Thermoelectric conversion materials and thermoelectric conversion elements

A polymer-based thermoelectric conversion material with aromatic hydrocarbon groups and conductive additives addresses the limitations of inorganic materials by enhancing conductivity and flexibility, enabling efficient and cost-effective thermoelectric elements.

JP7585628B2Active Publication Date: 2024-11-19TOYO INK MFG CO LTD +1
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020104431
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-17
Publication Date
2024-11-19
Estimated Expiration
2040-06-17

AI Technical Summary

Technical Problem

Existing thermoelectric conversion materials, particularly those containing inorganic materials, face challenges such as high cost, complexity in manufacturing, rigidity, heaviness, and limited flexibility, making them unsuitable for non-planar installations and requiring high energy and cost for production.

Method used

A thermoelectric conversion material comprising a polymer with monomer units derived from (meth)acrylonitrile and aromatic hydrocarbon groups, combined with a conductive material, enhances conductivity and stability, allowing for flexible and efficient thermoelectric conversion elements.

Benefits of technology

The material achieves both high thermoelectric conversion performance and conductivity, with improved flexibility and stability at room temperature, facilitating the production of high-performance thermoelectric elements suitable for various installations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585628000001
    Figure 0007585628000001
  • Figure 0007585628000002
    Figure 0007585628000002
Patent Text Reader

Abstract

To provide a thermoelectric conversion material that can achieve both thermoelectric conversion performance and electrical conductivity, and also to provide a thermoelectric conversion element with excellent thermoelectric conversion performance and resistance at room temperature.SOLUTION: The problem to be solved by the present invention can be solved by a thermoelectric conversion material including a polymer (A) and a conductive material (B), and the polymer (A) is a copolymer containing monomer units derived from (meth)acrylonitrile and monomer units having aromatic hydrocarbon groups.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermoelectric conversion material and a thermoelectric conversion element. [Background technology]

[0002] Thermoelectric conversion technology, which converts heat into electricity using thermoelectric conversion materials, has been attracting attention as a clean energy source that can effectively utilize minute thermal energy such as body heat and exhaust heat from factories, cars, and homes, as well as various types of heat in nature, as electricity. There are various thermoelectric effects that are used in thermoelectric conversion technology, but the mainstream system uses the Seebeck effect, in which an electromotive force is generated by an electron gradient that occurs within a material in response to the temperature difference when two different temperatures are applied to both ends of the material, which is made up of a combination of semiconductors and metals.

[0003] Thermoelectric materials that can convert between thermal energy and electrical energy are used in thermoelectric conversion elements such as thermoelectric power generation elements and Peltier elements. Thermoelectric conversion elements are elements that convert heat into electricity and are made up of a combination of semiconductors and metals. Representative thermoelectric conversion elements are classified into p-type semiconductors alone, n-type semiconductors alone, and combinations of p-type and n-type semiconductors. To obtain a larger potential difference, thermoelectric conversion elements generally use a combination of p-type and n-type semiconductors as materials.

[0004] Thermoelectric conversion elements, such as Peltier elements, are used as thermoelectric modules that combine a number of elements into a plate or cylinder. Because they can directly convert thermal energy into electricity, they can be used, for example, as a power source for wristwatches that operate with body heat, and for power generation on the ground and in artificial satellites. The performance of a thermoelectric conversion element depends on the performance of the thermoelectric conversion material and the durability of the module.

[0005] As described in Non-Patent Document 1, the dimensionless thermoelectric figure of merit ZT is used as an index representing the performance of a thermoelectric conversion material. In addition, the power factor PF (=S 2 ·σ) may also be used. The dimensionless thermoelectric figure of merit ZT is expressed by the following formula (1). ZT=((S 2 ·σ) / к)·T Equation (1) Here, S is the Seebeck coefficient (V / K), σ is the electrical conductivity (S / m), T is the absolute temperature (K), and κ is the thermal conductivity (W / (m K)). Thermal conductivity κ is expressed by the following formula (2). к=α·ρ·C Equation (2) where α is the thermal diffusivity (m 2 / s), ρ is density (kg / m 3 ), and C is the specific heat capacity (J / (kg K)). That is, in order to improve the thermoelectric conversion performance (hereinafter also referred to as thermoelectric properties), it is important to improve the Seebeck coefficient or electrical conductivity while decreasing the thermal conductivity.

[0006] Representative thermoelectric conversion materials include inorganic materials such as bismuth-tellurium (Bi-Te) systems for temperatures from room temperature to 500 K, lead-tellurium (Pb-Te) systems for temperatures from room temperature to 800 K, and silicon-germanium (Si-Ge) systems for temperatures from room temperature to 1000 K.

[0007] However, thermoelectric conversion materials containing these inorganic materials often contain rare elements and are expensive, or may contain harmful substances. In addition, inorganic materials are poorly processable, making the manufacturing process complicated. Therefore, thermoelectric conversion materials containing inorganic materials require high manufacturing energy and manufacturing costs, making it difficult to generalize them. Furthermore, since materials containing inorganic materials are rigid, it is difficult to form flexible thermoelectric conversion elements that can be installed on shapes that are not flat. In addition, thermoelectric conversion materials containing inorganic materials generally have a high specific gravity, so there is also the issue that they tend to become heavy when the elements are combined into a module.

[0008] In response to this, research is being conducted into thermoelectric conversion elements that use organic materials instead of conventional inorganic materials. Organic materials are lightweight, have excellent moldability, and are more flexible than inorganic materials, making them highly versatile within the temperature range in which they do not decompose. In addition, they are more advantageous than inorganic materials in terms of manufacturing energy and costs, as printing technology can be easily utilized.

[0009] For example, Patent Document 1 discloses a thermoelectric conversion material containing a polymer dispersant having an organic dye skeleton and carbon nanotubes (CNTs), and a thermoelectric conversion element using the same. Patent Document 2 discloses a thermoelectric conversion material containing a conductive compound in which a polycyclic aromatic ring having carrier transport properties is bonded to a substituent containing an alkyl group, and a thermoelectric conversion element using the same. However, the invention of Patent Document 1 does not provide sufficient performance as a thermoelectric conversion element. Also, the invention of Patent Document 2 discloses a thermoelectric conversion material having a conductivity of 10 -8 ~10 -7 The electrical conductivity is low at only S / cm, and it is not possible to obtain a practical value for use as a thermoelectric conversion element. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] International Publication No. 2015 / 050113 [Patent Document 2] International Publication No. 2015 / 129877 [Patent Document 3] International Publication No. 2017 / 104757 [Non-patent literature]

[0011] [Non-Patent Document 1] Takenobu Kajikawa, "Thermoelectric Conversion Technology Handbook (First Edition)", NTS Publishing, p. 19 Summary of the Invention [Problem to be solved by the invention]

[0012] The problem to be solved by the present invention is to provide a thermoelectric conversion material that can achieve both thermoelectric conversion performance and electrical conductivity, and to provide a thermoelectric conversion element that has excellent thermoelectric conversion performance and durability at room temperature. [Means for solving the problem]

[0013] The present inventors have conducted extensive research to solve the above problems and have arrived at the present invention. That is, the present invention relates to a thermoelectric conversion material comprising a polymer (A) and a conductive material (B), wherein the polymer (A) is a copolymer comprising a monomer unit derived from (meth)acrylonitrile and a monomer unit having an aromatic hydrocarbon group.

[0014] The present invention also relates to the above thermoelectric conversion material, wherein the monomer having an aromatic hydrocarbon group contains a styrene-based monomer.

[0015] The present invention also relates to the above thermoelectric conversion material, wherein the polymer (A) contains 40% by mass or more and less than 100% by mass of monomer units derived from (meth)acrylonitrile.

[0016] The present invention also relates to the above thermoelectric conversion material, wherein the polymer (A) contains from 1% by mass to 60% by mass of monomer units having an aromatic hydrocarbon group.

[0017] The present invention also relates to the above thermoelectric conversion material, which further contains at least one selected from the group consisting of inorganic metal salts, inorganic bases, and organic bases.

[0018] The present invention also relates to the above thermoelectric conversion material, wherein the content of the polymer (A) is 5 to 100 mass % based on the total amount of the conductive material (B).

[0019] The present invention also relates to a thermoelectric conversion element having a thermoelectric conversion film containing the above-mentioned thermoelectric conversion material and electrodes, the thermoelectric conversion film and the electrodes being electrically connected to each other. Effect of the Invention

[0020] The present invention provides a thermoelectric conversion material that can achieve both thermoelectric conversion performance and electrical conductivity. In addition, the material can be used to provide a thermoelectric conversion element that has excellent thermoelectric conversion performance and excellent resistance at room temperature. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, an embodiment of the present invention will be described. In this specification, unless otherwise specified, the terms "(meth)acrylic", "(meth)acrylo", "(meth)acrylic acid", "(meth)acrylate", and "(meth)acryloyloxy" refer to "acrylic or methacrylic", "acrylo or methacrylo", "acrylic acid or methacrylic acid", "acrylate or methacrylate", and "acryloyloxy or methacryloyloxy", respectively.

[0022] <Thermoelectric conversion materials> The thermoelectric conversion material of the present invention is a thermoelectric conversion material containing a polymer (A) and a conductive material (B), and is characterized in that the polymer (A) is a copolymer containing a monomer unit derived from (meth)acrylonitrile and a monomer unit having an aromatic hydrocarbon group. Hereinafter, an embodiment of the present invention will be described in detail.

[0023] <Polymer (A)> The polymer (A) is a copolymer containing a monomer unit derived from (meth)acrylonitrile and a monomer unit having an aromatic hydrocarbon group. The polymer (A) may be in the form of either a random copolymer or a block copolymer. It is presumed that the strong polarity of the cyano group in the (meth)acrylonitrile in the polymer (A) and the aromatic hydrocarbon group enhance the adsorption to the conductive material (B), suppress the aggregation of the conductive material (B) and the adsorption of moisture to the conductive material (B), and allow the conductive material (B) to exist stably in the thermoelectric conversion material.

[0024] First, the monomer having an aromatic hydrocarbon group, which is a constituent unit of the polymer (A), will be described. The monomer having an aromatic hydrocarbon group is not particularly limited as long as it is a monomer having at least one aromatic hydrocarbon group capable of forming a polymer, and the aromatic hydrocarbon group may have any substituent.

[0025] Examples of monomers having an aromatic hydrocarbon group include styrene, phenyl (meth)acrylate, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, α-methoxystyrene, 4-methoxystyrene, 4-vinylbiphenyl, 4-isopropenyltoluene, 2-isopropenyltoluene, 4-n-octylstyrene, 4-tert-butylstyrene, 1-vinylnaphthalene, m-vinylbenzyl cyanide, p-vinylbenzyl cyanide, phenoxyethyl (meth)acrylate, benzyl (meth)acrylate, allyl benzoate, and allyl benzyl ether.

[0026] The monomer having an aromatic hydrocarbon group preferably includes a styrene-based monomer. In this specification, the styrene-based monomer refers to a monomer in which a vinyl group or an isopropenyl group is bonded to the aromatic ring of an aromatic hydrocarbon. In addition, the aromatic hydrocarbon may be a monocyclic aromatic hydrocarbon, a condensed ring aromatic hydrocarbon, or a ring assembly hydrocarbon. Examples of the styrene-based monomer include styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 4-methoxystyrene, 4-methoxystyrene, 4-isopropenyltoluene, 2-isopropenyltoluene, 4-n-octylstyrene, 1-vinylnaphthalene, m-vinylbenzyl cyanide, and p-vinylbenzyl cyanide. Among the styrene-based monomers, styrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, and α-methylstyrene are preferred, and styrene is more preferred.

[0027] Of the structural units of the polymer (A), the unit derived from (meth)acrylonitrile is preferably contained in an amount of 40% by mass or more and less than 100% by mass, more preferably 65% ​​by mass or more and 99% by mass or less, even more preferably 65% ​​by mass or more and 95% by mass or less, and particularly preferably 75% by mass or more and 95% by mass or less. By containing the unit derived from (meth)acrylonitrile in the above range, good adsorption to the conductive material (B) can be obtained.

[0028] The monomer units having an aromatic hydrocarbon group are preferably contained in an amount of 1% by mass to 60% by mass, more preferably 10% by mass to 30% by mass, of all the monomer units in the copolymer. By containing the monomer units having an aromatic hydrocarbon group in this range, storage stability can be improved.

[0029] The polymer (A) may contain other monomers as constituent units other than the above monomers. Examples of the other monomers include: Vinyl ethers such as ethyl vinyl ether, n-propyl vinyl ether, isopropyl vinyl ether, n-butyl vinyl ether, and isobutyl vinyl ether; vinyl acetate, vinyl propionate and other vinyl fatty acids; heterocyclic (meth)acrylates such as tetrahydrofurfuryl (meth)acrylate and 3-methyloxetanyl (meth)acrylate; hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate; aliphatic unsaturated fatty acids such as (meth)acrylic acid and crotonic acid; Among other monomers, it is preferable to contain, as a constituent unit, an active hydrogen group-containing monomer such as hydroxyalkyl (meth)acrylates or aliphatic unsaturated fatty acids.

[0030] The method for producing the polymer (A) is not particularly limited, and may be any of, for example, a solution polymerization method, a suspension polymerization method, a bulk polymerization method, an emulsion polymerization method, a precipitation polymerization method, etc., with solution polymerization or precipitation polymerization being preferred, and precipitation polymerization being most preferred. The polymer (A) obtained by the precipitation polymerization method can be quickly removed after polymerization from low molecular weight components and residual monomers that dissolve in the solvent used during polymerization, so that it is possible to narrowly control the molecular weight distribution, and the amount of residual monomers can be reduced as much as possible, and a polymer (A) with a molecular weight that functions as a dispersant can be efficiently obtained. As the polymerization reaction system, addition polymerization such as ionic polymerization, free radical polymerization, and living radical polymerization can be used, and free radical polymerization or living radical polymerization is preferred. In addition, as the radical polymerization initiator, a compound selected from peroxides, azo-based initiators, etc., or a mixture thereof can be used, and a molecular weight regulator such as a chain transfer agent may be used as necessary.

[0031] The molecular weight of the polymer (A), in terms of polystyrene equivalent weight average molecular weight, is preferably in the range of 3000 to 500000, more preferably in the range of 4000 to 200000, further preferably in the range of 5000 to 100000, and particularly preferably in the range of 10000 to 100000. By setting the weight average molecular weight within the above range, good adsorption to the conductive material (B) can be obtained.

[0032] <Conductive material (B)> The conductive material (B) contributes to improving the conductivity. Therefore, the conductivity can be improved by increasing the content of the conductive material (B). The conductive material (B) is not particularly limited as long as it is a material having conductivity (carbon material, metal material, conductive polymer, etc.), and examples of the carbon material include graphite, carbon nanotubes, carbon black, graphene (including graphene nanoplates), etc. Examples of the metal material include metal powders such as gold, silver, copper, nickel, chromium, palladium, rhodium, ruthenium, indium, silicon, aluminum, tungsten, molybdenum, germanium, gallium, and platinum, as well as ZnSe, CdS, InP, GaN, SiC, SiGe, and alloys thereof, and composite powders thereof. In addition, fine particles coated with a core and a material different from the core material, specifically, for example, silver-coated copper powder in which the core material is copper and the surface is coated with silver, can be mentioned. Examples of the conductive polymer include powders of metal oxides such as silver oxide, indium oxide, tin oxide, zinc oxide, ruthenium oxide, ITO (tin-doped indium oxide), AZO (aluminum-doped zinc oxide), and GZO (gallium-doped zinc oxide), as well as powders surface-coated with these metal oxides. Examples of the conductive polymer include PEDOT / PSS (a composite of poly(3,4-ethylenedioxythiophene) and polystyrene sulfonic acid), polyaniline, polyacetylene, polypyrrole, polythiophene, and polyparaphenylene. The conductive material may be one type or a combination of two or more types. The shape of the conductive material (B) is not particularly limited, and may be amorphous, aggregated, scaly, microcrystalline, spherical, flake, wire, or the like, as appropriate.

[0033] From the viewpoint of achieving both a high Seebeck coefficient and electrical conductivity, at least one selected from the group consisting of carbon nanotubes, carbon black, and graphene (including graphene nanoplates) is preferred, more preferably carbon nanotubes, and particularly preferably single-walled carbon nanotubes.

[0034] Examples of carbon materials include flaky graphite such as CMX, UP-5, UP-10, UP-20, UP-35N, CSSP, CSPE, CSP, CP, CB-150, CB-100, ACP, ACP-1000, ACB-50, ACB-100, ACB-150, SP-10, SP-20, J-SP, SP-270, HOP, GR-60, LEP, F#1, and F manufactured by Nippon Graphite Industries Co., Ltd. Examples of the graphite include #2, F#3, BF-3AK, FBF, BF-15AK, CBR, CPB-6S, CPB-3, 96L, 96L-3, K-3, SC-120, SC-60, HLP, CP-150, and SB-1 manufactured by Chuetsu Graphite Industry Co., Ltd., EC1500, EC1000, EC500, EC300, EC100, and EC50 manufactured by Ito Graphite Industry Co., Ltd., and 10099M and PB-99 manufactured by Nishimura Graphite Co., Ltd. Examples of the spherical natural graphite include CGC-20, CGC-50, CGB-20, and CGB-50 manufactured by Nippon Graphite Industry Co., Ltd. Examples of the amorphous graphite include Blue P, AP, AOP, and P#1 manufactured by Nippon Graphite Industry Co., Ltd., and APR, K-5, AP-2000, AP-6, 300F, and 150F manufactured by Chuetsu Graphite Co., Ltd. Examples of artificial graphite include PAG-60, PAG-80, PAG-120, PAG-5, HAG-10W, and HAG-150 manufactured by Nippon Graphite Industries Co., Ltd.; G-4AK, G-6S, G-3G-150, G-30, G-80, G-50, SMF, EMF, SFF, SFF-80B, SS-100, BSP-15AK, BSP-100AK, and WF-15C manufactured by Chuetsu Graphite Co., Ltd.; and SGP-100, SGP-50, SGP-25, SGP-15, SGP-5, SGP-1, SGO-100, SGO-50, SGO-25, SGO-15, SGO-5, SGO-1, SGX-100, SGX-50, SGX-25, SGX-15, SGX-5, and SGX-1 manufactured by SEC Carbon Co., Ltd.

[0035] Examples of commercially available conductive carbon fibers and carbon nanotubes include vapor grown carbon fibers such as VGCF manufactured by Showa Denko K.K.; single-walled carbon nanotubes such as EC1.5 and EC1.5-P manufactured by Meijo Nano Carbon Co., Ltd., TUBALL manufactured by Kusumoto Chemicals Co., Ltd., and ZEONANO manufactured by Zeon Nano Technology Inc.; FloTube9000, FloTube7000, and FloTube2000 manufactured by CNano Corporation; NC7000 manufactured by Nanocyl Corporation; and 100T and 200P manufactured by Knano Corporation.

[0036] Examples of commercially available carbon black include Tokai Carbon's Tokablack #4300, #4400, #4500, and #5500; Degussa's Printex L; and Colombian's Raven7000, 5750, 5250, 5000ULTRAIII, and 500. Examples of the black include furnace blacks such as #2350, #2400B, #2600B, #3050B, #3030B, #3230B, #3350B, #3400B, and #5400B manufactured by Mitsubishi Chemical Corporation, MONARCH1400, 1300, and 900, VulcanXC-72R, and BlackPearls2000 manufactured by Cabot Corporation, Ensaco250G, Ensaco260G, Ensaco350G, and SuperP-Li manufactured by TIMCAL Corporation, Ketjen blacks such as EC-300J and EC-600JD manufactured by Lion Corporation, and acetylene blacks such as Denka Black, Denka Black HS-100, and FX-35 manufactured by Denki Kagaku Kogyo Co., Ltd., but are not particularly limited thereto.

[0037] When the monomer units derived from acrylonitrile in polymer (A) form a cyclic structure, the dispersibility, fluidity, and storage stability of the thermoelectric conversion material are improved. For example, when polymer (A) is treated with alkali, the monomer units derived from acrylonitrile are converted to a cyclic structure such as a hydrogenated naphthyridine ring, and dispersibility is improved. In addition, although the detailed mechanism is unknown, the formation of a cyclic structure also improves the thermoelectric performance of the thermoelectric conversion material. It is thought that the presence of a cyclic structure increases the adsorption to the conductive material (B), making it easier for carriers to move from polymer (A) to the conductive material (B).

[0038] The thermoelectric conversion material of the present invention preferably contains an inorganic base, an inorganic metal salt, or an organic base. This further improves the stability over time of the components constituting the thermoelectric conversion material. The inorganic base and inorganic metal salt preferably contain an alkali metal or an alkaline earth metal. For example, chlorides, hydroxides, carbonates, nitrates, sulfates, phosphates, tungstates, vanadates, molybdates, niobates, borates, etc. of alkali metals or alkaline earth metals. Among these, chlorides, hydroxides, and carbonates of alkali metals and alkaline earth metals are preferred in terms of being able to easily supply cations.

[0039] Examples of the hydroxide of an alkali metal include lithium hydroxide, sodium hydroxide, and potassium hydroxide. Examples of the hydroxide of an alkaline earth metal include calcium hydroxide and magnesium hydroxide. Examples of the carbonate of an alkali metal include lithium carbonate, lithium hydrogen carbonate, sodium carbonate, sodium hydrogen carbonate, potassium carbonate, and potassium hydrogen carbonate. Examples of the carbonate of an alkaline earth metal include calcium carbonate and magnesium carbonate. Among these, lithium hydroxide, sodium hydroxide, lithium carbonate, and sodium carbonate are more preferable. The metal in the inorganic base or inorganic metal salt may be a transition metal.

[0040] Examples of the organic base include primary, secondary or tertiary alkylamines and compounds containing a basic nitrogen atom, as shown below. Examples of primary alkylamines include propylamine, butylamine, isobutylamine, octylamine, 2-ethylhexylamine, laurylamine, stearylamine, oleylamine, 2-aminoethanol, 3-aminopropanol, 3-ethoxypropylamine, and 3-lauryloxypropylamine. Examples of secondary alkylamines include dibutylamine, diisobutylamine, N-methylhexylamine, dioctylamine, distearylamine, and 2-methylaminoethanol.

[0041] Examples of the tertiary alkylamine include triethylamine, tributylamine, N,N-dimethylbutylamine, N,N-diisopropylethylamine, dimethyloctylamine, trioctylamine, dimethyldecylamine, dimethyllaurylamine, dimethylmyristylamine, dimethylpalmitylamine, dimethylstearylamine, dilaurylmonomethylamine, triethanolamine, 2-(dimethylamino)ethanol, etc. The number of carbon atoms in the alkylamine is preferably 1 to 30, more preferably 1 to 20.

[0042] Further, examples of the organic base include compounds containing a basic nitrogen atom, such as 1,8-diazabicyclo[5.4.0]undecene-7 (DBU), 1,5-diazabicyclo[4.3.0]nonene-5 (DBN), 1,4-diazabicyclo[2.2.2]octane (DABCO), tri-n-butylamine, dimethylbenzylamine, monoethanolamine, imidazole, 1-methylimidazole, tetramethylammonium hydroxide, and tetraethylammonium hydroxide.

[0043] The blending amount of the inorganic base, inorganic metal salt, or organic base is preferably 1 to 50 parts by mass per 100 parts by mass of the polymer (A), which further improves dispersibility.

[0044] From the viewpoints of dispersing the conductive material (B) in the thermoelectric conversion material, improving the Seebeck coefficient, and achieving compatibility with electrical conductivity, the content of the polymer (A) is preferably 400% by mass or less, more preferably 200% by mass or less, even more preferably 120% by mass or less, and particularly preferably 100% by mass or less, based on the total amount of the conductive material (B). In order to exert the effects of the polymer (A), the lower limit of the polymer (A) is preferably 5% by mass or more, more preferably 20% by mass or more, even more preferably 25% by mass or more, and particularly preferably 40% by mass or more, based on the total amount of the conductive material (B).

[0045] In order to maintain the thermoelectric properties, the thermoelectric conversion material of the present invention preferably does not contain a compound that generates radicals, and more preferably consists of only the polymer (A) and the conductive material (B), or the polymer (A), the conductive material (B) and at least one selected from an inorganic metal salt, an inorganic base, and an organic base, but may contain other components as necessary.

[0046] (dispersion medium) The dispersion medium can be used as a medium when mixing the polymer (A) and the conductive material (B). The inclusion of the dispersion medium results in an ink or paste state, which can be used to form a thermoelectric conversion film by printing or coating. The dispersion medium that can be used is preferably one that can dissolve or disperse the polymer (A) and the conductive material (B), and examples of such dispersion medium include organic solvents and water. The dispersion medium may be used alone or in combination of two or more types.

[0047] Examples of organic solvents include alcohols such as methanol, ethanol, propanol, butanol, ethylene glycol methyl ether, diethylene glycol methyl ether, terpineol, dihydroterpineol, 2,4-diethyl-1,5-pentanediol, 1,3-butylene glycol, isobornylcyclohexanol, ethylene glycol, 1,3-propanediol, 1,4-butanediol, diethylene glycol, triethylene glycol, glycerin, polyethylene glycol, polypropylene glycol, trifluoroethanol, m-cresol, and thiodiglycol, ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, ethers such as tetrahydrofuran, dioxane, ethylene glycol dimethyl ether, and diethylene glycol dimethyl ether, hydrocarbons such as hexane, heptane, and octane, aromatics such as benzene, toluene, xylene, and cumene, esters such as ethyl acetate and butyl acetate, and N-methylpyrrolidone. These can be appropriately selected as needed. From the viewpoint of dispersibility and solubility of the polymer (A) and the conductive material (B), N-methylpyrrolidone is particularly preferred.

[0048] (resin) The thermoelectric conversion material of the present invention may contain a resin in addition to the polymer (A) for the purpose of adjusting the film-forming property and film strength, etc., within a range in which the properties are not affected by electrical conductivity and heat. The resin may be used alone or in combination of two or more. Also, it may be a copolymer of these resins. Although not particularly limited, in one embodiment, polyurethane resin, polyether resin, acrylic resin, and acrylamide resin are preferable. From the viewpoint of electrical conductivity, when a resin is contained, the content of the resin is preferably 99 mass% or less, more preferably 50 mass% or less, and even more preferably 20 mass% or less, based on the total mass of the polymer (A) and the conductive material (B).

[0049] (Inorganic thermoelectric conversion materials) The thermoelectric conversion material of the present invention may contain an inorganic thermoelectric conversion material as necessary in order to improve the thermoelectric conversion performance. The inorganic thermoelectric conversion material is not particularly limited, and any material generally known as a thermoelectric conversion material may be used. Impurities may be added to the inorganic thermoelectric conversion material to control the polarity (p-type, n-type) and electrical conductivity.

[0050] <Thermoelectric conversion element> The thermoelectric conversion element of the present invention has a thermoelectric conversion film formed using the thermoelectric conversion material of the present invention and electrodes, and the thermoelectric conversion film and the electrodes are electrically connected. The thermoelectric conversion film is excellent in heat resistance and flexibility in addition to electrical conductivity and thermoelectric properties. Therefore, a high-quality thermoelectric conversion element can be easily produced.

[0051] The thermoelectric conversion film may be a film obtained by applying a thermoelectric conversion material onto a substrate. Since the thermoelectric conversion material has excellent moldability, it is easy to obtain a good film by application or printing. The method for producing the thermoelectric conversion film is not particularly limited as long as the desired thermoelectric conversion film can be obtained, and can be appropriately selected according to the properties of the thermoelectric conversion material, such as viscosity, and the required film thickness, area, shape, and other conditions. For example, methods using various means such as spin coating, spray coating, roll coating, gravure coating, flexo coating, die coating, lip coating, knife coating, blade coating, comma coating, roll coating, curtain coating, bar coating, dip coating, dispenser, screen coating, and inkjet printing can be mentioned.

[0052] The thickness of the thermoelectric conversion film is not particularly limited and can be set according to the required electric properties such as current value, voltage value, and resistance, and thermoelectric properties, but as described later, it is preferable that the film is formed to have a certain thickness or more so that a temperature difference can be generated and transmitted in the thickness direction or surface direction of the thermoelectric conversion film. From the viewpoint of thermoelectric properties and flexibility, the film thickness of the thermoelectric conversion film is preferably in the range of 0.1 to 200 μm, more preferably in the range of 1 to 100 μm, and particularly preferably in the range of 1 to 60 μm.

[0053] The substrate is not particularly limited, and examples of the substrate that can be used include nonwoven fabric, paper, plastic films made of materials such as polyethylene, polyethylene terephthalate (PET), polyethylene naphthalate, polyethersulfone, polypropylene, polyimide, polycarbonate, and cellulose triacetate, and glass, etc. These substrates may have an aluminum deposition layer or a barrier layer on the substrate surface to prevent deterioration of the thermoelectric conversion material due to the effects of water and oxygen.

[0054] In order to improve the adhesion between the substrate and the thermoelectric conversion film, various treatments can be performed on the substrate surface. Specifically, prior to application of the thermoelectric conversion material, UV ozone treatment, corona treatment, plasma treatment, or easy-adhesion treatment can be performed.

[0055] The thermoelectric conversion film may be laminated with a substrate, or may be a free-standing film without a substrate. When preparing a free-standing film, there is no particular limitation, but for example, the film can be obtained by forming the thermoelectric conversion film on a release sheet and then removing the release coat.

[0056] Examples of the release sheet include release-treated plastic films such as polyester film, polyethylene film, polypropylene film, and polyimide film.

[0057] The thermoelectric conversion element can be constructed by applying techniques well known in the art, except that it is constructed using the above-mentioned thermoelectric conversion material. A more specific configuration of the thermoelectric conversion element and a manufacturing method thereof will be described below.

[0058] In a thermoelectric conversion element, a thermoelectric conversion film and an electrode are electrically connected. Here, "electrically connected" means that they are joined to each other or can be electrically connected via other components such as wires.

[0059] The material of the electrode is not particularly limited as long as it functions as an electrode, and can be selected from metals, alloys, and semiconductors. In one embodiment, metals and alloys are preferred because they have high electrical conductivity and low contact resistance of the thermoelectric conversion film. For example, it is preferred that the electrode contains at least one selected from the group consisting of gold, silver, copper, platinum, nickel, and aluminum. It is more preferred that the electrode contains silver.

[0060] The method for forming the electrodes is not particularly limited, and the electrodes can be formed by a method such as vacuum deposition, thermocompression bonding of an electrode material foil or a film having an electrode material film, application of a paste in which fine particles of the electrode material are dispersed, etc. From the viewpoint of process simplicity, a method using thermocompression bonding of an electrode material foil or a film having an electrode material film, or application of a paste in which the electrode material is dispersed is preferred.

[0061] Typical examples of the structure of a thermoelectric conversion element can be broadly classified into (1) a structure in which electrodes are formed on both ends of the thermoelectric conversion film of the present invention, and (2) a structure in which the thermoelectric conversion film of the present invention is sandwiched between two electrodes, based on the positional relationship between the thermoelectric conversion film and a pair of electrodes. The thermoelectric conversion element having the structure (1) above can be obtained, for example, by forming a thermoelectric conversion film on a substrate, and then applying silver paste to both ends of the film to form the first and second electrodes. In this way, a thermoelectric conversion element having electrodes formed on both ends of the thermoelectric conversion film can easily increase the distance between the two electrodes. Therefore, it is easy to generate a large temperature difference between the two electrodes and perform efficient thermoelectric conversion.

[0062] The thermoelectric conversion element having the structure of (2) above can be obtained, for example, by applying silver paste onto a substrate to form a first electrode, forming the thermoelectric conversion film of the present invention thereon, and further applying silver paste onto the first electrode to form a second electrode. In this way, a thermoelectric conversion element having the thermoelectric conversion film of the present invention sandwiched between two electrodes can utilize the temperature difference in the film thickness direction of the thermoelectric conversion film, that is, in the direction perpendicular to the substrate, and can be used in a form attached to a heat source. Therefore, it is preferable because it has the advantage of being able to extract heat from a wide range from the heat source. In the thermoelectric conversion element having the structure of (2) above, it is also possible to ensure a temperature difference by increasing the film thickness to widen the distance between the two electrodes.

[0063] Thermoelectric conversion elements can generate a high voltage by connecting them in series, and can generate a large current by connecting them in parallel. The thermoelectric conversion element may be one in which two or more thermoelectric conversion elements are connected. According to the present invention, since the thermoelectric conversion element has excellent flexibility, it can be well installed so as to conform to a heat source having a shape that is not flat. The thermoelectric conversion element may have a heat absorption layer or a heat storage layer for efficient heat transfer from a heat source, and may also have a heat insulation layer or a heat dissipation layer for ensuring a temperature difference. Furthermore, depending on the application and the amount of power required, the extracted electricity can be boosted using a boost circuit, or the extracted electric energy can be temporarily stored in a condenser, a capacitor, a secondary battery, or the like for use. EXAMPLES

[0064] The present invention will be described in more detail below with reference to the following experimental examples, but the present invention is not limited to these examples. In the examples, "parts" means "parts by mass" and "%" means "% by mass". "NMP" refers to N-methylpyrrolidone.

[0065] (Method of measuring weight average molecular weight (Mw)) The weight average molecular weight (Mw) was measured by gel permeation chromatography (GPC) equipped with an RI detector. The apparatus used was an HLC-8320GPC (manufactured by Tosoh Corporation), with three separation columns connected in series, and the packing materials used were Tosoh Corporation's "TSK-GELSUPERAW-4000", "AW-3000" and "AW-2500", respectively. The oven temperature was 40°C, and an N,N-dimethylformamide solution of 30 mM triethylamine and 10 mM LiBr was used as the eluent, at a flow rate of 0.6 mL / min. The measurement sample was adjusted to a concentration of 1% in the dispersion medium consisting of the above eluent, and 20 μL was injected. The molecular weight is a polystyrene equivalent value.

[0066] <Production of Polymer (A)> (Production Example 1) (Production of Polymer (A-1)) A reaction vessel equipped with a gas inlet tube, a thermometer, a condenser, and a stirrer was charged with 100 parts of acetonitrile, 99 parts of acrylonitrile, 1 part of styrene, and 1 part of 3-mercapto-1,2-propanediol as a chain transfer agent, and replaced with nitrogen gas. The reaction vessel was heated to 70°C, and a mixture consisting of 10 parts of acetonitrile and 0.4 parts of 2,2'-azobis(2,4-dimethylvaleronitrile) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.: V-65) was dropped into the reaction vessel over 6 hours to carry out a polymerization reaction. After the dropwise addition, the mixture was reacted at 70°C for 1 hour, and then 0.1 parts of V-65 was added, and the reaction was continued at 70°C for another 1 hour to obtain the target product as a precipitate. Thereafter, the conversion rate was confirmed to exceed 98% by measuring the nonvolatile content. The product was filtered out by vacuum filtration, washed with 100 parts of acetonitrile, and the solvent was completely removed by vacuum drying to obtain a polymer (A-1).

[0067] (Examples 2 to 14) (Production of Polymers (A-2) to (A-14)) Polymers (A-2) to (A-14) were produced in the same manner as in Production Example 1, except that the type and amount of monomer were changed as shown in Table 1. The Mw of each polymer is shown in Table 1. The synthesis of polymers (A-2) to (A-14) was performed by adjusting the Mw by adding a chain transfer agent, adjusting the amount of polymerization initiator, and appropriately changing the reaction conditions. In addition, 3-mercapto-1,2-propanediol was used as a chain transfer agent. In Table 1, unless otherwise specified, the numerical values ​​represent "parts", and blanks mean that no compound was added. The abbreviations in Table 1 are as follows. AA: Acrylic acid HEA: Hydroxyethyl acrylate St: styrene

[0068] <Production of Dispersion Containing Thermoelectric Conversion Material> [Example 1] (Dispersion 1) 0.3 parts of polymer (A-1), 0.4 parts of SWCNT (single-walled carbon nanotube "TUBALL" manufactured by OCSiAl Corporation), and 79.3 parts of NMP were weighed and mixed. Beads were further added, and the mixture was shaken for 4 hours with Scandex, and then filtered to remove the beads, to obtain a dispersion liquid 1 of a thermoelectric conversion material.

[0069] [Examples 2 to 38, Comparative Examples 1 and 2] (Dispersion 2~38) Thermoelectric conversion material dispersions 2 to 38 were obtained in the same manner as dispersion 1, except that the types and amounts of materials were changed as shown in Table 2.

[0070] The abbreviations for the materials listed in Table 2 are as follows. Conductive material (B) SWCNT: OCSiAl's single-walled carbon nanotube "TUBALL" MWCNT: (Kumho Petrochemical's multi-walled carbon nanotubes "Knanos100P") CB: (Lion Ketjen Black "EC-300J") Polymer that is not polymer (A) PVP: Nippon Shokubai, Polyvinylpyrrolidone K-30, 100% non-volatile content TMAOH: Tetramethylammonium hydroxide

[0071] <Evaluation of Thermoelectric Conversion Materials> The obtained dispersions 1 to 38, 101, and 102 were each applied to a 75 μm thick PET film, which was a sheet-like substrate, using an applicator, and then dried at 120° C. for 30 minutes to obtain a laminate having a thermoelectric conversion film with a thickness of 5 μm. The coating suitability when the dispersion was applied to the substrate was evaluated according to the method shown below. In addition, the electrical conductivity, Seebeck coefficient, and room temperature stability of the obtained laminate having a thermoelectric conversion film (hereinafter also referred to as a coating film) were evaluated according to the method shown below. The results are shown in Table 2.

[0072] (Electrical conductivity (resistivity)) The obtained laminate was cut into a size of 2.5 cm × 5 cm, and the conductivity was measured by a four-probe method using Loresta GX MCP-T700 (manufactured by Mitsubishi Chemical Analytech Co., Ltd.) in accordance with JIS-K7194. The conductivity is shown in Table 2 as a relative value when the conductivity of Comparative Example 1 is set to 1.

[0073] (Seebeck coefficient) The obtained laminate was cut into a size of 3 mm × 10 mm, and the Seebeck coefficient (μV / K) at 80° C. was measured using a ZEM-3LW manufactured by Advance Riko Co., Ltd. Table 2 shows the relative values ​​when the Seebeck coefficient of Comparative Example 1 was set to 1.

[0074] (Stability at room temperature) The laminate immediately after preparation was left to stand for 10 days under conditions of 25°C and 50%, and then the Seebeck coefficient was measured. The rate of change in the Seebeck coefficient relative to the Seebeck coefficient of the laminate immediately after preparation (the Seebeck coefficient listed in Table 2) was determined and evaluated based on the following criteria. ◎: The change in the Seebeck coefficient is 10% or less. (Very good) ○: The rate of change in the Seebeck coefficient is greater than 10% and less than 20% (good). △: The rate of change in the Seebeck coefficient is greater than 20% and less than 50%. (Usable) ×: The change in the Seebeck coefficient is more than 50% (poor).

[0075] As shown in Table 2, the thermoelectric conversion material of the present invention exhibited high electrical conductivity and Seebeck coefficient. Furthermore, it was confirmed that the material had high stability at room temperature (25°C, 50%). This is presumably because the introduction of aromatic hydrocarbon groups into the polymer prevents deterioration of the thermoelectric element due to moisture in the air, thereby improving stability at room temperature.

[0076] <Manufacturing of thermoelectric conversion elements> The above dispersions were applied onto a PET film having a thickness of 50 μm, and five thermoelectric conversion layers each having a thickness of 20 μm and a shape of 5 mm×30 mm were prepared at intervals of 10 mm. Next, four silver circuits (electrodes) having a thickness of 10 μm and a shape of 5 mm×33 mm were prepared using silver paste so that each thermoelectric conversion layer was connected in series, and thermoelectric conversion elements were manufactured. As the above silver paste, REXALPHA RA-FS 074 manufactured by Toyo Ink Co., Ltd. was used. When the electromotive force of each thermoelectric conversion element was measured, it was confirmed that the thermoelectric conversion elements manufactured using the dispersions manufactured in Examples 1 to 38 had a superior electromotive force to the thermoelectric conversion elements manufactured using the dispersions manufactured in Comparative Examples 101 and 102. [Industrial Applicability]

[0077] The thermoelectric conversion material according to an embodiment of the present invention has both electrical conductivity and a Seebeck coefficient and is also excellent in thermoelectric properties, and therefore a high-performance thermoelectric conversion element can be provided by using the material.

[0078] [Table 1]

[0079] [Table 2]

Claims

1. A thermoelectric conversion material comprising a polymer (A) and a conductive material (B), wherein the polymer (A) is a copolymer comprising a monomer unit derived from (meth)acrylonitrile and a monomer unit having an aromatic hydrocarbon group, and further comprises at least one selected from the group consisting of an inorganic metal salt, an inorganic base, and an organic base, wherein the inorganic base and the inorganic metal salt are an alkali metal hydroxide or an alkali metal carbonate.

2. 2. The thermoelectric conversion material according to claim 1, wherein the monomer having an aromatic hydrocarbon group includes a styrene-based monomer.

3. 3. The thermoelectric conversion material according to claim 1, wherein the polymer (A) contains 40% by mass or more and less than 100% by mass of monomer units derived from (meth)acrylonitrile.

4. 4. The thermoelectric conversion material according to claim 1, wherein the polymer (A) contains 1% by mass or more and 60% by mass or less of the monomer unit having an aromatic hydrocarbon group.

5. 5. The thermoelectric conversion material according to claim 1, wherein the content of the polymer (A) is 5 to 100 mass % based on the total amount of the conductive material (B).

6. A thermoelectric conversion element comprising a thermoelectric conversion film comprising the thermoelectric conversion material according to any one of claims 1 to 5 and electrodes, the thermoelectric conversion film and the electrodes being electrically connected to each other.

Citation Information

Patent Citations

  • Power generation device

    JP2015115447A

  • Thermoelectric conversion material-containing resin composition, and film formed by thermoelectric conversion material-containing resin composition

    JP2015170766A

  • Thermoelectric conversion element

    JP2016058475A

  • Carbon material complex composition

    JP2016127210A

  • Manufacturing method of molded article, molded article, and thermoelectric conversion material

    JP2019012831A