benzyl-2-(dimethylamino)-4'-morpholinobutyrophenone (OMNIRAD369, IGM) B-3: Bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (OMNIRAD819 manufactured by IGM) B-4: 1-Hydroxycyclohexyl phenyl ketone (OMNIRAD184 IGM)

[0059] (C) Component: Nonionic surfactant C-1: Fluorine-based nonionic surfactant (MEGAFAC RS-75-A manufactured by DIC Corporation, surface tension 23.8 mN / m when mixed with 0.1 part by mass in PGMEA) C-2: Fluorine-based nonionic surfactant (MEGAFAC RS-78, manufactured by DIC Corporation, surface tension 22.0 mN / m when mixed with 0.1 part by mass in PGMEA) C-3: Fluorine-based nonionic surfactant (MEGAFAC F-560 manufactured by DIC Corporation; surface tension 21.4 mN / m when mixed at 0.1 parts by weight in PGMEA) C-4: Fluorine-based nonionic surfactant (MEGAFAC F-477, manufactured by DIC Corporation; surface tension 25.4 mN / m when mixed with 0.1 parts by weight in PGMEA) C'-1: Fluorine-based anionic surfactant (MEGAFAC F-114 manufactured by DIC Corporation; surface tension 26.5 mN / m when mixed at 0.1 parts by mass in PGMEA)

[0060] Component (D): Hardener D-1: Dipentaerythritol hexakis(3-mercaptopropionate) (DPMP manufactured by SC Organic Chemicals Co., Ltd.: 6 functional groups, molecular weight 783)

[0061] (E) Ingredient: Diluent E-1: Methyl ethyl ketone E-2: Butyl acrylate

[0062] Components (A) to (E) were added to a mixing vessel in the proportions shown in Tables 1 and 2, and stirred with a three-one motor at room temperature (23°C) under UV protection until homogenous, to obtain a sample of a resin composition for water-repellent lens protective film. The obtained resin compositions for water-repellent lens protective film of each of the Examples and Comparative Examples were evaluated for viscosity, coatability, photocurability, retention, peelability, and lens contamination as described below. The results are shown in Tables 1 and 2.

[0063] [Protective film formation on super water-repellent lenses] For the evaluation, a plastic lens with an ultra-water-repellent layer having a contact angle of 150° with pure water was used. The resin compositions for water-repellent lens protective films of the Examples and Comparative Examples were coated onto the ultra-water-repellent lenses by dip coating. After coating, the lenses were left to stand for 10 minutes at room temperature (23°C) in a space that was protected from ultraviolet rays, and then dried. The lenses were then exposed to an LED ultraviolet ray irradiation device (Unijet E110IIHD-365 manufactured by Ushio Inc.) with an illumination intensity of 500 mW / cm. 2 The distance from the lens was adjusted so that the curing was even, and each side was irradiated at the same time. The same method was also used to cure the resin using an LED ultraviolet irradiation device (Ushio Electric Co., Ltd. Unijet E110IIHD-395) with a peak wavelength of 395 nm.

[0064] [Viscosity measurement] After leaving the sample at 25°C for 3 minutes, the "viscosity (mPa s)" was measured using an E-type viscometer (Toki Sangyo Co., Ltd. RE-85L, cone: CORD-1 1°34' × R24) under the following measurement conditions: 25°C, 20 rpm.

[0065] [Coatability evaluation] The resin composition for water-repellent lens protection film was coated on a super water-repellent lens by the dip coating method described above, and cured. If repelling was observed, the maximum width of the uncoated part from the edge of the lens was measured as the repelling size, and it was evaluated as follows. For the coatability, the repelling size must be 10 mm or less. ◎: No repelling. ◯: The uncoated portion from the edge is 10 mm or less. ×: The portion that is not coated from the edge is greater than 10 mm.

[0066] [Photocuring evaluation] When the resin composition for the water-repellent lens protective film after coating was cured with an LED ultraviolet irradiation device, the cumulative light amount at which the tack of the surface was removed by irradiation was confirmed and evaluated as follows. The cumulative light amount was determined to be 20,000 mJ / cm based on the thermal effect on the lens and the curing time. 2 It needs to be as follows: ◎: Accumulated light amount is 1000mJ / cm 2 The following is the result. ○: 1000mJ / cm 2 More than 20000mJ / cm 2 The following is the result. ×:20000mJ / cm 2 More.

[0067] [Retention strength evaluation] To evaluate the axial misalignment during edge processing, the retention strength of the protective film formed on the superhydrophobic lens was evaluated. The retention strength was measured by changing the load in accordance with JIS-Z0237. A 24 mm wide, 130 mm long adhesive tape (CT405AP-24 manufactured by Nichiban Co., Ltd.) was attached to the center of the superhydrophobic lens on which the protective film had been formed (see Figure 1). At this time, a mark was made with an oil-based pen so that it overlapped with the adhesive tape at the center of the concave part of the lens. A load of 14.7 N was applied to the end of the adhesive tape opposite the end attached to the lens, and the distance at which the marks on the convex and concave surfaces were misaligned after 10 minutes was measured (see Figure 2). The measurement results were evaluated as follows: ◎: The holding force measurement result is 0.0 mm. ◯: The retention force measurement result is greater than 0.0 mm and less than 2.0 mm. ×: The holding force measurement result is greater than 2.0 mm.

[0068] [Peelability] After tape was applied to the edge of the protective film formed on the super water repellent lens and the protective film was peeled off, the appearance and peelability of the lens were visually inspected and evaluated as follows. ○: Peeled off without leaving any residue. ×: Cracks or cracks occurred during peeling, or peeling was not possible.

[0069] [Lens contamination] After peeling the protective film from the ultra-water-repellent lens, a line was drawn on the lens with an oil-based marker (Teranishi Chemical Industry Co., Ltd.'s black magic ink) and the ink repelling was observed and rated as follows. Note that the ink of the oil-based marker repels before the protective film is formed, but if contaminants remain on the lens surface, the water repellency decreases and the repelling becomes poor. ○: A straight line drawn with ink appears as dots. ×: No ink repellency is observed in the straight line drawn.

[0070] As shown in Tables 1 and 2, all of the samples in the examples can be applied to superhydrophobic lenses and can be cured with an LED UV irradiation device with a peak wavelength of 395 nm. In addition, because they have sufficient retention strength to prevent axial misalignment during edging, even superhydrophobic lenses can be processed into the desired shape using conventional processing methods.

[0071] On the other hand, in Comparative Example 1, which does not contain the nonionic surfactant (C) and Comparative Example 2, which contains an anionic surfactant instead of the nonionic surfactant (C), it is not possible to coat the super water-repellent lens, and even a protective film cannot be formed. In Comparative Example 3, the curing is poor when using an LED ultraviolet irradiation device with a peak wavelength of 395 nm, and the allowable cumulative light amount is exceeded. Furthermore, the toughness of the cured film is low, so the peeling is poor, as it tears when peeled off. In Comparative Example 4, the photocuring is good, but the flexibility of the cured film is high, and the retention force is greater than the specified value. This causes axial misalignment during peripheral processing.

[0072] [Table 1]

[0073] [Table 2]

Claims

1. (A) a polyfunctional (meth)acrylate having a weight average molecular weight of 200 to 30,000; (B) a photopolymerization initiator; (C) a nonionic surfactant; (D) containing a polyfunctional thiol compound, A resin composition for use in a water-repellent lens protective film, in which the functional group ratio ((D) / (A)) of the number of thiol groups in (D) to the number of (meth)acryloxy groups in (A) is 0.3 to 2.

0.

2. 2. The resin composition for a water-repellent lens protective film according to claim 1, wherein the nonionic surfactant (C) is a fluorine-containing nonionic surfactant having a surface tension of 26.0 mN / mm or less when mixed in an amount of 0.1 part by mass in propylene glycol monomethyl ether acetate.

3. Illuminance 50-3000mW / cm 2 When using an LED light source, the cumulative light quantity is 5000 mJ / cm 2 3. The resin composition for a water-repellent lens protective film according to claim 1, which is curable at a temperature of 0.1 to 100° C.

4. A method for protecting a water-repellent lens by applying to the water-repellent lens a resin composition for a water-repellent lens protective film according to any one of claims 1 to 3 and curing the composition to provide a protective film thereon.

Citation Information

Patent Citations

  • Shaft slippage preventing kit for use in shaping lens for glasses and lens shaping method for glasses using the same

    JP2004122238A

  • Plastic spectacle lens with protective coat film

    JP2009109611A

  • Protecting film of lens and method for manufacturing the same

    JP2010085691A

  • Spectacle lens, method for manufacturing the spectacle lens, and treatment liquid

    JP2013228437A