DEAD FRONT FOR DISPLAYS WITH TOUCH PANELS ON DECORATIVE GLASS AND ASSOCIATED METHODS - Patent application

The deadfront product with a translucent and contrast layer, combined with a high optical density layer, addresses the issue of visible edges in displays by ensuring a seamless appearance and enhanced visibility of icons, improving aesthetic appeal in automotive and consumer electronics.

JP7595125B2Active Publication Date: 2024-12-05CORNING INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023133392
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-09-11
Filing Date
2023-08-18
Publication Date
2024-12-05
Estimated Expiration
2038-09-12

AI Technical Summary

Technical Problem

Existing display technologies struggle to achieve a seamless transition between display and non-display areas, resulting in visible edges when the display is off, which compromises aesthetic appeal and design consistency, particularly in automotive and consumer electronics.

Method used

The use of a deadfront product comprising a substrate with a translucent layer and a contrast layer to enhance visibility and contrast, combined with a high optical density layer to obscure non-display areas when the display is off, while allowing icons and graphics to be visible when activated, utilizing cold forming processes to create curved shapes.

Benefits of technology

The solution provides a high-quality deadfront appearance with visible icons and graphics when activated, while maintaining a unified appearance when off, enhancing aesthetic appeal and design consistency in vehicle and consumer electronics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595125000001
    Figure 0007595125000001
  • Figure 0007595125000002
    Figure 0007595125000002
  • Figure 0007595125000003
    Figure 0007595125000003
Patent Text Reader

Abstract

To provide a deadfront article capable of achieving both a good deadfront appearance and, when a display is on, a high-quality display.SOLUTION: The deadfront article includes a substrate having a first surface and a second surface. The deadfront article also includes a semi-transparent layer disposed on the second surface of the substrate. The semi-transparent layer has a region of a single color or a region of a design of two or more colors, and the semi-transparent layer has a first optical density. Further, the deadfront article includes a contrast layer disposed on the region. The contrast layer is configured to enhance visibility of the colors of the semi-transparent layer.SELECTED DRAWING: Figure 28
Need to check novelty before this filing date? Find Prior Art

Description

Related Applications

[0001] This application claims the benefit of priority under 35 U.S.C. § 119 of U.S. Provisional Application No. 62 / 729,695, filed September 11, 2018, U.S. Provisional Application No. 62 / 679,278, filed June 1, 2018, and U.S. Provisional Application No. 62 / 557,502, filed September 12, 2017, the contents of each of which are incorporated by reference in their entirety and herein. This application is also a divisional application of Patent Application No. 2020-514953, filed on September 12, 2018. [Technical field]

[0002] FIELD OF THE DISCLOSURE The present disclosure relates to deadfront products for displays, and in particular to vehicle interior systems including deadfront products for displays and methods of forming same. [Background technology]

[0003] In various applications involving displays, it is desirable to have a display surface or functional surface with a dead-front appearance. In general, a dead-front appearance is a way to conceal a display or functional surface such that there is a seamless transition between the display area and the non-display area or between the dead-front area of ​​a product and the non-dead-front area or other surface. For example, in a typical display with a glass or plastic cover surface, the edge of the display (or the transition from the display area to the non-display area) is visible even when the display is turned off. However, from an aesthetic appearance or design standpoint, it is often desirable to have a dead-front appearance such that when the display is off, the display area and the non-display area exist as indistinguishable from each other, and the cover surface presents a unified appearance. One application where a dead-front appearance is desirable is in automotive interiors, including in-car displays or touch interfaces, and other applications in consumer mobile or home electronics, including mobile devices and home appliances. However, it is difficult to achieve both a good dead-front appearance and a high-quality display when the display is on. Summary of the Invention

[0004] In one aspect, an embodiment of the present disclosure relates to a deadfront product. The deadfront product has a substrate, a translucent layer, and a contrast layer. The substrate has a first surface and a second surface opposite the first surface. The translucent layer is disposed on at least a first portion of the second surface of the substrate. Further, the translucent layer has a monochromatic area or an area of ​​a design of two or more colors. The contrast layer is disposed on at least a portion of the area. The contrast layer is configured to enhance the visibility of the color of the area or to enhance the contrast between the colors of the design of the area in the portion of the area where the contrast layer is disposed.

[0005] In another aspect, an embodiment of a device incorporating a deadfront product is provided. The device includes a deadfront product having a substrate, a semi-transparent layer disposed on a first side of the substrate, a contrast layer disposed on at least a portion of the semi-transparent layer, and a high optical density layer disposed on at least a portion of the contrast layer. The high optical density layer at least partially forms at least one icon. The device further includes a touch panel disposed behind the at least one icon.

[0006] Another embodiment of the present disclosure relates to a method for forming a curved dead-front product for display, the method comprising: curving a dead-front product having a glass layer on a support having a curved surface; and fixing the curved dead-front product to the support such that the dead-front product conforms to the curved shape of the curved surface of the support. During the curving and fixing of the dead-front product, the maximum temperature of the dead-front product is below the glass transition temperature of the glass layer. Additionally, the dead-front product has a translucent layer disposed on a first surface of the glass layer and a contrast layer. The translucent layer has a monochromatic area or an area of ​​a design of two or more colors, and the contrast layer is disposed on at least a portion of the area. The contrast layer is configured to enhance the visibility of the color of the area or to enhance the contrast between the colors of the design of the area in the portion of the area where the contrast layer is disposed.

[0007] Additional features and advantages will be set forth in the following detailed description, and in part will become readily apparent to those skilled in the art from that description, or may be learned by practicing the embodiments described herein, including the following detailed description, claims, and accompanying drawings.

[0008] It should be understood that both the foregoing general description and the following detailed description are merely exemplary and are intended to provide an overview or framework for understanding the nature and character of the claims. The accompanying drawings are included to provide a further understanding, and are incorporated in and constitute a part of this specification. The drawings illustrate one or more embodiments, and together with the description, serve to explain the principles and operation of the various embodiments. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a perspective view of a vehicle interior including a vehicle interior system utilizing a Deadfront product according to one or more of the embodiments described herein. [Diagram 2] 1 illustrates a display with a monochromatic dead-front product with the display turned off, according to one exemplary embodiment. [Diagram 3] 3 illustrates a display comprising the dead-front product of FIG. 2 with the display illuminated, according to one exemplary embodiment. [Figure 4] 1 illustrates a display with a patterned dead-front product with the display turned off, according to one exemplary embodiment. [Diagram 5] 5 illustrates a display comprising the dead-front product of FIG. 4 with the display illuminated, according to one exemplary embodiment. [Figure 6] FIG. 2 is a cross-sectional view of a dead-front product for a display having a translucent layer and a contrast layer according to one exemplary embodiment. [Figure 7] FIG. 2 is another cross-sectional view of a dead-front product for a display having a functional surface layer and an opaque layer according to one exemplary embodiment. [Figure 8] FIG. 1 is a cross-sectional view of an LED display having a dead-front product according to one exemplary embodiment. [Figure 9]FIG. 2 is a cross-sectional view of a DLP MEMS chip having a dead-front product according to one exemplary embodiment. [Figure 10] FIG. 1 is a cross-sectional view of a dead-front display with touch screen functionality according to one exemplary embodiment. [Figure 11] 1 is a leather textured front display for a vehicle interior according to one exemplary embodiment. [Figure 12] 1 is a woodgrain dead-front display for a vehicle interior according to one exemplary embodiment. [Figure 13A] 1 shows the front side of the glass layer with the semi-transparent layer printed on it. [Figure 13B] 1 shows the back side of the glass layer with the semi-transparent layer printed on it. [Figure 14A] 1 shows the front side of a glass layer printed with a translucent layer and a contrast layer according to one exemplary embodiment. [Figure 14B] 1 shows the back side of a glass layer printed with a translucent layer and a contrast layer according to one exemplary embodiment. [Figure 15] 1 illustrates a variable whiteness contrast layer printed on a glass sheet according to one exemplary embodiment. [Figure 16] 1 is a graph of transmittance for a variable transmittance contrast layer according to an exemplary embodiment. [Figure 17] 1 illustrates four different patterns of translucent layers for a deadfront product according to one exemplary embodiment. [Figure 18] 1 illustrates a deadfront product having a semi-transparent layer that transitions from leather grain to solid black color, according to one exemplary embodiment. [Figure 19] 1 shows a semi-transparent layer of a knit pattern for a deadfront product. [Figure 20] 1 illustrates a semi-transparent layer of a knit pattern for a deadfront product according to one exemplary embodiment, with a contrast layer printed behind the semi-transparent layer of the knit pattern. [Figure 21] 1 illustrates the front side of a deadfront product having a marble pattern translucent layer with a window in the contrast layer according to one exemplary embodiment. [Figure 22] 1 shows the backside of a deadfront product having a marble pattern translucent layer with windows in the contrast layer according to one exemplary embodiment. [Figure 23] FIG. 1 is a side view of a curved glass dead-front product for use with a display according to one exemplary embodiment. [Figure 24] FIG. 7 is a front perspective view of a glass layer for the glass dead-front product of FIG. 6 prior to curvature forming, according to an exemplary embodiment. [Diagram 25] 1 illustrates a curved dead-front product having a glass layer shaped to conform to a curved display frame according to one exemplary embodiment. [Figure 26] 1 illustrates a process for cold forming a dead-front product including a glass layer into a curved shape according to one exemplary embodiment. [Figure 27] 1 illustrates a process for forming a curved dead-front product including a curved glass layer according to one exemplary embodiment. [Figure 28] FIG. 1 illustrates an exploded view of layers of a deadfront product according to one exemplary embodiment. [Figure 29] 1 illustrates a wood grain deadfront product according to one exemplary embodiment. [Diagram 30] 1 illustrates a wood grain deadfront product with an illuminated backside according to one exemplary embodiment. [Diagram 31] 1 illustrates a wood grain dead front product with illuminated back and different colored icons according to one exemplary embodiment. [Diagram 32] Opacity is too high, carbon fiber pattern shows dead front of product. [Diagram 33]FIG. 32 shows a dead-front product with an illuminated backside, demonstrating that high levels of opacity can obscure icons. [Diagram 34] 1 illustrates a carbon fiber patterned deadfront product having an opacity within the disclosed ranges according to one exemplary embodiment. [Diagram 35] 35 shows the dead-front product of FIG. 34 with an illuminated backside, demonstrating better visibility of the icons. [Diagram 36] 1 illustrates a dead-front product with a touch panel according to one exemplary embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Referring generally to the drawings, vehicle interior systems may have a variety of different curved surfaces designed to be transparent, such as curved display surfaces, and the present disclosure provides products and methods for forming these curved surfaces. In one or more embodiments, such surfaces are formed from glass or plastic materials. Forming curved vehicle surfaces from glass materials may provide many advantages compared to typical curved plastic panels traditionally found in vehicle interiors. For example, glass is generally believed to provide enhanced functionality and user experience for many curved cover material applications, such as display and touch screen applications, compared to plastic cover materials.

[0011] Furthermore, it may be desirable in many applications to equip displays, particularly displays for vehicle interior systems, with a dead-front appearance. Generally, the dead-front appearance blocks the visibility of underlying display components, icons, graphics, etc. when the display is off, but allows the display components to be easily seen when the display is on or activated (in the case of touch-enabled displays). In addition, products that provide a dead-front effect (i.e., dead-front products) can be used to match the color or pattern of the product with adjacent components to eliminate visibility of the transition from the dead-front product to the surrounding components. This may be particularly effective when the dead-front product is of a different material than the surrounding components (e.g., the dead-front product is formed from a glass material but is surrounded by a center console covered in leather). For example, the dead-front product may have a wood grain pattern or leather pattern, where the leather pattern can be used to match the appearance of the display with the surrounding wooden or leather components (e.g., a wooden or leather dashboard) of the vehicle interior system in which the display is installed.

[0012] Various embodiments of the present disclosure relate to forming curved glass-based dead-front products utilizing a cold forming or cold bending process. As described herein, curved glass-based dead-front products and processes for forming the same are provided that avoid the shortcomings of typical glass hot forming processes. For example, hot forming processes require high energy, increasing the cost of forming curved glass components relative to the cold bending processes described herein. In addition, hot forming processes generally make the application of glass coating layers, such as dead-front ink or pigment layers, more difficult. For example, ink or pigment materials generally cannot withstand the high temperatures of the hot forming process, so not much ink or pigment material can be applied to a flat piece of glass material prior to the hot forming process. Furthermore, application of ink or pigment material to the surface of a curved glass product after hot bending is substantially more difficult than application to a flat glass product.

[0013] FIG. 1 illustrates a vehicle interior 10 having three different vehicle interior systems 100, 200, 300 according to one exemplary embodiment. Vehicle interior system 100 has a center console base 110 with a curved surface 120 with a display shown as a curved display 130. Vehicle interior system 200 has a dashboard base 210 with a curved surface 220 with a display shown as a curved display 230. Dashboard base 210 generally has an instrument panel 215, which may also have a curved display. Vehicle interior system 300 has a dashboard steering wheel base 310 with a curved surface 320 and a display shown as a curved display 330. In one or more embodiments, the vehicle interior system may have a base that is an armrest, pillar, seat back, floor panel, headrest, door panel, or any part of the vehicle's interior that has a curved surface.

[0014] The embodiments of the Deadfront products described herein may be used in any or all of the vehicle interior systems 100, 200, and 300. Although FIG. 1 illustrates an automobile interior, various embodiments of the vehicle interior system may be incorporated into any type of vehicle, including trains, automobiles (e.g., cars, trucks, buses, etc.), marine vehicles (boats, ships, submarines, etc.), and aircraft (e.g., drones, planes, jets, helicopters, etc.), including human-operated, semi-autonomous, and fully autonomous vehicles. Additionally, while the description herein primarily relates to the use of Deadfront embodiments for use in vehicle displays, it should be understood that the various Deadfront embodiments described herein may be used in any type of display application.

[0015] 2 and 3, a dead-front product 400 for a vehicle display, such as display 130, 230, and / or 330, is shown and described. FIG. 2 shows the appearance of the dead-front product 400 when the light source of the associated display is inactivated, and FIG. 3 shows the appearance of the dead-front product 400 when the light source of the associated display is activated. As shown in FIG. 3, when the light source is activated, a graphic 410 and / or a number of icons are visible through the dead-front product. When the light source is inactivated, the graphic 410 disappears and the dead-front product 400 displays a surface exhibiting a desired surface finish (e.g., a black surface in FIG. 2) uninterrupted by the graphic 410. In an embodiment, the light source is activated using a power button 420. As shown in the embodiment of FIG. 2 and FIG. 3, the power button 420 is illuminated and changes from red to green when activated. In an exemplary embodiment, the power button 420 is selected to comply with one of IEC 60417-5007, IEC 60417-5008, IEC 60417-5009 and IEC 60417-5010.

[0016] 4 and 5 show another embodiment of a dead-front product 400 for a vehicle display, such as displays 130, 230 and / or 330. In comparison to the monochromatic dead-front product 400 of FIG. 2, FIG. 4 shows a patterned dead-front product 400. When the light source of the associated display is inactivated as shown in FIG. 4, only the pattern of the dead-front product 400 is visible. In FIG. 5, the light source of the associated display is activated and the icon 430 is visible through the dead-front product 400. Thus, when the light source is inactivated, the icon 430 disappears and the dead-front product 400 displays a surface exhibiting a desired pattern uninterrupted by the icon 430 (e.g., the leather grain pattern in FIG. 4).

[0017] As described in more detail below, the dead-front product 400 provides this differential icon display by utilizing one or more colored layers disposed between the outer substrate and the light source. The optical properties of the colored layers are designed such that when the light source is turned off, the boundaries of the icons or other display structures below the colored layers are not visible, but when the light source is on, the graphics 410 and / or icons 430 are visible. In various embodiments, the dead-front products described herein are designed to provide a high quality dead-front appearance, including high contrast icons when the light source is on, combined with a uniform dead-front appearance when the light is off. Additionally, applicant provides these various dead-front products with materials suitable for cold forming into curved shapes, including complex curved shapes, as described below.

[0018] Referring now to FIG. 6, one embodiment of the structure of a deadfront product 400 is shown. In particular, the deadfront product 400 has at least a substrate 450, a semi-transparent layer 460, and a contrast layer 470. The substrate 450 has an outer surface 480 facing the viewer and an inner surface 490 on which the semi-transparent layer 460 and / or the contrast layer 470 are at least partially disposed. As used herein, the term "disposing" includes coating, depositing, and / or forming a material on a surface using any method known in the art. The disposed material may constitute a layer, as defined herein. As used herein, the phrase "disposed on" includes examples of forming a material on a surface such that the material is in direct contact with the surface, and also includes examples of forming a material on a surface such that there are one or more intervening materials between the disposed material and the surface. The intervening materials may constitute a layer, as defined herein. The term "layer" may include one layer or may include one or more sublayers. Such sublayers may be in direct contact with one another. The sublayers may be formed of the same material or two or more different materials. In one or more alternative embodiments, such sublayers may have intervening layers of different materials disposed between the sublayers. In one or more embodiments, a layer may include one or more adjacent uninterrupted layers and / or one or more discontinuous interrupted layers (i.e., layers having different materials formed adjacent to one another). A layer or sublayer may be formed by any method known in the art, including discrete deposition or continuous deposition processes. In one or more embodiments, a layer may be formed using only continuous deposition processes, or alternatively, using only discrete deposition processes.

[0019] The properties of the substrate 450 are described in more detail below, but in embodiments, the substrate 450 has a thickness of 0.05 to 2.0 mm. In one or more embodiments, the substrate may be a transparent plastic, such as PMMA, polycarbonate, or may include a glass material (which may be optionally reinforced). Also as described in more detail below, in embodiments, the semi-transparent layer 460 may be printed on at least a portion of the inner surface 490 of the substrate 450. In other embodiments, the semi-transparent layer 460 is deposited using non-conductive vacuum deposition. Additionally, in embodiments, the contrast layer 470 is printed on at least a portion of the inner surface 490 of the substrate 450 and / or at least a portion of the semi-transparent layer 460.

[0020] In certain embodiments, such as that shown in FIG. 7, the deadfront product 400 also has a functional surface layer 500 and / or an opaque layer 510 (also referred to as a "high optical density layer"). The functional surface layer 500 can be configured to provide one or more of a variety of functions. In another exemplary embodiment, the functional surface layer 500 is an optical coating configured to provide easy-cleaning capabilities, anti-glare properties, anti-reflective properties, and / or a half-mirror coating. Such optical coatings can be formed using one layer or multiple layers. In the case of an anti-reflective functional surface layer, such layers may be formed using multiple layers of alternating high and low refractive indexes. Non-limiting examples of low refractive index materials include SiO2, MgF2, and Al2O3, and non-limiting examples of high refractive index materials include Nb2O5, TiO2, ZrO2, HfO2, and Y2O3. In embodiments, the total thickness of such optical coatings (which may be disposed on the anti-glare surface or on a smooth substrate surface) is between 5 nm and 750 nm. Additionally, in embodiments, the functional surface layer 500 provides easy-cleaning capabilities, enhanced feel for touch screens, and / or coatings / treatments to reduce fingerprints. In some embodiments, the functional surface layer 500 is integral with the first side of the substrate. For example, such a functional surface layer may include an etched surface on the first side of the substrate 450 that provides an anti-dazzle surface (or haze, e.g., 2%-20%). The functional surface layer 500, when provided, together with the substrate 450, the translucent layer 460, and the contrast layer 470, constitute the translucent structure 520 of the deadfront product 400.

[0021] As described in more detail below, the opaque layer 510 has a high optical density to block light transmission. As used herein, "opaque layer" is used interchangeably with "high optical density layer." In embodiments, the opaque layer 510 is used to block light from passing through certain areas of the deadfront product 400. In some embodiments, the opaque layer 510 obscures functional or non-decorative elements provided for operation of the deadfront product 400. In other embodiments, the opaque layer 510 is provided to outline backlit icons and / or other graphics (such as the graphic 410 and / or power button 420 shown in FIGS. 2 and 3 and the icon 430 shown in FIG. 5), thereby enhancing contrast at the edges of such icons and / or graphics. Thus, in embodiments, the opaque layer 510 has breaks in the layer that form windows for the graphic 410, the power button 420, and / or the icon 430. That is, in embodiments, the opaque layer 510 extends continuously until it reaches the peripheral edges for the graphic 410, the power button 420, and / or the icons 430. At such edges, the opaque layer 510 is discontinued or, in some embodiments, substantially reduced in optical density (e.g., reduced material thickness, reduced material density, etc.). In embodiments, the opaque layer 510 intermittently recommences in the areas of the graphic 410, the power button 420, and / or the icons 430 to form features of the graphic 410, the power button 420, and / or the icons 430, such as forming the "I" and "O" of a given power button 420. Thus, in embodiments, the opaque layer 510 forms an image negative of the graphic 410, the power button 420, and / or the icons 430, by virtue of the portions of the graphic 410, the power button 420, and / or the icons 430 that are visible to a user through the exterior surface 480 of the substrate 450 being blank areas of the opaque layer 510.

[0022] The opaque layer 510 can be any color, but in certain embodiments, the opaque layer 510 is black or gray. In embodiments, the opaque layer 510 is provided by screen printing or inkjet printing on the semi-transparent layer 460 and / or the inner surface 490 of the substrate 450. Generally, the thickness of an inkjet printed opaque layer 510 is between 1 μm and 5 μm, whereas the thickness of a screen printed opaque layer 510 is between 5 μm and 20 μm. Thus, the printed opaque layer 510 can have a thickness in the range of 1 μm to 20 μm. However, in other embodiments, the opaque layer 510 is a metal layer deposited by physical vapor deposition and / or is an optical stack fabricated using the high index / low index stacking described above for color matching.

[0023] FIG. 28 shows an exploded view of the layers comprising the deadfront product 400 in one embodiment. As can be seen, the layers include a substrate 450, a translucent layer 460, a contrast layer 470, an opaque layer 510, and a color layer 650. As can be seen in FIG. 28, the translucent layer 460 is a wood grain pattern, and the opaque layer 510 provides a negative image of the icons 430 for the entertainment console, such as, for example, the power button 420, tuning control, volume control, presets, etc. The combination of the translucent layer 460, contrast layer 470, and opaque layer 510 provides the deadfront product 400 as shown in FIG. 29 and FIG. 30. In FIG. 29, the wood grain of the translucent layer 460 is visible when the deadfront product 400 is not backlit, and when the deadfront product 400 is backlit, the icons 430 are visible through the exterior surface 480 of the deadfront product 400. Referring again to Figure 28, when color layer 650 is disposed over opaque layer 510 (at least in the area of ​​icon 430), it can change the color of icon 430, as shown in Figure 31. Additionally, whereas a monochromatic layer 650 is shown in Figure 28, color layer 650 can include multiple colors across the layer and / or a particular color in the area of ​​a particular icon 430 or portion of icon 430, as shown in Figure 31. Thus, in some embodiments, color layer 650 is a continuous layer, while in other embodiments, color layer 650 is discontinuous, i.e., color is only provided in predetermined locations across opaque layer 510 and / or contrast layer 470 in the areas defining icon 430.

[0024] In embodiments, the optical densities of the layers are adjusted to enhance the visibility of the graphic 410, power button 420, and / or icon 430 when the deadfront product 400 is backlit. In certain embodiments, the combined optical density of the translucent layer 460 and the contrast layer 470 in the illuminated areas (i.e., the graphic 410, power button 420, and / or icon 430) is between 1.0 and 2.1. In other embodiments, the combined optical density is between 1.2 and 1.6, and in yet other embodiments, the combined optical density is about 1.4. When providing optical density in the illuminated areas, in embodiments, the optical density of the contrast layer 470 is between 0.9 and 2.0, and in embodiments, the optical density of the translucent layer 460 is between 0.1 and 0.5. In non-illuminated areas (i.e., areas surrounding the graphic 410, power button 420, and / or icon 430), the combined optical density of the translucent layer 460, contrast layer 470, and opaque layer 510 is at least 3.4. When providing optical density in non-illuminated areas, in embodiments, the optical density of the contrast layer 470 is between 0.9 and 2.0, in embodiments, the optical density of the translucent layer 460 is between 0.1 and 0.5, and in embodiments, the optical density of the opaque layer 510 is at least 2.4. In an exemplary embodiment, the optical density of the color layer 650 is between 0.3 and 0.7. Additionally, in embodiments, the optical density of a particular layer may vary across the layer to provide enhanced contrast or to preserve the ink or material that comprises the layer. For example, the optical density in the contrast layer 470 may be lower in illuminated areas than in non-illuminated areas. Additionally, the optical density of the color layer 650 may be lower (or zero) in non-illuminated areas than in illuminated areas.

[0025] 32 and 33, and 34 and 35 show different dead-front products with different levels of optical density, whereby these figures show the different appearances of a dead-front product 400 with too high optical density in the illuminated area (FIGS. 32 and 33) and a dead-front product 400 with optical density in the ranges mentioned above for the illuminated area (FIGS. 34 and 35). As seen in FIG. 32, the dead-front product has a carbon fiber pattern in which the optical density of the translucent layer is too high. This makes the illuminated area difficult to see, as seen in FIG. 33. In comparison, the dead-front product 400 in FIG. 34 is provided with a carbon fiber pattern with a translucent layer 460, a contrast layer 470 and an opaque layer 510 with optical density in the ranges mentioned above. Thus, as shown in FIG. 35, the icon 430 is significantly more crisp and clearly visible. As also shown in FIG. 35, the center icon 430 is a power button 420 provided with the color red using color layer 650.

[0026] As shown in FIG. 8 and FIG. 9, the deadfront product 400 is disposed on or in front of the display 530. In one or more embodiments, the display may include a touch-enabled display including a display and a touch panel. Exemplary displays include LED displays (FIG. 8), DLP MEMS chips (FIG. 9), LCDs, OLEDs, transmissive displays, reflective displays, and the like. In an embodiment, the display 530 is secured or attached to the deadfront product 400 using, for example, an optically clear adhesive 540. The deadfront product 400 has a transmittance of about 5% to about 30% across the visible spectrum, i.e., wavelengths from 400 nm to 700 nm. In other words, the deadfront product 400 has an average light transmittance in the range of about 5% to about 30% across the entire wavelength range of about 400 nm to about 700 nm. As used herein, the term "transmittance" is defined as the percentage of incident optical power in any wavelength range that is transmitted through a material (e.g., the deadfront product, a substrate or a layer thereof). In embodiments, the deadfront product 400 is a low transmission deadfront product having a light transmission of 10% or less across the visible spectrum. In such instances, the opaque layer 510 may not be necessary to obscure non-display areas such as the edges of the display 530, i.e., display borders, and / or wiring, connectors, etc. In other embodiments, the deadfront product 400 is a high transmission deadfront product having an average transmission of about 10% to about 30%. In such embodiments, the opaque layer 510 may be necessary to block non-display areas from being seen.

[0027] In one embodiment, the deadfront product 400 is provided with touch functionality as shown in FIG. 10. In FIG. 10, the deadfront product 400 has a substrate 450, a black semi-transparent layer 460, and a contrast layer 470 disposed on portions of the substrate 450 and the semi-transparent layer 460. In this case, the contrast layer 470 and the semi-transparent layer 460 form an icon or graphic, such as a power button 420 (e.g., as shown in FIG. 2 and FIG. 3). In one embodiment, the touch functionality is provided by capacitive sensing. In one embodiment, the capacitive sensor is formed by a transparent conductive film or coating 550. In one exemplary embodiment, the transparent conductive film 550 is a polyester (e.g., PET) film coated with a transparent conductive oxide (e.g., indium tin oxide (ITO)).

[0028] By activating the toggle switch (e.g., by touching the deadfront product 400 in the area of ​​the transparent conductive film 550), the light source 570 is activated or deactivated. In the embodiment of FIG. 10, the light source 570 includes a red LED 580 and a green LED 590. In a setting, such as a vehicle, the red LED 580 and the green LED 590 indicate the state of the deadfront product 400. For example, before starting the vehicle, the red LED 580 and the green LED 590 are both off, as shown at the bottom of the power button 420 state legend on the left side of FIG. 10. When the vehicle is started, before touching the power button 420, the red LED 580 is on while the green LED 590 is off (at the top of the power button 420 state legend), indicating that the display 530 is not activated. When the power button 420 is touched, the toggle switch 560 turns off the red LED 580 and turns on the green LED 590, activating the display 530. If the user wishes to deactivate the display 530 while continuing to run the vehicle, the user can again touch the power button 420 and the toggle switch 560 will turn off the green LED 590, turn on the red LED 580, and turn off the display 530. In one embodiment, a vibration motor 600 is provided to provide tactile feedback each time the toggle switch 560 is activated.

[0029] Although an exemplary embodiment of a power button 420 for a display 530 is shown, the touch functionality is suitable for other features. Continuing with the vehicle example, the touch functionality is suitable for use to control various vehicle systems, such as a climate control (i.e., heating and air conditioning) system, a radio / entertainment system, a dashboard display panel (e.g., for speedometer, odometer, trip odometer, tachometer, vehicle warning indicators, etc.), a center console display panel (e.g., for GPS display, in-car information, etc.), among others. In FIG. 11, a deadfront product 400 is shown with a speedometer 610 and a climate control 620. The deadfront product 400 has a leather grain pattern. FIG. 12 shows a substantially similar deadfront product 400 with a speedometer 610 and a climate control 620, but the deadfront product 400 has a wood grain pattern.

[0030] In certain embodiments, substrate 450 is treated (e.g., by sandblasting, etching, engraving, etc.) in the area of ​​the buttons to provide tactile feedback to a user's finger, allowing a user to feel the buttons of dead-front product 400 without taking their eyes off the road (in a road vehicle setting). Additionally, in embodiments, toggle switch 560 is provided with a delay, e.g., 1-3 seconds, to prevent accidental actuation of toggle switch 560.

[0031] FIG. 36 illustrates another embodiment of a dead-front product 400 with touch capabilities. In particular, the dead-front product 400 has a touch panel 660. The touch panel 660 can be any of a variety of suitable touch panels, such as a resistive touch panel, a capacitive (e.g., surface or raised) touch panel, a surface acoustic wave touch panel, an infrared touch panel, an optical imaging touch panel, a distributed signal touch panel, or an acoustic pulse recognition touch panel. In an embodiment, the touch panel 660 is laminated to the dead-front product 400 using an optically clear adhesive 540. In other embodiments, the touch panel 660 is printed on the dead-front product 400 such that an optically clear adhesive 540 is not required. Advantageously, the touch panel 660 is cold bendable to provide a three-dimensional shape. Cold bending of the dead-front product 400 (including the touch panel 660) is described in more detail further below.

[0032] Having generally described the structure of the deadfront product 400, attention is now directed to the semi-transparent layer 460 and the contrast layer 470. As discussed above, the semi-transparent layer 460 and the contrast layer 470 are disposed on the substrate 450. In an embodiment, the semi-transparent layer 460 is printed onto the substrate using a CMYK color model. In an embodiment where the contrast layer is not white, such as gray, the CMYK color model can also be used to print the contrast layer 470. In other embodiments where the contrast layer 470 is white, a color model including white ink can be used to print the contrast layer 470. The printed semi-transparent layer 460 and the printed contrast layer 470 each have a thickness between 1 μm and 6 μm. In an embodiment, the color layer 650 also has a thickness between 1 μm and 6 μm. In an embodiment, the contrast layer 470 has a thickness between 1 μm and 14 μm. Additionally, in an embodiment, the color layer 650 is printed onto the opaque layer 510 and / or the contrast layer 470. In one embodiment, the color layer 650 is printed onto the opaque layer 510 and / or the contrast layer 470 using the CMYK color model.

[0033] The inks used to print the semi-transparent layer 460, the contrast layer 470 and / or the color layer 650 can be heat curable or UV curable inks. In particular, the inks consist of at least one or more colorants and a vehicle. The colorants can be soluble or insoluble in the vehicle. In embodiments, the colorants are dry colorants in the form of fine powders. Such fine powders, in embodiments, have particles with sizes between 10 nm and 500 nm. Using the CMYK color model, the colorants provide the colors cyan, magenta, yellow and / or key (black). For white inks, the colorants can be any of a variety of suitable pigments, such as TiO2, Sb2O3, BaSO4, BaSO4:ZnS, ZnO and (PbCO3)2:Pb(OH)2. The colorants are dissolved or suspended in the vehicle.

[0034] The vehicle can function as a binder to provide adhesion to the surface to which the ink is applied. Additionally, in embodiments, additives are included in the vehicle to enhance adhesion, especially to glass / plastic surfaces. Non-limiting examples of vehicles for the colorant include propylene glycol monomethyl ether, diethylene glycol diethyl ether, dimethylacetamide, and toluene. Typically, such vehicles solidify at temperatures between 80° C. and 200° C. In embodiments, the ink includes 0.5% to 6% by volume of the colorant and 94% to 99.5% by volume of the vehicle.

[0035] As shown in Figures 13A and 13B, the leather grain semi-transparent layer 460 is printed on the substrate 450 using, among other things, an inkjet printer according to the CMYK color model (although in other embodiments, other printer types and / or printing models are used). In Figures 14A and 14B, a white contrast layer 470 is printed behind the semi-transparent layer 460. Figures 13B and 14B show the backside of these printed layers. As can be seen in a comparison of Figures 13A and 14A, the contrast of the leather grain pattern of the semi-transparent layer 460 is enhanced in Figure 14A by the white contrast layer 470. In fact, the use of the contrast layer 470 makes the overall appearance of the pattern or design in the semi-transparent layer 460 lighter and enhances the contrast between the colors in that pattern or design.

[0036] The thickness and composition of the contrast layer 470 can be tailored to exhibit a particular transmittance in the visible and infrared wavelength ranges. FIG. 15 shows a contrast layer 470 printed on a glass background. The contrast layer 470 has varying whiteness (W). "Whiteness" as used herein means CIE whiteness or ISO 11475:2004, which measures the amount of light reflected by a white surface across the visible spectrum (wavelengths 400 nm to 700 nm). In the lower left corner of FIG. 15 is a 100 W contrast layer. The whiteness of the contrast layer 470 decreases from left to right along the bottom row from 100 W to 60 W, and along the top row, the whiteness decreases from left to right from 50 W to 10 W. As can be seen, the relatively lower whiteness contrast layer 470 transmits more light than the relatively higher whiteness contrast layer 470. This is also demonstrated in the transmittance (T) graph in FIG. 16. As whiteness increases, the percent transmission (%T) across the visible spectrum decreases. The data to generate the graph of FIG. 16 was calculated after printing a white ink having a diethylene glycol diethyl ether solvent using 128 nozzles and a 40 pL printhead. The transmission (T) is controlled by manipulating the print resolution and layer thickness. In an embodiment, the deadfront product 400 is provided with a contrast layer 470 having a whiteness between 10W and 60W. In other embodiments, the contrast layer 470 has a whiteness between 20W and 50W. In a particular embodiment, the contrast layer 470 has a whiteness between 20W and 30W.

[0037] FIG. 17 shows four glass substrates 450 with a translucent layer 460 and a contrast layer 470 printed on the translucent layer 460. As seen in FIG. 17, the translucent layer 460 features a design of a knitted pattern, a leather grain pattern, and two wood grain patterns. FIG. 18 shows a translucent layer 460 that transitions from a leather grain pattern to a solid black pattern. In FIG. 18, a green power button is also printed in the lower left corner. FIG. 19 and FIG. 20 show a comparison between translucent layers 460 with the same knitted pattern. However, in FIG. 20, the contrast layer 470 is printed behind the translucent layer 460. In FIG. 20, the deadfront product 400 has a transmittance of 5% to 10% across the visible spectrum (wavelengths from 400 nm to 700 nm). FIG. 21 and FIG. 22 show a marble deadfront product 400. In particular, Figure 21 is the viewer's side of the deadfront product 400, while Figure 22 is the back side of the deadfront product 400. As can be seen in Figure 22, one section of the translucent layer 460 is not covered by the contrast layer 470. In an embodiment, a display can be attached to the section not covered by the contrast layer 470.

[0038] 23-27, various sizes, shapes, curvatures, glass materials, etc. for glass-based deadfront products are shown and described, along with various processes for forming the curved glass-based deadfront. For ease of explanation, FIGs. 23-27 are described with respect to a simplified curved deadfront product 2000, however, it should be understood that the deadfront product 2000 may be any of the deadfront embodiments described herein.

[0039] 23, in one or more embodiments, the deadfront product 2000 has a curved outer glass substrate 2010 having at least a first radius of curvature R1, and in various embodiments, the curved outer glass substrate 2010 is a compound curved sheet of glass material having at least one additional radius of curvature R1. In various embodiments, R1 ranges from about 60 mm to about 1500 mm.

[0040] The curved deadfront product 2000 has a deadfront color layer 2020 (e.g., an ink / pigment layer as described above) disposed along an inner major surface of a curved outer glass substrate 2010. Generally, the deadfront color layer 2020 is printed, colored, molded, etc. to provide a wood grain design, a leather grain design, a woven design, a brushed metal design, a graphic design, a solid color, and / or a logo. However, embodiments of the invention are not limited to these designs or patterns. The curved deadfront product 2000 may include any of the additional layers 2030 (e.g., high optical density layers, light guide layers, reflector layers, display modules, display stack layers, light sources, touch panels, etc.) that may be associated with a display or vehicle interior system as described above or herein.

[0041] As described in more detail below, in various embodiments, a curved dead-front product 2000 having a glass substrate 2010 and a colored layer 2020 may be cold-formed together into a curved shape, as shown in Figure 23. In some embodiments, a curved dead-front product 2000 having a glass substrate 2010, a colored layer 2020, and an additional layer 2030 may be cold-formed together into a curved shape, as in the dead-front product 2000 shown in Figure 23. In other embodiments, the glass substrate 2010 may be formed into a curved shape, and then the layers 2020 and 2030 may be provided after the curve forming.

[0042] Referring to Figure 24, there is shown the outer glass substrate 2010 prior to being formed into the curved shape shown in Figure 23. Generally, Applicant believes that the products and processes described herein provide high quality dead-front products utilizing glass in sizes, shapes, compositions, strengths, etc. not previously available.

[0043] As shown in FIG. 24, the outer glass substrate 2010 has a first major surface 2050 and a second major surface 2060 opposite the first major surface 2050. A minor or minor surface 2070 connects the first major surface 2050 and the second major surface 2060. The outer glass substrate 2010 has a thickness (t) that is substantially constant and defined as the distance between the first major surface 2050 and the second major surface 2060. In some embodiments, thickness (t) as used herein refers to the maximum thickness of the outer glass substrate 2010. The outer glass substrate 2010 has a width (W) defined as a first maximum dimension of one of the first or second major surfaces that is orthogonal to the thickness (t), and the outer glass substrate 2010 also has a length (L) defined as a second maximum dimension of one of the first or second surfaces that is orthogonal to both the thickness and the width. In other embodiments, the dimensions described herein are average dimensions.

[0044] In one or more embodiments, the outer glass substrate 2010 has a thickness (t) in the range of 0.05 mm to 2 mm. In various embodiments, the outer glass substrate 2010 has a thickness (t) of about 1.5 mm or less. For example, the thickness is about 0.1 mm to about 1.5 mm, about 0.15 mm to about 1.5 mm, about 0.2 mm to about 1.5 mm, about 0.25 mm to about 1.5 mm, about 0.3 mm to about 1.5 mm, about 0.35 mm to about 1.5 mm, about 0.4 mm to about 1.5 mm, about 0.45 mm ~1.5mm, 0.5mm~1.5mm, 0.55mm~1.5mm, 0.6mm~1.5mm, 0.65mm~1.5mm, 0.7mm~1.5mm, 0.1mm~1.4mm, 0.1mm~1.3mm, 0.1mm~1.5mm The range may be 1.2 mm, about 0.1 mm to about 1.1 mm, about 0.1 mm to about 1.05 mm, about 0.1 mm to about 1 mm, about 0.1 mm to about 0.95 mm, about 0.1 mm to about 0.9 mm, about 0.1 mm to about 0.85 mm, about 0.1 mm to about 0.8 mm, about 0.1 mm to about 0.75 mm, about 0.1 mm to about 0.7 mm, about 0.1 mm to about 0.65 mm, about 0.1 mm to about 0.6 mm, about 0.1 mm to about 0.55 mm, about 0.1 mm to about 0.5 mm, about 0.1 mm to about 0.4 mm, or about 0.3 mm to about 0.7 mm.

[0045] In one or more embodiments, the outer glass substrate 2010 has a width (W) in the range of about 5 cm to about 250 cm, about 10 cm to about 250 cm, about 15 cm to about 250 cm, about 20 cm to about 250 cm, about 25 cm to about 250 cm, about 30 cm to about 250 cm, about 35 cm to about 250 cm, about 40 cm to about 250 cm, about 45 cm to about 250 cm, about 50 cm to about 250 cm, about 55 cm to about 250 cm, about 60 cm to about 250 cm, about 65 cm to about 250 cm, about 70 cm to about 250 cm, about 75 cm to about 250 cm, about 80 cm to about 250 cm, about 85 cm to about 250 cm, about 90 cm to about 250 cm, about 95 cm to about 250 cm, about 100 cm to about 250 cm, about 110 cm to about 250 cm, about 120 cm to about 250 cm, about 130 cm to about 250 cm, about 140 cm to about 250 cm, about 150 cm to about 250 cm, about 5 cm to about 240 cm, about 5 cm to about 230 cm, about 5 cm to about 220 cm, about 5 cm to about 210 cm, about 5 cm to about 200 cm, about 5 cm to about 190 cm, about 5 cm to about 180 cm, about 5 cm to about 170 cm, about 5 cm to about 160 cm, about 5 cm to about 150 cm, about 5 cm to about 140 cm, about 5 cm to about 130 cm, about 5 cm to about 120 cm, about 5 cm to about 110 cm, about 5 cm to about 100 cm, about 5 cm to about 90 cm, about 5 cm to about 80 cm or about 5 cm to about 75 cm.

[0046] In one or more embodiments, the outer glass substrate 2010 has a thickness of about 5 cm to about 250 cm, about 10 cm to about 250 cm, about 15 cm to about 250 cm, about 20 cm to about 250 cm, about 25 cm to about 250 cm, about 30 cm to about 250 cm, about 35 cm to about 250 cm, about 40 cm to about 250 cm, about 45 cm to about 250 cm, about 50 cm to about 250 cm, about 55 cm to about 250 cm, about 60 cm to about 250 cm, about 65 cm to about 250 cm, about 70 cm to about 250 cm, about 75 cm to about 250 cm, about 80 cm to about 250 cm, about 85 cm to about 250 cm, about 90 cm to about 250 cm, about 95 cm to about 250 cm, about 100 cm to about 250 cm, about 110 cm to about 250 cm, about 120 cm to about 250 cm, about 130 cm to about 250 cm, about 140 cm to about 250 cm, about 150 cm to about 250 cm, about 160 cm to about 250 cm, about 170 cm to about 250 cm, about 180 cm to about 250 cm, about 190 cm to about 250 cm, about 200 cm to about 250 cm, about 210 cm to about 250 cm, about 220 cm to about 250 cm, about 230 cm to about 250 cm, about 240 cm to about 250 cm, about 250 cm to about 250 cm, about 260 cm to about 250 cm, about 260 cm to about m ~ about 250cm, about 120cm - about 250cm, about 130cm - about 250cm, about 140cm - about 250cm, about 150cm - about 250cm, about 5cm - about 24 0cm, about 5cm to about 230cm, about 5cm to about 220cm, about 5cm to about 210cm, about 5cm to about 200cm, about 5cm to about 190cm, about 5cm to about 180 cm, about 5cm to about 170cm, about 5cm to about 160cm, about 5cm to about 150cm, about 5cm to about 140cm, about 5cm to about 130cm, about 5cm to about 120cm m, has a length (L) in the range of about 5 cm to about 110 cm, about 5 cm to about 100 cm, about 5 cm to about 90 cm, about 5 cm to about 80 cm, or about 5 cm to about 75 cm.

[0047] 23, the outer glass substrate 2010 is formed into a curved shape having at least one radius of curvature shown as R1. In various embodiments, the outer glass substrate 2010 may be formed into the curved shape by any suitable process, including cold forming and hot forming.

[0048] In certain embodiments, the outer glass substrate 2010 is formed into the curved shape shown in FIG. 23 by a cold forming process, either alone or following attachment of layers 2020 and 2030. As used herein, the phrases "cold bent," "cold bending," "cold formed," or "cold forming" refer to curving a glass substrate at a cold forming temperature below the softening point of the glass (as described herein). A cold formed glass substrate is characterized by asymmetric surface compression between the first major surface 2050 and the second major surface 2060. In some embodiments, prior to the cold forming process or prior to being cold formed, the respective compressive stresses at the first major surface 2050 and the second major surface 2060 are substantially equal.

[0049] In some such embodiments in which the outer glass substrate 2010 is not strengthened, the first major surface 2050 and the second major surface 2060 exhibit no appreciable compressive stress prior to cold forming. In some such embodiments in which the outer glass substrate 2010 is strengthened (as described herein), the first major surface 2050 and the second major surface 2060 exhibit substantially equal compressive stresses relative to one another prior to cold forming. In one or more embodiments, after cold forming (e.g., as shown in FIG. 23 ), the compressive stress at the second major surface 2060 (e.g., the concave surface after bending) increases (i.e., the compressive stress at the second major surface 2060 is greater after cold forming than before cold forming).

[0050] Without being bound by theory, the cold forming process increases the compressive stress of the formed glass substrate to counteract the tensile stress imparted during the bending and / or forming operations. In one or more embodiments, the cold forming process causes the first major surface 2050 (e.g., the convex surface after bending) to experience tensile stress while the second major surface 2060 experiences compressive stress. The tensile stresses experienced at surface 2050 after bending result in a net reduction in surface compressive stress such that the compressive stress at surface 2050 of the strengthened glass sheet after bending is less than the compressive stress at surface 2050 when the glass sheet is flat.

[0051] Furthermore, if a strengthened glass substrate is utilized for the outer glass substrate 2010, the first and second major surfaces (2050, 2060) are already under compressive stress, and therefore the first major surface 2050 can develop greater tensile stresses during bending without risk of cracking. This allows the strengthened embodiment of the outer glass substrate 2010 to conform to more curved surfaces (e.g., molded to have a smaller R1 value).

[0052] In various embodiments, the thickness of the outer glass substrate 2010 is adjusted to allow the outer glass substrate 2010 to be more flexible to achieve the desired radius of curvature. Additionally, a thinner outer glass substrate 2010 may deform more easily, which can potentially counteract mismatches and gaps that may be caused by the shape of the supports or frame (as described below). In one or more embodiments, the thin and strengthened outer glass substrate 2010 exhibits greater flexibility, especially during cold forming. The greater flexibility of the glass substrates described herein may enable consistent bending without heating.

[0053] In various embodiments, the outer glass substrate 2010 (and the resulting dead-front product 2000) may have a compound curvature that includes a large radius and a lateral curvature. The complexly curved cold-formed outer glass substrate 2010 may have separate radii of curvature in two independent directions. Thus, in one or more embodiments, the complexly curved cold-formed outer glass substrate 2010 may be characterized as having a "lateral curvature," where the cold-formed outer glass substrate 2010 is curved along an axis parallel to any dimension (i.e., a first axis) and also curved along an axis perpendicular to the same dimension (i.e., a second axis). The curvature of the cold-formed outer glass substrate 2010 can become even more complex when a significant minimum radius is combined with a significant lateral curvature and / or a bend depth.

[0054] Referring to FIG. 25, a display assembly 2100 according to one exemplary embodiment is shown. In the illustrated embodiment, the display assembly 2100 has a frame 2110 that supports (directly or indirectly) both a light source, shown as a display module 2120, and a dead-front product 2000. As shown in FIG. 25, the dead-front product 2000 and the display module 2120 are coupled to the frame 2110, and the display module 2120 is positioned so that a user can view the light, images, etc. generated by the display module 2120 through the dead-front product 2000. In various embodiments, the frame 2110 may be formed from various materials, such as plastics (such as PC / ABS), metals (such as Al alloys, Mg alloys, Fe alloys, etc.). Various processes, such as casting, cutting, stamping, injection molding, etc., may be utilized to form the curved shape of the frame 2110. 25 shows a light source in the form of a display module, it should be understood that the display assembly 2100 may include any of the light sources described herein for generating graphics, icons, images, displays, etc. according to any of the dead-front embodiments described herein. Additionally, while the frame 2110 is shown as a frame associated with a display assembly, the frame 2110 may be any support or frame product associated with a vehicle interior system.

[0055] In various embodiments, the systems and methods described herein allow for shaping of the deadfront product 2000 to conform to a wide variety of curved shapes that the frame 2110 may have. As shown in FIG. 25, the frame 2110 has a support surface 2130 that has a curved shape, and the deadfront product 2000 is shaped to match the curved shape of the support surface 2130. As will be appreciated, the deadfront product 2000 may be shaped in a wide variety of shapes to match a desired frame shape of the display assembly 2100, which itself may be shaped to fit the shape of a portion of a vehicle interior system, as described herein.

[0056] In one or more embodiments, the dead-front structure 2000 (and particularly the outer glass substrate 2010) is shaped to have a first radius of curvature R1 of about 60 mm or more. For example, R1 can be from about 60 mm to about 1500 mm, from about 70 mm to about 1500 mm, from about 80 mm to about 1500 mm, from about 90 mm to about 1500 mm, from about 100 mm to about 1500 mm, from about 120 mm to about 1500 mm, from about 140 mm to about 1500 mm, from about 150 mm to about 1500 mm, from about 160 mm to about 1500 mm, from about 180 mm to about 1500 mm, from about 200 mm to about 1500 mm, from about 220 mm to about 1500 mm, from about 240 mm to about 1500 mm, or from about 260 mm to about 1500 mm. 00mm, about 250mm to about 1500mm, about 260mm to about 1500mm, about 270mm to about 1500mm, about 280mm to about 1500mm, about 290mm to about 1500mm, about 300mm to about 1500mm, about 3 50mm to about 1500mm, about 400mm to about 1500mm, about 450mm to about 1500mm, about 500mm to about 1500mm, about 550mm to about 1500mm, about 600mm to about 1500mm, about 650mm to about 15 00mm, approximately 700mm to approximately 1500mm, approximately 750mm to approximately 1500mm, approximately 800mm to approximately 1500mm, approximately 900mm to approximately 1500mm, approximately 950mm to approximately 1500mm, approximately 1000mm to approximately 1500mm, approximately 1250mm~1500mm, 60mm~1400mm, 60mm~1300mm, 60mm~1200mm, 60mm~1100mm, 60mm~1000mm, 60mm~950mm , about 60 mm to about 900 mm, about 60 mm to about 850 mm, about 60 mm to about 800 mm, about 60 mm to about 750 mm, about 60 mm to about 700 mm, about 60 mm to about 650 mm, about 60 mm to about 600 mm, about 60 mm to about 550 mm, about 60 mm to about 500 mm, about 60 mm to about 450 mm, about 60 mm to about 400 mm, about 60 mm to about 350 mm, about 60 mm to about 300 mm, or about 60 mm to about 250 mm.

[0057] In one or more embodiments, the support surface 2130 has a second radius of curvature of about 60 mm or more. For example, the second radius of curvature of the support surface 2130 can be about 60 mm to about 1500 mm, about 70 mm to about 1500 mm, about 80 mm to about 1500 mm, about 90 mm to about 1500 mm, about 100 mm to about 1500 mm, about 120 mm to about 1500 mm, about 140 mm to about 1500 mm, about 150 mm to about 1500 mm, about 160 mm to about 1500 mm, about 180 mm to about 1500 mm, about 200 mm to about 1500 mm, about 220 mm to about 1500 mm, Approximately 240mm to approximately 1500mm, approximately 250mm to approximately 1500mm, approximately 260mm to approximately 1500mm, approximately 270mm to approximately 1500mm, approximately 280mm to approximately 1500mm, approximately 290mm to approximately 1500mm, approximately 300mm to approximately 1 500mm, about 350mm to about 1500mm, about 400mm to about 1500mm, about 450mm to about 1500mm, about 500mm to about 1500mm, about 550mm to about 1500mm, about 600mm to about 1500mm, about 65 0mm~1500mm, 700mm~1500mm, 750mm~1500mm, 800mm~1500mm, 900mm~1500mm, 950mm~1500mm, 1000mm~150 0mm, about 1250mm to about 1500mm, about 60mm to about 1400mm, about 60mm to about 1300mm, about 60mm to about 1200mm, about 60mm to about 1100mm, about 60mm to about 1000mm, about 60mm to about 95 The range may be about 60 mm, about 60 mm to about 900 mm, about 60 mm to about 850 mm, about 60 mm to about 800 mm, about 60 mm to about 750 mm, about 60 mm to about 700 mm, about 60 mm to about 650 mm, about 60 mm to about 600 mm, about 60 mm to about 550 mm, about 60 mm to about 500 mm, about 60 mm to about 450 mm, about 60 mm to about 400 mm, about 60 mm to about 350 mm, about 60 mm to about 300 mm, or about 60 mm to about 250 mm.

[0058] In one or more embodiments, the dead-front structure 2000 is cold-formed to have a first radius of curvature R1 that is within 10% (e.g., about 10% or less, about 9% or less, about 8% or less, about 7% or less, about 6% or less, or about 5% or less) of the second radius of curvature of the support surface 2130 of the frame 2110. For example, the support surface 2130 of the frame 2110 has a radius of curvature of 1000 mm and the dead-front product 2000 is cold-formed to have a radius of curvature in the range of about 900 mm to about 1100 mm.

[0059] In one or more embodiments, the first major surface 2050 and / or the second major surface 2060 of the glass substrate 2010 have a functional coating layer as described herein. The functional coating layer may cover at least a portion of the first major surface 2050 and / or the second major surface 2060. Exemplary functional coatings include at least one of a glare reducing coating or surface, an anti-glare coating or surface, a scratch resistant coating, an anti-reflective coating, a half mirror coating, or an easy to clean coating.

[0060] 26, a method 2200 of forming a display assembly having a cold-formed dead-front product, such as dead-front product 2000, is shown. In step 2210, the method includes curving a dead-front product, such as dead-front product 2000, to a curved surface of a support. Generally, the support may be a frame of a display, such as frame 2110 that defines a curved shape around a vehicle display. Generally, the frame has a curved support surface, and one of the major surfaces 2050 and 2060 of the dead-front product 2000 is placed in contact with the curved support surface.

[0061] In step 2220, the method includes fixing the curved dead-front product to the support while bending the dead-front product to conform (or match) to the curved surface of the support. In this form, the curved dead-front product 2000 shown in FIG. 23 is formed from a generally flat dead-front product into a curved dead-front product. In this arrangement, bending the flat dead-front product forms a curved shape on the major surface facing the support, while also forming a corresponding (but complementary) curvature on the opposing major surface of the frame. Applicant believes that by bending the dead-front product directly in the curved frame, the need for a separate curved mold or die (which is typically required in other glass bending processes) is eliminated. Furthermore, Applicant believes that by forming the dead-front product directly into the curved frame, a wide range of curved radii may be achieved in a less complex manufacturing process.

[0062] In some embodiments, the force applied in step 2210 and / or step 2220 may be air pressure applied by a vacuum fixture. In some other embodiments, the air pressure differential is created by providing a vacuum to an airtight enclosure surrounding the frame and the dead-front product. In certain embodiments, the airtight enclosure is a flexible polymeric shell, such as a plastic bag or pouch. In other embodiments, the air pressure differential is created by creating increased air pressure around the dead-front product and frame by an overpressure device, such as an autoclave. Applicant has further found that air pressure provides a consistent and highly uniform bending force (compared to contact-based bending methods), which further translates to an error-free manufacturing process. In various embodiments, the air pressure difference is between 0.5 and 1.5 standard atmospheres (atm) (506.625 and 1519.88 hPa), particularly between 0.7 and 1.1 atm (709.275 and 1114.58 hPa), and more particularly between 0.8 and 1 atm (810.6 and 1013.25 hPa).

[0063] In step 2230, the temperature of the dead-front product is maintained below the glass transition temperature of the material of the outer glass layer between steps 2210 and 2220. Thus, method 2200 is a cold forming or cold bending process. In certain embodiments, the temperature of the dead-front product is maintained below 500° C., 400° C., 300° C., 200° C., or 100° C. In certain embodiments, the dead-front product is maintained at or below room temperature during bending. In certain embodiments, the dead-front product is not actively heated by heating elements, furnaces, ovens, etc. during bending, as is the case when hot forming glass into a curved shape.

[0064] In addition to providing processing advantages such as the elimination of expensive and / or slow heating steps as discussed above, it is believed that the cold forming processes described herein provide curved dead-front products with various properties believed to be superior to those achievable by hot forming processes. For example, Applicants believe that, for at least some glass materials, heating during the hot forming process degrades the optical properties of the curved glass substrate, such that curved glass-based dead-front products formed utilizing the cold bending processes / systems described herein provide both curved glass shapes and improved optical qualities that are believed not achievable by hot bending processes.

[0065] Furthermore, many materials used for the various coatings and layers (e.g., easy-clean coatings, anti-reflective coatings, etc.) are applied by deposition processes such as sputtering processes that are generally less suitable for coating on curved surfaces. In addition, many coating materials, such as dead-front ink / pigment materials, also cannot withstand the high temperatures associated with hot bending processes. Thus, in certain embodiments described herein, layer 2020 is applied to the outer glass substrate 2010 prior to cold bending. Thus, applicants believe that the processes and systems described herein perform the bending of the glass after one or more coating materials have been applied to the glass, as opposed to typical hot forming processes.

[0066] In step 2220, the curved dead-front product is attached or secured to the curved support. In various embodiments, the attachment between the curved dead-front product and the curved support may be via an adhesive material. Such adhesive may include any suitable optically clear adhesive for bonding the dead-front product in a predetermined position relative to a display assembly (e.g., a frame of a display). In one example, the adhesive may include an optically clear adhesive sold by 3M Corporation under the trade designation 8215. The thickness of the adhesive may range from about 200 μm to about 500 μm.

[0067] The adhesive material may be applied in a variety of ways. In one embodiment, the adhesive is applied using an applicator gun and leveled using a roller or drawdown die. In various embodiments, the adhesives described herein are structural adhesives. In certain embodiments, the structural adhesive may include an adhesive selected from one or more of the following categories: (a) toughened epoxy (Masterbond EP21TDCHT-LO, 3M Scotch Weld Epoxy DP460 Off-white), (b) flexible epoxy (Masterbond EP21TDC-2LO, 3M Scotch Weld Epoxy 2216 B / A Gray), (c) acrylic (LORD Adhesive 410 / Accelerator 19 w / LORD AP 134 primer, LORD Adhesive 852 / LORD Accelerator 25GB, Loctite HF 8000, Loctite AA4800), (d) urethane (3M Scotch Weld Urethane DP640 Brown), and (e) silicone (Dow Corning 995). In some cases, structural glues available in sheet format, such as (B-stage epoxy adhesives), may be utilized. Additionally, a pressure sensitive structural adhesive such as 3M VHB tape may be utilized. In such an embodiment, by utilizing a pressure sensitive adhesive, the curved dead front product is bonded to the frame without the need for a curing step.

[0068] In one or more embodiments, the method includes a step 2240 of securing the curved dead-front product to the display. In one or more embodiments, the method may include securing the display to the dead-front product before step 2210 and curving both the display and the dead-front product in step 2210. In one or more embodiments, the method includes placing or assembling the curved dead-front product and the display in the vehicle interior system 100, 200, 300.

[0069] Referring to FIG. 27, a method 2300 of forming a display utilizing a curved dead-front product is shown and described. In some embodiments, the substrate of the dead-front product (e.g., outer glass layer 2010) is formed into a curved shape in step 2310. The forming in step 2310 may be cold forming or hot forming. In step 2320, a dead-front ink / pigment layer (e.g., layer 2020) is applied to the substrate after forming to provide a curved dead-front product. Then, in step 2330, the curved dead-front product is attached to a frame, such as frame 2110 of display assembly 2100 or other frame that may be associated with a vehicle interior system.

[0070] Substrate Material The various substrates of the deadfront products described herein may be formed from any transparent material, such as a polymer (e.g., PMMA, polycarbonate, etc.) or glass. Suitable glass compositions include soda-lime glass, aluminosilicate glass, borosilicate glass, boroaluminosilicate glass, alkali-containing aluminosilicate glass, alkali-containing borosilicate glass, and alkali-containing boroaluminosilicate glass.

[0071] Unless otherwise specified, the glass compositions disclosed herein are listed in mole percent (mol %) analyzed on an oxide basis.

[0072] In one or more embodiments, the glass composition may include SiO in an amount ranging from about 66 mol% to about 80 mol%, about 67 mol% to about 80 mol%, about 68 mol% to about 80 mol%, about 69 mol% to about 80 mol%, about 70 mol% to about 80 mol%, about 72 mol% to about 80 mol%, about 65 mol% to about 78 mol%, about 65 mol% to about 76 mol%, about 65 mol% to about 75 mol%, about 65 mol% to about 74 mol%, about 65 mol% to about 72 mol%, or about 65 mol% to about 70 mol%, and all ranges and subranges therebetween.

[0073] In one or more embodiments, the glass composition includes Al2O3 in an amount greater than about 4 mol% or greater than about 5 mol%. In one or more embodiments, the glass composition includes Al2O3 in an amount greater than about 7 mol% to about 15 mol%, greater than about 7 mol% to about 14 mol%, about 7 mol% to about 13 mol%, about 4 mol% to about 12 mol%, about 7 mol% to about 11 mol%, about 8 mol% to about 15 mol%, about 9 mol% to about 15 mol%, about 10 mol% to about 15 mol%, about 11 mol% to about 15 mol%, or about 12 mol% to about 15 mol%, and all ranges and subranges therebetween. In one or more embodiments, the upper limit of Al2O3 may be about 14 mol%, 14.2 mol%, 14.4 mol%, 14.6 mol%, or 14.8 mol%.

[0074] In one or more embodiments, the glass layer herein is described as an aluminosilicate glass product or has an aluminosilicate glass composition. In such embodiments, the glass composition or products formed therefrom include SiO2 and Al2O3 and are not soda-lime silicate glass. In this regard, the glass composition or products formed therefrom include Al2O3 in an amount of about 2 mol% or more, 2.25 mol% or more, 2.5 mol% or more, about 2.75 mol% or more, or about 3 mol% or more.

[0075] In one or more embodiments, the glass composition includes B2O3 (e.g., about 0.01 mol% or more). In one or more embodiments, the glass composition includes B2O3 in an amount ranging from about 0 mol% to about 5 mol%, from about 0 mol% to about 4 mol%, from about 0 mol% to about 3 mol%, from about 0 mol% to about 2 mol%, from about 0 mol% to about 1 mol%, from about 0 mol% to about 0.5 mol%, from about 0.1 mol% to about 5 mol%, from about 0.1 mol% to about 4 mol%, from about 0.1 mol% to about 3 mol%, from about 0.1 mol% to about 2 mol%, from about 0.1 mol% to about 1 mol%, from about 0.1 mol% to about 0.5 mol%, and all ranges and subranges therebetween. In one or more embodiments, the glass composition is substantially free of B2O3.

[0076] As used herein, the phrase "substantially free" with respect to a component of a composition means that the component is not actively or intentionally added to the composition during initial batch processing, but may be present as an impurity in an amount less than about 0.001 mole percent.

[0077] In one or more embodiments, the glass composition optionally includes P2O5 (e.g., about 0.01 mol% or more). In one or more embodiments, the glass composition includes a non-zero amount of P2O5 up to and including 2 mol%, 1.5 mol%, 1 mol%, or 0.5 mol%. In one or more embodiments, the glass composition is substantially free of P2O5.

[0078] In one or more embodiments, the glass composition may include a total amount of RO (which is the total amount of alkali metal oxides, such as Li2O, Na2O, KO, Rb2O, and Cs2O) of about 8 mol% or more, about 10 mol% or more, or about 12 mol% or more. In some embodiments, the glass composition includes a total amount of RO in the range of about 8 mol% to about 20 mol%, about 8 mol% to about 18 mol%, about 8 mol% to about 16 mol%, about 8 mol% to about 14 mol%, about 8 mol% to about 12 mol%, about 9 mol% to about 20 mol%, about 10 mol% to about 20 mol%, about 11 mol% to about 20 mol%, about 12 mol% to about 20 mol%, about 13 mol% to about 20 mol%, about 10 mol% to about 14 mol%, or about 11 mol% to about 13 mol%, and all ranges and subranges therebetween. In one or more embodiments, the glass composition may be substantially free of Rb2O, Cs2O, or both Rb2O and Cs2O. In one or more embodiments, R2O may include a combined amount of only Li2O, Na2O, and K2O. In one or more embodiments, the glass composition may include at least one alkali metal oxide selected from Li2O, Na2O, and K2O, where the alkali metal oxide is present in an amount of about 8 mol % or greater.

[0079] In one or more embodiments, the glass composition includes Na2O in an amount of about 8 mol% or more, about 10 mol% or more, or about 12 mol% or more. In one or more embodiments, the composition includes Na2O in an amount of about 8 mol% to about 20 mol%, about 8 mol% to about 18 mol%, about 8 mol% to about 16 mol%, about 8 mol% to about 14 mol%, about 8 mol% to about 12 mol%, about 9 mol% to about 20 mol%, about 10 mol% to about 20 mol%, about 11 mol% to about 20 mol%, about 12 mol% to about 20 mol%, about 13 mol% to about 20 mol%, about 10 mol% to about 14 mol%, or about 11 mol% to about 16 mol% and all ranges and subranges therebetween.

[0080] In one or more embodiments, the glass composition includes less than about 4 mol% K2O, less than about 3 mol% K2O, or less than about 1 mol% K2O. In some examples, the glass composition may include KO in an amount ranging from about 0 mol% to about 4 mol%, from about 0 mol% to about 3.5 mol%, from about 0 mol% to about 3 mol%, from about 0 mol% to about 2.5 mol%, from about 0 mol% to about 2 mol%, from about 0 mol% to about 1.5 mol%, from about 0 mol% to about 1 mol%, from about 0 mol% to about 0.5 mol%, from about 0 mol% to about 0.2 mol%, from about 0 mol% to about 0.1 mol%, from about 0.5 mol% to about 4 mol%, from about 0.5 mol% to about 3.5 mol%, from about 0.5 mol% to about 3 mol%, from about 0.5 mol% to about 2.5 mol%, from about 0.5 mol% to about 2 mol%, from about 0.5 mol% to about 1.5 mol%, or from about 0.5 mol% to about 1 mol%, and all ranges and subranges therebetween. In one or more embodiments, the glass composition may be substantially free of K2O.

[0081] In one or more embodiments, the glass composition is substantially free of Li2O. In one or more embodiments, the amount of Na2O in the composition may be greater than the amount of Li2O. In some instances, the amount of Na2O may be greater than the combined amount of Li2O and K2O. In one or more alternative embodiments, the amount of Li2O in the composition may be greater than the amount of Na2O or the combined amount of Na2O and K2O.

[0082] In one or more embodiments, the glass composition may include a total amount of RO (the total amount of alkaline earth metal oxides, such as CaO, MgO, BaO, ZnO, and SrO) ranging from about 0 mol% to about 2 mol%. In some embodiments, the glass composition includes a non-zero amount of RO up to about 2 mol%. In one or more embodiments, the glass composition includes an amount of RO in an amount of about 0 mol% to about 1.8 mol%, about 0 mol% to about 1.6 mol%, about 0 mol% to about 1.5 mol%, about 0 mol% to about 1.4 mol%, about 0 mol% to about 1.2 mol%, about 0 mol% to about 1 mol%, about 0 mol% to about 0.8 mol%, about 0 mol% to about 0.5 mol%, and all ranges and subranges therebetween.

[0083] In one or more embodiments, the glass composition includes CaO in an amount less than about 1 mol%, less than about 0.8 mol%, or less than about 0.5 mol%. In one or more embodiments, the glass composition is substantially free of CaO.

[0084] In some embodiments, the glass composition includes MgO in an amount between about 0 mol% and about 7 mol%, between about 0 mol% and about 6 mol%, between about 0 mol% and about 5 mol%, between about 0 mol% and about 4 mol%, between about 0.1 mol% and about 7 mol%, between about 0.1 mol% and about 6 mol%, between about 0.1 mol% and about 5 mol%, between about 0.1 mol% and about 4 mol%, between about 1 mol% and about 7 mol%, between about 2 mol% and about 6 mol%, or between about 3 mol% and about 6 mol%, and all ranges and subranges therebetween.

[0085] In one or more embodiments, the glass composition includes ZrO2 in an amount of about 0.2 mol% or less, less than about 0.18 mol%, less than about 0.16 mol%, less than about 0.15 mol%, less than about 0.14 mol%, or less than about 0.12 mol%. In one or more embodiments, the glass composition includes ZrO2 in an amount of about 0.01 mol% to about 0.2 mol%, about 0.01 mol% to about 0.18 mol%, about 0.01 mol% to about 0.16 mol%, about 0.01 mol% to about 0.15 mol%, about 0.01 mol% to about 0.14 mol%, about 0.01 mol% to about 0.12 mol%, or about 0.01 mol% to about 0.10 mol%, and all ranges and subranges therebetween.

[0086] In one or more embodiments, the glass composition includes SnO2 in an amount of about 0.2 mol% or less, less than about 0.18 mol%, less than about 0.16 mol%, less than about 0.15 mol%, less than about 0.14 mol%, or less than about 0.12 mol%. In one or more embodiments, the glass composition includes SnO2 in an amount of about 0.01 mol% to about 0.2 mol%, about 0.01 mol% to about 0.18 mol%, about 0.01 mol% to about 0.16 mol%, about 0.01 mol% to about 0.15 mol%, about 0.01 mol% to about 0.14 mol%, about 0.01 mol% to about 0.12 mol%, or about 0.01 mol% to about 0.10 mol%, and all ranges and subranges therebetween.

[0087] In one or more embodiments, the glass composition may include oxides that provide color or tint to the glass product. In some embodiments, the glass composition includes oxides that prevent discoloration of the glass product when the glass product is exposed to ultraviolet radiation. Examples of such oxides include, without limitation, oxides of Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Ce, W, and Mo.

[0088] In one or more embodiments, the glass composition includes Fe, expressed as Fe2O3, where Fe is present in an amount up to and including about 1 mol%. In some embodiments, the glass composition is substantially free of Fe. In one or more embodiments, the glass composition includes Fe2O3 in an amount of about 0.2 mol% or less, less than about 0.18 mol%, less than about 0.16 mol%, less than about 0.15 mol%, less than about 0.14 mol%, or less than about 0.12 mol%. In one or more embodiments, the glass composition includes Fe2O3 in the range of about 0.01 mol % to about 0.2 mol %, about 0.01 mol % to about 0.18 mol %, about 0.01 mol % to about 0.16 mol %, about 0.01 mol % to about 0.15 mol %, about 0.01 mol % to about 0.14 mol %, about 0.01 mol % to about 0.12 mol %, or about 0.01 mol % to about 0.10 mol %, and all ranges and subranges therebetween.

[0089] If the glass composition includes TiO2, it may be present in an amount of about 5 mol% or less, about 2.5 mol% or less, about 2 mol% or less, or about 1 mol% or less. In one or more embodiments, the glass composition may be substantially free of TiO2.

[0090] A typical glass composition includes SiO2 in an amount ranging from about 65 mol% to about 75 mol%, Al2O3 in an amount ranging from about 8 mol% to about 14 mol%, Na2O in an amount ranging from about 12 mol% to about 17 mol%, K2O in an amount ranging from about 0 mol% to about 0.2 mol%, and MgO in an amount ranging from about 1.5 mol% to about 6 mol%. Optionally, SnO2 may be included in amounts otherwise disclosed herein.

[0091] Reinforced substrate In one or more embodiments, the substrate comprises any of the glass materials of the dead front product embodiments described herein (such as the outer glass substrate 2010 or other glass substrates). In one or more embodiments, such glass substrates may be strengthened. In one or more embodiments, the glass substrate may be strengthened to have compressive stresses extending from the surface to a depth of compression (DOC). The compressive stress areas are balanced by a central portion having tensile stresses. At the DOC, the stress changes from positive (compressive) to negative (tensile).

[0092] In one or more embodiments, the glass substrates used in the deadfront products described herein may be mechanically strengthened by taking advantage of the mismatch in thermal expansion coefficients between portions of the glass to create regions of compressive stress and a central region with tensile stress. In some embodiments, the glass substrate may be thermally strengthened by heating the glass to a temperature above the glass transition temperature and then rapidly quenching.

[0093] In one or more embodiments, the glass substrates used in the deadfront products described herein may be chemically strengthened by ion exchange. In an ion exchange process, ions at or near the surface of the glass substrate are replaced or exchanged with larger ions having the same valence or oxidation state. In embodiments where the glass substrate comprises an alkali aluminosilicate glass or a soda-lime silicate glass, the ions in the surface layer of the product and the larger ions are Li + , Na + , K + , Rb + and Cs + Alternatively, the monovalent cation in the surface layer is Ag + In such embodiments, the monovalent ions (or cations) exchanged into the glass substrate may be replaced with monovalent cations other than alkali metal cations, such as: In such embodiments, the monovalent ions (or cations) exchanged into the glass substrate create stress.

[0094] The ion exchange process is typically carried out by immersing the glass substrate in a molten salt bath (or two or more molten salt baths) containing the larger ions to be exchanged for the smaller ions in the glass substrate. It should be noted that aqueous salt baths may be utilized. In addition, the composition of the bath may contain two or more types of larger ions (e.g., Na + and K. + ) or one larger ion. It will be understood by those skilled in the art that the parameters for the ion exchange process, including but not limited to bath composition and temperature, immersion time, number of immersions of the glass substrate in the salt bath (or baths), use of multiple salt baths, additional steps such as annealing, washing, etc., are generally determined by the composition of the glass substrate (including the structure of the substrate and any crystalline phases present) and the desired DOC and CS of the substrate resulting from the strengthening.

[0095] Typical molten bath compositions may include nitrates, sulfates, and chlorides of larger alkali metal ions. Typical nitrates include KNO3, NaNO3, LiNO3, NaSO4, and combinations thereof. The temperature of the molten salt bath typically ranges from about 380°C to about 450°C, while immersion times range from about 15 minutes to about 100 hours depending on the glass thickness, bath temperature, and glass (or monovalent ion) diffusivity. However, temperatures and immersion times different from those mentioned above may be utilized.

[0096] In one or more embodiments, the glass substrate used in the deadfront product may be immersed in a molten salt bath of 100% NaNO3, 100% KNO3, or a combination of NaNO3 and KNO3 having a temperature of about 370°C to about 480°C. In some embodiments, the glass substrate of the deadfront product may be immersed in a mixed molten salt bath including about 5% to about 90% KNO3 and about 10% to about 95% NaNO3. In one or more embodiments, the glass substrate may be immersed in a second bath after immersion in the first bath. The first and second baths may have different compositions and / or temperatures from each other. The immersion times in the first and second baths may be different. For example, the immersion in the first bath may be longer than the immersion in the second bath.

[0097] In one or more embodiments, the glass substrate used to form the dead-front product may be immersed in a mixed molten salt bath including NaNO3 and KNO3 (e.g., 49% / 51%, 50% / 50%, 51% / 49%) having a temperature of less than about 420°C (e.g., about 400°C or about 380°C) for less than about 5 hours or even less than about 4 hours.

[0098] The ion exchange conditions can be adjusted to provide a "spike" or increase the gradient of the stress distribution at or near the surface of the resulting glass substrate of the dead front product. The spike can result in a larger surface CS value. This spike can be achieved with one bath or multiple baths, with one composition or mixed compositions, due to the unique properties of the glass compositions used in the glass substrate of the dead front product described herein.

[0099] In one or more embodiments, when two or more monovalent ions are exchanged into a glass substrate used in a dead-front product, different monovalent ions may be exchanged to different depths within the glass substrate (and may produce different amounts of stress within the glass substrate at different depths). The resulting relative depths of the stress-producing ions can be determined, which can result in different characteristics of the stress distribution.

[0100] CS is measured using means known in the art, such as by a surface stress meter (FSM) using commercially available equipment, such as the FSM-6000 manufactured by Orihara Industrial Co., Ltd. (Japan). Surface stress measurement relies on accurate measurement of the stress optical coefficient (SOC), which is related to the birefringence of the glass. SOC itself is measured by methods known in the art, such as the fiber and four-point bending methods, both of which are described in ASTM standard C770-98 (2013), entitled "Standard Test Method for Measurement of Glass Stress-Optical Coefficient," the entire contents of which are incorporated herein by reference, and also by the bulk cylinder method. As used herein, CS may be the "maximum compressive stress," which is the highest compressive stress value measured within the compressive stress layer. In some embodiments, the maximum compressive stress is present at the surface of the glass substrate. In other embodiments, the maximum compressive stress may occur at a predetermined depth within the surface, giving the appearance of a "buried peak" in the compression distribution.

[0101] DOC may be measured by FSM or by a scattered light polariscope (SCALP) (such as a SCALP-04 scattered light polariscope available from Glasstress Ltd., Tallinn, Estonia) depending on the strengthening method and conditions. If the glass substrate is chemically strengthened by an ion exchange process, FSM or SCALP may be used depending on which ions are exchanged into the glass substrate. If stress in the glass substrate is induced by exchanging potassium ions into the glass substrate, FSM is used to measure the DOC. If stress is induced by exchanging sodium ions into the glass substrate, SCALP is used to measure the DOC. If stress in the glass substrate is induced by exchanging both potassium and sodium ions into the glass, DOC is measured by SCALP. Because it is believed that the exchange depth of sodium indicates DOC, and the exchange depth of potassium ions indicates the change in the magnitude of compressive stress (but not the change in stress from compressive to tensile). The exchange depth of potassium ions in such glass substrates is measured by FSM. Central tension or CT is the maximum tensile stress and is measured by SCALP.

[0102] In one or more embodiments, the glass substrate used to form the dead-front product may be strengthened to have a DOC, described as a percentage of the thickness t of the glass substrate (as described herein). For example, in one or more embodiments, the DOC may be about 0.05t or more, about 0.1t or more, about 0.11t or more, about 0.12t or more, about 0.13t or more, about 0.14t or more, about 0.15t or more, about 0.16t or more, about 0.17t or more, about 0.18t or more, about 0.19t or more, about 0.2t or more, or about 0.21t or more. In some embodiments, the DOC is from about 0.08t to about 0.25t, from about 0.09t to about 0.25t, from about 0.18t to about 0.25t, from about 0.11t to about 0.25t, from about 0.12t to about 0.25t, from about 0.13t to about 0.25t, from about 0.14t to about 0.25t, from about 0.15t to about 0.25t, from about 0.08t to about 0. 24t, about 0.08t to about 0.23t, about 0.08t to about 0.22t, about 0.08t to about 0.21t, about 0.08t to about 0.2t, about 0.08t to about 0.19t, about 0.08t to about 0.18t, about 0.08t to about 0.17t, about 0.08t to about 0.16t, or about 0.08t to about 0.15t. In some examples, the DOC may be about 20 μm or less. In one or more embodiments, the DOC has a diameter of about 40 μm or more (e.g., about 40 μm to about 300 μm, about 50 μm to about 300 μm, about 60 μm to about 300 μm, about 70 μm to about 300 μm, about 80 μm to about 300 μm, about 90 μm to about 300 μm, about 100 μm to about 300 μm, about 110 μm to about 300 μm, about 120 μm to about 300 μm, about 140 μm to about 300 μm, about 150 μm to about 300 μm, about 40 μm to about 290 μm, about 40 μm to about 280 μm, about 40 μm to about 260 μm, about 40 μm to about 250 μm, about 40 μm to about 240 μm, about 40 μm to about 230 μm, about 40 μm to about 220 μm, about 40 μm to about 210 μm, about 40 μm to about 200 μm, about 40 μm to about 180 μm, about 40 μm to about 160 μm, about 40 μm to about 150 μm, about 40 μm to about 140 μm, about 40 μm to about 130 μm, about 40 μm to about 120 μm, about 40 μm to about 110 μm, or about 40 μm to about 100 μm).

[0103] In one or more embodiments, the glass substrate used to form the dead front product may have a CS (which may be found on the surface of the glass product or at a predetermined depth within the glass product) of about 200 MPa or more, 300 MPa or more, 400 MPa or more, about 500 MPa or more, about 600 MPa or more, about 700 MPa or more, about 800 MPa or more, about 900 MPa or more, about 930 MPa or more, about 1000 MPa or more, or about 1050 MPa or more.

[0104] In one or more embodiments, the glass substrate used to form the deadfront product may have a maximum tensile stress or central tension (CT) of about 20 MPa or more, about 30 MPa or more, about 40 MPa or more, about 45 MPa or more, about 50 MPa or more, about 60 MPa or more, about 70 MPa or more, about 75 MPa or more, about 80 MPa or more, or about 85 MPa or more. In some embodiments, the maximum tensile stress or central tension (CT) may range from about 40 MPa to about 100 MPa.

[0105] Aspect (1) of the present disclosure is a deadfront product, a substrate having a first surface and a second surface opposite the first surface; a translucent layer disposed on at least a first portion of the second surface of the substrate, the translucent layer having areas of a single color or areas of a design of two or more colors; a contrast layer disposed on at least a portion of the region, the contrast layer being configured to enhance the visibility of the color of the region or to enhance the contrast between colors of the design of the region in the portion of the region where the contrast layer is disposed; The present invention relates to a dead front product comprising:

[0106] Aspect (2) of the present disclosure relates to the deadfront product of aspect (1), wherein the area has a design of two or more colors, and the design is at least one of a leather grain pattern, a wood grain pattern, a woven pattern, a brushed metal finish pattern, a graphic or a logo.

[0107] Aspect (3) of the present disclosure relates to the deadfront product of aspect (1) or (2), wherein the translucent layer comprises a printed translucent layer.

[0108] Aspect (4) of the present disclosure relates to the deadfront product of any one of aspects (1) to (3), wherein the translucent layer has an average thickness of at most 6 μm.

[0109] Aspect (5) of the present disclosure relates to the deadfront product of any one of aspects (1) to (4), wherein the translucent layer has an average thickness of at least 1 μm.

[0110] Aspect (6) of the present disclosure relates to a deadfront product according to any one of aspects (1) to (5), wherein the semi-transparent layer is printed on the second surface of the substrate by an inkjet printer using a CMYK color model.

[0111] A seventh aspect of the present disclosure relates to the deadfront product of any one of the first to sixth aspects, wherein the contrast layer is white or gray in color.

[0112] An embodiment (8) of the present disclosure relates to the deadfront product of any one of embodiments (1) to (7), wherein the contrast layer has an average thickness of at most 6 μm.

[0113] Aspect (9) of the present disclosure relates to the deadfront product of any one of aspects (1) to (8), wherein the contrast layer has an average thickness of at least 1 μm.

[0114] Aspect (10) of the present disclosure relates to a deadfront product according to any one of aspects (1) to (9), wherein the second surface of the substrate has a second portion on which the contrast layer is disposed.

[0115] An embodiment (11) of the present disclosure relates to the deadfront product of any one of embodiments (1) to (10), wherein the contrast layer is white and has a whiteness of 20W or greater as measured according to ISO 11475:2004.

[0116] Aspect (12) of the present disclosure relates to the deadfront product of any one of aspects (1) to (11), wherein the translucent layer is disposed between the second surface and the contrast layer.

[0117] Aspect (13) of the present disclosure relates to the deadfront product of any one of aspects (1) to (12), wherein the combination of the translucent layer and the contrast layer has an average light transmittance in the range of about 5% to about 30% over a wavelength range of about 400 nm to about 700 nm.

[0118] Aspect (14) of the present disclosure relates to a deadfront product according to any one of aspects (1) to (13), having an average light transmittance in the range of about 5% to about 10% over a wavelength range of about 400 nm to about 700 nm.

[0119] Aspect (15) of the present disclosure relates to the deadfront product of any one of aspects (1) to (14), further comprising a high optical density layer disposed on at least a portion of the contrast layer, the contrast layer being disposed between the high optical density layer and the translucent layer.

[0120] A sixteenth aspect of the present disclosure relates to the deadfront product of the fifteenth aspect, wherein the high optical density layer is disposed on the contrast layer to form at least a portion of a graphic or logo.

[0121] Aspect (17) of the present disclosure relates to a deadfront product as described in aspect (16), further comprising a color layer disposed in the area of ​​the graphic or logo, and in at least a portion of the graphic or logo formed by the high optical density layer, the contrast layer is disposed between the translucent layer and the color layer.

[0122] An aspect (18) of the present disclosure relates to the deadfront product of any one of aspects (15) to (17), wherein the contrast layer has a first optical density of 0.9 to 2.0.

[0123] Aspect (19) of the present disclosure relates to the deadfront product of aspect (18), wherein the high optical density layer has a second optical density and the translucent layer has a third optical density, and the first optical density, the second optical density, and the third optical density together are at least 3.4.

[0124] Aspect (20) of the present disclosure relates to the deadfront product of aspect (19), wherein the second optical density is at least 2.4.

[0125] Aspect (21) of the present disclosure relates to the deadfront product of aspect (20), wherein the second optical density is at least 3.

[0126] Aspect (22) of the present disclosure relates to the deadfront product of any one of aspects (19) to (21), wherein the color layer has a fourth optical density of 0.3 to 0.7.

[0127] Aspect (23) of the present disclosure relates to a deadfront product according to any one of aspects (19) to (22), wherein in at least one region, the first optical density and the third optical density together are between 1.0 and 2.1.

[0128] Aspect (24) of the present disclosure relates to the deadfront product of aspect (23), wherein in at least one region, the first optical density and the third optical density together are between 1.2 and 1.6.

[0129] Aspect (25) of the present disclosure relates to the deadfront product of any one of aspects (1) to (24), wherein the substrate comprises a glass substrate and has an average thickness between the first surface and the second surface in the range of 0.05 mm to 2 mm.

[0130] Aspect (26) of the present disclosure relates to the deadfront product of any one of aspects (1) to (25), wherein the first surface of the substrate includes an anti-glare surface.

[0131] Aspect (27) of the present disclosure relates to a deadfront product according to any one of aspects (1) to (26), further comprising a functional layer disposed on the first surface of the substrate.

[0132] Aspect (28) of the present disclosure relates to a deadfront product according to aspect (27), wherein the functional layer has an average thickness of 5 nm to 600 nm.

[0133] Aspect (29) of the present disclosure relates to the deadfront product according to aspect (27) or (28), wherein the functional layer is an anti-glare layer, a scratch-resistant layer, an anti-reflection layer, a half-mirror layer, or an easy-cleaning layer.

[0134] An aspect (30) of the present disclosure relates to the deadfront product of any one of aspects (1) to (29), wherein the substrate is formed from a tempered glass material.

[0135] An aspect (31) of the present disclosure relates to the dead-front product of any one of aspects (1) to (30), wherein the substrate is curved to have a first radius of curvature.

[0136] A thirty-second aspect of the present disclosure relates to the deadfront product of the thirty-first aspect, wherein the first radius of curvature is in the range of about 60 mm to about 1500 mm.

[0137] Aspect (33) of the present disclosure relates to the dead-front product of aspect (31) or (32), wherein the substrate has a second radius of curvature different from the first radius of curvature.

[0138] An aspect (34) of the present disclosure relates to the deadfront product of any one of aspects (31) to (33), wherein the substrate is cold-formed into a curved shape.

[0139] Aspect (35) of the present disclosure relates to the deadfront product of any one of aspects (1) to (34), wherein a maximum thickness of the substrate measured between the first surface and the second surface is 1.5 mm or less.

[0140] Aspect (36) of the present disclosure relates to a deadfront product according to any one of aspects (1) to (35), wherein a maximum thickness of the substrate measured between the first surface and the second surface is between 0.3 mm and 0.7 mm.

[0141] Aspect (37) of the present disclosure relates to the deadfront product of any one of aspects (1) to (36), wherein the substrate has a width ranging from about 5 cm to about 250 cm and a length ranging from about 5 cm to about 250 cm.

[0142] An aspect (38) of the present disclosure is an apparatus, comprising: A deadfront product, comprising: A substrate; a semi-transparent layer disposed on a first surface of the substrate; a contrast layer disposed on at least a portion of the semi-transparent layer; a high optical density layer disposed on at least a portion of said contrast layer, said high optical density layer at least partially forming at least one icon; a touch panel disposed behind the at least one icon, the touch panel configured to respond to contact by a user; The present invention relates to an apparatus comprising:

[0143] Aspect (39) of the present disclosure relates to the device of aspect (38), wherein the touch panel is laminated behind the at least one icon using an optically clear adhesive.

[0144] Aspect (40) of the present disclosure relates to the device described in aspect (38), wherein the touch panel is printed behind the at least one icon.

[0145] Aspect (41) of the present disclosure relates to the device of any one of aspects (38) to (40), wherein the substrate has a second surface opposite the first surface, the first surface and the second surface defining a thickness of the substrate, and an area of ​​the second surface is modified to provide a tactile or visual indication of the at least one icon.

[0146] Aspect (42) of the present disclosure relates to the device of aspect (41), wherein the region has a greater surface roughness than a surrounding region of the second surface.

[0147] An aspect (43) of the present disclosure relates to the device according to aspect (41), wherein the thickness of the substrate is greater in the region.

[0148] An aspect (44) of the present disclosure relates to the device according to aspect (41), wherein the thickness of the substrate is smaller in the region.

[0149] Aspect (45) of the present disclosure relates to the device of aspect (41), wherein the area has a different anti-glare treatment than the surrounding area of ​​the second surface.

[0150] An embodiment (46) of the present disclosure relates to the device according to any one of embodiments (38) to (45), wherein the translucent layer has areas of a single color or areas of a design of two or more colors.

[0151] Aspect (47) of the present disclosure relates to the device of aspect (46), wherein the area has a design of two or more colors, the design being at least one of a leather grain pattern, a wood grain pattern, a woven pattern, a brushed metal finish pattern, a graphic, or a logo.

[0152] An embodiment (48) of the present disclosure relates to the device according to any one of embodiments (38) to (47), wherein the contrast layer is white or gray.

[0153] An aspect (49) of the present disclosure relates to the device of any one of aspects (38) to (48), wherein the contrast layer has a first optical density between 0.9 and 2.0.

[0154] An embodiment (50) of the present disclosure relates to the device of embodiment (49), wherein the high optical density layer has a second optical density, the second optical density being at least 2.4.

[0155] Aspect (51) of the present disclosure relates to the device according to aspect (50), wherein the second optical density is at least 3.

[0156] Aspect (52) of the present disclosure relates to a device described in any one of aspects (38) to (51), further comprising a color layer disposed in the area of ​​the icon, and in at least a portion of the icon formed by the high optical density layer, the contrast layer is disposed between the translucent layer and the color layer.

[0157] Aspect (53) of the present disclosure relates to the device of aspect (52), wherein the color layer has a third optical density of 0.3 to 0.7.

[0158] An aspect (54) of the present disclosure relates to the device of any one of aspects (38) to (53), wherein the contrast layer has a first optical density of 0.9 to 2.0, the translucent layer has a fourth optical density, and in the region of at least one icon, the first optical density and the fourth optical density together are between 1.0 and 2.1.

[0159] Aspect (55) of the present disclosure relates to the device described in aspect (54), wherein in the region of the at least one icon, the first optical density and the fourth optical density together are between 1.2 and 1.6.

[0160] Aspect (56) of the present disclosure relates to the device of any one of aspects (38) to (55), further comprising a vibration motor configured to provide tactile feedback when actuated.

[0161] Aspect (57) of the present disclosure relates to the device of aspect (56), wherein the vibration motor provides tactile feedback when the user touches the substrate.

[0162] Aspect (58) of the present disclosure relates to the device of any one of aspects (38) to (57), further comprising a dynamic display disposed on the same side of the substrate as the first surface.

[0163] Aspect (59) of the present disclosure relates to the device described in aspect (58), wherein the dynamic display includes at least one of an OLED display, an LCD display, an LED display, or a DLP MEMS chip.

[0164] Aspect (60) of the present disclosure relates to the device of any one of aspects (38) to (59), wherein one icon of the at least one icon is a power symbol according to one of IEC 60417-5007, IEC 60417-5008, IEC 60417-5009 and IEC 60417-5010.

[0165] Aspect (61) of the present disclosure relates to the device of any one of aspects (38) to (60), wherein the device is located in a vehicle dashboard, a vehicle center console, a vehicle climate control or radio control panel, or a vehicle occupant entertainment panel.

[0166] Aspect (62) of the present disclosure relates to the device of any one of aspects (38) to (61), wherein the substrate comprises a tempered glass material and has an average thickness between the first surface and a second surface opposite the first surface in a range of 0.05 mm to 2 mm.

[0167] Aspect (63) of the present disclosure relates to the apparatus of aspect (62), wherein the substrate has a radius of curvature along at least one of the first surface and the second surface of between 60 mm and 1500 mm.

[0168] An aspect (64) of the present disclosure relates to the device of any one of aspects (38) to (63), further comprising a light source, and wherein the deadfront product is disposed on the light source.

[0169] Aspect (65) of the present disclosure relates to the device of aspect (64), wherein in response to the user's contact, the light source changes the color of the icon.

[0170] An aspect (66) of the present disclosure is a method of forming a curved deadfront product, comprising: Curving the dead-front product on a support having a curved surface, the dead-front product comprising: A glass layer; a translucent layer disposed on a first surface of the glass layer, the translucent layer having areas of a solid color or areas of a design of two or more colors; a contrast layer disposed on at least a portion of the region, the contrast layer being configured to enhance visibility of a color of the region or to enhance contrast between colors of a design of the region in the portion of the region where the contrast layer is disposed; fastening said curved dead-front product to said support such that said dead-front product conforms to the curved shape of said curved surface of said support; Including, During bending and fixing of the dead-front product, the maximum temperature of the dead-front product is less than the glass transition temperature of the glass layer. It concerns the method.

[0171] In an aspect (67) of the present disclosure, the step of fixing the curved dead-front product comprises: providing an adhesive between the curved surface of the support and a surface of the deadfront product; bonding said deadfront product to a support surface of a frame with said adhesive while applying a force; The method according to embodiment (66), comprising:

[0172] An embodiment (68) of the present disclosure relates to the method according to embodiment (66) or (67), wherein the glass layer is tempered.

[0173] Aspect (69) of the present disclosure relates to the method of aspect (68), wherein the glass layer has a second surface opposite the first surface, and a maximum thickness of the glass layer measured between the first surface and the second surface is 1.5 mm or less.

[0174] An embodiment (70) of the present disclosure relates to the method of any one of embodiments (66) to (69), wherein the maximum temperature of the dead-front product during bending and fixing the dead-front product is less than 200° C.

[0175] Aspect (71) of the present disclosure relates to the method of any one of aspects (66) to (70), wherein the deadfront product further comprises a high optical density layer disposed on at least a portion of the contrast layer.

[0176] Aspect (72) of the present disclosure relates to the method of any one of aspects (66) to (71), wherein the deadfront product further comprises a touch panel disposed on at least one of the contrast layer or the high optical density layer.

[0177] An embodiment (73) of the present disclosure relates to the method of any one of embodiments (66) to (72), wherein the contrast layer has a first optical density of 0.9 to 2.0.

[0178] Embodiment (74) of the present disclosure relates to the method of any one of embodiments (71) to (73), wherein the high optical density layer has a second optical density of at least 2.4.

[0179] An embodiment (75) of the present disclosure relates to the method of embodiment (74), wherein the second optical density is at least 3.

[0180] An embodiment (76) of the present disclosure relates to the method of any one of embodiments (71) to (75), wherein the high optical density layer and the contrast layer together form at least one icon.

[0181] Aspect (77) of the present disclosure relates to the method of aspect (76), wherein the deadfront product further comprises a color layer disposed in the area of ​​the at least one icon, and in at least a portion of the at least one icon formed by the high optical density layer, the contrast layer is disposed between the translucent layer and the color layer.

[0182] A seventy-eighth aspect of the present disclosure relates to the method of the seventy-seventh aspect, wherein the color layer has a third optical density of 0.3 to 0.7.

[0183] A seventy-ninth aspect of the present disclosure relates to the method of the seventy-third aspect, wherein the semi-transparent layer has a fourth optical density, and the first optical density and the fourth optical density together are between 1.0 and 2.1.

[0184] An embodiment (80) of the present disclosure relates to the method of embodiment (79), wherein the first optical density and the fourth optical density together are 1.2 to 1.6.

[0185] Unless expressly stated otherwise, it is not intended that any method set forth herein be construed as requiring that its steps be performed in a particular order. Thus, unless a method claim actually recites the order in which its steps should be followed, or unless it is specifically stated otherwise in the claim or detailed description that the steps are to be limited to a particular order, no particular order is intended to be inferred. Additionally, as used herein, the article "a" is intended to include one or more components or elements, and is not intended to be construed as meaning only one.

[0186] It will be apparent to those skilled in the art that various improvements and modifications can be made without departing from the spirit or scope of the disclosed embodiments. Since improvements, combinations, subcombinations and variations of the disclosed embodiments incorporating the spirit and substance of the embodiments may occur to those skilled in the art, the disclosed embodiments should be interpreted as including all within the scope of the appended claims and their equivalents.

[0187] Preferred embodiments of the present invention will be described below in detail.

[0188] EMBODIMENT 1 A deadfront product, comprising: a substrate having a first surface and a second surface opposite the first surface; a translucent layer disposed on at least a first portion of the second surface of the substrate, the translucent layer having areas of a single color or areas of a design of two or more colors; a contrast layer disposed on at least a portion of the region, the contrast layer being configured to enhance the visibility of the color of the region or to enhance the contrast between colors of the design of the region in the portion of the region where the contrast layer is disposed; A dead front product that includes:

[0189] EMBODIMENT 2 2. The deadfront product of embodiment 1, wherein the area has a design in two or more colors, the design being at least one of a leather grain pattern, a wood grain pattern, a woven pattern, a brushed metal finish pattern, a graphic, or a logo.

[0190] EMBODIMENT 3 3. The deadfront product of embodiment 1 or 2, wherein the translucent layer comprises a printed translucent layer.

[0191] EMBODIMENT 4 4. The deadfront product of any one of the preceding claims, wherein the translucent layer has an average thickness of up to 6 μm.

[0192] EMBODIMENT 5 5. The deadfront product of any one of the preceding claims, wherein the translucent layer has an average thickness of at least 1 μm.

[0193] EMBODIMENT 6 6. The deadfront product of any one of claims 1 to 5, wherein the semi-transparent layer is printed on the second side of the substrate by an inkjet printer using a CMYK color model.

[0194] EMBODIMENT 7 7. The deadfront product of any one of the preceding claims, wherein the contrast layer is white or gray in color.

[0195] EMBODIMENT 8 8. The deadfront product of any one of the preceding claims, wherein the contrast layer has an average thickness of at most 6 μm.

[0196] EMBODIMENT 9 9. The deadfront product of any one of the preceding claims, wherein the contrast layer has an average thickness of at least 1 μm.

[0197] EMBODIMENT 10 10. The deadfront product of any one of claims 1 to 9, wherein the second surface of the substrate has a second portion on which the contrast layer is disposed.

[0198] EMBODIMENT 11 11. The deadfront product of any one of the preceding claims, wherein the contrast layer is white and has a whiteness of 20W or greater as measured according to ISO 11475:2004.

[0199] EMBODIMENT 12 12. The deadfront product of any one of claims 1 to 11, wherein the translucent layer is disposed between the second surface and the contrast layer.

[0200] EMBODIMENT 13 13. The deadfront product of any one of claims 1 to 12, wherein the combination of the translucent layer and the contrast layer has an average light transmittance in the range of about 5% to about 30% over a wavelength range of about 400 nm to about 700 nm.

[0201] EMBODIMENT 14 14. The deadfront product of any one of embodiments 1 to 13, having an average light transmittance in the range of about 5% to about 10% over a wavelength range of about 400 nm to about 700 nm.

[0202] EMBODIMENT 15 15. The deadfront product of any one of claims 1 to 14, further comprising a high optical density layer disposed on at least a portion of the contrast layer, the contrast layer being disposed between the high optical density layer and the translucent layer.

[0203] EMBODIMENT 16 16. The deadfront product of embodiment 15, wherein the high optical density layer is disposed on the contrast layer so as to form at least a portion of a graphic or logo.

[0204] EMBODIMENT 17 The deadfront product of embodiment 16 further comprises a color layer disposed in the area of ​​the graphic or logo, and in at least a portion of the graphic or logo formed by the high optical density layer, the contrast layer is disposed between the translucent layer and the color layer.

[0205] EMBODIMENT 18 18. The deadfront product of any one of embodiments 15 to 17, wherein the contrast layer has a first optical density of 0.9 to 2.0.

[0206] EMBODIMENT 19 19. The deadfront product of embodiment 18, wherein the high optical density layer has a second optical density and the translucent layer has a third optical density, and the first optical density, the second optical density and the third optical density together are at least 3.4.

[0207] EMBODIMENT 20 20. The deadfront product of embodiment 19, wherein the second optical density is at least 2.4.

[0208] EMBODIMENT 21 21. The deadfront product of embodiment 20, wherein the second optical density is at least 3.

[0209] EMBODIMENT 22 22. The deadfront product of any one of claims 19 to 21, wherein the color layer has a fourth optical density of 0.3 to 0.7.

[0210] EMBODIMENT 23 23. The deadfront product of any one of claims 19 to 22, wherein in at least one region, the first optical density and the third optical density together are between 1.0 and 2.1.

[0211] EMBODIMENT 24 24. The deadfront product of embodiment 23, wherein in at least one region, the first optical density and the third optical density together are between 1.2 and 1.6.

[0212] EMBODIMENT 25 25. The deadfront product of any one of claims 1 to 24, wherein the substrate comprises a glass substrate and has an average thickness between the first surface and the second surface in the range of 0.05 mm to 2 mm.

[0213] EMBODIMENT 26 26. The deadfront product of any one of claims 1 to 25, wherein the first surface of the substrate comprises an anti-glare surface.

[0214] EMBODIMENT 27 A deadfront product according to any one of claims 1 to 26, further comprising a functional layer disposed on the first surface of the substrate.

[0215] EMBODIMENT 28 28. The deadfront product of embodiment 27, wherein the functional layer has an average thickness of 5 nm to 600 nm.

[0216] EMBODIMENT 29 29. The deadfront product of embodiment 27 or 28, wherein the functional layer is an anti-glare layer, a scratch-resistant layer, an anti-reflection layer, a half-mirror layer or an easy-cleaning layer.

[0217] EMBODIMENT 30 30. The deadfront product of any one of claims 1 to 29, wherein the substrate is formed from a tempered glass material.

[0218] EMBODIMENT 31 31. The deadfront product of any one of claims 1 to 30, wherein the substrate is curved to have a first radius of curvature.

[0219] EMBODIMENT 32 32. The deadfront product of embodiment 31, wherein the first radius of curvature is in the range of about 60 mm to about 1500 mm.

[0220] EMBODIMENT 33 33. The deadfront product of embodiment 31 or 32, wherein the substrate has a second radius of curvature different from the first radius of curvature.

[0221] EMBODIMENT 34 34. The deadfront product of any one of embodiments 31 to 33, wherein the substrate is cold-formed into a curved shape.

[0222] EMBODIMENT 35 35. The deadfront product of any one of claims 1 to 34, wherein the maximum thickness of the substrate measured between the first side and the second side is 1.5 mm or less.

[0223] EMBODIMENT 36 36. The deadfront product of any one of claims 1 to 35, wherein a maximum thickness of the substrate measured between the first surface and the second surface is between 0.3 mm and 0.7 mm.

[0224] EMBODIMENT 37 37. The deadfront product of any one of claims 1 to 36, wherein the substrate has a width ranging from about 5 cm to about 250 cm and a length ranging from about 5 cm to about 250 cm.

[0225] EMBODIMENT 38 1. An apparatus comprising: A deadfront product, comprising: A substrate; a semi-transparent layer disposed on a first surface of the substrate; a contrast layer disposed on at least a portion of the semi-transparent layer; a high optical density layer disposed on at least a portion of said contrast layer, said high optical density layer at least partially forming at least one icon; a touch panel disposed behind the at least one icon, the touch panel configured to respond to contact by a user; An apparatus comprising:

[0226] EMBODIMENT 39 39. The device of embodiment 38, wherein the touch panel is laminated behind the at least one icon using an optically clear adhesive.

[0227] EMBODIMENT 40 39. The device of embodiment 38, wherein the touch panel is printed behind the at least one icon.

[0228] EMBODIMENT 41 The device of any one of embodiments 38 to 40, wherein the substrate has a second surface opposite the first surface, the first surface and the second surface defining a thickness of the substrate, and an area of ​​the second surface is modified to provide a tactile or visual indication of the at least one icon.

[0229] EMBODIMENT 42 42. The apparatus of embodiment 41, wherein the region has a greater surface roughness than a surrounding region of the second surface.

[0230] EMBODIMENT 43 42. The apparatus of embodiment 41, wherein the thickness of the substrate is greater in the region.

[0231] EMBODIMENT 44 42. The apparatus of embodiment 41, wherein the thickness of the substrate is smaller in the region.

[0232] EMBODIMENT 45 42. The device of embodiment 41, wherein the area has a different anti-glare treatment than the surrounding area of ​​the second surface.

[0233] EMBODIMENT 46 46. ​​The device of any one of embodiments 38 to 45, wherein the translucent layer has areas of a single color or areas of a design of two or more colors.

[0234] EMBODIMENT 47 47. The device of embodiment 46, wherein the area has a design of two or more colors, the design being at least one of a leather grain pattern, a wood grain pattern, a woven pattern, a brushed metal finish pattern, a graphic, or a logo.

[0235] EMBODIMENT 48 48. The device of any one of embodiments 38 to 47, wherein the contrast layer is white or gray.

[0236] EMBODIMENT 49 49. The device of any one of embodiments 38 to 48, wherein the contrast layer has a first optical density of 0.9 to 2.0.

[0237] EMBODIMENT 50 50. The device of embodiment 49, wherein the high optical density layer has a second optical density, the second optical density being at least 2.4.

[0238] EMBODIMENT 51 51. The device of embodiment 50, wherein the second optical density is at least 3.

[0239] EMBODIMENT 52 The device of any one of embodiments 38 to 51, further comprising a color layer disposed in the area of ​​the icon, wherein in at least a portion of the icon formed by the high optical density layer, the contrast layer is disposed between the translucent layer and the color layer.

[0240] EMBODIMENT 53 53. The device of embodiment 52, wherein the color layer has a third optical density of 0.3 to 0.7.

[0241] EMBODIMENT 54 54. The device of any one of embodiments 38 to 53, wherein the contrast layer has a first optical density of 0.9 to 2.0, the translucent layer has a fourth optical density, and in the region of at least one icon, the first optical density and the fourth optical density together are 1.0 to 2.1.

[0242] EMBODIMENT 55 55. The device of embodiment 54, wherein in the region of the at least one icon, the first optical density and the fourth optical density together are between 1.2 and 1.6.

[0243] EMBODIMENT 56 56. The device of any one of embodiments 38 to 55, further comprising a vibration motor configured to provide tactile feedback when activated.

[0244] EMBODIMENT 57 57. The apparatus of embodiment 56, wherein the vibration motor provides tactile feedback when the user touches the substrate.

[0245] EMBODIMENT 58 The device of any one of embodiments 38 to 57, further comprising a dynamic display disposed on the same side of the substrate as the first surface.

[0246] EMBODIMENT 59 59. The device of embodiment 58, wherein the dynamic display includes at least one of an OLED display, an LCD display, an LED display, or a DLP MEMS chip.

[0247] EMBODIMENT 60 60. The device of any one of embodiments 38 to 59, wherein one of the at least one icons is a power symbol according to one of IEC 60417-5007, IEC 60417-5008, IEC 60417-5009 and IEC 60417-5010.

[0248] EMBODIMENT 61 The device of any one of embodiments 38 to 60, wherein the device is located in a vehicle dashboard, a vehicle center console, a vehicle climate control or radio control panel, or a vehicle occupant entertainment panel.

[0249] EMBODIMENT 62 62. The device of any one of embodiments 38 to 61, wherein the substrate comprises a reinforced glass material and has an average thickness between the first surface and a second surface opposite the first surface in the range of 0.05 mm to 2 mm.

[0250] EMBODIMENT 63 63. The apparatus of embodiment 62, wherein the substrate has a radius of curvature along at least one of the first surface and the second surface of between 60 mm and 1500 mm.

[0251] EMBODIMENT 64 64. The apparatus of any one of embodiments 38 to 63, further comprising a light source, and the deadfront product is disposed on the light source.

[0252] EMBODIMENT 65 65. The device of embodiment 64, wherein in response to the user's contact, the light source changes the color of the icon.

[0253] EMBODIMENT 66 1. A method of forming a curved deadfront product, comprising: Curving the dead-front product on a support having a curved surface, the dead-front product comprising: A glass layer; a translucent layer disposed on a first surface of the glass layer, the translucent layer having areas of a solid color or areas of a design of two or more colors; a contrast layer disposed on at least a portion of the region, the contrast layer being configured to enhance visibility of a color of the region or to enhance contrast between colors of a design of the region in the portion of the region where the contrast layer is disposed; fastening said curved dead-front product to said support such that said dead-front product conforms to the curved shape of said curved surface of said support; Including, During bending and fixing of the dead-front product, the maximum temperature of the dead-front product is less than the glass transition temperature of the glass layer. method.

[0254] EMBODIMENT 67 The step of fixing the curved deadfront product includes: providing an adhesive between the curved surface of the support and a surface of the deadfront product; bonding said deadfront product to a support surface of a frame with said adhesive while applying a force; 67. The method of embodiment 66, comprising:

[0255] EMBODIMENT 68 68. The method of claim 66 or 67, wherein the glass layer is tempered.

[0256] EMBODIMENT 69 69. The method of claim 68, wherein the glass layer has a second surface opposite the first surface, and a maximum thickness of the glass layer measured between the first surface and the second surface is 1.5 mm or less.

[0257] EMBODIMENT 70 70. The method of any one of embodiments 66 to 69, wherein the maximum temperature of the dead-front product during bending and fixing the dead-front product is less than 200° C.

[0258] EMBODIMENT 71 71. The method of any one of claims 66 to 70, wherein the deadfront product further comprises a high optical density layer disposed on at least a portion of the contrast layer.

[0259] EMBODIMENT 72 72. The method of any one of claims 66 to 71, wherein the deadfront product further comprises a touch panel disposed on at least one of the contrast layer or the high optical density layer.

[0260] EMBODIMENT 73 73. The method of any one of embodiments 66 to 72, wherein the contrast layer has a first optical density of 0.9 to 2.0.

[0261] EMBODIMENT 74 74. The method of any one of embodiments 71 to 73, wherein the high optical density layer has a second optical density of at least 2.4.

[0262] EMBODIMENT 75 75. The method of embodiment 74, wherein the second optical density is at least 3.

[0263] EMBODIMENT 76 76. The method of any one of embodiments 71 to 75, wherein the high optical density layer and the contrast layer together form at least one icon.

[0264] EMBODIMENT 77 The method of embodiment 76, wherein the deadfront product further comprises a color layer disposed in the area of ​​the at least one icon, and in at least a portion of the at least one icon formed by the high optical density layer, the contrast layer is disposed between the translucent layer and the color layer.

[0265] EMBODIMENT 78 78. The method of embodiment 77, wherein the color layer has a third optical density of 0.3 to 0.7.

[0266] EMBODIMENT 79 74. The method of embodiment 73, wherein the semi-transparent layer has a fourth optical density, and the first optical density and the fourth optical density together are between 1.0 and 2.1.

[0267] EMBODIMENT 80 80. The method of embodiment 79, wherein the first optical density and the fourth optical density together are between 1.2 and 1.6.

Claims

1. A deadfront product, comprising: a substrate having a first surface and a second surface opposite the first surface; a semi-transparent layer disposed on the second surface of the substrate, the semi-transparent layer having an optical density between 0.1 and 0.5 and forming a pattern of two or more colors, the semi-transparent layer being printed on the second surface of the substrate using a CMYK color model; a contrast layer disposed on at least a portion of said translucent layer, said contrast layer including a reflective surface that reflects light in the visible spectrum and causes said pattern to be visible when said deadfront product is viewed from said first side; a color layer disposed on the contrast layer, the color layer being made up of a plurality of colors; Equipped with A deadfront product, wherein the semi-transparent layer is printed onto the contrast layer using a CMYK color model.

2. The deadfront product of claim 1 , wherein the contrast layer is white or gray.

3. 3. The deadfront product of claim 2, wherein the contrast layer is white and has a whiteness of 20W or greater measured according to ISO 11475:2004.

4. the semi-transparent layer is disposed between the contrast layer and the substrate; 4. The deadfront product of claim 1, wherein the contrast layer is disposed between the color layer and the translucent layer.

5. the semi-transparent layer is a first thermally curable ink or a UV curable ink; the contrast layer being a second thermal or UV curable ink; the color layer is a third heat curable ink or a UV curable ink; 4. The deadfront product of claim 1, wherein the deadfront product is at least one of:

6. The deadfront product of claim 1 , wherein the two or more color patterns are at least one of a leather grain pattern, a wood grain pattern, a woven pattern, a brushed metal finish pattern, a graphic, or a logo.

7. the semi-transparent layer has an average thickness of 1 μm to 6 μm; said contrast layer having an average thickness of 1 μm to 14 μm; A deadfront product according to any one of claims 1 to 3, wherein the colour layer has an average thickness of 1 µm to 6 µm.

8. 4. The deadfront product of claim 1, further comprising a high optical density layer disposed on at least a portion of the contrast layer, the contrast layer being disposed between the high optical density layer and the translucent layer.

9. 9. The deadfront product of claim 8, wherein the contrast layer has a first optical density, the high optical density layer has a second optical density, and the translucent layer has a third optical density, the first optical density, the second optical density, and the third optical density collectively being at least 3.

4.

10. the color layer has a fourth optical density of 0.3 to 0.7; 10. The deadfront product of claim 9, wherein in at least one region, said first optical density and said third optical density together are between 1.2 and 1.6.

Citation Information

Patent Citations

  • Display device

    JP2001331132A

  • Illuminating display unit

    JP2004045529A

  • Article with display structure

    JP2007206577A

  • Organic electroluminescence panel module

    WO2016152792A1