Two-wheel vehicle tire

The motorcycle tire design addresses the challenge of enhancing grip and stability by dividing the tread into specific rubber zones with tailored properties and additives, resulting in improved grip and stability without compromising workability or wear resistance.

WO2024241612A1PCT designated stage expired Publication Date: 2024-11-28BRIDGESTONE CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/043723
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-23
Filing Date
2023-12-06
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Motorcycle tires face challenges in achieving high grip properties and turning stability, particularly during high-speed turns, due to limitations in dry and wet grip performance, and existing methods to improve grip, such as adding fillers or resin, compromise workability and turning stability.

Method used

A motorcycle tire design with a tread portion divided into five parts, featuring center, traction, and edge rubbers with specific storage elastic modulus and loss tangent values, and containing fillers and resins, along with fine particle size silica, to enhance grip and stability without impairing workability.

Benefits of technology

The tire achieves improved grip and turning stability performance while maintaining workability and wear resistance, with the edge rubber containing fine particle size silica and a balanced filler and resin content, optimizing both dry and wet grip conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023043723_28112024_PF_FP_ABST
    Figure JP2023043723_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide a two-wheel vehicle tire having excellent grip performance, without impairing turning stability. In order to solve the problem, the present invention provides a two-wheel vehicle tire having a tread portion divided, on a tread portion surface, into five portions by a center portion including a tire equatorial plane, a pair of edge portions including tread ends, and a pair of traction portions between the center portion and each of the edge portions in the tire width direction, the two-wheel vehicle tire being characterized in that a storage modulus E' at 60° C in a center rubber forming the center portion, a traction rubber forming the traction portions, and an edge rubber forming the edge portions satisfies the following expressions (1) and (2). (1): E' of center rubber > E' of edge rubber > E' of traction rubber (2): E' of edge rubber > the average value of E' of center rubber and E' of traction rubber
Need to check novelty before this filing date? Find Prior Art

Description

Motorcycle tires

[0001] The present invention relates to a tire for a motorcycle.

[0002] Motorcycle tires are required to have high grip because the inclination of the tire's equatorial plane relative to the road surface increases when the vehicle is cornering. Grip can be broadly divided into dry grip (steering stability on dry roads) and wet grip (braking performance on wet roads). Motorcycle tires, especially sports tires, are also required to have high levels of handling stability.

[0003] Thus, it is desirable to achieve a high level of balance between dry grip performance and wet grip performance in the tread portion of motorcycle tires (see, for example, Patent Document 1). However, although the motorcycle tire of Patent Document 1 is suitable for long-distance driving on public roads, there is room for further improvement in dry grip performance and wet grip performance during high-speed cornering.

[0004] In order to improve the grip of the tread portion of motorcycle tires during high-speed cornering, methods of incorporating a large amount of filler into the tread portion have been studied. However, this method has the problem of deteriorating workability during tire production.

[0005] Furthermore, in order to further improve the grip performance described above, a method of incorporating a resin into the tread portion has been considered. However, when a resin is incorporated, the peak temperature of the loss tangent tanδ of the rubber in the tread portion increases, which results in a problem that the ease with which grip performance is expressed (operability) is not excellent.

[0006] JP 2016-112998 A

[0007] Therefore, an object of the present invention is to provide a motorcycle tire that has excellent gripping properties without impairing cornering stability.

[0008] The gist of the tire of the present invention that solves the above problems is as follows.

[0009] [1] A motorcycle tire comprising a pair of bead portions, a pair of sidewall portions, and a tread portion connected to both sidewall portions, wherein the tread portion is divided into five sections on the tread portion surface in the tire width direction by a center portion including the tire equatorial plane, a pair of edge portions including tread edges, and a pair of traction portions between the center portion and the edge portions, wherein the storage moduli E' at 60°C of a center rubber constituting the center portion, a traction rubber constituting the traction portions, and an edge rubber constituting the edge portions satisfy the following formulas (1) and (2): E' of center rubber > E' of edge rubber > E' of traction rubber (1) E' of edge rubber > average value of E' of center rubber and E' of traction rubber (2) The tire of the present invention described in [1] above has excellent grip without compromising cornering stability.

[0010] [2] The motorcycle tire according to [1], characterized in that the loss tangent tanδ of the center rubber, the traction rubber, and the edge rubber at 60°C satisfy the following formula (3): tanδ of edge rubber > tanδ of traction rubber > tanδ of center rubber (3). The motorcycle tire according to [2] above can achieve higher levels of cornering stability and grip.

[0011] [3] Peak temperature T of loss tangent of the center rubber, the traction rubber, and the edge rubber p is expressed by the following formula (4): T of traction rubber p > Edge rubber T p > Center rubber T p The motorcycle tire according to [1] or [2], characterized in that it satisfies the following condition (4): The motorcycle tire according to [4] above can achieve even better gripping properties.

[0012] [4] The motorcycle tire according to any one of [1] to [3], characterized in that the center rubber, the traction rubber, and the edge rubber all contain a filler, and the content of the filler is 100 parts by mass or more per 100 parts by mass of the rubber component. The motorcycle tire according to [4] above can achieve better gripping performance.

[0013] [5] The motorcycle tire according to any one of [1] to [4], wherein the center rubber, the traction rubber, and the edge rubber all contain oil and resin, and the total content of the oil and resin is 50 to 150 parts by mass per 100 parts by mass of the rubber component. The motorcycle tire according to [5] above can achieve better gripping performance without impairing workability during manufacturing.

[0014] [6] The motorcycle tire according to any one of [1] to [5], characterized in that the edge rubber contains fine particle silica having a cetyltrimethylammonium bromide adsorption specific surface area (CTAB) of at least 180. The motorcycle tire according to [6] above can achieve better gripping performance without impairing workability during manufacturing.

[0015] [7] The motorcycle tire according to any one of [1] to [6], wherein the edge rubber contains fine particle silica having a cetyltrimethylammonium bromide adsorption specific surface area (CTAB) of 180 or more. The motorcycle tire according to [7] above can achieve excellent wear resistance.

[0016] [8] The motorcycle tire according to [4], characterized in that the silica content in the filler of the edge rubber is less than 55% by mass. The motorcycle tire according to [8] can achieve better gripping performance without compromising workability during manufacturing.

[0017] According to the present invention, it is possible to provide a motorcycle tire that has excellent gripping performance without impairing cornering stability.

[0018] Fig. 1 is a schematic diagram showing a widthwise cross section of a motorcycle tire according to one embodiment of the present invention, and Fig. 2 is a schematic diagram showing a widthwise cross section of a motorcycle tire according to another embodiment of the present invention.

[0019] Hereinafter, embodiments of the present invention will be described. These descriptions are for the purpose of illustrating the present invention and are not intended to limit the present invention in any way.

[0020] In the present invention, the storage modulus E' at 60 ° C, the loss tangent tanδ at 60 ° C, and the peak temperature T p can be measured by the method described in the Examples.

[0021] In this specification, both dry grip property and wet grip property may be collectively referred to simply as grip property.

[0022] In the present invention, unless otherwise specified, the amount of a component in the rubber refers to the amount in each of the rubber in the center portion, traction portion and edge portion, and not the amount in the rubber in the entire tread portion.

[0023] In the present invention, Mw is calculated as a value converted into standard polystyrene by gel permeation chromatography (GPC).

[0024] <Tire for Motorcycles> A tire for motorcycles according to the present invention includes a pair of bead portions, a pair of sidewall portions, and a tread portion continuous with both sidewall portions, wherein the tread portion is divided into five portions on the surface of the tread portion in the tire width direction: a center portion including the tire equatorial plane, a pair of edge portions including tread ends, and a pair of traction portions between the center portion and the edge portions.

[0025] The tire of this embodiment has a carcass layer including steel cords, the steel cords being composed of steel filaments, and 20 mass % or more of the total mass of the steel filaments in the carcass layer being derived from recycled iron. When the proportion of the steel filaments derived from recycled iron in the entire steel cords of the carcass layer is 20 mass % or more, resources can be fully recycled while suppressing a decrease in durability of the carcass layer.

[0026] Here, Fig. 1 is a schematic diagram showing a widthwise cross section of a motorcycle tire according to one embodiment of the present invention. In Fig. 1, a motorcycle tire 10 includes a pair of bead portions 11, a pair of sidewall portions 12, and a tread portion 13 connected to both sidewall portions 12. The tread portion 13 is divided into five portions on the tread surface in the tire width direction: a center portion 15 including a tire equatorial plane 14, a pair of edge portions 17 including tread edges 16, and a pair of traction portions 18 between the center portion 15 and the edge portions 17. In the example shown in Fig. 1, each bead portion 11 has a bead core 19, and one or more carcass layers 20 are provided between the pair of bead cores 19 so as to extend in a toroidal shape. The carcass layer 20 is formed by rubber-coating a plurality of carcass cords.

[0027] The tread portion 13 extends across both sidewall portions 12. In the present invention, as described above, the tread portion is a divided tread divided into five portions: a center portion, two traction portions, and two edge portions.

[0028] (Tread portion) As described above, the tread portion is a divided tread divided into five portions, and is characterized in that the storage moduli E' at 60°C of the center rubber constituting the center portion, the traction rubber constituting the traction portion, and the edge rubber constituting the edge portion satisfy the following formulas (1) and (2): E' of center rubber > E' of edge rubber > E' of traction rubber ... (1) E' of edge rubber > average value of E' of center rubber and E' of traction rubber ... (2)

[0029] When the tread portion is divided into five parts, the edge portion and the traction portion tend to be required to have grip performance during cornering, the center portion and the traction portion tend to be required to have grip performance during straight running, and the center portion tends to be required to have wear resistance. Therefore, in the present invention, by satisfying the above formula (1), it is possible to improve grip performance during cornering and wear resistance during straight running, and by satisfying the above formula (2), it is possible to achieve both cornering stability and grip performance.

[0030] The storage moduli E' at 60°C of the center rubber, traction rubber, and edge rubber are not particularly limited as long as they satisfy the relationships of the above formulas (1) and (2). For example, the storage modulus E' at 60°C of the center rubber can be set to 8 to 12 Pa, the storage modulus E' at 60°C of the traction rubber can be set to 4 to 8 Pa, and the storage modulus E' at 60°C of the edge rubber can be set to 7 to 11 Pa.

[0031] In addition, it is preferable that the loss tangent tanδ of the center rubber, the traction rubber, and the edge rubber at 60°C in the tread portion satisfy the following formula (3): tanδ of edge rubber > tanδ of traction rubber > tanδ of center rubber ... (3) When the loss tangent tanδ of the center rubber, the traction rubber, and the edge rubber at 60°C satisfy the above formula (3), grip performance, particularly grip performance during straight running, can be further improved.

[0032] The loss tangent tanδ of the center rubber, the traction rubber, and the edge rubber at 60° C. is not particularly limited as long as it satisfies the relationship of the above formula (3). For example, the loss tangent tanδ of the center rubber at 60° C. can be 0.20 to 0.30 Pa, the loss tangent tanδ of the traction rubber at 60° C. can be 0.28 to 0.42 Pa, and the loss tangent tanδ of the edge rubber at 60° C. can be 0.35 to 0.50 Pa.

[0033] Furthermore, the tread portion has a peak temperature Tp is expressed by the following formula (4): T of traction rubber p > Edge rubber T p > Center rubber T p It is preferable that the following condition (4) is satisfied: the peak temperature T p However, by satisfying the above formula (4), it is possible to improve grip performance while maintaining wear resistance. In the five-divided tread, grip performance is required particularly in cornering in the edge portion and traction portion, and wear resistance is required in the center portion. In order to ensure the grip performance of the tread rubber, it is effective to raise the peak temperature of the loss tangent tanδ of the tread rubber. However, if this peak temperature is raised, grip performance is not easily achieved unless the temperature of the rubber is high, resulting in low operability. Furthermore, if the peak temperature is raised, the elastic modulus of the tread rubber increases, making the rubber hard and making it difficult to follow the shape of the road surface. On the other hand, in order to improve the wear resistance of the tread rubber, it is effective to lower the peak temperature of the loss tangent tanδ of the tread rubber. Therefore, in the present invention, the peak temperatures T p However, by satisfying the above formula (4), the wear resistance is improved and the grip performance is also improved.

[0034] The peak temperature T of the loss tangent of the traction rubber and the edge rubber p is not particularly limited as long as it satisfies the above formula (4), but can be, for example, −40 to 20° C. In addition, from the viewpoint of achieving a higher balance between abrasion resistance and gripping properties, the peak temperature T p It is preferable that the temperature of the edge rubber is in the range of -10 to 5°C. p And the next highest traction rubber is T p The difference between the T and the T of the traction rubber is not particularly limited, but may be, for example, 1 to 15°C. p And the lowest center rubber T pThe difference between the temperature is not particularly limited, but can be, for example, 1 to 15°C.

[0035] (Rubber Composition Constituting Tread Portion) The rubber composition constituting the center rubber, the traction rubber, and the edge rubber in the tread portion (hereinafter, a rubber composition applicable to all of the center rubber, the traction rubber, and the edge rubber may be simply referred to as the "rubber composition") is not particularly limited as long as it satisfies the relationships of the above-mentioned formulas (1) and (2). As the rubber composition, for example, a rubber composition containing a rubber component and a filler can be used.

[0036] Rubber Component The rubber component contained in the rubber composition is not particularly limited, but from the viewpoint of improving grip performance and manufacturing workability, it preferably contains at least one selected from styrene-butadiene rubber (SBR) and butadiene rubber (BR), and it is preferable to contain both styrene-butadiene rubber (SBR) and butadiene rubber (BR).

[0037] The styrene-butadiene rubber (SBR) and butadiene rubber (BR) are relatively difficult to adhere to each other and have excellent fracture properties. Furthermore, the styrene-butadiene rubber is highly effective in improving the grip performance of tires, while the butadiene rubber is highly effective in improving abrasion resistance. Therefore, when the rubber component contains at least one selected from the styrene-butadiene rubber (SBR) and the butadiene rubber (BR), a rubber composition suitable for treads is obtained. The styrene-butadiene rubber (SBR) and the butadiene rubber (BR) may be unmodified or modified, or may be a blend of unmodified and modified rubbers.

[0038] In the rubber component, the total proportion of the styrene-butadiene rubber (SBR) and the butadiene rubber (BR) is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and may be 100% by mass. In the rubber component, the proportion of the styrene-butadiene rubber (SBR) is preferably 70% by mass or more, more preferably 80% by mass or more, and is preferably 100% by mass or less, more preferably 90% by mass or less. In addition, in the rubber component, the proportion of the butadiene rubber (BR) is preferably 0% by mass or more, more preferably 10% by mass or more, and is preferably 30% by mass or less, more preferably 20% by mass or less.

[0039] The rubber component may further contain other rubbers. In that case, the content of the other rubbers in the rubber component is preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 10% by mass or less, and may even be 0% by mass. Examples of such other rubbers include natural rubber (NR), isoprene rubber (IR), chloroprene rubber (CR), styrene-isoprene rubber (SIR), acrylonitrile-butadiene rubber (NBR), butyl rubber (IIR), and halogenated butyl rubber. These other rubbers may be used alone or in combination of two or more.

[0040] The rubber component may be partially or entirely oil-extended. However, when the rubber component is oil-extended, the extender oil is classified as an oil, which will be described later.

[0041] Filler: The rubber compositions constituting the center rubber, the traction rubber, and the edge rubber preferably further contain a filler in addition to the rubber component. When the rubber composition contains a filler, the content thereof is preferably 90 parts by mass or more, more preferably 100 parts by mass or more, and even more preferably 110 parts by mass or more, per 100 parts by mass of the rubber component. This can further improve physical properties such as grip, cornering stability, and abrasion resistance.

[0042] The filler preferably contains at least one of silica and carbon black, and more preferably contains both silica and carbon black, which can further improve physical properties such as grip, cornering stability, and abrasion resistance.

[0043] The carbon black reinforces the tread portion, improving the breaking characteristics, and also contributes to improving the grip performance of the tire.

[0044] The carbon black is not particularly limited, and examples thereof include GPF, FEF, HAF, ISAF, and SAF grade carbon black. These carbon blacks may be used alone or in combination of two or more. The carbon black may also be recycled carbon black.

[0045] In this specification, "recycled carbon black" refers to carbon black recovered from raw materials that are waste materials that have been recycled. Examples of the waste materials that have been recycled include rubber products (particularly vulcanized rubber products) containing carbon black, such as used rubber and used tires, and waste oil. "Recycled carbon black" differs from carbon black that is produced directly from hydrocarbons such as petroleum and natural gas, i.e., non-recycled carbon black. Note that "used" here refers not only to carbon black that has been discarded after actual use, but also to carbon black that has been produced but discarded without actually being used.

[0046] From the viewpoints of abrasion resistance and tire grip performance, the content of the carbon black in the rubber composition is preferably 10 parts by mass or more, and more preferably 20 parts by mass or more, per 100 parts by mass of the rubber component. Also, from the viewpoint of low heat buildup of the rubber composition, the content of the carbon black in the rubber composition is preferably 140 parts by mass or less, and more preferably 130 parts by mass or less, per 100 parts by mass of the rubber component.

[0047] The silica contributes to improving the grip performance (particularly wet grip performance) of a tire to which the rubber composition is applied.

[0048] The content of silica in the filler may be adjusted as appropriate. Silica may be used alone or in combination of two or more.

[0049] For example, when the rubber composition is used for the center rubber, the silica content relative to the total amount of the filler is 60 to 95% by mass, preferably 85 to 95% by mass. When the rubber composition is used for the traction rubber, the silica content relative to the total amount of the filler is 60 to 95% by mass, preferably 70 to 90% by mass. Furthermore, when the rubber composition is used for the edge rubber, the silica content relative to the total amount of the filler is 30 to 60% by mass, preferably 30% by mass or more and less than 55% by mass.

[0050] The silica is not particularly limited and can be appropriately selected depending on the purpose. Examples of silica include wet silica (hydrated silicic acid), dry silica (anhydrous silicic acid), calcium silicate, and aluminum silicate. Among these, wet silica and dry silica are preferred from the viewpoint of improving abrasion resistance and wet grip performance.

[0051] From the viewpoint of reducing environmental impact, silica derived from siliceous plants is also preferred as the silica. Examples of siliceous plants include mosses, ferns, horsetails, Cucurbitaceae, Urticaceae, and Gramineae plants. Among these plants, grasses are preferred. Examples of grasses include rice, bamboo, and sugarcane, with rice being preferred. Rice is widely cultivated for food and therefore can be procured locally over a wide area. Furthermore, rice husks are generated in large quantities as industrial waste, making it easy to secure a sufficient supply. Therefore, from the viewpoint of availability, silica derived from rice husks (hereinafter also referred to as "rice husk silica") is particularly preferred as silica. The use of rice husk silica allows for the effective use of rice husks, which are industrial waste, and also allows for the local procurement of raw materials near tire manufacturing plants, thereby reducing the energy and costs involved in transportation and storage, which is environmentally preferable from various viewpoints. The rice husk silica may be a powder of rice husk charcoal obtained by carbonizing rice husks by heating, or may be precipitated silica produced by a wet process using an alkali silicate aqueous solution, which is prepared by extracting rice husk ash generated when rice husks are burned as fuel in a biomass boiler with an alkali. The method for producing the rice husk charcoal is not particularly limited, and various known methods can be used. For example, rice husk charcoal can be obtained by pyrolyzing rice husks by steaming them in a kiln. The rice husk charcoal obtained in this manner can be pulverized using a known pulverizer (e.g., a ball mill), and then sorted and classified into a predetermined particle size range to obtain rice husk charcoal powder. The rice husk-derived precipitated silica can be produced by the method described in JP 2019-38728 A, for example.

[0052] The silica has a nitrogen adsorption specific surface area (BET method) of 80 m 2 / g or more 330m 2 The nitrogen adsorption specific surface area (BET method) of silica is preferably less than 80 m 2 / g or more, a tire using the rubber composition can be sufficiently reinforced. 2When the specific surface area of ​​silica is less than 100 m / g, the elastic modulus of the rubber composition does not become too high, and the wet grip performance of a tire using the rubber composition is improved. 2 / g or more, and 2 / g or more, and 2 / g or more, and 2 / g or more, and 2 / g or more, and 2 / g or more, and 2 / g or more, and 2 From the viewpoint of further improving the wet grip performance of the tire, the nitrogen adsorption specific surface area (BET method) of the silica is more preferably 300 m 2 / g or less, and 2 / g or less is more preferable, and 270m 2 It is more preferable that the tensile strength is 1 / g or less.

[0053] The silica preferably has a cetyltrimethylammonium bromide adsorption specific surface area (CTAB) of 150 m 2 / g or more, more preferably 150 to 300m 2 / g. CTAB is 150m 2 When the CTAB is 300 m / g or more, a tire to which the rubber composition is applied can be sufficiently reinforced. 2 When the modulus of elasticity of the rubber composition is not too high, the wet grip performance of a tire using the rubber composition is improved.

[0054] Furthermore, the silica contained in the rubber composition constituting the edge rubber is preferably fine-particle silica having a cetyltrimethylammonium bromide adsorption specific surface area (CTAB) of at least 180. This allows the motorcycle tire to achieve both higher levels of cornering stability and grip.

[0055] Oil and Resin The rubber compositions constituting the center rubber, the traction rubber, and the edge rubber preferably contain oil and resin, because this allows the motorcycle tire to achieve both higher levels of cornering stability and grip.

[0056] Furthermore, when the rubber composition contains oil and resin, the total content thereof is preferably 50 to 150 parts by mass, and more preferably 20 to 100 parts by mass, per 100 parts by mass of the rubber component, which can further improve cornering stability and grip performance of motorcycle tires without impairing wear resistance or handling stability.

[0057] The oil may be any oil contained in known rubber compositions, such as petroleum-based softeners such as aromatic oils, paraffinic oils, and naphthenic oils; and plant-based softeners such as palm oil, castor oil, cottonseed oil, and soybean oil.

[0058] The content of the oil is not particularly limited and can be adjusted as appropriate. For example, the content of the oil per 100 parts by mass of the rubber component is preferably 5 to 150 parts by mass, and more preferably 40 to 60 parts by mass. In the present invention, the oil may be an extender oil for the rubber component or a compounding agent, and the content refers to the combined amount of the extender oil content and the compounding agent content. From the viewpoint of workability, the mass ratio of extender oil to compounding agent oil is preferably 1:1 to 10:1.

[0059] The resin is not particularly limited and can be appropriately selected depending on the purpose. 5 based resin, C 5 -C 9 based resin, C 9 These resins may be used singly or in combination of two or more.

[0060] Said C 5 As a resin based on C, there is C obtained by thermal decomposition of naphtha in the petrochemical industry.5 and aliphatic petroleum resins obtained by (co)polymerizing the distillate. 5 The fraction usually contains olefinic hydrocarbons such as 1-pentene, 2-pentene, 2-methyl-1-butene, 2-methyl-2-butene, and 3-methyl-1-butene, and diolefinic hydrocarbons such as 2-methyl-1,3-butadiene, 1,2-pentadiene, 1,3-pentadiene, and 3-methyl-1,2-butadiene. 5 Commercially available resins can be used.

[0061] Said C 5 -C 9 The C-based resin is 5 -C 9 It refers to synthetic petroleum resin, 5 -C 9 Examples of the resin include petroleum-derived C 5 -C 11 The fraction was treated with AlCl 3 , B.F. 3 More specifically, copolymers containing styrene, vinyltoluene, α-methylstyrene, indene, etc. as the main component may be mentioned. 5 -C 9 As the resin, 9 Resins containing less of the above components are preferred from the viewpoint of compatibility with the rubber component. 9 "The above components are low" means that the C 9 This means that the above components are contained in an amount of less than 50% by mass, preferably 40% by mass or less. 5 -C 9 Commercially available resins can be used.

[0062] Said C 9 The C-based resin is 9 This refers to synthetic petroleum resins, such as AlCl 3 or BF 3 Using a Friedel-Crafts type catalyst such as C 9 It refers to a solid polymer obtained by polymerizing the fraction. 9Examples of the resin include copolymers containing indene, α-methylstyrene, vinyltoluene, etc. as main components.

[0063] The terpene resin is a solid resin obtained by blending turpentine, which is obtained simultaneously with the extraction of rosin from pine trees, or a polymerization component separated therefrom, and polymerizing the blend using a Friedel-Crafts catalyst. Examples of such resins include β-pinene resin and α-pinene resin. Terpene resins also include terpene-aromatic compound resins, representative examples of which include terpene-phenol resin and styrene-terpene resin. Terpene-phenol resins can be obtained by reacting terpenes with various phenols using a Friedel-Crafts catalyst, or by further condensing the terpene with formalin. Styrene-terpene resins can be obtained by reacting styrene with terpenes using a Friedel-Crafts catalyst. The terpenes used as raw materials are not particularly limited; monoterpene hydrocarbons such as α-pinene and limonene are preferred, with those containing α-pinene being more preferred, and α-pinene being particularly preferred.

[0064] The dicyclopentadiene resin is, for example, AlCl 3 or BF 3 This refers to a resin obtained by polymerizing dicyclopentadiene using a Friedel-Crafts catalyst such as

[0065] The resin may be, for example, C 5 A resin (C) copolymerized with the fraction and dicyclopentadiene (DCPD) 5 -DCPD-based resin). When the dicyclopentadiene-derived component is 50% by mass or more in the total amount of the resin, C 5 -DCPD-based resins are included in dicyclopentadiene-based resins. When the dicyclopentadiene-derived component is less than 50% by mass in the total amount of resin, C 5 -DCPD resin is C 5 The same applies to cases where a small amount of a third component is contained.

[0066] Furthermore, from the viewpoint of obtaining better grip performance of the tire, it is preferable that the rubber composition constituting the edge rubber contains a hydrogenated resin as the resin. The hydrogenated resin means a resin obtained by reducing and hydrogenating a resin.

[0067] In addition, the resins that can be used as raw materials for the hydrogenated resin include, among the above-mentioned resins, C 5 based resin, C 5 -C 9 based resin, C 9 Examples of resins that can be used include cyclopentadiene-based resins, terpene-based resins (including terpene-aromatic compound-based resins), and dicyclopentadiene-based resins. These resins may be used alone or in combination of two or more.

[0068] The hydrogenated resin used herein has a softening point of more than 110° C. and a weight average molecular weight of 200 to 1600 g / mol in terms of polystyrene.

[0069] If the softening point of the hydrogenated resin is 110°C or lower, the edge portion to which the rubber composition is applied cannot be sufficiently reinforced. From the viewpoint of the fracture characteristics and abrasion resistance of the tire, the softening point of the hydrogenated resin is preferably 116°C or higher, more preferably 120°C or higher, more preferably 123°C or higher, more preferably 126°C or higher, and even more preferably 128°C or higher. Furthermore, from the viewpoint of the grip performance of the tire, the softening point of the hydrogenated resin is preferably 160°C or lower, more preferably 150°C or lower, more preferably 145°C or lower, and even more preferably 141°C or lower.

[0070] Furthermore, if the weight-average molecular weight of the hydrogenated resin in terms of polystyrene is less than 200 g / mol, the hydrogenated resin will precipitate from the tire, making it difficult to fully exhibit the effects of the hydrogenated resin, and if it exceeds 1600 g / mol, the hydrogenated resin will be less compatible with the rubber component. From the viewpoint of suppressing precipitation of the hydrogenated resin from the tire and suppressing deterioration of the tire appearance, the weight-average molecular weight in terms of polystyrene of the hydrogenated resin is preferably 300 g / mol or more, preferably 400 g / mol or more, more preferably 500 g / mol or more, preferably 550 g / mol or more, more preferably 600 g / mol or more, more preferably 650 g / mol or more, and even more preferably 700 g / mol or more. Furthermore, from the viewpoint of improving the compatibility of the hydrogenated resin with the rubber component and further enhancing the effects of the hydrogenated resin, the polystyrene-equivalent weight average molecular weight of the hydrogenated resin is more preferably 1570 g / mol or less, more preferably 1530 g / mol or less, more preferably 1500 g / mol or less, more preferably 1470 g / mol or less, more preferably 1430 g / mol or less, more preferably 1400 g / mol or less, more preferably 1370 g / mol or less, more preferably 1330 g / mol or less, more preferably 1300 g / mol or less, more preferably 1200 g / mol or less, more preferably 1100 g / mol or less, more preferably 1000 g / mol or less, and even more preferably 950 g / mol or less.

[0071] The weight average molecular weight (Mw HR ) (unit: g / mol) of the hydrogenated resin to the softening point (Ts HR ) (unit: °C) ratio (Ts HR / Mw HR) is preferably 0.075 or more, more preferably 0.083 or more, more preferably 0.095 or more, more preferably 0.104 or more, more preferably 0.14 or more, more preferably 0.155 or more, and even more preferably 0.158 or more. HR / Mw HR The softening point and polystyrene-equivalent weight average molecular weight of the hydrogenated resin can be determined by the method described in the Examples below.

[0072] In addition, from the viewpoint of increasing the compatibility between the rubber component and the hydrogenated resin and further improving the grip performance of a tire using the rubber composition, the hydrogenated resin is preferably a hydrogenated C 5 based resin, hydrogenated C 5 -C 9 The resin is preferably at least one selected from the group consisting of hydrogenated dicyclopentadiene resins (hydrogenated DCPD resins) and hydrogenated terpene resins, and hydrogenated C 5 Resin and hydrogenated C 5 -C 9 It is more preferable that the resin is at least one selected from the group consisting of hydrogenated C 5 Furthermore, it is preferable that the resin has at least a hydrogenated DCPD structure or a hydrogenated cyclic structure in the monomer.

[0073] The content of the resin in the rubber composition constituting the center rubber, the traction rubber, and the edge rubber is not particularly limited and can be adjusted appropriately. For example, it is preferably 5 to 150 parts by mass, and more preferably 15 to 100 parts by mass, per 100 parts by mass of the rubber component.

[0074] Styrene-Based Thermoplastic Elastomer The rubber composition constituting the center rubber, the traction rubber, and the edge rubber may contain a styrene-based thermoplastic elastomer (TPS). The styrene-based thermoplastic elastomer (TPS) has a styrene-based polymer block (hard segment) and a conjugated diene-based polymer block (soft segment). The styrene-based polymer portion forms physical crosslinks to serve as crosslinking points, while the conjugated diene-based polymer block provides rubber elasticity. The double bonds of the conjugated diene-based polymer block (soft segment) may be partially or completely hydrogenated. Note that while the styrene-based thermoplastic elastomer (TPS) is thermoplastic, the rubber component (preferably, a diene-based rubber) is not. Therefore, in this specification, the styrene-based thermoplastic elastomer (TPS) is not included in the rubber component. The content of the styrene-based thermoplastic elastomer (TPS) is preferably in the range of 1 to 30 parts by mass per 100 parts by mass of the rubber component.

[0075] Examples of the styrene-based thermoplastic elastomer (TPS) include styrene / butadiene / styrene (SBS) block copolymers, styrene / isoprene / styrene (SIS) block copolymers, styrene / butadiene / isoprene / styrene (SBIS) block copolymers, styrene / isoprene (SI) block copolymers, styrene / butadiene / isoprene (SBI) block copolymers, styrene / ethylene / butylene / styrene (SEBS) block copolymers, styrene / ethylene / propylene / styrene (SEPS) block copolymers, styrene / ethylene / ethylene / propylene / styrene (SEEPS) block copolymers, styrene / ethylene / butylene (SEB) block copolymers, styrene / ethylene / propylene (SEP) block copolymers, and styrene / ethylene / ethylene / propylene (SEEP) block copolymers.

[0076] Other Components In addition to the rubber component, filler, oil, resin, and styrene-based thermoplastic elastomer described above, the rubber composition for tires of the present invention may contain, as necessary, various components commonly used in the rubber industry, such as silane coupling agents, antioxidants, stearic acid, zinc oxide (zinc white), vulcanization accelerators, vulcanizing agents, etc., appropriately selected within ranges that do not impair the object of the present invention. Commercially available products can be suitably used as these compounding ingredients.

[0077] Examples of the silane coupling agent include bis(3-triethoxysilylpropyl)tetrasulfide, bis(3-triethoxysilylpropyl)trisulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 2-mercaptoethyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, 3-trimethoxysilylpropyl-N,N-dimethylthiocarbamoyltetrasulfide, 3-triethoxysilylpropyl-N ,N-dimethylthiocarbamoyl tetrasulfide, 2-triethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, 3-trimethoxysilylpropyl benzothiazolyl tetrasulfide, 3-triethoxysilylpropyl benzothiazolyl tetrasulfide, 3-triethoxysilylpropyl methacrylate monosulfide, 3-trimethoxysilylpropyl methacrylate monosulfide, bis(3-diethoxymethylsilylpropyl)tetrasulfide, 3-mercaptopropyldimethoxymethylsilane, dimethoxymethylsilylpropyl-N,N-dimethylthiocarbamoyl tetrasulfide, dimethoxymethylsilylpropyl benzothiazolyl tetrasulfide, etc. The content of the silane coupling agent is preferably in the range of 2 to 20 parts by mass, more preferably in the range of 5 to 15 parts by mass, per 100 parts by mass of the silica.

[0078] Examples of the antioxidant include N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine (6C), 2,2,4-trimethyl-1,2-dihydroquinoline polymer (TMDQ), 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline (AW), N,N'-diphenyl-p-phenylenediamine (DPPD), etc. The content of the antioxidant is not particularly limited, and is preferably in the range of 0.1 to 15 parts by mass, and more preferably 1 to 10 parts by mass, per 100 parts by mass of the rubber component.

[0079] Examples of the vulcanization accelerator include sulfenamide-based vulcanization accelerators, guanidine-based vulcanization accelerators, thiazole-based vulcanization accelerators, thiuram-based vulcanization accelerators, and dithiocarbamate-based vulcanization accelerators. Examples of the vulcanizing agent include sulfur. The total content of the vulcanization system (vulcanization package) containing the vulcanization accelerator, vulcanizing agent, and stearic acid is not particularly limited, and is preferably in the range of 1 to 25 parts by mass, and more preferably 5 to 20 parts by mass, per 100 parts by mass of the rubber component.

[0080] Tread Section The center rubber, traction rubber, and edge rubber constituting the tread section can be produced by blending components such as the rubber components described above, kneading them using a known kneading machine such as a Banbury mixer, roll, or internal mixer, and vulcanizing them. The components may be kneaded in a single stage or in two or more stages. For example, when kneading in two stages, the maximum temperature in the first stage of kneading is preferably 140 to 160°C, and the maximum temperature in the second stage is preferably 90 to 120°C. The vulcanization conditions are not particularly limited, and known vulcanization conditions for motorcycle tires can be used.

[0081] As shown in Fig. 1, the periphery length (curved length) in the width direction on the surface of the tread portion of the center portion 15, the traction portion 18, and the edge portion 17 may be adjusted as appropriate. C is the curve length from point T1 to point T2. In FIG. 1, the curve length L in the width direction on the surface of the tread portion of the traction portion 18 is Sis the sum of the curve length from point T3 to point T1 and the curve length from point T4 to point T2. In FIG. 1, the curve length L in the width direction on the surface of the tread portion of the edge portion 17 is E is the sum of the curved length from the left tread edge 16 to point T3 and the curved length from the right tread edge 16 to point T4. In the present invention, the periphery length (curved length) does not include the length of the irregularities of the tread grooves.

[0082] The curve length L of the center portion 15 C is the overall curve length L of the tread surface in the width direction (i.e., the curve length L of the center portion 15) C , the curve length L of the traction portion 18 S and the curve length L of the edge portion 17 E The curve length L of the traction portion 18 is preferably 10 to 50%, and more preferably 20 to 40% of the curve length L of the traction portion 18. S is preferably 20 to 60% of the overall curve length L in the width direction of the tread surface, and more preferably 30 to 50%.

[0083] The curve length L of the edge portion 17 E is preferably 10 to 50% of the overall curve length L in the width direction of the tread surface, and more preferably 20 to 40%.

[0084] The tread portion 13 may be divided into five portions on the surface of the tread portion: a center portion 15, a traction portion 18, and an edge portion 17. The portion of the tread portion 13 adjacent to the carcass layer 20 may be a single portion (identical to either the center portion 15, the traction portion 18, or the edge portion 17), or may be divided into three portions (either the center portion 15 and the traction portion 18, the center portion 15 and the edge portion 17, or the traction portion 18 and the edge portion 17), or may be divided into five portions.

[0085] FIG. 2 is a schematic diagram showing a widthwise cross section of a motorcycle tire according to another embodiment of the present invention. The same reference numerals as in FIG. 1 denote the same objects. In FIG. 2, the tread portion 13 is divided into five parts on the surface of the tread portion 13 in the tire width direction: a center portion 15 including the tire equatorial plane 14; a pair of edge portions 17 including tread edges 16; and a pair of traction portions 18 between the center portion 15 and the edge portions 17. In the example shown in FIG. 2, the rubber in the center portion 15 functions as base rubber 21 on the carcass layer 20 side of the traction portions 18 and the edge portions 17. In the traction portion 18, the rubber of the traction portion 18 is provided on the base rubber 21, and in the edge portions 17, the rubber of the edge portions 17 is provided on the base rubber 21.

[0086] The motorcycle tire according to the present invention may be a tire for a motorcycle, and may be a tire for a motorbike. The motorcycle is not particularly limited and may be appropriately selected depending on the purpose, and examples include racing motorcycles, motorcycles for general public roads, motorcycles for on-road use, and motorcycles for off-road use. Among these, motorcycles in which the effects of the present invention are particularly likely to be exhibited are preferably motorcycles for general public roads and motorcycles for on-road use, and more preferably motorcycles for general public roads.

[0087] The motorcycle tire according to the present invention may be used as a tire for a motorcycle, and may be used as at least one of a front tire and a rear tire, or may be used as tires for both wheels.

[0088] The present invention will be described in more detail below by way of examples, but these examples are intended to illustrate the present invention and are not intended to limit the present invention in any way.

[0089] Example 1, Comparative Examples 1 to 4 Each rubber composition constituting the center rubber, traction rubber, and edge rubber was prepared in the compounding amounts (parts by mass) shown in Table 1. The prepared rubber compositions were used in the center, traction, and edge portions of the tread, and a prototype motorcycle tire (size: 180 / 55ZR17) was produced in a conventional manner, divided into five sections as shown in Figure 1. The ratios of the center, traction, and edge portions in the tread were L c = 30%, Ls = 40%, L E = 30%.

[0090] <Storage Modulus E' of Tread Rubber at 60°C> The storage modulus E' of the center rubber, traction rubber, and edge rubber obtained in each Example and Comparative Example was measured at 60°C. Specifically, the measurement was carried out using a spectrometer manufactured by Ueshima Seisakusho under conditions of 60°C, a frequency of 52 Hz, and a dynamic strain of 1.0%. Measurements were carried out for each of the center rubber, traction rubber, and edge rubber, and the results are shown in Table 1.

[0091] <Performance Evaluation> (1) Cornering Stability A test rider performed cornering on a dry road course for the motorcycle tires obtained in each Example and Comparative Example, and evaluated the feeling of stability during cornering. The evaluation results are shown in Table 1. The numerical values ​​are evaluated on a scale of 1 to 10, and are shown as the score difference from Comparative Example 1. The larger the positive numerical value, the better the performance compared to Comparative Example 1, and the larger the negative numerical value, the worse the performance.

[0092] (2) Grip (Dry Grip Test) For the motorcycle tires obtained in each Example and Comparative Example, a test rider performed various driving tests on a dry road course and evaluated the dry grip feeling of the tire during driving. The evaluation results are shown in Table 1. The numerical values ​​are evaluated on a scale of 1 to 10, and are shown as the score difference from Comparative Example 1. The larger the positive value, the better the result compared to Comparative Example 1, and the larger the negative value, the worse the result.

[0093] (3) Steering Stability For the motorcycle tires obtained in each Example and Comparative Example, a test rider evaluated the steering stability on a dry road course. The evaluation results are shown in Table 1. The numerical values ​​were evaluated on a scale of 10 points, and are shown as the score difference from Comparative Example 1. The larger the positive numerical value, the better the performance compared to Comparative Example 1, and the larger the negative numerical value, the worse the performance.

[0094]

[0095] * 1 BR: Butadiene rubber, manufactured by ENEOS Material Corporation, trade name "BR54" * 2 Low Tg SBR: Styrene-butadiene rubber, proportion of styrene units (bound styrene amount) = 17% by mass, manufactured by Asahi Kasei Corporation, trade name "TUFDENE1834" * 3 Medium Tg SBR: Styrene-butadiene rubber, proportion of styrene units (bound styrene amount) = 35.5% by mass, manufactured by Asahi Kasei Corporation, trade name "Tufden E581", oil-extended rubber containing 37.5 parts by mass of extender oil (liquid softener component, liquid at 25 ° C.) per 100 parts by mass of rubber component * 4 High Tg SBR: Styrene-butadiene copolymer rubber, manufactured by ENEOS Material Corporation, emulsion-polymerized styrene-butadiene copolymer rubber, product name "HP755B", oil-extended rubber containing 37.5 parts by mass of extender oil (liquid softener component, liquid at 25 ° C) per 100 parts by mass of rubber component * 5 Carbon black: manufactured by Asahi Carbon Co., Ltd., product name "Asahi #107" * 6 Silica: CTAB specific surface area = 150 m 2 / g * 7 Fine particle silica: CTAB specific surface area = 191 m 2 / g * 8 Oil: Liquid softener component (liquid at 25 ° C.), manufactured by JX Nippon Oil & Energy Corporation, trade name "A / O MIX" * 9 Resin A: Aliphatic petroleum resin, manufactured by Nippon Zeon Co., Ltd., Quinton M100 * 10 Resin B: C5C9 resin, manufactured by ENEOS Corporation, T-REZ RD104 * 11 Resin C: Hydrogenated resin (hydrogenated C5 resin), manufactured by Eastman, trade name "registered trademark Impera E1780", softening point = 130 ° C., weight average molecular weight (Mw) = 800 g / mol * 12 Resin D: Terpene phenol resin, manufactured by Yasuhara Chemical Co., Ltd., YS Polystar S145 * 14 Antioxidant A: Seiko Chemical Nonflex RD * 15 Antioxidant B: Ouchi Shinko Chemical Industry Co., Ltd., Nocrac 6C * 16 Vulcanization accelerator A: Soxinol (registered trademark) D, manufactured by Sumitomo Chemical Co., Ltd. *17 Vulcanization accelerator B: Nocceler (registered trademark) CZ-G, manufactured by Ouchi Shinko Chemical Industry Co., Ltd. *18 Vulcanization accelerator C: Nocceler TOT-N, manufactured by Ouchi Shinko Chemical Industry Co., Ltd. *19 Silane coupling agent: Product name "ABC-856" manufactured by Shin-Etsu Chemical Co., Ltd. *20 Other chemicals: total amount of wax, antioxidant, vulcanizing agent, vulcanization accelerator, vulcanization acceleration aid, workability improver, silane coupling agent, vulcanization acceleration aid, and workability improver. Note that the same parts were used in all examples and comparative examples.

[0096] It can be seen that the motorcycle tire of Example 1 is able to achieve both cornering stability and grip at a higher level than the motorcycle tires of Comparative Examples 1 to 3.

[0097] According to the present invention, it is possible to provide a motorcycle tire that has excellent gripping performance without impairing cornering stability.

[0098] 10: Motorcycle tire 11: Bead portion 12: Sidewall portion 13: Tread portion 14: Tire equatorial plane 15: Center portion 16: Tread edge 17: Edge portion 18: Traction portion 19: Bead core 20: Carcass layer 21: Base rubber

Claims

1. A motorcycle tire comprising a pair of bead portions, a pair of sidewall portions, and a tread portion connected to both sidewall portions, wherein the tread portion is divided into five portions on the tread portion surface in the tire width direction: a center portion including the tire equatorial plane, a pair of edge portions including tread ends, and a pair of traction portions between the center portion and the edge portions, wherein the storage moduli E' at 60°C of a center rubber constituting the center portion, a traction rubber constituting the traction portions, and an edge rubber constituting the edge portions satisfy the following formulas (1) and (2): E' of center rubber > E' of edge rubber > E' of traction rubber ... (1) E' of edge rubber > average value of E' of center rubber and E' of traction rubber ... (2).

2. The motorcycle tire according to claim 1, wherein the loss tangent tan δ of the center rubber, the traction rubber and the edge rubber at 60° C. satisfies the following formula (3): tan δ of edge rubber > tan δ of traction rubber > tan δ of center rubber ... (3).

3. Peak temperature T of the loss tangent of the center rubber, the traction rubber and the edge rubber p is expressed by the following formula (4): T of the traction rubber p > Edge rubber T p > Center rubber T p The tire for a motorcycle according to claim 1 or 2, characterized in that the following condition is satisfied:

4. A motorcycle tire as set forth in claim 1 or 2, characterized in that the center rubber, the traction rubber and the edge rubber all contain a filler, and the content of the filler is 100 parts by mass or more per 100 parts by mass of the rubber component.

5. A motorcycle tire as set forth in claim 1 or 2, characterized in that the center rubber, the traction rubber and the edge rubber all contain oil and resin, and the total content of the oil and resin is 50 to 150 parts by mass per 100 parts by mass of the rubber component.

6. A motorcycle tire as set forth in claim 1 or 2, characterized in that the edge rubber contains fine particle silica having a cetyltrimethylammonium bromide adsorption specific surface area (CTAB) of 180 or more.

7. A motorcycle tire as set forth in claim 1 or 2, characterized in that the edge rubber contains carbon black.

8. A motorcycle tire as set forth in claim 4, characterized in that the edge rubber has a silica content in the filler of less than 55 mass %.

9. A motorcycle tire as set forth in claim 5, characterized in that the edge rubber contains a hydrogenated resin as the resin.

Citation Information

Patent Citations

  • Tire

    JP2016112998A

  • Method for producing precipitated silica

    JP2019038728A

  • Tire for motorcycle

    JP2007168531A

  • Pneumatic tire for motorcycle

    JP2009051350A

  • Pneumatic tire for motorcycle

    JP2010023761A