Method for producing bifunctional cyclic carbonate having a spiro structure and method for producing polyhydroxyurethane
By reacting pentaerythritol and diaryl carbonate without a catalyst, the method simplifies and enhances the yield of bifunctional cyclic carbonates, facilitating the production of novel polyhydroxyurethanes.
Patent Information
- Application Number
- JP2020083001
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-05-11
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2040-05-11
AI Technical Summary
The synthesis of bifunctional cyclic carbonates requires multiple steps and catalysts, leading to complications such as the use of toxic phosgene derivatives and high reactivity with amines, which complicates the purification process and reduces yield.
A method for producing a bifunctional cyclic carbonate with a spiro structure by reacting pentaerythritol and diaryl carbonate without a catalyst, optimizing reaction conditions such as temperature, molar ratios, and concentration to enhance yield and simplify the process.
This method results in a simple and efficient production of bifunctional cyclic carbonates with improved yield, enabling the synthesis of novel polyhydroxyurethanes through a one-step reaction.
Smart Images

Figure 0007594368000016 
Figure 0007594368000017 
Figure 0007594368000018
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a difunctional cyclic carbonate having a spiro structure and a method for producing a polyhydroxyurethane. [Background technology]
[0002] Polyhydroxyurethanes (PHUs), which are synthesized by the ring-opening polyaddition reaction of bifunctional cyclic carbonates with diamines, have attracted attention in recent years as a novel method for synthesizing polyurethanes (PUs) without using diisocyanates. In addition, this reaction generates primary and tertiary hydroxyl groups in the side chains due to the structure of the ring-opening cyclic carbonate, allowing the side chains of PHUs to be modified in various ways. However, most bifunctional five- and six-membered cyclic carbonates require linking two cyclic carbonates with a linker, and their synthesis requires several steps. It is also known that six-membered cyclic carbonates are more reactive with amines than five-membered cyclic carbonates.
[0003] On the other hand, the bifunctional cyclic carbonate 2,4,8,10-tetraoxaspiro[5,5]-undecane-3,9-dione, which can be synthesized in one step by the reaction of the inexpensive polyol pentaerythritol (PE) with diethyl carbonate (dimethyl carbonate; DMC), has a spiro structure consisting of two six-membered cyclic carbonates, so it does not require a linker moiety. Furthermore, in the ring-opening reaction of 2,4,8,10-tetraoxaspiro[5,5]-undecane-3,9-dione with an amine, only primary hydroxyl groups are produced, unlike bifunctional cyclic carbonates with low symmetry. For example, Patent Document 1 discloses that 2,4,8,10-tetraoxaspiro[5,5]-undecane-3,9-dione can be obtained by reacting PE with 2,2,2-Trichloethyl Chloroformate (TrocCl). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2018 / 109714 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the reaction of PE with DMC requires a catalyst and a complicated purification procedure, while the reaction of PE with TrocCl produces TrocCl derived from toxic phosgene and containing chlorine components, which can cause coloring and other problems.
[0006] The present invention has been made in consideration of the above circumstances, and provides a method for producing a bifunctional cyclic carbonate simply and in an improved yield, and a method for producing a novel polyhydroxyurethane using the bifunctional cyclic carbonate. [Means for solving the problem]
[0007] That is, the present invention includes the following aspects. (1) A reaction step of reacting pentaerythritol with a diaryl carbonate to obtain a bifunctional cyclic carbonate having a spiro structure, The bifunctional cyclic carbonate having a spiro structure is 2,4,8,10-tetraoxaspiro[5,5]-undecane-3,9-dione. the law of nature, In the reaction step, no catalyst is used. Method for producing bifunctional cyclic carbonates having a spiro structure 。 (2 In the reaction step, the reaction is carried out at a temperature of 40° C. or higher and 100° C. or lower. (1 ) The manufacturing method described above. ( 3 In the reaction step, the reaction is carried out at a temperature of 50° C. or higher and 100° C. or lower. (1) Or (2) The manufacturing method described in ( 4In the reaction step, the molar ratio of the diaryl carbonate to pentaerythritol is 2 / 1 or more and 10 / 1 or less. 3 The manufacturing method according to any one of the preceding claims. ( 5 In the reaction step, the molar ratio of diaryl carbonate to pentaerythritol is 4 / 1 or more and 10 / 1 or less. 4 The manufacturing method according to any one of the preceding claims. ( 6 In the reaction step, the concentration of pentaerythritol is 10 mmol / L or more and 100 mmol / L or less with respect to the total volume of the reaction solution. 5 The manufacturing method according to any one of the preceding claims. ( 7 In the reaction step, the concentration of pentaerythritol is 10 mmol / L or more and 80 mmol / L or less with respect to the total volume of the reaction solution. 6 The manufacturing method according to any one of the preceding claims. ( 8 ) the diaryl carbonate is diphenyl carbonate, 7 The manufacturing method according to any one of the preceding claims. ( 9 ) A bifunctional cyclic carbonate having a spiro structure is produced by the production method according to any one of (1) to (8), The method includes a polymerization step of reacting a bifunctional cyclic carbonate having a spiro structure with a diamine represented by the following general formula (Ia) to obtain a polyhydroxyurethane, A method for producing polyhydroxyurethane, wherein the bifunctional cyclic carbonate having a spiro structure is 2,4,8,10-tetraoxaspiro[5,5]-undecane-3,9-dione.
[0008] [ka]
[0009] In the general formula (Ia), X is an alkylene group, an aralkylene group, or -R 11 -Ar 11 -R 12 - is a group represented by Ar 11is a divalent aromatic hydrocarbon group, and R 11 and R 12 are each independently an alkylene group having 1 to 20 carbon atoms.
[0010] ( 10 In the polymerization step, the polymerization reaction is carried out at 5° C. or less, and the content of polyhydroxyurethane having a branched structure is controlled to be 4 mol % or less based on the total molar amount of polyhydroxyurethane. 9 ) The manufacturing method described in the above. ( 11 In the polymerization step, the polymerization reaction is carried out at 50° C. or higher, and the content of polyhydroxyurethane having a branched structure is controlled to be 11 mol % or more based on the total molar amount of polyhydroxyurethane. 9 ) The manufacturing method described in the above. Effect of the Invention
[0011] According to the above-mentioned embodiment of the method for producing a bifunctional cyclic carbonate, it is possible to provide a method for producing a bifunctional cyclic carbonate easily and with improved yield. According to the above-mentioned embodiment of the method for producing a polyhydroxyurethane, it is possible to obtain a novel polyhydroxyurethane. [Brief description of the drawings]
[0012] [Figure 1A] 1 is a 1H-NMR spectrum of compound (I) in Example 1. [Figure 1B] 1 is a 13C-NMR spectrum of compound (I) in Example 1. [Diagram 2] 1 is a 1H-NMR spectrum of the product in Example 2. [Diagram 3] 1 is a graph showing the relationship between the yield (selectivity) of compound (I) and the initial PE concentration. [Figure 4] 1 is a graph showing the relationship between the yield (selectivity) of compound (I) and the reaction temperature. [Diagram 5] 1 is a graph showing the relationship between the yield (selectivity) of compound (I) and the molar ratio of DPC to PE. [Figure 6] FIG. 1H-NMR spectra of a mixture (A) of compound (I) and compound (IV), a reaction product (B) of compound (IV) with a monoamine, a reaction product (C) of compound (I) with a monoamine, and a reaction product (D) of a mixture of compound (I) and compound (IV) with a monoamine in Example 16. [Figure 7] 1 shows gel permeation chromatograms of the reaction product of compound (I) and 1,6-diaminohexane in Example 17 (reaction times: 1, 2, 3, 4, 5, 7 and 9 hours). [Figure 8] 1 is a graph showing the relationship between the reaction time of compound (I) and 1,6-diaminohexane in Example 17 and the number average molecular weight or molecular weight distribution of the product. [Figure 9] 22 is a graph showing the results of thermogravimetric analysis of each of the polyhydroxyurethanes obtained in Examples 18 to 21 in Example 22. [Figure 10] 2 is a graph showing the results of differential scanning calorimetry of each of the polyhydroxyurethanes obtained in Examples 18 to 21 in Example 22. [Figure 11] 1 is a 1H-NMR spectrum of compound (V) in Example 23. [Figure 12] 1H-NMR spectra of the reaction product (crude product) of compound (I) and 1-hexylamine in Example 24 and the purified by-product (compound V'). [Figure 13] FIG. 1H-NMR spectrum of the reaction product of compound (I) and 1,6-diaminohexane in Example 25 (reaction temperature: 50° C.). [Figure 14] FIG. 1H-NMR spectrum of the reaction product of compound (I) and 1,6-diaminohexane in Example 26 (reaction temperature: 0° C.). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, an embodiment for carrying out the present invention (hereinafter, abbreviated as "present embodiment") will be described in detail. Note that the present invention is not limited to the following embodiment, and can be carried out in various modifications within the scope of the gist of the present invention.
[0014] <Method for producing bifunctional cyclic carbonate> The method for producing a bifunctional cyclic carbonate having a spiro structure according to the present embodiment (hereinafter also referred to as the "method for producing a bifunctional cyclic carbonate according to the present embodiment") includes a reaction step of reacting pentaerythritol (PE) with a diaryl carbonate to obtain a bifunctional cyclic carbonate having a spiro structure. The bifunctional cyclic carbonate having a spiro structure is 2,4,8,10-tetraoxaspiro[5,5]-undecane-3,9-dione. 2,4,8,10-tetraoxaspiro[5,5]-undecane-3,9-dione is a compound represented by the following formula (I) (hereinafter sometimes referred to as "compound (I)"). The CAS number of compound (I) is 84056-48-4.
[0015] [ka]
[0016] In a conventional method for producing a bifunctional cyclic carbonate, PE and dimethyl carbonate are reacted in the presence of a catalyst (1,4-Diazabicyclo[2.2.2]octane; DABCO) to obtain a bifunctional cyclic carbonate having a spiro structure. In contrast, in the method for producing a bifunctional cyclic carbonate of the present embodiment, 2,4,8,10-tetraoxaspiro[5,5]-undecane-3,9-dione, which is a bifunctional cyclic carbonate having a spiro structure, is obtained in a one-step reaction without using a catalyst.
[0017] The steps constituting the method for producing a bifunctional cyclic carbonate of this embodiment will be described in detail below.
[0018] [Reaction process] In the reaction step, as shown in the following reaction formula, pentaerythritol is reacted with diaryl carbonate to obtain the above-mentioned compound (I), which is a bifunctional cyclic carbonate having a spiro structure. This reaction to obtain compound (I) is a known intramolecular cyclization reaction.
[0019] [ka]
[0020] (Pentaerythritol (PE)) Pentaerythritol (PE) is a compound having the structure shown in the above reaction formula. PE can be synthesized, for example, by condensing acetaldehyde and formaldehyde in a basic environment. Commercially available PE may also be used. The CAS number of PE is 115-77-5.
[0021] (Diaryl carbonate) Examples of diaryl carbonates include a compound represented by the following general formula (III) (hereinafter, sometimes referred to as "compound (III)").
[0022] [ka]
[0023] In general formula (III), Ar 31 and Ar 32 are each independently a monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms.
[0024] Ar 31 and Ar 32is an aromatic hydrocarbon group having 6 to 20 carbon atoms, preferably an aromatic hydrocarbon group having 6 to 12 carbon atoms, and more preferably an aromatic hydrocarbon group having 6 to 10 carbon atoms. The aromatic hydrocarbon group may have a substituent. Examples of the substituent in the aromatic hydrocarbon group include an alkyl group, an alkoxy group, a dialkylamino group, a halogen group, a nitro group, a trifluoromethyl group, and a cyano group. Such an Ar 31 and Ar 32 Specifically, examples of the phenyl group, methylphenyl group (each isomer), ethylphenyl group (each isomer), propylphenyl group (each isomer), butylphenyl group (each isomer), pentylphenyl group (each isomer), hexylphenyl group (each isomer), dimethylphenyl group (each isomer), methylethylphenyl group (each isomer), methylpropylphenyl group (each isomer), methylbutylphenyl group (each isomer), methylpentylphenyl group (each isomer), diethylphenyl group (each isomer), ethylpropylphenyl group (each isomer), ethyl Examples of such groups include a butylphenyl group (each isomer), a dipropylphenyl group (each isomer), a trimethylphenyl group (each isomer), a triethylphenyl group (each isomer), a naphthyl group (each isomer), a methoxyphenyl group, a dimethoxyphenyl group, a trimethoxyphenyl group, a dimethylaminophenyl group, a chlorophenyl group, a dichlorophenyl group, a trichlorophenyl group, a fluorophenyl group, a difluorophenyl group, a trifluorophenyl group, a perfluorophenyl group, a nitrophenyl group, a dinitrophenyl group, and a trinitrophenyl group. Among these, Ar 31 and Ar 32 As the alkyl group, a phenyl group is preferable. Ar 31 and Ar 32 may be the same or different, but from the viewpoint of ease of production, it is preferable that they are the same.
[0025] Preferred diaryl carbonates include Ar 31 and Ar 32is an aromatic hydrocarbon group having 6 to 10 carbon atoms. Specific examples of such diaryl carbonates include diphenyl carbonate, di(methylphenyl) carbonate (each isomer), di(diethylphenyl) carbonate (each isomer), and di(methylethylphenyl) carbonate (each isomer). Note that these compounds are merely examples of preferred diaryl carbonates, and preferred diaryl carbonates are not limited to these. Furthermore, these diaryl carbonates may be used alone or in combination of two or more. Among these, diphenyl carbonate is particularly preferred as the diaryl carbonate.
[0026] Known methods can be used as a method for producing diaryl carbonate. Among them, a method described in WO 2009 / 139061 (Reference 1) is preferred, which involves reacting an organotin compound having a tin-oxygen-carbon bond with carbon dioxide to produce an aliphatic carbonate, and then producing an aromatic carbonate (i.e., diaryl carbonate) from the aliphatic carbonate and an aromatic hydroxy compound. The diaryl carbonate can be produced, for example, by using the production apparatus described in WO 2009 / 139061 (Reference 1). Commercially available diaryl carbonate may also be used.
[0027] The reaction step can be carried out in the presence or absence of a solvent. The solvent may be any solvent capable of dissolving PE, and is preferably a highly polar solvent having no hydroxyl group. Specific examples of such a solvent include the following:
[0028] (1) Ketones such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, and methylcyclohexanone; (2) Nitriles such as acetonitrile, butyronitrile, and caprylnitrile; (3) Esters such as methyl formate, ethyl formate, propyl formate, methyl acetate, ethyl acetate, dimethyl phthalate, diethyl phthalate, dipropyl phthalate, dibutyl phthalate, diamyl phthalate, dibutyl fumarate, dimethyl maleate, diethyl maleate, and dibutyl maleate; (4) Ethers such as furan, tetrahydrofuran, propyl oxide, dioxane, dibenzyl ether, and diphenyl ether; (5) Glycol ether esters such as ethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, cyclohexanol acetate, propylene glycol diacetate, 1,4-butanediol diacetate, 1,3-butylene glycol diacetate, and 1,6-hexanediol diacetate; (6) Phosphite esters such as triphenyl phosphite; (7) Sulfur compounds such as dimethyl sulfide, thiophene, and carbon disulfide; (8) Halogenated hydrocarbons, such as methyl chloride, ethyl chloride, dichloropropane, dichloroethylene, trichloroethylene, tetrachloroethylene, pentachloroethane, chloroform, methyl bromide, ethyl bromide, methyl iodide, and ethyl iodide; (9) N,N-dimethylformamide (DMF), N,N-dimethylacetamide, N,N-dimethylpropionamide, 1-methyl-2-pyrrolidone, 1-ethyl-2-pyrrolidone, 1,5-dimethyl-2-pyrrolidone; (10) Pyrrolidines such as 1-acetylpyrrolidine; (11) Ureas such as 1,3-dimethyl-2-imidazolidinone; (12) Sulfoxide compounds such as dimethyl sulfoxide (DMSO), diethyl sulfoxide, dipropyl sulfoxide, dibutyl sulfoxide, diphenyl sulfoxide, methyl ethyl sulfoxide, methyl propyl sulfoxide, methyl butyl sulfoxide, and methyl phenyl sulfoxide.
[0029] These solvents may be used alone or in combination of two or more. When two or more types are used in combination, the combination and ratio thereof can be selected arbitrarily.
[0030] The reaction step is preferably carried out, for example, under an inert gas atmosphere. Examples of the inert gas include argon gas, helium gas, and nitrogen gas.
[0031] In the reaction step, the amount of PE used, i.e., the concentration of PE in the reaction solution, is preferably 10 mmol / L or more and 100 mmol / L or less, more preferably 10 mmol / L or more and 80 mmol / L or less, even more preferably 10 mmol / L or more and 60 mmol / L or less, particularly preferably 10 mmol / L or more and 40 mmol / L or less, and most preferably 10 mmol / L or more and 30 mmol / L or less, relative to the total volume of the reaction solution. When the concentration of PE is equal to or higher than the lower limit, the PE can be reacted more thoroughly with the diaryl carbonate. On the other hand, when the concentration of PE is equal to or lower than the upper limit, the carbonation of PE can be preferentially caused intramolecularly rather than intermolecularly, and the yield (selectivity) of compound (I) can be further improved.
[0032] In the reaction step, the amount of diaryl carbonate used can be expressed as a molar ratio of diaryl carbonate to PE. The molar ratio of diaryl carbonate to PE is preferably 2 / 1 or more and 10 / 1 or less, more preferably 4 / 1 or more and 10 / 1 or less. When the molar ratio of diaryl carbonate to PE is equal to or greater than the lower limit, carbonation of PE can occur preferentially intramolecularly rather than intermolecularly, and the yield (selectivity) of compound (I) can be improved. When the molar ratio of diaryl carbonate to PE is equal to or less than the upper limit, the abundance ratio of diaryl carbonate can be prevented from becoming excessive, and compound (I) can be produced more efficiently while suppressing production costs.
[0033] In the reaction step, the reaction temperature can be 20°C or higher and 100°C or lower, preferably 40°C or higher and 100°C or lower, more preferably 50°C or higher and 100°C or lower, and even more preferably 75°C or higher and 100°C or lower. By keeping the reaction temperature at or above the lower limit, the carbonation of PE can be preferentially caused intramolecularly rather than intermolecularly, and the yield (selectivity) of compound (I) can be improved. On the other hand, by keeping the reaction temperature at or below the upper limit, the application of excess heat can be suppressed, and compound (I) can be produced more efficiently while suppressing production costs.
[0034] The reaction time can be, for example, from 1 hour to 24 hours, and can be from 6 hours to 18 hours.
[0035] [Other processes] The method for producing a bifunctional cyclic carbonate of this embodiment may further include a purification step of compound (I) after the reaction step, i.e., after completion of the reaction.
[0036] In the purification step, post-treatment is carried out as necessary by a known method to extract compound (I). Specifically, post-treatment operations such as filtration, washing, extraction, pH adjustment, dehydration, and concentration are carried out individually or in combination as necessary, and compound (I) is roughly purified by concentration, crystallization, reprecipitation, column chromatography, etc.
[0037] In order to increase the purity of the above-mentioned roughly purified compound (I), it is preferable to carry out, as necessary, one or more of the following operations, such as crystallization, reprecipitation, column chromatography, extraction, and stirring and washing of the crystals with a solvent, either alone or in combination.
[0038] In the method for producing a bifunctional cyclic carbonate of this embodiment, after the reaction step, the product may be used in the method for producing polyhydroxyurethane described below without carrying out a purification step. However, from the viewpoint of improving the yield of polyhydroxyurethane, it is preferable to carry out a purification step of compound (I).
[0039] The structure of Compound (I) can be confirmed by known techniques such as nuclear magnetic resonance (NMR) spectroscopy, mass spectrometry (MS), and infrared spectroscopy (IR).
[0040] <Uses of Compound (I)> Compound (I) obtained by the production method of the present embodiment is suitably used, for example, as a raw material for polyhydroxyurethane described later, a raw material for a diol having two urethane groups obtained by the reaction of compound (I) with a monoamine, a raw material for polycarbonate, a raw material for copolymerization with lactone or lactide, a raw material for a crosslinking agent, and the like.
[0041] <Method of producing polyhydroxyurethane> The method for producing polyhydroxyurethane of the present embodiment includes a polymerization step of reacting a bifunctional cyclic carbonate having a spiro structure with a diamine represented by the above general formula (Ia) to obtain polyhydroxyurethane. The bifunctional cyclic carbonate having a spiro structure is 2,4,8,10-tetraoxaspiro[5,5]-undecane-3,9-dione.
[0042] According to the method for producing polyhydroxyurethane of the present embodiment, a novel polyhydroxyurethane can be obtained.
[0043] [Polymerization process] In the polymerization step, as shown in the reaction formula below, a bifunctional cyclic carbonate having a spiro structure is reacted with a diamine represented by the following general formula (Ia) to obtain polyhydroxyurethane. This reaction to give polyhydroxyurethane is a known ring-opening polyaddition reaction.
[0044] [ka]
[0045] In the above reaction formula, X is an alkylene group, an aralkylene group, or -R 11 -Ar11 -R 12 - is a group represented by Ar 11 is a divalent aromatic hydrocarbon group, and R 11 and R 12 are each independently an alkylene group having 1 to 20 carbon atoms, and n is an integer of 1 or greater.
[0046] (Bifunctional cyclic carbonates having spiro structures) The bifunctional cyclic carbonate having a spiro structure is 2,4,8,10-tetraoxaspiro[5,5]-undecane-3,9-dione (compound (I)). Compound (I) may be a commercially available product or may be synthesized using a known method, but it is preferable that the compound (I) is obtained by the above-mentioned method for producing a bifunctional cyclic carbonate, since the compound (I) can be obtained easily and in good yield.
[0047] (Diamine) The diamine is a compound represented by the following general formula (Ia) (hereinafter, sometimes referred to as "diamine (Ia)").
[0048] [ka]
[0049] In the general formula (Ia), X is an alkylene group, an aralkylene group, or -R 11 -Ar 11 -R 12 - is a group represented by Ar 11 is a divalent aromatic hydrocarbon group, and R 11 and R 12 are each independently an alkylene group having 1 to 20 carbon atoms.
[0050] The alkylene group in X is preferably a linear alkylene group having 2 to 20 carbon atoms, and specific examples thereof include an ethylene group, a propylene group, a butylene group, a pentylene group, a hexylene group, a heptylene group, an octylene group, a nonylene group, a decylene group, an undecylene group, a dodecylene group, a tetradecylene group, a hexadecylene group, an octadecylene group, a nonylene group, and a decylene group. Among these, the alkylene group in X is preferably a propylene group, a butylene group, a pentylene group, a hexylene group, a heptylene group, an octylene group, a nonylene group, or a decylene group, and more preferably a propylene group, a butylene group, a pentylene group, a hexylene group, a heptylene group, or an octylene group.
[0051] The aralkylene group in X is preferably an aralkylene group having 3 to 20 carbon atoms, and specific examples thereof include a benzylene group, a phenethylene group, a phenylbutylene group, a naphthylmethylene group, and a naphthylethylene group. Of these, the aralkylene group in X is preferably a benzylene group or a phenethylene group.
[0052] -R in X 11 -Ar 11 -R 12 In the group represented by -, R 11 and R 12 may be the same or different, but is preferably the same. R 11 and R 12 Examples of the alkylene group having 1 to 20 carbon atoms in R include a methylene group and the same as those exemplified in the alkylene group in X. 11 and R 12 As the alkylene group having 1 to 20 carbon atoms in the formula (I), a methylene group or an ethylene group is preferable.
[0053] -R in X 11 -Ar 11 -R 12Specific examples of the group represented by - include a group represented by -CH2-Ph-CH2- (Ph is a phenylene group, the same applies below), and a group represented by -CH2CH2-Ph-CH2CH2-. 11 -Ar 11 -R 12 As the group represented by -, a group represented by -CH2-Ph-CH2- is preferable.
[0054] Examples of preferred diamines (Ia) include 1,2-diaminoethane, 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, 1,7-diaminoheptane, 1,8-diaminooctane, 1,9-diaminononane, 1,10-diaminodecane, 1,11-diaminoundecane, 1,12-diaminododecane, p-xylylenediamine, etc. Among them, 1,3-diaminopropane, 1,6-diaminohexane, 1,8-diaminooctane, or p-xylylenediamine is preferred as diamine (Ia).
[0055] The polymerization step can be carried out in the presence or absence of a solvent. Examples of the solvent include the same solvents as those exemplified in the reaction step of the above-mentioned method for producing a bifunctional cyclic carbonate. The solvent may be used alone or in combination of two or more. When two or more types are used in combination, the combination and ratio thereof can be selected arbitrarily.
[0056] The polymerization process can be carried out without the use of a catalyst.
[0057] The reaction step is preferably carried out, for example, under an inert gas atmosphere. Examples of the inert gas include argon gas, helium gas, and nitrogen gas.
[0058] In the polymerization step, the amount of diamine (Ia) used is preferably 0.5 to 1.5 times, more preferably 0.7 to 1.3 times, the amount of compound (I) used by molar ratio.
[0059] In the polymerization step, as shown in the examples described later, in the latter stage of the reaction, the molar concentration of the amino group at the polymer chain end of the polyhydroxyurethane produced is significantly lower than the molar concentration of the hydroxy group end produced. Therefore, there is a risk that the compound (I) reacts with the hydroxy group instead of the amino group, crosslinking the polymer chain and causing gelation of the polyhydroxyurethane. Therefore, in order to suppress the gelation of the polyhydroxyurethane, it is preferable to add diamine (Ia) in an amount of 0.05 to 0.3 times the molar amount of the compound (I) used, preferably 0.07 to 0.2 times the molar amount, during the reaction, for example, 30 minutes, 1 hour, 2 hours, and 3 hours after the start of the reaction. This can prevent the formation of a crosslinked structure in the polyhydroxyurethane, and can effectively suppress the gelation of the polyhydroxyurethane produced. In addition, the amount of diamine (Ia) used throughout the reaction should be within the above range, and for example, at the start of the reaction, diamine (Ia) is added in an amount of more than half the amount of diamine (Ia) used throughout the reaction, and during the reaction, diamine (Ia) is further added in an amount of less than half the amount of diamine (Ia) used throughout the reaction.In addition, for example, it is preferable to add diamine (Ia) in an amount equivalent to the amount of compound (I) used at the start of the reaction, and further add diamine (Ia) in an amount 0.1 times the amount of compound (I) used 3 hours after the start of the reaction.
[0060] In the polymerization step, as shown in the examples described later, the structure of the resulting polyhydroxyurethane can be controlled by adjusting the polymerization temperature. When producing a polyhydroxyurethane having a branched structure in a relatively large amount, specifically when producing a polyhydroxyurethane having a branched structure in an amount of 11 mol % or more relative to the total molar amount of the obtained polyhydroxyurethane, the polymerization temperature is preferably 50° C. or higher, and more preferably 60° C. or higher. By setting the polymerization temperature to the above lower limit or higher, the production of polyhydroxyurethane having a linear structure can be more effectively suppressed, and the yield of polyhydroxyurethane having a branched structure can be further improved. On the other hand, the upper limit of the reaction temperature is not particularly limited, and can be set to, for example, 100°C.
[0061] On the other hand, when producing polyhydroxyurethane having a linear structure in a relatively large amount, specifically when producing polyhydroxyurethane having a branched structure in an amount of 4 mol % or less based on the total molar amount of the obtained polyhydroxyurethane, the polymerization temperature is preferably 5°C or less, and more preferably 0°C. By setting the polymerization temperature to the above upper limit or lower, the production of polyhydroxyurethane having a branched structure can be more effectively suppressed, and the yield of polyhydroxyurethane having a linear structure can be further improved. On the other hand, the lower limit of the reaction temperature is not particularly limited, and can be, for example, 0°C.
[0062] When a diamine (Ia) having an alkenyl group with 7 or more carbon atoms is used and the solubility in a solvent is low, the polymerization temperature can be temporarily increased to more than 60°C and not more than 100°C, and maintained for a short period of time, such as for 10 minutes to 1 hour, to dissolve the diamine (Ia) and make the reaction solution homogenous, and then the polymerization temperature can be decreased to a temperature not more than the above upper limit.
[0063] The polymerization time can be, for example, from 1 hour to 24 hours, and can be from 6 hours to 20 hours.
[0064] [Other processes] The method for producing polyhydroxyurethane of the present embodiment may further include a step of purifying the polyhydroxyurethane after the polymerization step, i.e., after completion of the reaction.
[0065] In the purification step, polyhydroxyurethane is extracted by performing post-treatment according to a known method as necessary. Specifically, post-treatment operations such as filtration, washing, extraction, pH adjustment, dehydration, and concentration are performed alone or in combination as necessary, and polyhydroxyurethane is roughly purified by concentration, crystallization, reprecipitation, column chromatography, etc.
[0066] In order to increase the purity of the above-mentioned roughly refined polyhydroxyurethane, it is preferable to carry out, as necessary, one or more of the following operations, such as crystallization, reprecipitation, column chromatography, extraction, and stirring and washing of the crystals with a solvent, either alone or in combination.
[0067] In the method for producing polyhydroxyurethane of this embodiment, a purification step does not have to be carried out after the reaction step. However, from the viewpoint of the storage stability of polyhydroxyurethane and the use of polyhydroxyurethane in a variety of applications, it is preferable to carry out a purification step of polyhydroxyurethane.
[0068] The structure of the polyhydroxyurethane can be confirmed by known techniques such as nuclear magnetic resonance (NMR) spectroscopy, mass spectrometry (MS), and infrared spectroscopy (IR).
[0069] <Uses of polyhydroxyurethane> The polyhydroxyurethane obtained by the production method of this embodiment is suitable for use as an industrial material, such as a molding material or a binder for paint. EXAMPLES
[0070] The present embodiment will be described in more detail below with reference to specific examples and comparative examples, but the present embodiment is not limited to the following examples and comparative examples as long as the gist of the present embodiment is not exceeded. Various analyses performed in the examples and comparative examples described below were measured by the following methods.
[0071] [Rating 1] (Yield of Compound (I)) The yield (also called selectivity) of compound (I) is 1 The analytical conditions were as follows:
[0072] (Analysis conditions) Equipment: JEOL ECS-400 spectrometer Sample preparation: A portion of the reaction solution (approximately 0.1 mL) was concentrated under reduced pressure and dissolved in deuterated DMSO (DMSO-d6) (approximately 0.55 mL).
[0073] 1 Specifically, the yield (selectivity) analysis method using H-NMR analysis is as follows: 1 H-NMR measurement was performed to identify the target compound, 2,4,8,10-tetraoxaspiro[5,5]-undecane-3,9-dione (compound (I)), and the by-products (impurities). 1 The yield (selectivity) of compound (I) was calculated from the integral ratio of the 1 H signal.
[0074] [Example 1] As shown in the reaction formula below, pentaerythritol (PE) and diphenyl carbonate (DPC) were reacted to obtain 2,4,8,10-tetraoxaspiro[5,5]-undecane-3,9-dione (compound (I)).
[0075] [ka]
[0076] Detailed reaction conditions are as follows. DPC (29.15 g, 0.136 mol) and N,N-dimethylformamide (DMF) (800 mL) were added to a 1000 mL flask and heated to 100 ° C. A DMF solution (40 mL) of PE (3.09 g, 0.023 mol) was quickly added thereto, the flask was replaced with nitrogen, and the mixture was stirred at 100 ° C for 12 hours. After returning to room temperature, DMF was distilled off under reduced pressure, ethyl acetate (EtOAc) / n-hexane (about 100 mL / about 100 mL) was added to the residue, and the precipitated white solid was collected. Furthermore, the obtained white solid was dissolved in hot DMF (about 60 mL), and recrystallized by adding diethyl ether (Et2O) (about 120 mL), to obtain compound (I) (yield 3.16 g, yield 74%) as a white solid.
[0077] Compound (I), 1 H-NMR, 13 The results of analysis by C-NMR, melting point measurement, and infrared spectrophotometer (IR) are shown below. 1 The H-NMR spectrum is shown in Figure 1A. 13 The C-NMR spectrum is shown in Figure 1B.
[0078] 1 H NMR (400 MHz, DMSO-d6, rt): δ 4.42 (s, 8H, CH2). 13 C NMR (100 MHz, DMSO-d6, rt): δ 147.056 (C=O), 68.84 (CH2-O-), 29.67 (-C-). Mp: 220-225℃(dec.). IR (ATR, cm -1 ): 1737 (ν C=O ), 1254 (ν C-O ), 1171 (ν C-O ), 1125 (ν C-O ), 1094 C-O ).
[0079] The DMF used as the reaction solvent was recovered and reused as a solvent, but this had almost no effect on the yield or purity, and it was confirmed that it could be reused at least five times.
[0080] <Study on Pentaerythritol (PE) Concentration> Next, in the presence of an excess amount of DPC (10 molar equivalents) relative to 1 molar equivalent of PE, the initial pentaerythritol (PE) concentration in the reaction solution was changed from 100 mM (mmol / L) to 20 mM (mmol / L) and the reaction was carried out at 100°C, and the yield of compound (I) was examined.
[0081] [Example 2] (Initial PE concentration: 100mM) DPC (428 mg, 2.0 mmol) and DMF (1.5 mL) were added to a 10 mL flask and heated to 100°C. A DMF solution (0.5 mL) of PE (27.2 mg, 0.20 mmol) was quickly added thereto, the atmosphere in the flask was replaced with nitrogen, and the mixture was stirred at 100°C for 12 hours. A part of the solution was distilled off under reduced pressure, and the residue was dissolved in DMSO-d6 and 1 H-NMR measurement was performed. As a result, the yield (selectivity) of compound (I) was 43.8%. 1 The results of H-NMR measurement are shown in Figure 2.
[0082] [Example 3] (Initial PE concentration: 80mM) DPC (428 mg, 2.0 mmol) and DMF (2.0 mL) were added to a 10 mL flask and heated to 100°C. A DMF solution (0.5 mL) of PE (27.2 mg, 0.20 mmol) was quickly added thereto, the atmosphere in the flask was replaced with nitrogen, and the mixture was stirred at 100°C for 12 hours. A portion of the solution was distilled off under reduced pressure, and the residue was dissolved in DMSO-d6. 1 H-NMR measurement was performed, and the result was that the yield (selectivity) of compound (I) was 55.0%.
[0083] [Example 4] (Initial PE concentration: 60mM) DPC (428 mg, 2.0 mmol) and DMF (2.8 mL) were added to a 10 mL flask and heated to 100°C. A DMF solution (0.5 mL) of PE (27.2 mg, 0.20 mmol) was quickly added thereto, the atmosphere in the flask was replaced with nitrogen, and the mixture was stirred at 100°C for 12 hours. A part of the solution was distilled off under reduced pressure, and the residue was dissolved in DMSO-d6 and 1 H-NMR measurement was performed, and the result was that the yield (selectivity) of compound (I) was 64.0%.
[0084] [Example 5] (Initial PE concentration: 40mM) DPC (428 mg, 2.0 mmol) and DMF (4.5 mL) were added to a 10 mL flask and heated to 100°C. A DMF solution (0.5 mL) of PE (27.2 mg, 0.20 mmol) was quickly added thereto, the atmosphere in the flask was replaced with nitrogen, and the mixture was stirred at 100°C for 12 hours. A portion of the solution was distilled off under reduced pressure, and the residue was dissolved in DMSO-d6. 1 H-NMR measurement was performed, and the result was that the yield (selectivity) of compound (I) was 78.3%.
[0085] [Example 6] (Initial PE concentration: 20mM) DPC (428 mg, 2.0 mmol) and DMF (9.5 mL) were added to a 25 mL flask and heated to 100°C. A DMF solution (0.5 mL) of PE (27.2 mg, 0.20 mmol) was quickly added thereto, the atmosphere in the flask was replaced with nitrogen, and the mixture was stirred at 100°C for 12 hours. Part of the solution was distilled off under reduced pressure, and the residue was dissolved in DMSO-d6. 1 H-NMR measurement was performed, and the result was that the yield (selectivity) of compound (I) was 86.8%.
[0086] Figure 3 is a graph showing the relationship between the yield (selectivity) of compound (I) obtained in Examples 2 to 6 and the initial PE concentration. As shown in Figure 3, the selectivity of compound (I) increased from 43.8% to 86.8% with a decrease in the initial PE concentration, and a linear relationship was observed between the initial PE concentration and the production ratio of compound (I). From this result, it is considered that at low concentrations, carbonation of PE occurs preferentially intramolecularly rather than intermolecularly, resulting in more selective production of compound (I).
[0087] <Temperature considerations> Based on the results of Examples 2 to 6 above, the yield of compound (I) was examined when the reaction was carried out at an initial PE concentration of 20 mM, which had the highest selectivity, in the presence of an excess amount of DPC (10 molar equivalents) relative to 1 molar equivalent of PE, and at a reaction temperature changed from 20°C to 100°C.
[0088] [Example 7] (Reaction temperature: 20℃) DPC (428 mg, 2.0 mmol) and DMF (9.5 mL) were added to a 25 mL flask and the temperature was adjusted to 20°C. A DMF solution (0.5 mL) of PE (27.2 mg, 0.20 mmol) was quickly added thereto, the atmosphere in the flask was replaced with nitrogen, and the mixture was stirred at 20°C for 12 hours. A part of the solution was distilled off under reduced pressure, and the residue was dissolved in DMSO-d6, whereupon insoluble parts were observed. Using the soluble parts of the solution, 1 As a result of H-NMR measurement, the yield (selectivity) of compound (I) was 8.5%.
[0089] [Example 8] (Reaction temperature: 50°C) DPC (428 mg, 2.0 mmol) and DMF (9.5 mL) were added to a 25 mL flask and heated to 50°C. A DMF solution (0.5 mL) of PE (27.2 mg, 0.20 mmol) was quickly added thereto, the atmosphere in the flask was replaced with nitrogen, and the mixture was stirred at 50°C for 12 hours. A portion of the solution was distilled off under reduced pressure, and the residue was dissolved in DMSO-d6. 1 H-NMR measurement was performed, and the result was that the yield (selectivity) of compound (I) was 69.1%.
[0090] [Example 9] (Reaction temperature: 75°C) DPC (428 mg, 2.0 mmol) and DMF (9.5 mL) were added to a 25 mL flask and heated to 75°C. A DMF solution (0.5 mL) of PE (27.2 mg, 0.20 mmol) was quickly added thereto, the atmosphere in the flask was replaced with nitrogen, and the mixture was stirred at 75°C for 12 hours. Part of the solution was distilled off under reduced pressure, and the residue was dissolved in DMSO-d6. 1 H-NMR measurement was performed, and the result was that the yield (selectivity) of compound (I) was 84.5%.
[0091] [Example 10] (Reaction temperature: 100℃) DPC (428 mg, 2.0 mmol) and DMF (9.5 mL) were added to a 25 mL flask and heated to 100°C. A DMF solution (0.5 mL) of PE (27.2 mg, 0.20 mmol) was quickly added thereto, the atmosphere in the flask was replaced with nitrogen, and the mixture was stirred at 100°C for 12 hours. Part of the solution was distilled off under reduced pressure, and the residue was dissolved in DMSO-d6. 1 H-NMR measurement was performed, and the result was that the yield (selectivity) of compound (I) was 86.8%.
[0092] FIG. 4 is a graph showing the relationship between the yield (selectivity) of compound (I) obtained in Examples 7 to 10 and the reaction temperature. As shown in FIG. 4, the selectivity of compound (I) increased with increasing temperature and leveled off at around 75° C. Furthermore, no unreacted PE was observed in any of the cases. From this, as shown in the reaction formula below, at high temperatures, an intermediate produced by the reaction of a part of the OH group of PE with DPC is likely to form an entropically disadvantageous cyclic carbonate, whereas at low temperatures, the intermediate preferentially produces an entropically advantageous intermolecular chain carbonate, and therefore, it is considered that the selectivity of compound (I) decreased with decreasing temperature.
[0093] [ka]
[0094] <Examination of the molar ratio of DPC to PE ([DPC]0 / [PE]0)> From the results in Examples 2 to 10 above, when the initial PE concentration was 20 mM, the reaction temperature was fixed at 100 °C, and the reaction was carried out with the molar ratio of DPC to PE varied from 10 / 1 to 2 / 1, the yield of compound (I) was examined.
[0095] [Example 11] ([DPC]0 / [PE]0: 10 / 1) DPC (214 mg, 1.0 mmol) and DMF (4.5 mL) were added to a 10 mL flask and heated to 100 °C. A DMF solution (0.5 mL) of PE (13.6 mg, 0.10 mmol) was quickly added thereto, the inside of the flask was purged with nitrogen, and the mixture was stirred at 100 °C for 12 hours. A part of the solution was distilled off under reduced pressure, and the residue was dissolved in DMSO-d6 1 for 1H-NMR measurement. As a result, the yield (selectivity) of compound (I) was 86.8%.
[0096] [Example 12] ([DPC]0 / [PE]0: 8 / 1) DPC (171.4 mg, 0.80 mmol) and DMF (4.5 mL) were added to a 10 mL flask and heated to 100 °C. A DMF solution (0.5 mL) of PE (13.6 mg, 0.10 mmol) was quickly added thereto, the inside of the flask was purged with nitrogen, and the mixture was stirred at 100 °C for 12 hours. A part of the solution was distilled off under reduced pressure, and the residue was dissolved in DMSO-d6 1 for 1H-NMR measurement. As a result, the yield (selectivity) of compound (I) was 94.2%.
[0097] [Example 13] ([DPC]0 / [PE]0: 6 / 1) DPC (128.5 mg, 0.60 mmol) and DMF (4.5 mL) were added to a 10 mL flask and heated to 100 °C. A DMF solution (0.5 mL) of PE (13.6 mg, 0.10 mmol) was quickly added thereto, the inside of the flask was purged with nitrogen, and the mixture was stirred at 100 °C for 12 hours. A part of the solution was distilled off under reduced pressure, and the residue was dissolved in DMSO-d6 1H-NMR measurement was performed, and the result was that the yield (selectivity) of compound (I) was 93.9%.
[0098] [Example 14] ([DPC]0 / [PE]0:4 / 1) DPC (85.7 mg, 0.40 mmol) and DMF (4.5 mL) were added to a 10 mL flask and heated to 100°C. A DMF solution (0.5 mL) of PE (13.6 mg, 0.10 mmol) was quickly added thereto, the atmosphere in the flask was replaced with nitrogen, and the mixture was stirred at 100°C for 12 hours. Part of the solution was distilled off under reduced pressure, and the residue was dissolved in DMSO-d6. 1 H-NMR measurement was performed, and the result was that the yield (selectivity) of compound (I) was 91.2%.
[0099] [Example 15] ([DPC]0 / [PE]0:2 / 1) DPC (42.8 mg, 0.20 mmol) and DMF (4.5 mL) were added to a 10 mL flask and heated to 100°C. A DMF solution (0.5 mL) of PE (13.6 mg, 0.10 mmol) was quickly added thereto, the atmosphere in the flask was replaced with nitrogen, and the mixture was stirred at 100°C for 12 hours. A part of the solution was distilled off under reduced pressure, and the residue was dissolved in DMSO-d6, and an insoluble portion was observed. Using the soluble portion of the solution, 1 As a result of H-NMR measurement, the yield (selectivity) of compound (I) was 86.6%.
[0100] The products of Examples 11 to 15 1 In the H-NMR measurements, no signals of unreacted OH groups were observed in any of the measurements. Fig. 5 is a graph showing the relationship between the yield (selectivity) of compound (I) obtained in Examples 11 to 15 and the molar ratio of DPC to PE. As shown in Fig. 5, when the molar ratio of DPC to PE was 2 / 1, an insoluble portion was observed, but the selectivity of compound (I) in the soluble portion did not differ significantly from that when the molar ratio of DPC to PE was from 10 / 1 to 4 / 1. On the other hand, when the molar ratio of DPC to PE was from 10 / 1 to 4 / 1, no insoluble portion was observed, and no significant difference was observed in the selectivity. From the above results, it is considered that when the molar ratio of DPC to PE was 2 / 1, as in the case of reactions at low temperatures of around 20°C in the above reaction temperature study, there was an excess of unreacted PE compared to the intermediate produced when some of the OH groups of PE reacted with DPC, and as a result, by-products such as oligomers were produced by reacting with the OH groups of PE or the intermediate before the intermediate could undergo intramolecular cyclization.
[0101] [Example 16] (Reactivity of Compound (I)) Since compound (I) has a spiro structure consisting of two six-membered cyclic carbonates, it was expected that the ring strain would be greater and the reactivity would be higher than that of similar six-membered cyclic carbonates. Therefore, 5,5-dimethyl-1,3-dioxan-2-one (hereinafter sometimes referred to as "compound (IV)") was used as a model compound, and in the coexistence of compound (I) and compound (IV) (molar ratio: [compound (I)] 0 / The reactivity of compound (I) and compound (IV) was compared by reacting them with 0.9 molar equivalents of monoamine (1-hexylamine) in DMSO-d6 at room temperature. 1 The H-NMR measurement results are shown in Figure 6.
[0102] As shown in Figure 6, compound (I) selectively reacted with monoamine (1-hexylamine), whereas compound (IV) was hardly consumed (yield: 1% or less). In other words, it was revealed that the reactivity of compound (I) with amines is more than 100 times higher than that of compound (IV).
[0103] <Production of polyhydroxyurethane> [Example 17] (Ring-opening polyaddition behavior of compound (I) and diamine) As shown in the reaction formula below, polyhydroxyurethane is obtained by reacting compound (I) with a diamine.
[0104] [ka]
[0105] In the following reaction formula, X represents an alkylene group, an aralkylene group, or -R 11 -Ar 11 -R 12 - is a group represented by Ar 11 is a divalent aromatic hydrocarbon group, and R 11 and R 12 are each independently an alkylene group having 1 to 20 carbon atoms. n is an integer of 1 or more. n is an integer of 1 or more.
[0106] We attempted to synthesize polyhydroxyurethane (C6) by polyaddition of spiro-biscarbonate compound (I) with 1,6-diaminohexane in DMSO at 85°C. As a result, gelation occurred after 24 hours of reaction. Therefore, in order to verify the polyaddition behavior of compound (I) and 1,6-diaminohexane, the polyaddition behavior was followed in DMSO at 50°C by gel permeation chromatography (GPC) measurement (see reaction formula below). The results of the GPC measurement are shown in Figure 7. Figure 8 is a graph showing the relationship between the reaction time of compound (I) and 1,6-diaminohexane and the number average molecular weight or molecular weight distribution of the product.
[0107] [ka]
[0108] From Figures 7 and 8, a new peak appeared on the high molecular weight side after about 3 hours of reaction, and as the reaction time increased, the peak area increased and shifted to the high molecular weight side. This is probably because in the later stages of the reaction, the concentration of the amino groups at the ends of the polymer chains decreased significantly compared to the concentration of the hydroxyl groups produced, and the six-membered cyclic carbonate groups at the ends of the polymer chains reacted with the hydroxyl groups in the side chains instead of the amino groups, resulting in crosslinking of the polymer chains. Similar gelation has also been reported in the polyaddition of other bifunctional six-membered cyclic carbonates with diamines. Therefore, in order to prevent this side reaction, 0.1 molar equivalents of 1,6-diaminohexane was added to the reaction system after 3 hours of reaction, but no gelation was observed even after one night.
[0109] Based on the above results, we standardized the polyaddition reaction conditions as shown in the reaction formula below: in DMSO, at 50°C, 0.1 molar equivalent of diamine was added after 3 hours of reaction. We produced a total of four types of polyhydroxyurethanes (PHUs) (C3, C6, C8, p-Xyl) with different diamines.
[0110] [ka]
[0111] Specific production methods are shown in Examples 18 to 21 below.
[0112] [Example 18] (Production of polyhydroxyurethane (C3)) Compound (I) (250 mg, 1.33 mmol) was added to a 5 mL vial, the vial was capped with a silicon septum, and the inside of the vial was replaced with nitrogen. Dry DMSO (2 mL) was added to this and suspended, and then 1,3-diaminopropane (112 μL, 1.33 mmol) was added at room temperature (immediately became a homogeneous solution). This solution was heated to 50 ° C and stirred under a nitrogen atmosphere. After 3 hours, 1,3-diaminopropane (11 μL, 0.13 mmol) was added and stirred at 50 ° C for 16 hours. After cooling to room temperature, the solution was added dropwise to CHCl3 (about 125 mL) and left to stand at about 4 ° C for 4 hours. The precipitated solid was collected, dissolved in DMF (about 4 mL), and added dropwise to CHCl3 (about 100 mL) to collect the precipitated solid, which was then dried under reduced pressure to obtain polyhydroxyurethane (C3) (330 mg, yield 95%), which is a white solid. 1 H-NMR spectrum and 13 The structure of polyhydroxyurethane (C3) was confirmed by C-NMR spectrum. 1 The proportion of side reactions calculated from the integral ratio of the H-NMR spectrum was approximately 22%, and the content of polyhydroxyurethane (C3) having a branched structure relative to the total molar amount of polyhydroxyurethane (C3) was approximately 11 mol %.
[0113] [Example 19] (Production of polyhydroxyurethane (C6)) Compound (I) (250 mg, 1.33 mmol) and 1,6-diaminohexane (154 mg, 1.33 mmol) were added to a 5 mL vial, the vial was capped with a silicon septum, and the inside of the vial was replaced with nitrogen. Dry DMSO (2 mL) was added to this at room temperature (immediately became a homogeneous solution), heated to 50 ° C, and stirred under a nitrogen atmosphere. After 3 hours, 1,6-diaminohexane (15.4 mg, 0.13 mmol) was added and stirred at 50 ° C for 12 hours. After cooling to room temperature, the solution was added dropwise to CHCl3 (about 125 mL) and left to stand at about 4 ° C for 1 hour. The precipitated solid was collected, dissolved in MeOH (about 5 mL), and added dropwise to CHCl3 (about 100 mL), and the precipitated solid was collected and dried under reduced pressure to obtain polyhydroxyurethane (C6) (356 mg, 88% yield) as a white solid. 1 H-NMR spectrum and 13 The structure of polyhydroxyurethane (C6) was confirmed by C-NMR spectrum.
[0114] [Example 20] (Production of polyhydroxyurethane (C8)) Compound (I) (250 mg, 1.33 mmol) and 1,8-diaminooctane (191.7 mg, 1.33 mmol) were added to a 5 mL vial, the vial was capped with a silicon septum, and the inside of the vial was replaced with nitrogen. Dry DMSO (3 mL) was added to this at room temperature (partially insoluble), heated to 95 ° C, and stirred under a nitrogen atmosphere for 0.5 hours and at 50 ° C for 2.5 hours. 1,8-diaminooctane (19.7 mg, 0.13 mmol) was added to this, and the mixture was stirred at 95 ° C for 3.5 hours and at 50 ° C for 2.5 hours. After cooling to room temperature, the solution was added dropwise to CHCl3 (about 125 mL) and left to stand at about 4 ° C for 3 hours. The precipitated solid was collected, dissolved in MeOH (approximately 5 mL), and added dropwise to CHCl3 / n-hexane (approximately 100 mL / approximately 50 mL). The precipitated solid was collected and dried under reduced pressure to obtain polyhydroxyurethane (C8) (375 mg, yield 85%) as a white solid. 1 H-NMR spectrum and 13 The structure of polyhydroxyurethane (C8) was confirmed by C-NMR spectrum.
[0115] [Example 21] (Production of polyhydroxyurethane (p-Xyl)) Compound (I) (250 mg, 1.33 mmol) and p-xylylenediamine (181 mg, 1.33 mmol) were added to a 5 mL vial, the vial was capped with a silicon septum, and the inside of the vial was replaced with nitrogen. Dry DMSO (2 mL) was added at room temperature (partially insoluble), and after stirring for 5 minutes, the mixture was heated to 50 ° C and stirred under a nitrogen atmosphere for 3 hours. p-xylylenediamine (18.1 mg, 0.13 mmol) was added to the mixture and stirred at 50 ° C for 12.5 hours. After cooling to room temperature, the solution was added dropwise to CHCl3 (about 125 mL) and allowed to stand at about 4 ° C for 1 hour. The precipitated solid was collected, dissolved in DMF (about 5 mL), and added dropwise to CHCl3 (about 125 mL), and the precipitated solid was collected and dried under reduced pressure to obtain a light yellow solid polyhydroxyurethane (p-Xyl) (407 mg, yield 94%). 1 H-NMR spectrum and 13 The structure of polyhydroxyurethane (p-Xyl) was confirmed by C-NMR spectrum. 1 The proportion of side reactions calculated from the integral ratio of the H-NMR spectrum was approximately 22%, and the content of polyhydroxyurethane (p-Xyl) having a branched structure relative to the total molar amount of polyhydroxyurethane (p-Xyl) was approximately 11 mol%.
[0116] The polyhydroxyurethanes obtained in Examples 18 to 21 were identified by GPC measurement and Fourier transform infrared spectroscopy (FT-IR). The polymerization conditions, yield, number average molecular weight (Mn), and molecular weight distribution (Mw / Mn) are summarized in Table 1.
[0117] [Table 1]
[0118] From the FT-IR results, in all polyhydroxyurethanes, the peak at 1737 cm was due to the C=O stretching vibration of compound (I), which is a spiro-type cyclic carbonate. -1The peak completely disappeared, and the peak at 1686 cm -1 over 1690cm -1 The following peaks are due to the C=O stretching vibration of urethane and at 3310 cm -1 A peak due to NH / OH stretching vibration was observed around 1 In the H-NMR spectrum, signals corresponding to the NH of the urethane group (cis / trans mixture: 6.8 ppm to 7.1 ppm), the OH of the hydroxyl group (4.3 ppm to 4.7 ppm), and other protons were observed in all polyhydroxyurethanes. 13 From the C-NMR spectrum, in all polyhydroxyurethanes, a C=O-derived urethane group was observed at around 156 ppm. 13 C signal was observed. The number average molecular weight Mn of each polyhydroxyurethane obtained was 3.5 × 10 3 Over 14.2 x 10 3 Hereinafter, the molecular weight distribution Mw / Mn was 2.0 or more and 5.8 or less. From these results, it was found that each of the produced polyhydroxyurethanes was a polyurethane having a hydroxy group in the side chain, and the desired polyhydroxyurethane was produced.
[0119] As shown in Table 1, polyhydroxyurethane (C8) had the highest number-average molecular weight Mn. However, the molecular weight distribution Mw / Mn was broad at 5.5, and a bimodal peak was observed in the GPC measurement. From these findings, polyhydroxyurethane (C8) is considered to contain a partially branched structure, which was presumed to be due to heating at 95°C at the beginning of the reaction. In addition, polyhydroxyurethane (p-Xyl), which was not heated at 95°C, also showed a wide molecular weight distribution (Mw / Mn=5.8). The reason for this is unclear, but it is thought that the nucleophilicity of the amino group at the benzyl position of p-xylenediamine is lower than that of other diamines, which makes it easier for the reaction to occur between the six-membered cyclic carbonate group at the end of the polymer chain and the hydroxyl group in the side chain.
[0120] [Example 22] (Thermal properties of polyhydroxyurethane) Thermogravimetric differential thermal analysis (TGA-DTA) and differential scanning calorimetry (DSC) were performed on each of the polyhydroxyurethanes obtained in Examples 18 to 21. The results of TGA-DTA are shown in FIG. 9, and the results of DSC are shown in FIG.
[0121] From Figure 9, the 5% mass loss temperature (T d5 ) rose from 236°C to 286°C with an increase in the carbon number of the diamine, except for polyhydroxyurethane (p-Xyl). This is probably because the polyhydroxyurethane depolymerizes upon heating and is converted into the corresponding monomer (compound (I) and diamine), and the higher the boiling point of the polyhydroxyurethane, the higher the T d5 On the other hand, although the boiling point of the diamine p-xylylenediamine produced by the depolymerization of polyhydroxyurethane (p-Xyl) is higher than that of other aliphatic diamines, the T d5 The T value of polyhydroxyurethane (p-Xyl) was 269°C, which is lower than that of polyhydroxyurethane (p-Xyl). In addition, the mass loss of polyhydroxyurethane (p-Xyl) did not reach 100% even at 500°C. These results suggest that p-xylylenediamine produced by heating was carbonized, and as a result, the T value of polyhydroxyurethane (p-Xyl) was d5 It is considered that the value was lower than that of polyhydroxyurethane (C8). In fact, when the sample of polyhydroxyurethane (p-Xyl) was examined after TGA-DTA, black solid matter was observed.
[0122] From FIG. 10, the glass transition temperatures Tg of polyhydroxyurethanes (C3), (C6) and (C8) were 42.5°C or higher and 47.4°C or lower, and no particular correlation was observed between the number of carbon chains of the diamine residue and Tg. Considering that Tg is affected by the molecular weight of the polymer, the reason for the lack of correlation is that the number average molecular weights Mn of polyhydroxyurethanes (C3), (C6) and (C8) are different. On the other hand, polyhydroxyurethane (p-Xyl) having an aromatic group in the main chain showed a higher Tg (85.7°C) than polyhydroxyurethanes (C3), (C6) and (C8). Furthermore, no melting point was observed in any of the polyhydroxyurethanes, indicating that they were amorphous.
[0123] [Example 23] (Conversion of compound (I) into a dihydroxyurethane derivative) By reacting 1 molar equivalent of compound (I) with 2 molar equivalents of monoamine, it is possible to derive the corresponding dihydroxyurethane. By polyaddition of this dihydroxyurethane derivative with diisocyanate, it is possible to synthesize polyurethanes having urethane groups in the side chains. In addition, the dihydroxyurethane derivative may be converted to a novel six-membered cyclic carbonate having two urethane groups by reaction with DPC. Based on these findings, the synthesis of a dihydroxyurethane derivative of compound (I) was investigated.
[0124] As shown in the reaction formula below, a dihydroxyurethane derivative (hereinafter sometimes referred to as "compound (V)") was obtained by reacting 1 molar equivalent of compound (I) with 2 molar equivalents of monoamine. The specific synthesis procedure is described below.
[0125] [ka]
[0126] Compound (I) (500 mg, 2.66 mmol) was suspended in dry DMF (5 mL), 1-hexylamine (592 mg, 5.85 mmol) was slowly added at room temperature, and the mixture was stirred at room temperature for 14.5 hours. DMF was removed under reduced pressure, and the residue was purified with a silica gel column (eluent: EtOAc / n-hexane = 3 / 1, vol / vol) to obtain compound (V) (744 mg, 72% yield) as a white solid.
[0127] Electrospray ionization mass spectrometry (ESI-MS) of compound (V); 1 H-NMR, 13 The results of analysis by C-NMR, melting point measurement, and infrared spectrophotometer (IR) are shown below. 1 The H-NMR spectrum is shown in Figure 11.
[0128] HRMS (ESI-MS) (positive): m / z calcd for [M + Na]+, 413.2628, found, 413.2629. 1 H NMR (400 MHz, DMSO-d6, rt): δ (trans-urethane isomer) 7.06 (t, J = 5.7 Hz, 2H, NH), 4.46 (t, J = 5.0 Hz, 2H, OH), 3.87 (s, 4H, -NHCOOCH2-), 3.36 (d, J = 5.3 Hz, partially overlapping with residual H2O signal, -CH2OH), 2.93 (q, J = 6.7 Hz, 4H, -NHCH2-), 1.37 (t, J = 6.7 Hz, 4H, -NHCH2CH2-), 1.29-1.21 (m, 12H, -CH2-(CH2)3-CH3), 0.85 (t, J = 6.8 Hz, 6H, -CH3). 13C NMR (100 MHz, DMSO-d6, rt): δ (trans-urethane isomer) 156.46, 62.59, 59.69, 44.39, 40.26, 31.06, 29.45, 26.00, 22.13, 13.97. Mp: 79.0-81.0℃. IR (ATR, cm -1 ): 3278 (ν N-H and / or ν O-H ), 1687 (ν C=O ), 1545 (ν N-H ), 1252 (ν C-O ), 1048(ν C-O ).
[0129] [Example 24] (Identification of by-products from model reactions of compound (I) with monoamines) A model reaction was carried out using compound (I) and a monoamine. The specific synthesis procedure is as follows. Compound (I) (500 mg, 2.66 mmol) was suspended in dry DMF (5 mL), 1-hexylamine (592 mg, 5.85 mmol) was slowly added at room temperature, and the mixture was stirred at 50° C. for 14.5 hours. DMF was removed from a portion of the reaction solution by distillation under reduced pressure, and the residue was dissolved in DMSO-d6. 1 H-NMR measurement was performed. In addition, the remaining reaction solution was purified with a silica gel column (eluent: CHCl3 / EtOAc = 2 / 8, vol / vol), and the obtained solid was dissolved in DMSO-d6. 1 H-NMR measurements were performed. 1 The results of H-NMR measurement are shown in Figure 12. In addition, the reaction products were identified by ESI-MS analysis. As a result, it was revealed that in addition to the target product, compound (V), by-products, compound (V') and compound (V''), were produced, as shown in the reaction formula below. In the reaction formula, R is a hexyl group.
[0130] [ka]
[0131] <Study of manufacturing conditions for polyhydroxyurethane> [Example 25] (Reaction temperature: 50°C) Compound (I) (250 mg, 1.33 mmol) and 1,6-diaminohexane (154 mg, 1.33 mmol) were added to a 5 mL vial, the vial was sealed with a silicon septum, and the atmosphere in the vial was replaced with nitrogen. Dry DMSO (2 mL) was added to the vial at room temperature, and the vial was heated to 50°C and stirred under a nitrogen atmosphere. After 3 hours, 1,6-diaminohexane (15.4 mg, 0.13 mmol) was added and stirred at 50°C for 12 hours. After cooling to room temperature, the solution was added dropwise to CHCl3 (approximately 125 mL) and allowed to stand at approximately 4°C for 1 hour. The precipitated solid was collected, dissolved in MeOH (approximately 5 mL), and added dropwise to CHCl3 (approximately 100 mL), and the precipitated solid was collected and dried under reduced pressure to obtain polyhydroxyurethane (C6) (356 mg, 88% yield) as a white solid. Polyhydroxyurethane (C6) 1 The H-NMR spectrum is shown in Figure 13.
[0132] From FIG. 13, it was confirmed that in addition to polyhydroxyurethane (C6), by-products corresponding to compound (V') and compound (V'') which were by-products identified in the model reaction in Example 24 were produced. The production ratio of polyhydroxyurethane (C6), compound (V') and compound (V'') was calculated as follows: 1 The product ratio was calculated from the integral ratio of the H-NMR spectrum. The product ratio was polyhydroxyurethane (C6): compound (V'): compound (V'') = 6.3:1:1, and the proportion of side reactions was approximately 24%.
[0133] These results suggest that polyhydroxyurethane (C6) contains a monomer unit having two hydroxy groups in the side chain (corresponding to the structure of compound (V)) and a monomer unit having one hydroxy group and one urethane group in the side chain (corresponding to the structure of compound (V')), and thus has a branched structure. It is also suggested that the terminal structures of the main chain and side chain of polyhydroxyurethane (C6) have terminal structures corresponding to the structure of compound (V''), which has three hydroxy groups in addition to the amino terminal.
[0134] [Example 26] (Reaction temperature: 0℃) 1,6-diaminohexane (154 mg, 1.33 mmol) was added to a 5 mL vial, the vial was capped with a silicon septum, and the inside of the vial was replaced with nitrogen. Dry DMF (2 mL) was added to this at room temperature, cooled to 0°C, and compound (I) (250 mg, 1.33 mmol) was added as a powder. After stirring at 0°C for 18 hours, 1,6-diaminohexane (15.4 mg, 0.13 mmol) was added at 0°C, and then stirred at 50°C for 5 hours. After cooling to room temperature, the solution was added dropwise to CHCl3 (approximately 125 mL) and allowed to stand at approximately 4°C for 1 hour. The precipitated solid was collected, dissolved in MeOH (approximately 5 mL), and added dropwise to CHCl3 (approximately 100 mL), and the precipitated solid was collected and dried under reduced pressure to obtain polyhydroxyurethane (C6) (305 mg, 80%) as a white solid. Polyhydroxyurethane (C6) 1 The H-NMR spectrum is shown in Figure 14. The production ratio of polyhydroxyurethane (C6), compound (V') and compound (V'') was 1 It was calculated from the integral ratio of the H-NMR spectrum. The product ratio was polyhydroxyurethane (C6): compound (V'): compound (V'') = 25:1:1, the proportion of side reactions was about 7%, and the content of polyhydroxyurethane (C6) having a branched structure relative to the total molar amount of polyhydroxyurethane (C6) was about 3.5 mol%.
[0135] From the above results, it was found that in this example, in which polyhydroxyurethane (C6) was synthesized at 0°C, side reactions were significantly suppressed compared to Example 25, in which polyhydroxyurethane (C6) was synthesized at 50°C (proportion of side reactions: approximately 24%).
[0136] [Example 27] (Production of polyhydroxyurethane (C3): reaction temperature 0°C) 1,3-diaminopropane (112μL, 1.33mmol) and dry DMF (2mL) were added to a 5mL vial at room temperature, cooled to 0℃, and compound (I) (250mg, 1.33mmol) was added as a powder and stirred at 0℃ for 18 hours. 1,3-diaminopropane (11μL, 0.13mmol) was added to this at 0℃, and then stirred at 50℃ for 5 hours. After cooling to room temperature, the solution was added dropwise to CHCl3 (about 100mL), the precipitated solid was collected, dissolved in DMF (about 4mL), and added dropwise to CHCl3 (about 100mL), the precipitated solid was collected, and dried under reduced pressure to obtain polyhydroxyurethane (C3) (312mg, yield 90%), which is a white solid. 1 The proportion of side reactions calculated from the integral ratio of the H-NMR spectrum was approximately 8%, and the content of polyhydroxyurethane (C3) having a branched structure relative to the total molar amount of polyhydroxyurethane (C3) was approximately 4 mol %.
[0137] [Example 28] (Production of polyhydroxyurethane (p-Xyl): Reaction temperature 0°C) Add p-xylylenediamine (181 mg, 1.33 mmol) and dry DMF (2 mL) to a 5 mL vial at room temperature, cool to 0 ° C, add compound (I) (250 mg, 1.33 mmol) as a powder, and stir at 0 ° C for 18 hours. Add p-xylylenediamine (18.1 mg, 0.13 mmol) to this at 0 ° C, and then stir at 50 ° C for 5 hours. After cooling to room temperature, the solution was dropped into CHCl3 (about 100 mL), and the precipitated solid was collected, dissolved in DMF (about 4 mL), dropped into CHCl3 (about 100 mL), and the precipitated solid was collected and dried under reduced pressure to obtain a white solid polyhydroxyurethane (p-Xyl) (396 mg, yield 92%). 1 The proportion of side reactions calculated from the integral ratio of the H-NMR spectrum was approximately 8%, and the content of polyhydroxyurethane (p-Xyl) having a branched structure relative to the total molar amount of polyhydroxyurethane (p-Xyl) was approximately 4 mol%.
[0138] From the above results, it was found that in Examples 27 and 28, in which polyhydroxyurethane (C3) and polyhydroxyurethane (p-Xyl) were synthesized at 0°C, side reactions were significantly suppressed compared to Examples 18 and 21, in which polyhydroxyurethane (C3) and polyhydroxyurethane (p-Xyl) were synthesized at 50°C (proportion of side reactions: approximately 11%). [Industrial Applicability]
[0139] According to the production method of this embodiment, it is possible to provide a simple method for producing a bifunctional cyclic carbonate with an improved yield, and a novel method for producing a polyhydroxyurethane using a bifunctional cyclic carbonate.
Claims
1. The method includes a reaction step of reacting pentaerythritol with a diaryl carbonate to obtain a bifunctional cyclic carbonate having a spiro structure, The bifunctional cyclic carbonate having a spiro structure is 2,4,8,10-tetraoxaspiro[5,5]-undecane-3,9-dione, A method for producing a bifunctional cyclic carbonate having a spiro structure, the method comprising the step of:
2. The method according to claim 1 , wherein the reaction is carried out at a temperature of 40° C. or higher and 100° C. or lower in the reaction step.
3. The method according to claim 1 or 2, wherein the reaction is carried out at a temperature of 50° C. or higher and 100° C. or lower in the reaction step.
4. The method according to any one of claims 1 to 3, wherein in the reaction step, a molar ratio of diaryl carbonate to pentaerythritol is 2 / 1 or more and 10 / 1 or less.
5. The method according to any one of claims 1 to 4, wherein in the reaction step, a molar ratio of diaryl carbonate to pentaerythritol is 4 / 1 or more and 10 / 1 or less.
6. The method according to any one of claims 1 to 5, wherein in the reaction step, a concentration of pentaerythritol is 10 mmol / L or more and 100 mmol / L or less with respect to a total volume of the reaction solution.
7. The method according to any one of claims 1 to 6, wherein in the reaction step, a concentration of pentaerythritol is 10 mmol / L or more and 80 mmol / L or less with respect to a total volume of the reaction solution.
8. The process according to any one of claims 1 to 7, wherein the diaryl carbonate is diphenyl carbonate.
9. A method for producing a bifunctional cyclic carbonate having a spiro structure by the production method according to any one of claims 1 to 8, The method includes a polymerization step of reacting the bifunctional cyclic carbonate having a spiro structure with a diamine represented by the following general formula (Ia) to obtain polyhydroxyurethane, The method for producing polyhydroxyurethane, wherein the bifunctional cyclic carbonate having a spiro structure is 2,4,8,10-tetraoxaspiro[5,5]-undecane-3,9-dione. 【Chemistry 1】 In the general formula (Ia), X is an alkylene group, an aralkylene group, or -R 11 -Ar 11 -R 12 Ar is a group represented by the formula -. 11 is a divalent aromatic hydrocarbon group, R 11 and R 12 are each independently an alkylene group having 1 to 20 carbon atoms.
10. The method according to claim 9, wherein in the polymerization step, the polymerization reaction is carried out at 5° C. or less, and the content of polyhydroxyurethane having a branched structure is controlled to be 4 mol % or less based on the total molar amount of polyhydroxyurethane.
11. The method according to claim 9, wherein in the polymerization step, the polymerization reaction is carried out at 50° C. or higher, and the content of polyhydroxyurethane having a branched structure is controlled to be 11 mol % or higher based on the total molar amount of polyhydroxyurethane.
Citation Information
Patent Citations
Novel cyclic carbonic acid derivative, manufacture and copolymer component for polycarbonate manufacture
JP1982144282A
Recovery of polyoxyalkylene alcohol polymerization catalyst
JP1996269189A
Method for producing polyhydroxyurethane
JP2006009001A
Ring-opened norbornene polymer, method of preparing the same and application thereof
JP2007204605A
Active energy line curing resin composition
JP2010132895A