Semiconductor material for thermoelectric conversion and thermoelectric conversion element using the same
By dispersing low-resistance, high-melting-point substances at grain boundaries in FeSi or SiSnGe-based semiconductors, the thermoelectric conversion efficiency and output are improved without changing the semiconductor's composition, achieving high-performance thermoelectric conversion elements.
Patent Information
- Application Number
- JP2020122022
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-16
- Publication Date
- 2024-11-25
- Estimated Expiration
- 2040-07-16
AI Technical Summary
Conventional thermoelectric conversion technologies and elements do not achieve the required thermoelectric conversion efficiency and output, necessitating further improvements.
Incorporating low-resistance substances with higher melting points and lower specific resistance than the semiconductor into a sintered body of FeSi or SiSnGe-based materials at the grain boundaries, without altering the semiconductor's composition or dopant content, to reduce internal resistance and maintain thermoelectromotive force.
This approach results in thermoelectric conversion materials and elements with enhanced efficiency and output, leveraging existing production technologies and maintaining thermoelectromotive voltage while lowering internal resistance.
Smart Images

Figure 0007588811000003 
Figure 0007588811000004 
Figure 0007588811000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a semiconductor material for thermoelectric conversion and a thermoelectric conversion element using the same. [Background technology]
[0002] 2. Description of the Related Art In recent years, with the trend toward a green society and more efficient energy use, power generation using waste heat from factory equipment, thermal and nuclear power generation equipment, engines, etc. has attracted attention, and various technologies have been developed. One of the power generation technologies is thermoelectric conversion using semiconductors, which has been put to practical use as thermoelectric conversion elements.
[0003] The biggest engine for increasing the output and conversion efficiency of thermoelectric conversion elements is the semiconductor material for thermoelectric conversion. For example, Patent Documents 1 to 3 and Non-Patent Document 1 disclose some of the efforts in this area.
[0004] However, conventional thermoelectric conversion technologies and thermoelectric conversion elements do not necessarily satisfy the required values in terms of thermoelectric conversion efficiency and output, and there is a demand for further improvement in thermoelectric conversion efficiency and higher output. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2013-8747 A [Patent Document 2] JP 2018-59160 A [Patent Document 3] JP 2015-93788 A [Non-patent literature]
[0006] [Non-Patent Document 1] Journal of Alloys Compounds, Volume 690,5 January 2017, Pages652-657 Summary of the Invention [Problem to be solved by the invention]
[0007] The problem to be solved by the present invention is to provide a thermoelectric conversion semiconductor material and a thermoelectric conversion element having high thermoelectric conversion efficiency and high thermoelectric conversion output, thereby resolving the problems described above in the Background Art section. Here, an object of the present invention is to provide a thermoelectric conversion semiconductor material and a thermoelectric conversion element that have high thermoelectric conversion efficiency and high thermoelectric conversion output, without modifying the composition or dopant amount of the host semiconductor that performs thermoelectric conversion, so that the continuity of technologies that have been developed thus far and production technologies can be utilized. [Means for solving the problem]
[0008] The configuration of the present invention for solving the problems is shown below. (Configuration 1) A semiconductor material for thermoelectric conversion, comprising a sintered body in which one or more low-resistance substances selected from the group consisting of metals, alloys and metal compounds, which have a higher melting point and lower resistivity than those of a semiconductor made of FeSi2 containing a dopant, are dispersed as particles in the semiconductor. (Configuration 2) The semiconductor material for thermoelectric conversion according to configuration 1, wherein the semiconductor is made of FeSi2 containing one or more dopants selected from the group consisting of Ni, Co, Pt, Pd, B, Mn, Cr, V, Ti, Al, and P. (Configuration 3) A semiconductor material for thermoelectric conversion, comprising a sintered body in which one or more low-resistance substances selected from the group consisting of metals, alloys and metal compounds, which have a higher melting point and lower resistivity than those of the semiconductor, are dispersed as particles in a semiconductor made of a Mg2SiSnGe-based material containing a dopant. (Configuration 4) The semiconductor material for thermoelectric conversion according to configuration 3, wherein the dopant is one or more selected from the group consisting of Cu, Ag, Cd, Zn, Al, Ga, In, Au, Ni, Co, Fe, Li, Na, Ca, K, N, P, As, Sb, Bi, S, Se, Te, Cl, Br, and I. (Configuration 5) half The conductor has the general formula A 2r Mg 2-2r (Si 1-x-y Sn x Ge y ) 1-s Bs (A and B are at least one selected from the group consisting of Cu, Ag, Cd, Zn, Al, Ga, In, Au, Ni, Co, Fe, Li, Na, Ca, K, N, P, As, Sb, Bi, S, Se, Te, Cl, Br, and I, 0≦r<1, 0≦s < 1, 0≦x≦1, 0≦y≦1, r+s>0, x+y<1 5. The semiconductor material for thermoelectric conversion according to claim 3 or 4, which is made of a material represented by the formula (1). (Configuration 6) The above 6. The semiconductor material for thermoelectric conversion according to any one of configurations 1 to 5, wherein the resistivity of the low resistance material is 1 / 1000 or less of the resistivity of the semiconductor. (Configuration 7) The semiconductor material for thermoelectric conversion according to any one of configurations 1 to 6, wherein the low resistance material is one or more selected from the group consisting of WSi2, TiB2, W, TaC, WC, ZrN, ZrB2, HfB2, VB2, W2B5, LaB6, TiSi2, and MoSi2. (Configuration 8) 7. The semiconductor material for thermoelectric conversion according to any one of claims 1 to 6, wherein the low resistance material is one or more selected from the group consisting of WSi2 and W. (Configuration 9) 9. The semiconductor material for thermoelectric conversion according to any one of claims 1 to 8, wherein the volume ratio of the low resistance material is 0.01 volume % or more and 2.5 volume % or less with respect to the semiconductor. (Configuration 10) 10. The semiconductor material for thermoelectric conversion according to any one of claims 1 to 9, wherein the ratio of the number of atoms of the dopant to the semiconductor is 100 ppm or more and 5.3% or less. (Configuration 11) 11. The semiconductor material for thermoelectric conversion according to any one of configurations 1 to 10, wherein the semiconductor forms grain boundaries, and the low resistance material is present between grain boundaries of the semiconductor. (Configuration 12) A thermoelectric conversion element, comprising a p-type semiconductor layer and an n-type semiconductor layer electrically connected to each other, and at least one of the p-type semiconductor layer and the n-type semiconductor layer contains the semiconductor according to any one of structures 1 to 11. (Configuration 13) 13. The thermoelectric conversion element of claim 12, wherein the connection is made via an electrode. Effect of the Invention
[0009] According to the present invention, it is possible to provide a thermoelectric conversion semiconductor material and a thermoelectric conversion element having high thermoelectric conversion efficiency and thermoelectric conversion output without modifying the composition of the thermoelectric semiconductor material or the amount of dopant. In the present invention, the composition of the host thermoelectric semiconductor material and the amount of dopant are based on conventional technology, so that it is possible to follow various existing technologies and utilize existing production technologies. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is an explanatory diagram showing a schematic structure of a semiconductor material of the present invention. [Diagram 2] FIG. 2 is an explanatory diagram showing the configuration of a main part of a thermoelectric conversion element, where (a) is a bird's-eye view and (b) is a cross-sectional view. [Diagram 3] 1 is a SEM photograph of a semiconductor material of the present invention. [Figure 4] FIG. 2 is a characteristic diagram showing the relationship between the weight ratio and the volume ratio of the materials of the present invention, where (a) is an n-type material and (b) is a p-type material. [Diagram 5] FIG. 2 is a characteristic diagram showing the dependence of resistivity of FeSi2 thermoelectric semiconductor material on the amount of WSi2 mixed. [Figure 6] FIG. 2 is a characteristic diagram showing the dependency of the resistivity of an n-type Mg2SiSn-based thermoelectric semiconductor material on the amount of low-resistance, high-melting-point material mixed therein. [Figure 7] FIG. 2 is a characteristic diagram showing the dependency of resistivity of a p-type Mg2SiSn-based thermoelectric semiconductor material on the amount of low-resistance, high-melting-point material mixed therein. [Figure 8] FIG. 1 is a characteristic diagram showing the dependence of the Seebeck coefficient of an n-type Mg2SiSn-based thermoelectric semiconductor material on the amount of low-resistance, high-melting-point material mixed therein. [Figure 9]FIG. 1 is a characteristic diagram showing the dependence of the Seebeck coefficient of a p-type Mg2SiSn-based thermoelectric semiconductor material on the amount of low-resistance, high-melting-point material mixed therein. [Figure 10] FIG. 1 is a characteristic diagram showing the dependency of the electrical figure of merit of an n-type Mg2SiSn-based thermoelectric semiconductor material on the amount of low-resistance, high-melting-point material added. [Figure 11] FIG. 1 is a characteristic diagram showing the dependency of the electrical figure of merit of a p-type Mg2SiSn-based thermoelectric semiconductor material on the amount of low-resistance, high-melting-point material added. [Figure 12] This is a characteristic diagram showing the temperature dependence of the electrical and physical properties of n-type Mg2SiSn-based thermoelectric semiconductor material, where (a) is the Seebeck coefficient, (b) is the resistivity, (c) is the thermal conductivity, and (d) is the dimensionless figure of merit ZT. [Figure 13] This is a characteristic diagram showing the temperature dependence of the electrical and physical properties of p-type Mg2SiSn-based thermoelectric semiconductor material, where (a) is the Seebeck coefficient, (b) is the resistivity, (c) is the thermal conductivity, and (d) is the dimensionless figure of merit ZT. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.
[0012] (First embodiment) The first embodiment (Embodiment 1) relates to a semiconductor material for thermoelectric conversion. Here, we will first explain thermoelectric conversion elements that use semiconductor materials for thermoelectric conversion, and then describe the characteristics required of the semiconductor materials for thermoelectric conversion in order to improve their performance, as well as the material structure and manufacturing method for obtaining those characteristics.
[0013] The thermoelectric conversion element mainly comprises an n-type thermoelectric power generating semiconductor material and a p-type thermoelectric power generating semiconductor material electrically connected in series. The power output (electric power) P of a thermoelectric conversion element is calculated by using the thermoelectromotive voltage E generated in the element made of the semiconductor material in response to the temperature difference and its internal resistance r, as follows: P=E×E / (4r) (Formula 1) It is expressed as: For this reason, one method of improving the power generation output P is to increase the thermoelectromotive force E and reduce the internal resistance r. However, in thermoelectric conversion materials made of semiconductors, both the thermoelectromotive force E and the internal resistance r change depending on the amount of dopant and the material composition. In general, there is a trade-off between the effects of the thermoelectromotive force E and the internal resistance r; that is, if the thermoelectromotive force E increases, the internal resistance r also increases (conductance decreases), and if the thermoelectromotive force E decreases, the internal resistance r also decreases (conductance increases).
[0014] In the present invention, the semiconductor material itself that causes thermoelectric conversion is basically left untouched, and a sintered body in which particles 13 of a low resistance material are dispersed in a semiconductor 12 is used as the thermoelectric conversion material, as shown in Figure 1. This configuration and structure suppresses the resistance of the thermoelectric conversion material 11, lowering the internal resistance r. Here, the particles 13 are made of a substance that has a higher melting point and a significantly smaller resistivity than the semiconductor 12, and are formed at the grain boundaries of the semiconductor 12. In this method, the particles 13 are formed in a mixed form outside the host semiconductor 12, and the material of the semiconductor 12 itself is not modified, so the thermoelectromotive voltage E basically remains unchanged. Meanwhile, the internal resistance r of the thermoelectric conversion material 11 decreases. This makes it possible to supply thermoelectric conversion materials and thermoelectric conversion elements with high power generation output P.
[0015] The semiconductor 12 is iron disilicide (FeSi2) containing a dopant. Here, the dopant may be one or more selected from the group consisting of nickel (Ni), cobalt (Co), platinum (Pt), palladium (Pd), boron (B), manganese (Mn), chromium (Cr), vanadium (V), titanium (Ti), aluminum (Al), and phosphorus (P). Here, the semiconductor 12 becomes an n-type semiconductor when nickel (Ni), cobalt (Co), boron (B), platinum (Pt), or palladium (Pd) is selected as the dopant, and becomes a p-type semiconductor when manganese (Mn), chromium (Cr), vanadium (V), titanium (Ti), aluminum (Al), or phosphorus (P) is selected. Alternatively, the semiconductor 12 may be a dimagnesium silicon tin germanium (MgSiSnGe) based material (MgSi 1-x-y Sn x Ge y (0≦x≦1, 0≦y≦1)). Here, the dopant may be one or more selected from the group consisting of copper (Cu), silver (Ag), cadmium (Cd), zinc (Zn), aluminum (Al), gallium (Ga), indium (In), gold (Au), nickel (Ni), cobalt (Co), iron (Fe), lithium (Li), sodium (Na), calcium (Ca), potassium (K), nitrogen (N), phosphorus (P), arsenic (As), antimony (Sb), bismuth (Bi), sulfur (S), selenium (Se), tellurium (Te), chlorine (Cl), bromine (Br), and iodine (I). Here, the semiconductor 12 becomes an n-type semiconductor when copper (Cu), gold (Au), nickel (Ni), cobalt (Co), iron (Fe), antimony (Sb), bismuth (Bi), sulfur (S), selenium (Se), tellurium (Te), chlorine (Cl), bromine (Br), or iodine (I) is selected as the dopant, and becomes a p-type semiconductor when silver (Ag), cadmium (Cd), zinc (Zn), aluminum (Al), gallium (Ga), indium (In), lithium (Li), sodium (Na), calcium (Ca), potassium (K), nitrogen (N), phosphorus (P), or arsenic (As) is selected. The dopant-containing Mg2SiSnGe-based material is represented by the general formula A 2r Mg 2-2r (Si 1-x-y Sn x Ge y ) 1-s Here, A and B are dopant elements and are at least one selected from the group consisting of Cu, Ag, Cd, Zn, Al, Ga, In, Au, Ni, Co, Fe, Li, Na, Ca, K, N, P, As, Sb, Bi, S, Se, Te, Cl, Br, and I, and 0≦r<1, 0≦s < 1, 0≦x≦1, 0≦y≦1 , r+s>0, x+y<1 There is a relationship between the two. End
[0016] The semiconductor 12 is prepared using a granular material. This allows the particles 13 to be formed at the grain boundaries of the semiconductor to reduce the resistance of the thermoelectric conversion material 11, and prevents elements of the particles 13 from being taken into the semiconductor 12, thereby preventing the characteristics of the semiconductor 12 from changing.
[0017] The size of the granular semiconductor can be, for example, 1 μm or more and 75 μm or less, specifically 38 μm to 75 μm. When the semiconductor is in this size range, the semiconductor 12 has sufficient thermoelectric conversion function. Furthermore, the grain boundary surface area is sufficient to allow a large number of particles 13 to be arranged, so the resistance of the thermoelectric conversion material 11 can be significantly reduced. Moreover, mechanical problems such as cracking can be suppressed. This size can be defined by the average length of the longest part measured by, for example, SEM.
[0018] The ratio of the dopant to the semiconductor 12 is preferably 100 ppm or more and 5.3% or less in terms of atomic ratio in order to obtain high thermoelectric conversion efficiency. The semiconductor 12 is a proven semiconductor that has high performance as a thermoelectric conversion semiconductor material.
[0019] As described above, the particles 13 are made of a material having a higher melting point and a significantly lower resistivity than the semiconductor 12, and may be one or more materials selected from the group consisting of metals, alloys, and metal compounds. The resistivity of the particles 13 is preferably smaller than that of the semiconductor 12 by about three orders of magnitude or more. By making the resistivity 1 / 1000 or less, it is possible to sufficiently reduce the internal resistance r of the thermoelectric conversion material 11. There is no particular lower limit, but there are suitable materials with low resistivity of 7 / 10000 compared to that of the semiconductor 12.
[0020] The melting point of the particles 13 is higher than that of the semiconductor 12. Preferably, the melting point is higher by 1000° C. or more, and more preferably by 2000° C. or more than the melting point of the semiconductor 12. This prevents elements of the particles 13 from diffusing into the semiconductor 12 during the sintering process of the thermoelectric conversion material 11 and from adversely affecting the characteristics of the semiconductor 12, and maintains the thermoelectromotive force E of the semiconductor 12.
[0021] Specific examples of particles 13 include one or more selected from the group consisting of tungsten disilicide (WSi2), titanium diboride (TiB2), tungsten (W), tantalum carbide (TaC), tungsten carbide (WC), zirconium nitride (ZrN), zirconium diboride (ZrB2), hafnium diboride (HfB2), vanadium diboride (VB2), tungsten pentaboride (W2B5), lanthanum hexaboride (LaB6), titanium disilicide (TiSi2), and molybdenum disilicide (MoSi2).
[0022] These materials have a higher melting point than semiconductor 12, and a resistivity in the range of 7 / 10,000 to 1 / 1,000 of semiconductor 12. For reference, Table 1 lists the melting points, specific gravities, and resistivities of semiconductors useful as semiconductor 12, and Table 2 lists the melting points, specific gravities, and resistivities of the above-mentioned examples of particle 13.
[0023] [Table 1]
[0024] [Table 2]
[0025] The size of the particles 13 is preferably 50 nm or more and 2 μm or less. When the particles 13 are in this size range, they are sufficiently dispersed at the grain boundaries of the semiconductor 12, and the resistance of the thermoelectric conversion material 11 can be uniformly reduced. The form of the particles 13 may be either individual or clustered.
[0026] The volume ratio of the particles 13 to the semiconductor 12 is preferably 0.01% or more and 2.5% or less, more preferably 0.05% or more and 2.0% or less, and even more preferably 0.1% or more and 1.5% or less. By making the volume fraction 0.01% or more, it is possible to reduce the internal resistance r of the thermoelectric conversion material 11, by making it 0.05% or more, it is possible to significantly reduce the internal resistance r, and by making it 0.1% or more, it is possible to further reduce the internal resistance r. Furthermore, by making it 2.5% or less, problems such as cracking of the thermoelectric conversion material 11 are unlikely to occur, and by making it 2.0% or less, it becomes even less likely to crack. At 1.5% or less, no cracking defects have been observed.
[0027] The volume ratio of the particles 13 to the semiconductor 12 can be obtained from image observation using an SEM or the like, or can be calculated by separately obtaining a calibration curve of the weight ratio and the volume ratio. In the method using the calibration curve of the weight ratio and the volume ratio, the volume ratio can be controlled by the weight ratio of the materials according to the calibration curve. For reference, the relationship between the volume ratio and weight ratio of the particles 13 to the semiconductor 12 is shown in Fig. 4. An almost linear relationship is observed between the two.
[0028] The thermoelectric conversion material 11 is produced as follows. First, a predetermined amount of semiconductor powder having a composition of semiconductor 12 containing a dopant, powder of particles 13, is prepared and mixed. Thereafter, the mixture is sintered using a hot press or the like to produce a thermoelectric conversion material 11 made of the sintered body. For example, in the case of hot pressing, the sintering conditions can be a pressure of 50 MPa to 100 MPa, a temperature of 650° C. to 1200° C., and a time of 60 minutes to 5 hours. Note that, in addition to hot pressing, other sintering methods such as a spark plasma sintering method and an ultra-high pressure sintering method can also be used.
[0029] In addition, Non-Patent Document 1 reports the results of mixing powders of semiconductor materials CrSi2 and WSi2, producing a sintered body by pulse current sintering, and investigating its electrical properties. In this paper, it is reported that the thermoelectric material CrSi2 becomes Cr by adding WSi2. 1-x W x The CrSi2 compound is formed, and the Cr-rich hexagonal (CrW)Si2 phase and the W-rich tetragonal (WCr)Si2 phase are generated, and the grain size of the CrSi2 phase becomes smaller. From another perspective, this method is a method in which the CrSi2 semiconductor is changed into a different compound. On the other hand, the present invention is characterized in that there is no change in composition between the semiconductor 12 and the mixed powder. That is, the present invention follows FeSi2 and Mg2SiSnGe-based semiconductors, which have a proven track record in high-quality technology and high-efficiency production technology as thermoelectric semiconductor materials. Therefore, the semiconductor material for thermoelectric conversion of the present invention has the characteristic that it is possible to supply products with sufficiently high quality and productivity by utilizing the technology, knowledge, facilities, etc. that have been accumulated up to now.
[0030] (Second embodiment) The second embodiment (second embodiment) relates to a thermoelectric conversion element using the semiconductor material according to the first embodiment.
[0031] In thermal power plants and engines, a large amount of energy is wasted as waste heat. Thermoelectric conversion elements using semiconductors are elements that recover thermal energy such as waste heat and directly convert it into useful electrical energy, and have features such as easy maintenance as they have no moving parts and good scalability.
[0032] A thermoelectric conversion element is an element that has a structure in which an n-type semiconductor and a p-type semiconductor are electrically connected. If this connection is made via electrodes, the n-type semiconductor and the p-type semiconductor can be arranged side by side, which has the advantage of being highly productive and making it easier to make the thermoelectric conversion element compact, but the n-type semiconductor and the p-type semiconductor can also be directly connected. 2, which is a configuration diagram of the main part of the thermoelectric conversion element 31, an n-type semiconductor 32 and a p-type semiconductor 33 are electrically connected in series between an electrode 34 (34a) on the low temperature side and an electrode 34 (34b) on the high temperature side, via these electrodes. Here, FIG. 2(a) is a bird's-eye view, and FIG. 2(b) is a cross-sectional view. In the second embodiment, the thermoelectric conversion semiconductor described in the first embodiment is used for at least one of the n-type semiconductor 32 and the p-type semiconductor 33. That is, an FeSi2 or Mg2SiSnGe-based material containing a dopant is used as a host semiconductor part, and an n-type or p-type semiconductor in which particles with low resistivity and high melting point are formed on the grain boundaries of the semiconductor part is used. These semiconductors can supply high-output power with high conversion efficiency, so the thermoelectric conversion element 31 becomes a high-output thermoelectric conversion element with high thermoelectric conversion efficiency. Here, it is preferable to use the thermoelectric conversion semiconductors described in the first embodiment for both the n-type semiconductor 32 and the p-type semiconductor 33. In this way, the thermoelectric conversion element 31 becomes a high-output thermoelectric conversion element with extremely high thermoelectric conversion efficiency. EXAMPLES
[0033] The present invention will be described in more detail below with reference to examples. However, these examples are provided merely to aid in the understanding of the present invention and are not intended to limit the present invention thereto.
[0034] Example 1 In Example 1, a sintered body was produced by mixing WSi2 powder with FeSi2 powder to which an n-type dopant had been added, using a hot press, and the resistivity of the sintered body was measured. The process for producing the sintered body is described in detail below. First, FeSi2 powder with added cobalt (Co) (atomized powder, purity: 99%, manufactured by Fukuda Metal Foil Powder Co., Ltd.) was prepared and weighed to a predetermined weight percentage with WSi2 powder (manufactured by Fujifilm Wako Pure Chemical Industries, purity: 99%). Here, the average particle sizes of FeSi2 powder and WSi2 powder are 7 μm and 2 to 5 μm, respectively. These powders were mixed in an inclined planetary ball mill (Plant M2-3F, manufactured by Nagao System Co., Ltd.) at room temperature in an argon atmosphere. The mixing time was 20 minutes. The melting point and resistivity of WSi2 are about 1.4 times and 1 / 640 times those of FeSi2, respectively, as shown in Table 1. The mixture was then hot-pressed to produce a sintered compact. The hot-pressing conditions were a pressure of 50 MPa, a temperature of 1174°C, and a time of 30 minutes. The mixture ratio was 0 to 0.1 mol%. After hot pressing, the material was heat-treated at 800°C for 20 hours to obtain the β phase.
[0035] The resistivity ρ of the resulting sintered body at room temperature was measured by the four-probe method. The resistivity ρ decreased monotonically with increasing mixing ratio, from approximately 8.5 μΩm for the unmixed sample to approximately 5.1 μΩm for the 0.1 mol% mixed sample, as shown in Figure 5. This result confirmed that the addition of high-melting-point, low-resistivity particles significantly reduces the resistivity of the sintered body.
[0036] Example 2 In Example 2, a number of sintered bodies were produced by mixing WSi2 or W with an Mg2SiSnGe-based material, and their electrical and physical properties were evaluated.
[0037] The first sintered body is an example of an n-type semiconductor, Mg2Si 0.4625 Sn 0.4625 Sb 0.075 The powder with the above composition and WSi2 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., purity: 99%) or W powder (manufactured by Japan New Metals Co., Ltd., purity: 99.9%) were sealed in a glass tube and mixed by rotating, and a sintered body was produced using a hot press. The hot press conditions were a pressure of 80 MPa, a temperature of 780°C, and 5 hours. The second sintered body is an example of a p-type semiconductor, Mg 1.97 Ag 0.25 Li 0.05 S 0.25 Sn 0.75 The powder with the above composition and WSi2 or W powder were enclosed in a glass tube, mixed by rotating, and sintered using a hot press. The hot press conditions were a pressure of 80 MPa, a temperature of 650°C, and a time of 4 hours.
[0038] The resistivities ρ of the first and second sintered bodies at room temperature are shown in Figures 6 and 7, respectively. The Seebeck coefficients α at room temperature are shown in Figures 8 and 9, respectively, and the electrical figure of merit PW calculated from the Seebeck coefficients α and resistivities ρ are shown in Figures 10 and 11, respectively.
[0039] The first sintered body is an n-type semiconductor, Mg2Si 0.4625 Sn 0.4625 Sb 0.075 The resistivity ρ of the unmixed sample without WSi2 or W powder is 2.34×10 -5 Ωm, whereas the WSi2 mixed sample is 1.12×10 -5 Ωm(2wt%), 1.01×10 -5 Ωm (4 wt%), and 8.96×10 for the W-mixed sample. -6 Ωm (2% by weight), 2.42×10 -6 The effect of mixing was remarkable, with a significant decrease to Ωm (4 wt%). The second sintered body is a p-type semiconductor, Mg 1.97 Ag 0.025 Li 0.005 S 0.25 Sn 0.75 The resistivity ρ of the unmixed sample is 2.09×10 -5 Ωm, whereas the WSi2 mixed sample is 2.00×10 -5 Ωm (2% by weight), 1.92×10 -5 The W-mixed sample showed a slight decrease to 1.41×10 -5 The resistance was significantly reduced to Ωm.
[0040] The Seebeck coefficient α at room temperature for the first sintered body (n-type sample) was -177.3 μV / K for the unmixed sample, -153.2 μV / K (2 wt%) and -181.0 μV / K (4 wt%) for the WSi2 mixed sample, and -128.2 μV / K (2 wt%) and -127.4 μV / K (4 wt%) for the W mixed sample, showing a tendency to decrease with increasing mixing ratio. For the second sintered body (p-type sample), the Seebeck coefficient α at room temperature was 128.7 μV / K for the unmixed sample, 134.4 μV / K (2 wt%) and 152.2 μV / K (4 wt%) for the WSi2 mixed sample, and 137.4 μV / K (2 wt%) and 155.7 μV / K (4 wt%) for the W mixed sample. This means that the Seebeck coefficient α at room temperature increased by mixing WSi2 and W.
[0041] The calculated electrical figure of merit PW for the first sintered body was 1.39 mW / mK for the unmixed sample. 2 , and 2.03mW / mK for the WSi2 mixed sample. 2 (2% by weight), 1.82mW / mK 2 (4 wt%), and 1.93 mW / mK for the W-mixed sample. 2 (2% by weight), 1.78mW / mK 2 (4 wt%), which was a maximum 46% improvement in performance compared to the unmixed sample. For the second sintered body, the unmixed sample had a value of 0.95 mW / mK. 2 , and 1.04mW / mK for the WSi2 mixed sample. 2 (2% by weight), 1.11mW / mK 2 (4 wt%), and 1.11 mW / mK for the W-mixed sample. 2 (2% by weight), 1.21mW / mK 2 (4 wt%), which was a maximum 27% improvement in performance compared to the unmixed sample. Here, the increase in the electrical figure of merit PW by mixing WSi2 and W with high melting points and low resistivity means that the thermoelectric power generation output P has increased significantly.
[0042] FIG. 12 shows the temperature dependence of the thermoelectric characteristics of the first sintered body, and FIG. 13 shows the temperature dependence of the thermoelectric characteristics of the second sintered body. The Seebeck coefficient α of the first sintered body (n-type sample) shows a tendency for its absolute value to increase with increasing temperature. The Seebeck coefficient α of the unmixed sample showed a maximum absolute value at approximately 700 K and decreased above that temperature. However, the Seebeck coefficient α of the mixed sample was smaller than that of the unmixed sample within the measurement temperature range (Figure 12(a)).
[0043] On the other hand, the Seebeck coefficient α of the second sintered body (p-type sample) showed no significant difference between the unmixed and mixed samples, and showed a maximum value at approximately 550 K (FIG. 13(a)).
[0044] The temperature dependence of resistivity ρ increased with increasing temperature for all samples. For the first sintered body, the n-type sample, the mixed sample showed a large decrease in resistivity compared to the unmixed sample within the measurement temperature range (Figure 12(b)). For the second sintered body, the p-type sample, the resistivity entered the intrinsic region above approximately 550 K and decreased linearly (Figure 13(b)). Here, the first sintered body containing 4 wt% WSi2 has a higher resistivity ρ than the first sintered body containing 2 wt% WSi2, which is believed to be caused by the increase in resistance due to cracks that occurred inside the first sintered body containing 4 wt% WSi2. The cracks were confirmed by SEM.
[0045] The temperature dependence of thermal conductivity κ of the first sintered body, which is an n-type sample, was large only for the sample containing 4 wt% WSi2, while the other mixed samples and the unmixed sample were almost the same (Figure 12(c)). On the other hand, for the second sintered body, which is a p-type sample, the unmixed sample was smaller, while the mixed samples were almost the same for all samples but larger than the unmixed sample (Figure 13(c)).
[0046] The dimensionless figure of merit ZT=(α 2The maximum value of T / ρκ) was smallest for the first sintered body (n-type sample) for the sample containing 4 wt% WSi2, and was larger than the unmixed sample (0.8) for the other mixed samples. The 4 wt% W sample was 1.25, 1.6 times that of the unmixed sample (Fig. 12(d)). In the second sintered body (p-type sample), the resistivity ρ decreased, but the Seebeck coefficient α also decreased, and the thermal conductivity κ was almost the same, so the maximum value of the dimensionless figure of merit ZT was almost the same for both the unmixed sample and the mixed sample (Figure 13(d)).
[0047] As described above, due to the improvement in the electrical figure of merit PW at room temperature, when used near room temperature, the output performance of thermoelectric power generation is improved by mixing particles 13. Since there is a large demand for IoT power sources near room temperature, it is expected that they will be widely used in industry. [Industrial Applicability]
[0048] The thermoelectric conversion semiconductor material according to the present invention and the thermoelectric conversion element using the same are elements having high thermoelectric conversion output that directly convert heat into electricity, and are therefore expected to be widely used in industry, for example, for waste heat recovery. [Explanation of symbols]
[0049] 11: Thermoelectric conversion semiconductor 12: Semiconductors 13: Particles (low resistance particles) 14: Grain interface 31: Thermoelectric generation element 32: n-type semiconductor 33: p-type semiconductor 34: Electrode 35: Current
Claims
1. Dopant-containing FeSi 2 and a sintered body in which one or more low-resistance substances selected from the group consisting of metals, alloys, and metal compounds having a higher melting point and a lower resistivity than the semiconductor are dispersed as particles in the semiconductor. The ratio of the number of atoms of the dopant to the number of atoms of the semiconductor is 100 ppm or more and 5.3% or less, The semiconductor forms grain boundaries, The resistivity of the low resistance material is 1 / 350 or less of the resistivity of the semiconductor, A semiconductor material for thermoelectric conversion, wherein the low resistance object is present at grain boundaries of the semiconductor.
2. The semiconductor is FeSi containing one or more elements selected from the group consisting of Ni, Co, Pt, Pd, B, Mn, Cr, V, Ti, Al, and P as a dopant. 2 The semiconductor material for thermoelectric conversion according to claim 1, comprising:
3. Mg containing dopants 2 S 1-x-y Sn x Ge y (0≦x≦1, 0≦y≦1) and one or more low-resistance substances selected from the group consisting of metals, alloys and metal compounds, which have a higher melting point and a lower resistivity than the semiconductor, are dispersed as particles in the semiconductor. The ratio of the number of atoms of the dopant to the number of atoms of the semiconductor is 100 ppm or more and 5.3% or less, the semiconductor forms a grain boundary, and the resistivity of the low resistance material is 1 / 100 or less of the resistivity of the semiconductor; A semiconductor material for thermoelectric conversion, wherein the low resistance object is present at grain boundaries of the semiconductor.
4. The dopant is at least one selected from the group consisting of Cu, Ag, Cd, Zn, Al, Ga, In, Au, Ni, Co, Fe, Li, Na, Ca, K, N, P, As, Sb, Bi, S, Se, Te, Cl, Br, and I. The semiconductor material for thermoelectric conversion according to claim 3.
5. A sintered body comprising a semiconductor containing a dopant and one or more low-resistance substances selected from the group consisting of metals, alloys, and metal compounds having a higher melting point and lower resistivity than the semiconductor dispersed as particles in the semiconductor, The semiconductor has the general formula A 2 rMg 2-2r (Si 1-x-y Sn x Ge y ) 1- sBs (A and B are dopants, each of which is one or more selected from the group consisting of Cu, Ag, Cd, Zn, Al, Ga, In, Au, Ni, Co, Fe, Li, Na, Ca, K, N, P, As, Sb, Bi, S, Se, Te, Cl, Br, and I, and is a material represented by 0≦r<1, 0≦s<1, 0≦x≦1, 0≦y≦1, r+s>0, and x+y<1); The semiconductor forms grain boundaries, A semiconductor material for thermoelectric conversion, wherein the resistivity of the low resistance material is 1 / 100 or less of the resistivity of the semiconductor, and the low resistance material is present at grain boundaries of the semiconductor.
6. 6. The semiconductor material for thermoelectric conversion according to claim 1, wherein the resistivity of the low resistance material is 7 / 10,000 or more and 1 / 1,000 or less of the resistivity of the semiconductor.
7. The low resistance material is WSi 2 , TiB 2 , W, TaC, WC, ZrN, ZrB 2 , HfB 2 , V.B. 2 , W 2 B 5 , LaB 6 , TiSi 2 , MoSi 2 The semiconductor material for thermoelectric conversion according to any one of claims 1 to 6, which is one or more selected from the group consisting of:
8. The low resistance material is WSi 2 7. The semiconductor material for thermoelectric conversion according to claim 1, wherein the SiC layer is at least one selected from the group consisting of Mn, Fe, and W.
9. 9. The semiconductor material for thermoelectric conversion according to claim 1, wherein a volume ratio of the low resistance material is 0.01 volume % or more and 2.5 volume % or less with respect to the semiconductor.
10. A thermoelectric conversion element comprising a p-type semiconductor layer and an n-type semiconductor layer electrically connected to each other, and at least one of the p-type semiconductor layer and the n-type semiconductor layer contains the semiconductor according to any one of claims 1 to 9.
11. The thermoelectric conversion element according to claim 10 , wherein the connection is made via an electrode. End
Citation Information
Patent Citations
P-type and beta-type FeSi2-base thermalelectric material containing dispersion-distribution nitride granule
CN1438202A
Thermoelectric material and manufacture thereof
JP1997298317A
Thermoelectric conversion material and manufacture thereof
JP1997321347A
Semiconductor material for thermoelectric conversion and manufacture of the same
JP2000261048A
Nano-composite thermoelectric conversion material, method for manufacturing the same, and thermoelectric conversion element
JP2012104560A