Thermoelectric conversion device and method for manufacturing same

Stable interconnects in thermoelectric devices are achieved using recrystallized silicon-containing materials and specific metals, addressing stability and performance issues at high temperatures.

JP7596152B2Active Publication Date: 2024-12-09RGS DEVMENT BV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020570642
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-03-07
Filing Date
2019-03-07
Publication Date
2024-12-09
Estimated Expiration
2039-03-07

AI Technical Summary

Technical Problem

Existing thermoelectric devices using silicon-containing materials face issues with interconnect stability due to metal diffusion, formation of brittle silicides, and thermal stress, leading to performance degradation and limited lifetime at high temperatures.

Method used

A method involving interconnects made of recrystallized silicon-containing materials and specific metals like Ag, Al, Ge, Sn, Zn, or their alloys, which do not form silicides, allowing for stable connections by melting and recrystallization, ensuring low resistance and mechanical stability.

Benefits of technology

The solution provides stable, low-resistance interconnects that maintain mechanical integrity and conductivity, enabling efficient thermoelectric operation at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596152000001
    Figure 0007596152000001
  • Figure 0007596152000002
    Figure 0007596152000002
  • Figure 0007596152000003
    Figure 0007596152000003
Patent Text Reader

Abstract

The thermoelectric device includes an active element containing a thermoelectric material of silicon, a silicon alloy, a metal-silicide, or a silicon composite, and an interconnect zone consisting of a metallic interconnect and a recrystallized phase of material from the active thermoelectric element. The metallic interconnect is from a metal that does not form a metal silicide in the solid state and has some solubility for the components of the thermoelectric element in the liquid phase and low solubility for these components in the solid phase. The active thermoelectric element is formed with a first contact interface and a second contact interface. The interconnect between different thermoelectric elements consists of at least two phase materials, one of which is primarily the metallic interconnect material and the other of which is formed by the recrystallized components of the thermoelectric material.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermoelectric conversion device made from a silicon-containing material. Additionally, the present invention relates to a method for manufacturing such a thermoelectric conversion device. [Background technology]

[0002] Thermoelectric elements based on bismuth telluride-containing materials are well known and widely applied in different application fields. However, due to the material properties of bismuth telluride materials, such devices are typically limited to a maximum operating temperature of 250 °C. In the so-called high-temperature range, with hot-side device operating temperatures exceeding 500 °C, these materials are no longer useful.

[0003] On the other hand, silicon, silicon composite, silicon alloy, and metal-silicide based thermoelectric devices are expected to be low-cost, environmentally benign thermoelectric devices well suited for high-temperature operation with device hot-side temperatures exceeding 500°C. As a result, such devices are ideal candidates for applications, for example, in process industries where large amounts of waste heat are generated at very high temperature levels (often between 800°C and 1200°C) or in cogeneration situations where heat and electricity are generated by gas or biomass combustion. Promising material classes for such high-temperature thermoelectric devices are the group of silicon, silicon composites, silicon alloys, or metal-silicides, denoted here as silicon-containing materials, in particular silicon with encapsulated nanostructures, silicon germanium alloys (SiGe), high manganese silicide (HMS), iron silicide (FeSi2), and magnesium silicide (Mg2Si) (silicides). These silicides are usually adjusted to the desired properties such as Seebeck voltage, electrical resistivity, and thermal conductivity by adding small amounts of dopant materials. A well-known example is the combination of boron-doped SiGe with phosphorus-doped SiGe, which allows the production of p-type conductive materials (boron-doped SiGe) and n-type conductive materials (phosphorus-doped SiGe). Other examples are aluminum-doped manganese silicide as the p-type conductive material, or iron-doped manganese silicide as the n-type material.

[0004] Since the voltage generated by the Seebeck effect on one thermoelectric element in such a thermoelectric conversion device is typically on the order of 100 mV, the thermoelectric conversion device typically consists of multiple thermoelectric elements electrically connected in series by conductive interconnects. Most preferably, such a thermoelectric conversion device consists of two types of thermoelectric elements, with so-called p-type conductive elements and n-type conductive elements. Alternating these thermoelectric elements in an electrical series interconnection is the preferred method for fabricating a thermoelectric conversion device. However, as known to those skilled in the art, parallel interconnections and devices consisting of only one type of thermoelectric element (i.e., p-type or n-type) are possible. In many practical cases, such conductive interconnects utilize high-temperature resistant metals such as nickel or copper. In oxygen-free environments, molybdenum and tungsten are also useful elements for electrical interconnects. However, due to the high operating temperatures and long intended operating lives of thermoelectric generators, the technical requirements for these conductive interconnects are very stringent.

[0005] In the process of making a thermoelectric conversion device, at least one, but preferably two, silicon-containing material thermoelectric elements comprising silicon, silicon composites, silicon alloys or metal-silicide based materials (one n-type, one p-type material) are connected in series using electrical interconnects with low electrical resistance. These interconnects must meet several requirements. - Low electrical resistivity - No performance degradation or at least acceptably small performance degradation under high temperature operation - Sufficient mechanical stability to allow continuous operation of the thermoelectric module under cyclic temperature operation and even under long-term constant high temperature operation The accepted state of the art is that silicon-containing material-metal direct interconnects cannot meet the above technical requirements. The reason is that metal from the metal interconnect layer will diffuse into the thermoelectric (silicide) material and degrade the electrical properties, while silicon from the thermoelectric material will react with the metal interconnect and often form very brittle metal silicides at the interface. Since these diffusion processes will continue during device operation, such interconnects are not stable under operation. Furthermore, silicon, silicon composites, silicon alloys or metal-silicide based materials-metal interconnects often exhibit differences in thermal expansion coefficients, which induce thermal stresses in the interconnects and lead to the formation of cracks or the interconnects breaking.

[0006] As a result, layered interface structures are used to overcome stability issues and produce the required properties.

[0007] WO2013145843 discloses a thermoelectric conversion module with manganese silicide as the active material in contact with Ni, Mo, or W electrodes using a Cr-Cu alloy stress relief layer in combination with a Ni diffusion barrier layer to prevent solid-state diffusion of Cr or Cu into the manganese silicide. However, the inventors' test results showed that the proposed structure including the manganese silicide-Ni interface was not stable under long-term operation in a high-temperature environment. Such a system is expected to have a limited life span under high-temperature operation.

[0008] Taiwan Patent Publication No. 201234688 discloses a resistive electrical contact on, for example, magnesium silicide, where the electrode material itself is a transition metal silicide or a mixture of a transition metal silicide (e.g., nickel silicide, chromium silicide, cobalt silicide, titanium silicide) and possibly a metal. Although such a structure provides a low electrical resistance contact with the thermoelectric material itself, it is not useful for thermoelectric module fabrication because transition metal silicides are not always mechanically stable enough and, in combination with a metal, e.g., Ni, do not prevent silicon diffusion into the metal and ultimately the conversion of the metal layer to a metal silicide.

[0009] Japanese Patent Application Publication No. 2005317834 discloses a thermoelectric conversion module comprising a thermoelectric conversion element of p-type iron silicide (FeSi2), a thermoelectric conversion element of n-type iron silicide (FeSi2), and an electrode member whose surface layer is at least copper, molybdenum, cobalt, or tungsten. At least the high temperature side of the thermoelectric conversion element is connected to the electrode member through an intervening layer of silver by a brazing filler metal member. The melting point of the brazing filler metal member is 600-820°C. This publication describes a method in which Ag particles are sintered within the above temperature range. Such a method does not produce a stable silver-metal interconnection and is subject to further sintering of Ag particles during thermoelectric operation and is therefore highly unstable.

[0010] Generally, these prior art disclosures for creating resistive electrical contacts with silicides lack long-term stability due to diffusion of the metal components of the contact into the thermoelectric silicide material, or diffusion of silicon from the thermoelectric material into the metallization layer where undesirable or harmful silicides are formed that often form mechanically brittle materials. Furthermore, differences in thermal expansion coefficients can cause high thermal stresses in the interconnect, leading to the formation of cracks and ultimately the rupture of the contact.

[0011] An alternative approach for connecting different materials based on silicon, silicon composites, silicon alloys or metal-silicides is the direct connection of two thermoelectric elements without an interconnecting metal by a so-called pn junction. This can be achieved by laser welding of the semiconducting metals together, by crystallizing the connected pn-type legs from the melt, or by diffusing dopants from the surface of the material at high temperature. An example of such a device is described in WO0184641(A1). By eliminating the metal interconnecting contact on the hot side of the element, such a technique overcomes the technical problems around the interconnection between silicon or metal silicide materials and metal interconnects. However, pn junctions are less conductive than metal contacts, the conductivity is strongly temperature dependent, and when a sufficient thermally generated charge carrier concentration is reached, the rectifying behavior of the pn junction changes to a more ohmic behavior. At lower temperatures, such p-n junctions are not necessarily conductive enough, and thus p-n junction-based thermoelectric devices have limited performance at low and moderate temperatures (depending on the bandgap of the material, ohmic conductivity of the p-n junction may require temperatures of at least 500°C or higher).

[0012] In summary, the current state of the art in thermoelectric devices based on silicon-containing materials such as silicon, silicon composites, silicon alloys, or metal-silicide based materials is that high conductivity Schottky-type contacts between semiconductors and interconnect metals are not always stable enough due to metal silicide formation at the interface and metal interdiffusion into the semiconductor material. A direct interconnect between two silicon, silicon composite, silicon alloy, or metal silicide thermoelectric elements in the form of a p-n junction can provide a stable interconnection, but the higher resistivity of the p-n junction degrades the device performance. Summary of the Invention

[0013] It is an object of the present invention to provide a thermoelectric conversion device based on silicon, silicon composite, silicon alloy, or metal-silicide based materials, and a method for manufacturing the thermoelectric conversion device, which overcomes or mitigates the above-mentioned deleterious effects.

[0014] The above object is achieved by a thermoelectric conversion device comprising a first active element and a second active element containing silicon, silicon composite, silicon alloy, or metal-silicide. Depending on the desired conductivity type, such first and second active elements can be doped with different dopants to allow a combination of n-type and p-type conductivity. These elements are interconnected by an interconnect layer consisting of a combination of an interconnect metal and a recrystallized material phase consisting of silicon, silicon composite, silicon alloy, and metal-silicide based elemental components. The interconnect metal has the following properties: - Interconnect metals are Does not react with silicon and does not form interconnecting metal-silicide phases in the solid state . The interconnect metal is either the first thermoelectric element or the second thermoelectric element. Reno At temperatures below the melting point too It will melt. In the molten state, the interconnect metal will dissolve at least one of the components of the thermoelectric element, preferably the element silicon, or all components of the thermoelectric element in the composition present in the element. The solubility of the components of the thermoelectric element in the molten interconnect metal will be limited to a certain value, but will increase if the temperature of the liquid interconnect metal is increased. - In the solid state, the interconnect metal is one of the components of the thermoelectric element. Regarding this It has low solubility.

[0015] A silicon-containing material, such as silicon, silicon composites, silicon alloys, or metal-silicide based materials, is considered to contain at least 50 at% Si.

[0016] As described below in the examples, metals that do not form interconnect metal-silicides exist in the case of silicon, silicon composites, silicon alloys, and metal-silicide based thermoelectric materials. Examples are tin, zinc, aluminum, silver, and germanium. Other metals are beryllium, gold, and antimony.

[0017] Examples of some frequently used metals that form interconnect metal-silicides and therefore do not meet the above description are iron, copper, chromium, nickel, platinum, and titanium. Such a thermoelectric element in combination with an interconnect metal would allow for an interconnect process in which the assembly of two thermoelectric elements with an interconnect metal between them is heated to a temperature above the melting point of the interconnect metal. In contrast to the interconnect process outlined in the above patent, this interconnect metal is completely melted and liquid in the process. During heating of the liquid interconnect metal, a quantity of at least one component, but preferably all components of the thermoelectric element, is melted in the melt. After a point in the interconnect process, the assembly would be cooled, causing the melted components of the thermoelectric material to crystallize from the liquid interconnect metal melt due to their reduced solubility. At the freezing point of the interconnect metal melt, the remaining components of the thermoelectric element in the liquid interconnect melt must also crystallize due to the low solubility of the elements in the solidified interconnect metal.

[0018] As a result of this process, an electrical and mechanical interconnection between at least two thermoelectric elements is created that consists of at least two different phases: a recrystallized phase of the components from the thermoelectric elements and a solidified interconnecting metallic phase.

[0019] The advantage of such a process compared to the current state of the art is that the properties of the selected interconnect metal make the assembly chemically inert in the solid state. In the area where the interconnect metal connects the two thermoelectric materials, a low electrical resistance interconnect is realized due to the Schottky contact behavior at the metal-thermoelectric element interface. The connected, recrystallized thermoelectric materials form a low conductivity pn junction that provides high mechanical stability to the interconnect system.

[0020] The ratio of recrystallized thermoelectric elements to interconnect metal can be adjusted by process parameters such as the maximum temperature during the interconnect metal melting process. The morphology of the recrystallized thermoelectric element phase can be adjusted by the resolidification temperature trajectory. By doing so, the recrystallized phase can be controlled to form a homogenous layer on the thermoelectric elements with a solidified metal layer in between. Such conditions lead to a high electrical conductivity with reduced mechanical strength of the interconnect. If the recrystallization process is performed at different cooling rates, the recrystallization front is destabilized, leading to recrystallized interconnects between the thermoelectric elements. Such a system has advantages in terms of mechanical stability at the expense of a slightly lower electrical conductivity. As a result, such a process produces the necessary process adjustments to enable the manufacture of thermoelectric generators according to their functional requirements.

[0021] Another advantage of this system is that the amount of metal in the metal interconnects is typically low, with preferred interconnect metal layer thicknesses being between 5 μm and 500 μm. [Brief description of the drawings]

[0022] The present invention will now be described in detail with reference to the drawings in which exemplary embodiments thereof are shown, which are for illustrative purposes only and are not intended to limit the inventive concepts defined by the appended claims. [Figure 1] 1 is a cross-sectional view of a thermoelectric conversion device according to an embodiment of the present invention. [Diagram 2] FIG. 4 is a cross-sectional view of another thermoelectric conversion device according to an embodiment of the present invention. [Diagram 3] 2A-2C are cross-sectional views of an interconnection scheme for a thermoelectric conversion device according to one embodiment of the present invention prior to the fabrication process. [Figure 4] 3A-3C are cross-sectional views of an interconnection scheme for a thermoelectric conversion device according to one embodiment of the present invention after a fabrication process. [Diagram 5] 4A-4C are cross-sectional views of an interconnection scheme for a thermoelectric device according to another embodiment of the present invention after a manufacturing process. [Figure 6] 4A-4C are cross-sectional views of an interconnection scheme for a thermoelectric device according to another embodiment of the present invention after a manufacturing process. [Figure 7] 4 is a cross-sectional micrograph of an actual interconnect of a thermoelectric conversion device according to one embodiment of the present invention after a fabrication process. [Figure 8] Phase diagram of the silver-silicon system. [Figure 9] 1 is a schematic perspective view of a thermoelectric device constructed in accordance with one embodiment of the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] FIG. 1 shows a cross-sectional view of a thermoelectric conversion device according to one embodiment of the present invention.

[0024] According to one embodiment, the thermoelectric conversion device comprises a plurality of thermoelectric elements 1001 and 1003, also denoted as "active elements", made of silicon, silicon composite, silicon alloy, or metal-silicide based material. Such thermoelectric elements may have a rod shape.

[0025] Each thermoelectric element 1001, 1003 comprises a contact interface with a first interconnection zone 1002 and a second interconnection zone 1004. For example, these contact interfaces and counter interfaces are formed at respective ends of a rod shape. During use of the thermoelectric element, one contact interface (for example, the first contact interface) is kept at a relatively high temperature, i.e. is the hot side located in a zone having a relatively high temperature, and the other first counter interface as the cold side is kept at a relatively low temperature and is located in a zone having a relatively low temperature compared to the zone having the high temperature.

[0026] Thermoelectric elements 1001, 1003 are connected in series by providing a metallic interconnection zone 1002. According to the invention, the interconnection zone 1002, which may be a strip-shaped element, consists of a volume of interconnect metal and a volume of recrystallized components of the thermoelectric elements.

[0027] The second interconnect zone 1004 may preferably be made of the same components as the first interconnect zone 1002. However, due to differences in operating temperatures, other interconnect metallurgies may also be applied.

[0028] In one embodiment, the thermoelectric elements 1001, 1003 are "L" shaped and made in one piece. Alternatively, the thermoelectric elements 1001, 1003 may each consist of two legs of the same material joined by a heat treatment to form the L shape.

[0029] FIG. 2 shows a cross-sectional view of a thermoelectric conversion device according to one embodiment of the present invention.

[0030] According to one embodiment, the thermoelectric conversion device comprises a plurality of thermoelectric elements 2001 and 2003, also denoted as "active elements", made of silicon, silicon composite, silicon alloy, or metal-silicide based material. Such thermoelectric elements may have a rod shape.

[0031] Each thermoelectric element 2001, 2003 comprises on its hot and cold sides a contact interface with an interconnection zone 2002. According to the invention, the interconnection zone 2002, which may be a strip-shaped element, consists of a volume of interconnect metal and a volume of recrystallized components of the thermoelectric element.

[0032] Figure 3 shows a cross-sectional view of the interconnect prior to the fabrication process. Thermoelectric elements 3001, 3003 are positioned with a metal interconnect layer 3002 sandwiched between their respective contact interfaces.

[0033] 4 shows a cross-section of the interconnect after the fabrication process. The thermoelectric elements 4001, 4003 were partially dissolved in the liquid interconnect metal and recrystallized during the cooling process. Such recrystallization can be in the form of pillars 4004 connecting the thermoelectric elements 4001, 4003. Between the pillars, the solidified interconnect metal 4002 forms a conductive contact.

[0034] 5 shows a cross section of the interconnect after the manufacturing process: one of the two thermoelectric elements 5001 is connected to a connecting element 5003 of the same material through a recrystallized element-interconnect metal layer 5005. The connecting element 5003 is then connected to a second thermoelectric element through a recrystallized element-interconnect metal layer 5004.

[0035] 6 shows a cross section of another thermoelectric device after the fabrication process. Thermoelectric elements 6001 and 6002 are connected together via a recrystallized thermoelectric element-metal interconnect layer 6003. Onto the thermoelectric element 6001, a third silicon, silicon composite, silicon alloy, or metal-silicide based component 6004 is conductively connected using the same interconnect process 6005. Such a structure is useful as a heat exchanger when the heat flux across the thermoelectric system is transferred from a liquid or gaseous material.

[0036] 7 shows a micrograph of an actual cross section of two thermoelectric elements 7001, 7003 connected according to one embodiment of the present invention. In the recrystallized interconnect zone, the interconnect metal 7002 is visible as a bright area. Between the interconnect metal 7002, the thermoelectric material has been recrystallized 7004.

[0037] FIG. 8 shows the phase diagram of the silver-silicon system according to R.W. Olesinski and G.J. Abbaschian (Binary Alloy Phase Diagrams, American Society for Metals, 1986). The dashed line 8004 indicates the processing temperature of 1000° C. In a typical embodiment of the invention, there will be a large amount of silicon in the thermoelectric element and a limited amount of liquid silver. The system will therefore be at a thermodynamic steady-state point 8001. During cooling, the system will evolve along the solid line Si-liquid Ag towards the eutectic point 8002. During this cooling period, the grey area 8003 indicates the amount of silicon that must solidify under steady-state conditions. It should be clear that this two-element system is a simplification of the actual system and only serves to illustrate the principles.

[0038] FIG. 9 shows a schematic cross-section of an actual thermoelectric conversion device fabricated according to one embodiment of the present invention.

[0039] As an example, a phosphorus-doped SiGe alloy can be used to fabricate a first type of n-type conductive thermoelectric element 9001, and a boron-doped SiGe can be used as a second type of p-type conductive thermoelectric element 9002, and these first and second elements 9001, 9002 can be interconnected between the first element 9001 and the connecting element 9003, and between the second element 9002 and the connecting element 9003, using a connecting element 9003 and a silver interconnect metal, similar to that shown in FIG. 5.

[0040] All components are mounted in a positioning fixture with a layer of Ag interconnect metal between the contacting surfaces. During a furnace process in which the Ag interconnect metal layer is melted, an interface is produced according to the invention. The furnace process can have an overhead temperature higher than the melting point of Ag of 962°C, such as 1000°C. After holding the overhead temperature for a period of time to allow dissolution of material from the thermoelectric element components in the interconnect metal melt, cooling initiates a recrystallization process. Depending on the change in solidification temperature due to the melted components of the thermoelectric element, the solidification temperature will vary from the melting temperature of Ag.

[0041] For manufacturing purposes, the Ag interconnect metal layer in this example may be applied in the form of an Ag foil that is placed between the thermoelectric elements, other application methods are evaporation of Ag on the surface, plating of an Ag layer, or screen printing a paste containing Ag particles, however many other manufacturing processes such as chemical or physical vapor deposition, plasma deposition, or sputtering are well known in the art and can be applied in accordance with the present invention.

[0042] Such interconnect metallurgy may include: - Does not react with silicon and does not form interconnecting metal-silicide phases in the solid state . - either the first thermoelectric element or the second thermoelectric element Reno At temperatures below the melting point too It will melt, - in the molten state, it will dissolve at least one of the components of the thermoelectric element, preferably the silicon element, and most preferably all components of the thermoelectric element in the composition present in the element, with the solubility of the components of the thermoelectric element in the molten interconnect metal being limited to a certain value but increasing if the temperature of the liquid interconnect metal is increased; - In the solid state, any of the components of the thermoelectric element Regarding this It is also possible to use other metals or metal alloys that are characterized by having low solubility.

[0043] Commercially available examples of such interconnect metal alloys are, for example, AgAl, or AgGe. Other metals exhibiting the desired characteristics are, for example, Zn, Sn, Al, Ge. Also Au, Be, and Sb have these desired characteristics. It is clear that alloys or mixtures of metals from these families can also be applied.

[0044] It is also possible to use mixtures or alloys of such interconnect metals with the components of the thermoelectric element, and such compositions can be useful for controlling the melting and solidification temperatures, as well as the amount of melted components of the thermoelectric element.

[0045] Furthermore, it should be mentioned that since the operating temperatures within the thermoelectric device at the interfaces are typically different, it may be advantageous to apply different interconnect metals, for example, to the hot side of the thermoelectric generator and to the cold side of the thermoelectric generator. Such a thermoelectric device may use Ag interconnect metal for establishing the interconnection of the elements of the thermoelectric device in areas operating at high temperatures, in combination with the lower melting temperature Zn for establishing the interconnection of a portion of the thermoelectric device in the colder areas. It is now clear that by using the present invention for the high temperature interconnects, thermoelectric devices combining the present invention with other known interconnection processes in the colder portions are possible.

[0046] The interconnection method of the present invention also allows for mechanical, thermal and electrical interconnection of thermoelectric elements of the same type or other structural components as part of a thermoelectric generator. Thus, the method can be used to attach structural components such as highly thermally conductive fins of a heat exchanger to thermoelectric elements. Another possibility is to create more complex geometries of thermoelectric elements of the same type by connecting them together with the interconnection process of the present invention. This allows for a very efficient and flexible design of thermoelectric generators, as will be apparent to those skilled in the art.

[0047] Another example is the use of a high manganese silicide material with, for example, vanadium, chromium, or aluminum dopants as the p-type thermoelectric element in combination with a high manganese silicide material with iron or ruthenium dopants as the n-type thermoelectric element.

[0048] Provided that the thermal expansion coefficients of the silicide materials are sufficiently matched, it is also possible to combine silicides from different families in the manufacturing process described in the present invention. Such material combinations are typically found when the thermoelectric or structural materials differ only in minor components, such as the addition of dopants or small percentages of alloying components.

[0049] In one embodiment, the method of the present invention uses a single high-temperature process that allows the thermoelectric device to be manufactured in a controlled manner. The process itself can be described as mechanically stacking a thermoelectric silicon alloy in contact with an interconnect metal material. This mechanical stack is heated in a gas atmosphere, which substantially prevents the formation of surface oxides in a furnace where the mechanical stack is heated to a temperature where only the interconnect metal, as the component with the lowest melting temperature, becomes liquid. As soon as the interconnect metal becomes liquid, components from the thermoelectric material will be melted in the interconnect metal up to their solubility limit. The amount of melted components of the thermoelectric element can be controlled by overheating the melt depending on the amount and solubility of the liquid interconnect metal. After a certain holding time, the furnace temperature will be reduced to allow the solidification of the melted components of the thermoelectric element from the interconnect metal melt. At the solidification temperature of the mixture of the molten interconnect metal and the melted components of the thermoelectric element, the system will solidify.

[0050] It will be clear to those skilled in the art that this process can be easily modified by changing the process environment (vacuum, protective gas, reducing atmosphere), process time, and process temperature. It may be useful to enforce a time interval along with the holding temperature to allow surface contaminants such as water to leave the surface of the components in the furnace during heating. Also, surface oxides of silver or metal components can be removed in a suitable heating cycle. It is also possible and advantageous to lower the melting temperature of the interconnect metal by adding alloying materials. There are many other mixtures or alloy compositions possible for the interconnect metal, as long as the interconnect metal components do not form a silicide phase. Such non-silicide forming materials are, for example, Ag, Al, Ge, Sn, Zn. Also, Au, Be, and Sb can be used.

[0051] In this process, the desired layered structure is formed in a single process step, although a two-step process using different interconnect metals at different furnace temperatures will now become apparent.

[0052] In the foregoing description of the drawings, the invention has been described with reference to specific embodiments thereof. However, it will be apparent that various modifications and changes can be made without departing from the scope of the invention as outlined in the appended claims.

[0053] In addition, modifications may be made to adapt to a particular situation or material to the teachings of the invention without departing from its essential scope. Therefore, it is not intended that the invention be limited to the particular embodiments disclosed, but the invention will include all embodiments falling within the scope of the appended claims.

[0054] In particular, combinations of specific features of the various aspects of the invention may be made. One aspect of the invention may be further advantageously enhanced by the addition of features that have been mentioned in relation to another aspect of the invention.

[0055] It is to be understood that the present invention is limited only by the appended claims and their technical equivalents. In this specification and in the claims, the verb "comprise" and its conjugations are used in their open-ended sense to mean that the items following the word are included without excluding items not specifically mentioned. Furthermore, the reference of an element by the indefinite article "a" or "an" does not exclude the possibility of the presence of a plurality of those elements, unless the context clearly requires that there is only one of those elements. Thus, the indefinite article "a" or "an" usually means "at least one". The following is a summary of the claims as originally filed: [1] A thermoelectric conversion device comprising at least a first active thermoelectric element and a second active thermoelectric element, each of the first active thermoelectric element and the second active thermoelectric element being based on a silicon-containing material, further comprising an interconnect zone between the first active thermoelectric element and the second active thermoelectric element, the interconnect metallic phase material being a recrystallized thermoelectric element constituent phase material, the interconnect metallic phase material being does not react with silicon and does not form metal-silicide phases in the solid state; melts at a temperature below the melting point of either the first active thermoelectric element material or the second active thermoelectric element material; in a molten state, melting at least one of the components of the thermoelectric element, preferably silicon, and most preferably all of the components of said thermoelectric element, while the solubility of one or more components of said thermoelectric element in the melt is limited but increases with increasing temperature; A thermoelectric conversion device, characterized in that any of the components of said thermoelectric element in a solid state has a solubility that is lower than the solubility of said components in a molten state. [2] The thermoelectric conversion device of [1], wherein the silicon-containing material comprises one selected from the group consisting of silicon, a silicon composite, a silicon alloy, or a metal-silicide. [3] The thermoelectric conversion device of [1] or [2], wherein the interconnect metallic phase material forms a junction between two portions of the first active thermoelectric element or the second active thermoelectric element. [4] The thermoelectric conversion device of any one of [1] to [3], wherein the interconnecting metallic phase material is in contact with one or more other functional components of the thermoelectric conversion device that provide thermal or electrical conductivity in the thermoelectric conversion device, each of the other functional components being based on the silicon-containing material. [5] The thermoelectric conversion device according to any one of [1] to [4], wherein the interconnecting metallic phase material is based on at least one element from the group consisting of Ag, Al, Ge, Sn, Zn, or a mixture or alloy of at least two elements from said group. [6] The thermoelectric conversion device according to any one of [1] to [5], wherein the interconnecting metallic phase material is based on at least one element from the group comprising Ag, Al, Ge, Sn, Zn, or a mixture or alloy of at least two elements from said group plus one or more of the components of the thermoelectric material. [7] The thermoelectric conversion device of any one of [1] to [6], wherein the interconnect metallic phase material has a thickness at the start of the interconnect process of between 5 μm and 500 μm. [8] A thermoelectric conversion device according to any one of [1] to [7], comprising a first interconnect metal phase and a recrystallized thermoelectric element component phase for interconnecting components of the thermoelectric device in the region of a hot side junction, and a second interconnect metal phase and a second recrystallized thermoelectric element component phase for interconnecting components of the thermoelectric device in the region of a cold side junction. [9] A method for manufacturing a thermoelectric device according to any one of [1] to [8], comprising the steps of: Assembling at least a first active thermoelectric element and a second active thermoelectric element with a first interconnect metal disposed between first surfaces to which the first active thermoelectric element and the second active thermoelectric element will be connected, the assembly having a desired geometry of the thermoelectric device to be formed; heating the assembly of the first active thermoelectric element and the second active thermoelectric element to a first temperature above a freezing point of the first interconnect metal to create a first liquid interconnect metal while allowing components of the first active thermoelectric element and the second active thermoelectric element to dissolve in the first liquid interconnect metal; cooling the assembly in a controlled manner to form a first interconnect zone between the first surfaces of the first and second active thermoelectric elements, the first interconnect metallic phase material and a first recrystallized thermoelectric element component phase material. A method for providing the above.

[10] during the heating of the assembly, a component of the silicon-containing material dissolves into the liquid interconnect metal at an interface between the interconnect metal and one or more functional components of the thermoelectric conversion device; and during cooling, an interconnect zone is formed at said interface comprising a recrystallized metallic phase and a recrystallized silicon-containing material. The manufacturing method described in [9], further comprising:

[11] during the assembly of at least the first active thermoelectric element and the second active thermoelectric element having a desired geometry of the thermoelectric device to be formed; and disposing a second interconnect metal disposed between a second surface to which the first active thermoelectric element and the second active thermoelectric element will be connected; heating the assembly of the first active thermoelectric element and the second active thermoelectric element to the first temperature above a freezing point of the second interconnect metal includes creating a second liquid interconnect metal while allowing components of the first active thermoelectric element and the second active thermoelectric element to dissolve in the second liquid interconnect metal; the controlled cooling of the assembly includes forming a second interconnect zone between the second surfaces of the first active thermoelectric element and the second active thermoelectric element, the second interconnect zone being comprised of a second recrystallized metallic phase material and a second recrystallized thermoelectric element component phase material; The method of any one of [9] to

[10] , wherein the second interconnect metallic phase material is different from the first interconnect metallic phase material.

[12] forming the first interconnect zone between the first surfaces of the first active thermoelectric element and the second active thermoelectric element, the first interconnect zone being comprised of the first recrystallized metallic phase material and the first recrystallized thermoelectric element component phase material; disposing a second interconnect metal disposed between a second surface to which the first active thermoelectric element and the second active thermoelectric element will be connected; heating the assembly of the first active thermoelectric element and the second active thermoelectric element to a second temperature above a freezing point of the second interconnect metal to create a second liquid interconnect metal while allowing components of the first active thermoelectric element and the second active thermoelectric element to dissolve in the second liquid interconnect metal; and controlling cooling of the assembly to form a second interconnection zone between the second surfaces of the first active thermoelectric element and the second active thermoelectric element, the second interconnection zone being comprised of a second recrystallized metallic phase material and a second recrystallized thermoelectric element component phase material; The method of any one of claims 9 to 10, wherein the second interconnect metal is different from the first interconnect metal and the second temperature is lower than the first temperature.

[13] The method according to any one of [9] to

[12] , wherein the interconnect metallic phase material is mainly based on at least one element from the group comprising Ag, Al, Ge, Sn, Zn, or a mixture or alloy of at least two elements from said group.

[14] The method according to any one of [9] to

[12] , wherein the interconnect metal is based on at least one element from the group of Ag, Al, Ge, Sn, Zn, or a mixture or alloy of at least two elements from said group plus one or more of the components of the thermoelectric material.

[15] The method of any one of [9] to

[14] , wherein the interconnect metal has an initial thickness of between 5 μm and 500 μm when disposed between the surfaces to which the first active thermoelectric element and the second active thermoelectric element will be connected, prior to heating of the assembly.

Claims

1. A thermoelectric conversion device comprising at least a first active thermoelectric element and a second active thermoelectric element, each of the first active thermoelectric element and the second active thermoelectric element being based on a silicon-containing material, the thermoelectric conversion device further comprising an interconnect zone between the first active thermoelectric element and the second active thermoelectric element, the interconnect zone being made of an interconnect metallic phase material and a recrystallized thermoelectric element constituent phase material; The interconnect metallic phase material comprises: does not react with silicon and does not form metal-silicide phases in the solid state; melts at a temperature below the melting point of either the material of the first active thermoelectric element or the material of the second active thermoelectric element; In the molten state, at least silicon of the components of the thermoelectric element is melted, while the solubility of one or more components of the thermoelectric element in the melt is limited but increases with increasing temperature; having a lower solubility for any of the components of the thermoelectric element in the solid state than the solubility thereof in the molten state; A thermoelectric conversion device comprising:

2. 10. The thermoelectric conversion device of claim 1, wherein the silicon-containing material comprises one selected from the group comprising silicon, a silicon composite, a silicon alloy, or a metal-silicide.

3. The thermoelectric conversion device of claim 1 or 2, wherein the interconnect metallic phase material forms a junction between two portions of the first active thermoelectric element or the second active thermoelectric element.

4. The thermoelectric conversion device according to any one of claims 1 to 3, wherein the interconnecting metallic phase material is based on at least one element from the group comprising Ag, Al, Ge, Sn, Zn, or a mixture or alloy of at least two elements from said group.

5. 5. The thermoelectric conversion device according to claim 1, wherein the interconnecting metallic phase material is based on at least one element from the group comprising Ag, Al, Ge, Sn, Zn, or a mixture or alloy of at least two elements from said group plus one or more of the components of the materials of the first and second active thermoelectric elements.

6. 6. The thermoelectric conversion device according to claim 1, wherein the interconnection zone comprises a first interconnection zone in the region of the high temperature side junction, the first interconnection zone being made of a first interconnect metallic phase material and a first recrystallized thermoelectric element component phase material for interconnecting components of the thermoelectric conversion device, and a second interconnection zone in the region of the low temperature side junction, the second interconnection zone being made of a second interconnect metallic phase material and a second recrystallized thermoelectric element component phase material for interconnecting components of the thermoelectric conversion device.

7. 1. A method for manufacturing a thermoelectric conversion device, comprising: Assembling at least a first active thermoelectric element based on a silicon-containing material and a second active thermoelectric element based on a silicon-containing material with a first interconnect metal disposed between first surfaces to which the first active thermoelectric element and the second active thermoelectric element are to be connected, the assembly having a desired geometry of the thermoelectric conversion device to be formed; heating the assembly of the first and second active thermoelectric elements to a first temperature above a freezing point of the first interconnect metal to allow components of the first and second active thermoelectric elements to dissolve in a first liquid interconnect metal to create the first liquid interconnect metal; and cooling the assembly in a controlled manner to form a first interconnect zone between the first surfaces of the first active thermoelectric element and the second active thermoelectric element, the first interconnect zone being comprised of a first interconnect metallic phase material and a first recrystallized thermoelectric element component phase material; The first interconnect metallic phase material comprises: does not react with silicon and does not form metal-silicide phases in the solid state; melts at a temperature below the melting point of either the material of the first active thermoelectric element or the material of the second active thermoelectric element; In the molten state, at least silicon of the components of the thermoelectric element is melted, while the solubility of one or more components of the thermoelectric element in the melt is limited but increases with increasing temperature; having a lower solubility for any of the components of the thermoelectric element in the solid state than the solubility thereof in the molten state; A method for manufacturing a thermoelectric conversion device.

8. 8. The method of claim 7, wherein the first interconnect metallic phase material has a thickness between 5 μm and 500 μm at the start of the interconnect process.

9. while forming at least the first active thermoelectric element and the second active thermoelectric element into the assembly having a desired geometry of the thermoelectric conversion device to be formed; and disposing a second interconnect metal disposed between a second surface to which the first active thermoelectric element and the second active thermoelectric element are to be connected; heating the assembly of the first active thermoelectric element and the second active thermoelectric element to the first temperature above a freezing point of the second interconnect metal includes allowing components of the first active thermoelectric element and the second active thermoelectric element to dissolve in a second liquid interconnect metal to create the second liquid interconnect metal; Controlled cooling of the assembly includes forming a second interconnect zone between the second surfaces of the first active thermoelectric element and the second active thermoelectric element, the second interconnect zone being comprised of a second interconnect metallic phase material and a second recrystallized thermoelectric element constituent phase material; The method of claim 7 or 8, wherein a second interconnect metallic phase material is different from the first interconnect metallic phase material.

10. After forming the first interconnect zone, disposing a second interconnect metal disposed between a second surface to which the first active thermoelectric element and the second active thermoelectric element are to be connected; heating the assembly of the first and second active thermoelectric elements to a second temperature above a freezing point of the second interconnect metal to allow components of the first and second active thermoelectric elements to dissolve in the second liquid interconnect metal to create the second liquid interconnect metal; and controlling cooling of the assembly to form a second interconnect zone between the second surfaces of the first and second active thermoelectric elements, the second interconnect zone being comprised of a second interconnect metallic phase material and a second recrystallized thermoelectric element component phase material; The method of claim 7 , wherein the second interconnect metal is different from the first interconnect metal, and the second temperature is lower than the first temperature.

11. 11. The method for producing a thermoelectric conversion device according to claim 9 or 10, wherein the first and second interconnecting metallic phase materials are mainly based on at least one element from the group comprising Ag, Al, Ge, Sn, Zn, or a mixture or alloy of at least two elements from said group.

12. 11. The method for producing a thermoelectric conversion device according to claim 9 or 10, wherein the first and second interconnecting metallic phase materials are based on at least one element from the group of Ag, Al, Ge, Sn, Zn, or a mixture or alloy of at least two elements from said group plus one or more of the components of the materials of the first and second active thermoelectric elements.

13. 13. The method of claim 9, wherein the first and second interconnect metallic phase materials have an initial thickness of between 5 μm and 500 μm when disposed between surfaces to which the first and second active thermoelectric elements are to be connected, prior to heating of the assembly.

Citation Information

Patent Citations

  • Manufacture of semiconductor device

    JP1990128425A

  • Thick film paste for fire-through in solar cells

    JP2010538466A

  • Thermoelectric conversion module and manufacturing method thereof

    JP2014049713A

  • Thermoelectric element

    WO1999034450A1