NiCo-MOF co-immobilized glycosyl transferase and sucrose synthase as well as preparation method and application thereof
Co-immobilized glycosyltransferase and sucrose synthase through NiCo-MOF, the problems of instability of free enzymes and complex preparation of immobilized enzymes are solved, high loading, stability and reusability are achieved, and the ginseng saponin Rh2 is improved Conversion rate provides a low-cost, environmentally friendly industrial enzyme catalytic method.
Patent Information
- Application Number
- CN202411100789.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-01
AI Technical Summary
In the prior art, free enzymes are unstable and difficult to separate from the reaction system, the preparation process of immobilized enzymes is complex and costly, especially purification and environmental changes affect the enzyme activity, and the material synthesis time is long and costly.
Using NiCo-MOF co-immobilized glycosyltransferase and sucrose synthase, the one-step purification and immobilization is achieved by using Ni2+ and Co2+ in phosphate buffer to achieve one-step purification and immobilization, reducing material costs and environmentally friendly.
The high loading, stability and reusability of enzymes are achieved, the enzyme activity is maintained, and the conversion rate of ginseng saponin Rh2 is improved by optimizing the coupling reaction, providing a low-cost and environmentally friendly industrial enzyme catalytic method.
Smart Images

Figure CN118879675A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of preparation and application of immobilized enzyme biocatalysts, and in particular to NiCo-MOF co-immobilized glycosyltransferase and sucrose synthase, and a preparation method and application thereof. Background Art
[0002] The rare ginsenoside Rh2 has multiple biological functions such as anti-cancer, anti-aging, promoting cell differentiation and anti-tumor, but its content in ginseng is extremely low and it is difficult to directly extract and synthesize in large quantities, which limits the application of ginsenoside Rh2 in the medical, health care and other industries.
[0003] There are many methods for synthesizing the rare ginsenoside Rh2, mainly chemical synthesis, plant extraction and biotransformation. Biotransformation is widely used because it is more environmentally friendly while maintaining high yields. UDP-glucose (UDPG) is an important substrate for the synthesis of ginsenoside Rh2 as a glycosyl donor, but it is expensive. Therefore, the method of coupling glycosyltransferase with sucrose synthase is currently mainly applied to the biosynthesis of ginsenosides, so that it can increase the yield of Rh2 while regenerating UDPG.
[0004] However, the two enzymes used in this method are first purified and then directly put into the reaction in a free state. The purification operation is complicated and increases the cost. After being put into the reaction, they cannot be separated and continued to be used. The addition of organic solvents and environmental changes during the purification process will also affect the activity of the enzyme. Immobilized enzyme is a technology that fixes free biological enzymes on specific materials so that they can be separated from the reaction system for repeated use. It can not only reduce operating costs and maintain enzyme activity, but also improve the stability of the enzyme.
[0005] Metal organic frameworks (MOFs) have been widely used in immobilized enzymes due to their high specific surface area, adjustable and ultra-high porosity, and good thermal stability. Wang et al. embedded peroxidase in FeNi-MOF through a one-step biomimetic mineralization technique, and the immobilized enzyme showed high stability. Long et al. modified the hydrothermally synthesized CoCu-MOF-H with (3-aminopropyl) triethoxysilane (APTES), and then fixed laccase (Lac) with glutaraldehyde. The stability of the obtained Lac-CoCu-MOF-H-APTE was 1.8 times that of the free enzyme, and the removal rate of Congo red was still 89.18% after 6 cycles. However, the preparation method of the above-mentioned immobilized enzyme has certain defects, that is, the addition of organic solvents and organic ligands with acidity and alkalinity will cause the enzyme to lose a certain amount of activity before being fixed. Wang et al. successfully expressed OsEUGT11 (UGT1) and SrUGT76G1 (UGT2) in E. coli and covalently immobilized them on chitosan beads, retaining 72.5% and 53.1% of their original activities, respectively, while showing high stability. However, the operation of purifying the target protein from the crude enzyme solution and then immobilizing it is very cumbersome and costly.
[0006] The covalent binding of protein affinity tags to carriers provides an effective solution to these problems, such as the covalent binding of histidine tags to transition metal ions (Cu 2+ 、Zn 2+ 、Ni 2+ and Co 2+ etc.) to achieve enzyme immobilization. Andrade et al. used β-galactosidase as a model and synthesized magnetic nanoparticles (Fe3O4-His-Ni) functionalized with histidine and nickel as carriers for directional immobilization of recombinant enzymes, which showed higher substrate affinity and thermal stability (about 50 times) than free enzymes. After repeated use for 15 times, the hydrolysis rate of lactose was still over 50%. However, the synthesis time of the materials in the above methods is very long and requires a high cost, so it is very meaningful to find a balanced material. To this end, the present invention provides a NiCo-MOF co-fixed glycosyltransferase and sucrose synthase and a preparation method and application thereof. Summary of the invention
[0007] The present invention provides a NiCo-MOF co-immobilized glycosyltransferase and sucrose synthase, and a preparation method and application thereof, which effectively solve the problem that the free enzyme used in the preparation of ginsenoside Rh2 is unstable and difficult to separate from the reaction system, involving a complex purification process, and the addition of organic solvents and environmental changes during purification affect the enzyme activity; when immobilized enzymes are used, organic solvents and organic ligands with acidity and alkalinity cause the enzyme to lose enzyme activity before being immobilized, and the operation of purifying the target protein from the crude enzyme solution and then immobilizing it is very cumbersome and costly; the covalent binding of the protein affinity tag to the carrier solves this problem, and at the same time provides a simple, low-cost, environmentally friendly and rapid bimetallic NiCo-MOF specific adsorption enzyme, which successfully purifies and immobilizes the recombinant glycosyltransferase and the recombinant sucrose synthase in one step, and obtains the immobilized enzyme NiCo-MOF@UGT&SUSy with high load, strong stability and strong reusability, while maintaining the enzyme activity, and then converts it into a high-yield ginsenoside Rh2 by a coupling reaction.
[0008] The first object of the present invention is to provide a method for preparing NiCo-MOF co-immobilized glycosyltransferase and sucrose synthase, characterized in that it comprises the following steps:
[0009] To soluble Ni 2+ Salt and soluble Co 2+ Add H3BTC and NaOH mixture to the mixed salt solution and stir at room temperature to make Ni 2+ and Co 2+ Coordinate reaction with H3BTC, centrifuge, freeze-dry, and obtain NiCo-MOF powder;
[0010] The NiCo-MOF powder was dispersed in a phosphate buffer to obtain a dispersion, and a mixed enzyme solution of glycosyltransferase (UGT) and sucrose synthase (SUSy) was added to the dispersion, and the mixture was stirred at room temperature. 2+ and Co 2+ Specific adsorption of Ni to the histidine tag in glycosyltransferase and sucrose synthase 2+ and Co 2+ The glycosyltransferase and sucrose synthase are co-immobilized and centrifuged to obtain NiCo-MOF co-immobilized glycosyltransferase and sucrose synthase (NiCo-MOF@UGT&SUSy).
[0011] Preparation of phosphate buffer: The buffer contains 137mmol / L NaCl, 2.7mmol / L KCl, 10mmol / LNa2HPO4, and 2mmol / LKH2PO4. Weigh 7.946g of NaCl, 0.201g of KCl, 3.581g of Na2HPO4, and 0.272g of KH2PO4 to make a 1000mL solution, and adjust the pH to 7.4.
[0012] As a preferred embodiment, the soluble Ni 2+ The molar ratio of salt, H3BTC and NaOH is 1-3:1:3-3.5.
[0013] As a preferred embodiment, the mixed salt solution is an ethanol aqueous solution of mixed salts, and the soluble Ni 2+ Salt and soluble Co 2+ The molar ratio of the salt is 0.5-1.5:0.5-1.5.
[0014] As a preferred embodiment, the dosage ratio of the NiCo-MOF powder to the mixed enzyme solution of glycosyltransferase and sucrose synthase is 10 mg: 0.4-1.6 mL.
[0015] As a preferred embodiment, in the mixed enzyme solution of the glycosyltransferase and sucrose synthase, the concentrations of the glycosyltransferase and sucrose synthase are both 1.5 mg / mL, and the volume ratio is 1:1.2-1.7.
[0016] As a preferred embodiment, the soluble Ni 2+ The salt is NiCl2·6H2O, the soluble Co 2+ The salt is CoCl2·6H2O.
[0017] As a preferred embodiment, the glycosyltransferase is the glycosyltransferase gene GE02773 mined from the genome of Bacillus subtilis SL-44, and a glycosyltransferase expression engineering bacterium BL21-GE02773-28a is constructed, and induced to express as a soluble protein glycosyltransferase (UGT);
[0018] It should be noted that the Bacillus subtilis SL-44 genome used in the present invention is disclosed in Yufei Zhang et al. Heterologous expression of Bacillus subtilis SL-44glycosyltransferasecatalyzed synthesis of ginsenoside Rh2.Applied Mathematics and Nonlinear Sciences, pages 1-13, published on 20231011. The method disclosed in the paper can be used to obtain the glycosyltransferase SL-44 genome, express and prepare the glycosyltransferase expression engineering bacteria BL21-GE02773-28a, and induce its expression as a soluble protein glycosyltransferase (UGT);
[0019] As a preferred embodiment, the sucrose synthase is a sucrose synthase gene mined from the genome of the genus Mytilus punctatus, and a sucrose synthase expression engineering bacterium pRSF-McSUSy-S31D is constructed and induced to express as a soluble protein sucrose synthase.
[0020] It should be noted that the Micractinium genome used in the present invention is disclosed in Kai Chen et al. Identification of sucrose synthase from Micractinium conductrix to favor biocatalytic glycosylation. Frontiers in Microbiology, pages 1-11, published on 20230815. The Micractinium genome can be obtained by the method disclosed in the paper, and the sucrose synthase expression engineered bacteria pRSF-McSUSy-S31D can be expressed and prepared by gene mutation and plasmid construction, and induced to express as soluble protein sucrose synthase.
[0021] Specifically, 1% of the engineered bacteria BL21-GE02773-28a and pRSF-McSUSy-S31D were inoculated into 200 mL LB medium containing 25 μg / mL kanamycin, and cultured at 180 rpm and 37°C for a period of time until OD 600When the p-value reaches 0.6-0.8, IPTG with a final concentration of 0.1 mmol / L is added to induce expression, and the mixture is incubated at 16°C on a shaker for 21 hours to obtain an induced expression bacterial solution; the induced expression bacterial solution is centrifuged at 8000 rpm for 3 minutes, washed twice with PBS buffer at pH = 7.4, and then resuspended. The resuspended bacterial solution is then ultrasonically disrupted at 400 W in an ice water bath for 5 seconds, with an interval of 5 seconds for a total of 30 minutes. Finally, the solution is centrifuged at 4°C and 12000 rpm for 10 minutes, and the supernatants containing soluble proteins UGT and SUSy are collected respectively.
[0022] The second object of the present invention is to provide a NiCo-MOF co-immobilized glycosyltransferase and sucrose synthase prepared by the above preparation method.
[0023] The third object of the present invention is to provide an application of the above-mentioned NiCo-MOF co-immobilized glycosyltransferase and sucrose synthase in the synthesis of ginsenoside Rh2, characterized in that the application is: mixing protopanaxadiol, uridine diphosphate, sucrose and NiCo-MOF co-immobilized glycosyltransferase and sucrose synthase in a phosphate buffer solution with a pH of 7.4 in a mass ratio of 1:1:10:8-12, shaking in a water bath at 35-40°C for 2-4h, extracting with n-butanol, centrifuging, and freeze-drying to obtain ginsenoside Rh2.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] (1) The present invention provides a NiCo-MOF co-immobilized glycosyltransferase and sucrose synthase and a preparation method and application thereof. Using cheap trimesic acid as a ligand, NiCo-MOF with better performance is prepared in a short time through exploration and optimization, and then Ni 2+ and Co 2+ The specific adsorption of the his tag was used to co-immobilize the recombinant glycosyltransferase (UGT) and recombinant sucrose synthase (SUSy) while purifying them, and the NiCo-MOF-immobilized glycosyltransferase and sucrose synthase (NiCo-MOF@UGT&SUSy) were obtained. The immobilized enzyme can be reused while maintaining the enzyme activity, and finally applied to the optimization of the coupling reaction to convert the target product PPD-type ginsenoside Rh2. The materials used in the present invention are all clean energy and the preparation process is simple. The loading amount, enzyme activity, morphology, reusability, stability and other aspects of the immobilized enzyme were studied and optimized, and the conversion mechanism was revealed through molecular docking. The present invention provides new insights for the use of his tag to immobilize enzymes, and also lays a foundation for the industrial implementation of enzyme-catalyzed synthesis of high-value-added natural products.
[0026] (2) The NiCo-MOF co-immobilized glycosyltransferase and sucrose synthase (NiCo-MOF@UGT&SUSy) prepared by the present invention has better pH stability, thermal stability, excellent reusability and storage stability. When the NiCo-MOF@UGT&SUSy prepared by the present invention is used as an enzyme biocatalyst to synthesize ginsenoside Rh2, a higher ginsenoside Rh2 conversion rate can be achieved.
[0027] (3) The preparation method of NiCo-MOF@UGT&SUSy provided by the present invention has simple and easy-to-obtain raw materials and low cost; the required equipment is very conventional and easy to prepare and control. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a SEM image of NiCo-MOF prepared in Example 1 of the present invention;
[0029] Figure 2 This is a SEM image of NiCo-MOF@UGT&SUSy prepared in Example 1 of the present invention;
[0030] Figure 3 This is an atomic force microscope image of NiCo-MOF@UGT&SUSy prepared in Example 1 of the present invention;
[0031] Figure 4 The SEM image and EDS element distribution map of NiCo-MOF@UGT&SUSy prepared in Example 1 of the present invention;
[0032] Figure 5 This is the energy dispersion spectrum of NiCo-MOF@UGT&SUSy prepared in Example 1 of the present invention;
[0033] Figure 6 The water contact angle diagrams of NiCo-MOF and NiCo-MOF@UGT&SUSy prepared in Example 1 of the present invention; wherein (a) is NiCo-MOF, and (b) is NiCo-MOF@UGT&SUSy;
[0034] Figure 7 Infrared spectra of NiCo-MOF and NiCo-MOF@UGT&SUSy prepared in Example 1 of the present invention, as well as free sucrose synthase SUSy and free glycosyltransferase UGT;
[0035] Figure 8 A proportional diagram of the secondary structures of free glycosyltransferase UGT, free sucrose synthase SUSy and NiCo-MOF@UGT&SUSy prepared in Example 1 of the present invention;
[0036] Fig. 9XRD patterns of NiCo-MOF and NiCo-MOF@UGT&SUSy prepared in the embodiments of the present invention; wherein (a) is NiCo-MOF and NiCo-MOF@UGT&SUSy prepared in Example 1, and (b) is NiCo-MOF@UGT&SUSy formed at different synthesis times;
[0037] Fig.10 TGA curves of NiCo-MOF and NiCo-MOF@UGT&SUSy prepared in Example 1 of the present invention;
[0038] Fig.11 Energy spectra of NiCo-MOF and NiCo-MOF@UGT&SUSy prepared in Example 1 of the present invention; wherein (a) is the total energy spectrum, (b) is the scanning image of Ni2p, (c) is the scanning image of Co2p, and (d) is the scanning image of N1s;
[0039] Fig.12 Figure 1 is a graph of thermal deformation kinetic parameters of UGT, SUSy, and NiCo-MOF@UGT&SUSy of the present invention; wherein (a) is an image of the thermal treatment activity change of the free enzyme UGT&SUSy, and (b) is an image of the treatment time and lnA of the free enzyme UGT&SUSy. RA (c) The relationship between the treatment temperature and lnk of the free enzyme UGT&SUSy, (d) The image of the change of the thermal treatment activity of NiCo-MOF@UGT&SUSy, (e) The relationship between the treatment time and lnA of NiCo-MOF@UGT&SUSy RA Relationship diagram, (f) Figure shows the relationship between treatment temperature and lnk of NiCo-MOF@UGT&SUSy;
[0040] Fig.13 Figures are related to recombinant UGT and recombinant SUSy; wherein (a) shows the alignment of homologous sequences of recombinant UGT, (b) shows the location of his tag and key amino acids of recombinant SUSy, and (c) shows the alignment of homologous sequences of recombinant SUSy;
[0041] Fig.14 This is an image showing the location of the his tag of the recombinant UGT of the present invention and its docking with PPD;
[0042] Fig.15 It is a two-dimensional visualization image of the docking of the recombinant UGT and PPD of the present invention;
[0043] Fig.16 This is an image of the docking of recombinant UGT and UDPG of the present invention;
[0044] Fig.17It is a two-dimensional visualization image of the docking of the recombinant UGT and UDPG of the present invention;
[0045] Fig.18 This is a schematic diagram of the combination of NiCo-MOF and his tag of the present invention;
[0046] Fig.19 The stability analysis diagrams are free glycosyltransferase UGT, free sucrose synthase SUSy, Ni-MOF@UGT&SUSy of comparative example 1, Co-MOF@UGT&SUSy of comparative example 2, and NiCo-MOF@UGT&SUSy of example 1; wherein (a) is a pH stability diagram, (b) is a temperature stability diagram, (c) is a storage stability diagram, and (d) is a diagram showing the yield of NiCo-MOF@UGT&SUSy in converting ginsenoside Rh2 and the reusability of NiCo-MOF@UGT&SUSy;
[0047] Fig. 20 The present invention is a flow chart of the preparation process of NiCo-MOF co-immobilized glycosyltransferase and sucrose synthase. DETAILED DESCRIPTION
[0048] In order to enable those skilled in the art to better understand the technical solution of the present invention and implement it, the present invention is further described below in conjunction with specific embodiments and drawings, but the embodiments are not intended to limit the present invention. The following test methods and detection methods, unless otherwise specified, are conventional methods; the reagents and raw materials, unless otherwise specified, are commercially available.
[0049] In view of the problems mentioned in the background technology of the present invention: first, when preparing ginsenoside Rh2, the free enzyme is unstable and difficult to separate from the reaction system, involving a complex purification process and the problem that the addition of organic solvents and environmental changes during purification affect the enzyme activity; second, when using immobilized enzymes, organic solvents and organic ligands with acidity and alkalinity cause the enzyme to lose a certain amount of enzyme activity before being fixed, and the operation of purifying the target protein from the crude enzyme solution and then fixing it is very cumbersome and costly; third, the cost problem is solved by covalently binding the protein affinity tag to the carrier. The present invention provides a NiCo-MOF co-fixed glycosyltransferase and sucrose synthase and a preparation method and application thereof. Using cheap trimesic acid as a ligand, NiCo-MOF with better performance is prepared in a short time through exploration and optimization, and then Ni 2+ and Co 2+The specific adsorption of the his tag is used to co-immobilize the recombinant glycosyltransferase (UGT) and the recombinant sucrose synthase (SUSy) while purifying them, and obtain NiCo-MOF-immobilized glycosyltransferase and sucrose synthase (NiCo-MOF@UGT&SUSy). The immobilized enzyme can be reused while maintaining the enzyme activity, and finally applied to the optimization of the coupling reaction to convert the target product PPD (protopanaxadiol) type ginsenoside Rh2. The immobilized glycosyltransferase UGT and sucrose synthase SUSy of the present invention have better pH stability, thermal stability, excellent reusability and storage stability.
[0050] The technical effects of the present invention are described below through embodiments and comparative examples.
[0051] Example 1
[0052] A method for preparing NiCo-MOF co-immobilized glycosyltransferase and sucrose synthase, such as Fig. 20 As shown, the following steps are included:
[0053] S1, dissolving 1 mmol H3BTC and 3 mmol NaOH in 15 mL water under magnetic stirring to form solution B; adding ethanol aqueous solution to a mixed salt of 1.5 mmol NiCl2·6H2O and 0.5 mmol CoCl2·6H2O to form solution C; slowly adding solution B to solution C, magnetically stirring at room temperature for 25 min, centrifuging at 10000 rpm for 3 min to obtain a precipitate, washing the precipitate with anhydrous ethanol and deionized water for 3 times, and freeze-drying to obtain NiCo-MOF powder;
[0054] S2, dispersing 10 mg of the NiCo-MOF powder in a phosphate buffer solution with a pH of 7.4 to obtain a dispersion, adding 1 mL of a mixed enzyme solution of glycosyltransferase (UGT) and sucrose synthase (SUSy) with a mass concentration of 1.5 mg / mL to the dispersion to make the total system reach 10 mL, the volume ratio of the glycosyltransferase (UGT) to the sucrose synthase (SUSy) is 1:1.5, magnetic stirring is carried out at room temperature for 2 h, and centrifugation is carried out at 10000 rpm for 5 min to obtain a precipitate, and the precipitate is washed 3 times with deionized water to obtain NiCo-MOF co-immobilized glycosyltransferase and sucrose synthase (NiCo-MOF@UGT&SUSy).
[0055] Example 2
[0056] A method for preparing NiCo-MOF co-immobilized glycosyltransferase and sucrose synthase, comprising the following steps:
[0057] S1, dissolving 1mmol H3BTC and 3mmolNaOH in 15mL water under magnetic stirring to form solution B; adding ethanol aqueous solution to a mixed salt of 1mmolNiCl2·6H2O and 1mmolCoCl2·6H2O to form solution C; slowly adding solution B to solution C, magnetically stirring at room temperature for 25min, centrifuging at 10000rpm for 3min to obtain a precipitate, washing the precipitate with anhydrous ethanol and deionized water for 3 times, and freeze-drying to obtain NiCo-MOF powder;
[0058] S2, dispersing 10 mg of the NiCo-MOF powder in a phosphate buffer solution with a pH of 7.4 to obtain a dispersion, adding 0.4 mL of a mixed enzyme solution of glycosyltransferase (UGT) and sucrose synthase (SUSy) with a mass concentration of 1.5 mg / mL to the dispersion to make the total system reach 10 mL, the volume ratio of the glycosyltransferase (UGT) to the sucrose synthase (SUSy) is 1:1.2, magnetic stirring is performed at room temperature for 2 h, and centrifugation is performed at 10000 rpm for 5 min to obtain a precipitate, and the precipitate is washed 3 times with deionized water to obtain NiCo-MOF co-immobilized glycosyltransferase and sucrose synthase (NiCo-MOF@UGT&SUSy).
[0059] Example 3
[0060] A method for preparing NiCo-MOF co-immobilized glycosyltransferase and sucrose synthase, comprising the following steps:
[0061] S1, dissolving 1mmol H3BTC and 3mmolNaOH in 15mL water under magnetic stirring to form solution B; adding ethanol aqueous solution to a mixed salt of 0.5mmol NiCl2·6H2O and 1.5mmol CoCl2·6H2O to form solution C; slowly adding solution B to solution C, magnetically stirring at room temperature for 25min, centrifuging at 10000rpm for 3min to obtain a precipitate, washing the precipitate with anhydrous ethanol and deionized water for 3 times, and freeze-drying to obtain NiCo-MOF powder;
[0062] S2, dispersing 10 mg of the NiCo-MOF powder in a phosphate buffer solution with a pH of 7.4 to obtain a dispersion, adding 1.6 mL of a mixed enzyme solution of glycosyltransferase (UGT) and sucrose synthase (SUSy) with a mass concentration of 1.5 mg / mL to the dispersion to make the total system reach 10 mL, the volume ratio of the glycosyltransferase (UGT) to the sucrose synthase (SUSy) is 1:1.7, magnetically stirring at room temperature for 2 h, centrifuging at 10000 rpm for 5 min to obtain a precipitate, washing the precipitate 3 times with deionized water to obtain NiCo-MOF co-immobilized glycosyltransferase and sucrose synthase (NiCo-MOF@UGT&SUSy).
[0063] The NiCo-MOF@UGT&SUSy prepared in the above Examples 1 to 3 was used to synthesize ginsenoside Rh2, specifically: 1 mg PPD, 1 mg UDP and 10 mg sucrose were dissolved in 1 mL PBS buffer with pH = 7.4, 10 mg of the NiCo-MOF co-immobilized glycosyltransferase and sucrose synthase were added, and the reaction was oscillated in a water bath at 40°C for 2 h, 700 μL of n-butanol was added for extraction, and the mixture was centrifuged at 12000 rpm for 3 min. 400 μL of the supernatant was freeze-dried to obtain a mixed powder, 600 μL of methanol (75%) was used to dissolve the mixed powder and filtered with a 0.22 μm organic microporous membrane, and finally the samples were analyzed by liquid phase using HPLC (Shimadzu LC-16) and Agilent ZORBAX Eclipse Plus C18 column (4.6×250 mm, 5 μm), respectively.
[0064] In order to further demonstrate the technical effect of the present invention, the present invention also provides a comparative example, which is as follows:
[0065] Comparative Example 1
[0066] Compared with Example 1, no cobalt salt was added.
[0067] A method for preparing Ni-MOF-immobilized glycosyltransferase and sucrose synthase comprises the following steps:
[0068] S1, dissolving 1 mmol H3BTC and 3 mmol NaOH in 15 mL water under magnetic stirring to form solution B; adding ethanol aqueous solution to 1.5 mmol NiCl2·6H2O salt solution to form solution C; slowly adding solution B to solution C, magnetically stirring at room temperature for 20 min, centrifuging at 10000 rpm for 3 min to obtain a precipitate, washing the precipitate with anhydrous ethanol and deionized water for 3 times, and freeze-drying to obtain Ni-MOF powder;
[0069] S2, dispersing 10 mg of the Ni-MOF powder in a phosphate buffer solution with a pH of 7.4 to obtain a dispersion, adding 1 mL of a mixed enzyme solution of glycosyltransferase (UGT) and sucrose synthase (SUSy) with a mass concentration of 1.5 mg / mL to the dispersion to make the total system reach 10 mL, the volume ratio of the glycosyltransferase (UGT) to the sucrose synthase (SUSy) is 1:1.5, magnetic stirring is performed at room temperature for 2 h, and centrifugation is performed at 10000 rpm for 5 min to obtain a precipitate, and the precipitate is washed 3 times with deionized water to obtain Ni-MOF-immobilized glycosyltransferase and sucrose synthase (Ni-MOF@UGT&SUSy).
[0070] Comparative Example 2
[0071] Compared with Example 1, no nickel salt is added.
[0072] A method for preparing Co-MOF-immobilized glycosyltransferase and sucrose synthase, comprising the following steps:
[0073] S1, dissolving 1mmol H3BTC and 3mmol NaOH in 15mL water under magnetic stirring to form solution B; adding ethanol aqueous solution to 1.5mmol CoCl2·6H2O salt solution to form solution C; slowly adding solution B to solution C, magnetically stirring at room temperature for 15min, centrifuging at 10000rpm for 3min to obtain a precipitate, washing the precipitate with anhydrous ethanol and deionized water for 3 times, and freeze-drying to obtain Co-MOF powder;
[0074] S2, dispersing 10 mg of the Co-MOF powder in a phosphate buffer solution with a pH of 7.4 to obtain a dispersion, adding 1 mL of a mixed enzyme solution of glycosyltransferase (UGT) and sucrose synthase (SUSy) with a mass concentration of 1.5 mg / mL to the dispersion to make the total system reach 10 mL, the volume ratio of the glycosyltransferase (UGT) to the sucrose synthase (SUSy) is 1:1.5, magnetic stirring is carried out at room temperature for 2 h, and centrifugation is carried out at 10000 rpm for 5 min to obtain a precipitate, and the precipitate is washed 3 times with deionized water to obtain Co-MOF-immobilized glycosyltransferase and sucrose synthase (Co-MOF@UGT&SUSy).
[0075] Comparative Example 3
[0076] Free glycosyltransferase UGT.
[0077] Comparative Example 4
[0078] Free sucrose synthase SUSy.
[0079] Since the performance of the NiCo-MOF-immobilized glycosyltransferase and sucrose synthase prepared in the above Examples 1 to 3 is similar, the effect is described by taking Example 1 as an example. The various performance tests of the NiCo-MOF-immobilized glycosyltransferase and sucrose synthase prepared in Example 1 of the present invention and the immobilized enzymes are as follows:
[0080] The enzyme loading and relative activity of NiCo-MOF@UGT&SUSy prepared in Example 1 of the present invention, Ni-MOF@UGT&SUSy of Comparative Example 1, and Co-MOF@UGT&SUSy of Comparative Example 2 are shown in Table 1.
[0081] Table 1 Enzyme loading and relative activity of NiCo-MOF@UGT&SUSy, Co-MOF@UGT&SUSy and Ni-MOF@UGT&SUSy
[0082] Immobilization materials Ni-MOF Co-MOF NiCo-MOF Loading amount (mg / g) 85.9 75.4 115.9 Relative activity (%) 77 72 89
[0083] To observe the morphological characteristics of the material, such as Figure 1 As shown in Figure 2, the SEM image shows that the NiCo-MOF particles are rectangular in shape, with a length of about 2.5 μm, a width of about 400 nm, a flat and smooth surface, and a large particle size. Figure 2 As shown, the surface of NiCo-MOF@UGT&SUSy becomes rough with many uniform small protrusions, which are the fixed UGT and SUSy.
[0084] Through atomic force microscopy images, such as Figure 3 As shown, it was observed that the height of the loaded UGT&SUSy on the NiCo-MOF microstructure was about 3.3 nm and was uniformly distributed.
[0085] In addition, we also performed elemental analysis on the surfaces of the three immobilized enzymes by EDS, e.g. Figure 4 and Figure 5 As shown in the figure, the two elements were detected simultaneously in NiCo-MOF@UGT&SUSy particles. In addition, the particles all have N and S elements on their surfaces, which are caused by the amino groups in proteins and the R groups in amino acids, respectively, indicating that the enzymes were successfully immobilized by the material.
[0086] In addition, the hydrophilicity and hydrophobicity of the materials before and after enzyme loading were measured by water contact angle, e.g. Figure 6 As shown in the figure, it was found that the contact angles of the materials increased after loading the enzyme, which was attributed to the hydrophobic amino acids in the enzyme molecules, which also showed that the enzyme was successfully immobilized by the material. Among them, the contact angle of NiCo-MOF increased from 20.1° to 85.3° after loading the enzyme, which was a large change, indicating that its loading capacity was large.
[0087] In order to better prove that the enzyme was successfully immobilized by the material, the changes in the functional groups of the material and the immobilized enzyme during the synthesis process were analyzed by FTIR, such as Figure 7 As shown. At 747cm -1 It was observed that both NiCo-MOF and NiCo-MOF@UGT&SUSy have characteristic stretching vibration peaks of aromatic rings, and at 1639 cm -1 The peak of asymmetric stretching of carboxyl group appears at 1389 cm -1 The symmetrical stretching peak of the carboxyl group appears at 1535 cm. This is because NiCo-MOF is made of trimesic acid and indicates the successful synthesis of MOF. -1 The deformation vibration peaks of the amino groups of UGT and SUSy appeared at 2922 cm -1 The CH vibration peaks of amino acids can only be observed in free enzyme and immobilized enzyme. These data indicate that the enzyme was successfully immobilized on MOF.
[0088] In order to better prove that the enzyme was successfully immobilized by the material, we analyzed the structure of the material and the immobilized enzyme by FTIR. -1 Up to 1700cm -1 We performed Gaussian deconvolution and second-order derivative fitting on the infrared images, and the results are shown in Figure 8 As shown in the figure, the total contents of α-helix and random coil in each sample are ranked as NiCo-MOF@UGT&SUSy>free UGT>free SUSy, accounting for 36.25%, 27.68% and 26.95% of the total respectively. The more α-helix and random coil, the more stable the structure. This shows that after the enzyme is fixed, its structure is not only more stable, but also has a more flexible conformation, thus having higher catalytic performance.
[0089] XRD tests were used to detect the changes in the crystal structure during the formation of immobilized enzymes, such as Fig. 9 As shown in Figure (a), after the enzyme was fixed to MOF, the intensity of the diffraction peak corresponding to the immobilized enzyme was only moderately weakened. Compared with before fixation, the position of the peak did not change, and no new peaks appeared, so the crystal structure of the material was not changed after the enzyme was fixed. We also conducted further research on the formation time of the immobilized material NiCo-MOF and the corresponding XRD results. Fig. 9In Figure (b), as the synthesis time increases, the diffraction peaks at 18° and 19.19° first increase and then weaken, and the peak intensity reaches the highest at 25 minutes of synthesis. This shows that when the formation time of NiCo-MOF is 25 minutes, its crystal growth is the best and the crystal form is the best. At this time, the amount of metal ions retained in NiCo-MOF is the largest, thus tending to the complete transformation of NiCo-MOF, and the structure also tends to be stable, so the peak intensity is the highest.
[0090] TGA is used to show the pyrolysis behavior of NiCo-MOF and NiCo-MOF@UGT&SUSy prepared in Example 1 of the present invention between room temperature and 700°C, such as Fig.10 As shown. From room temperature to 150°C, all samples lost weight due to the loss of water molecules. From 150°C to 400°C, the cobalt ions in NiCo-MOF and NiCo-MOF@UGT&SUSy were gradually oxidized to cobalt oxide, and the nickel ions in NiCo-MOF and NiCo-MOF@UGT&SUSy were gradually oxidized to nickel oxide, which resulted in the loss of sample mass. Among them, from 200°C to 400°C, the enzyme molecules in NiCo-MOF@UGT&SUSy further lost mass due to the gradual decomposition of the structure. From 400°C to 550°C, the weight loss continued due to the collapse of the MOF structure of each material. In general, the weight change of the immobilized enzyme is relatively gentle compared to the immobilized material, which indicates that the enzyme is successfully immobilized on the material and the immobilized enzyme has a high thermal stability.
[0091] In order to analyze the elements and main forms in NiCo-MOF and NiCo-MOF@UGT&SUSy, we performed XPS tests, such as Fig.11 The complete spectra of NiCo-MOF and NiCo-MOF@UGT&SUSy are shown in Fig.11 Figure (a) shows that Ni, Co, O and C are present in both materials. NiCo-MOF@UGT&SUSy also contains N and S due to the protein loading after immobilization, indicating that the immobilized enzyme was successfully prepared. In the Co2p spectrum, Fig.11 Figure (c) shows that the binding energies of Co2p3 / 2 and Co2p1 / 2 appear at 780.9eV and 797.3eV, respectively, and the satellite peaks appear at 785.7eV and 802.3eV, respectively. Ni2p spectrum, such as Fig.11Figure (b) shows two main peaks at 855.8eV and 874.0eV, corresponding to Ni2p3 / 2 and Ni2p1 / 2, respectively, and satellite peaks at 879.8eV and 861.4eV. After fixation, the binding energies of Ni2p3 / 2 and Co2p3 / 2 in NiCo-MOF@UGT and SUSy increased by 0.1eV and 0.2eV, respectively. This shift is caused by the strong electronic absorption of nitrogen atoms, which leads to an increase in the binding energy of nickel and cobalt, indicating that Co 2+ and Ni 2+ Coordinated with N, such as Fig.11 In Figure (d), the binding energies of NH and N-Ni or N-Co bonds present in the N spectrum are 400.0 eV and 399.4 eV, respectively, further confirming this coordination.
[0092] The kinetic parameters of free UGT&SUSy and NiCo-MOF@UGT&SUSy are shown in Table 2.
[0093] Table 2 Kinetic parameters of free UGT&SUSy and NiCo-MOF@UGT&SUSy
[0094] sample <![CDATA[v max (μM min -1 )]]> <![CDATA[K m (mM)]]> <![CDATA[k cat (min -1 )]]> <![CDATA[k cat / K m (mM) -1 ·min -1 )]]> Free UGT&SUSy <![CDATA[8.31×10 -4 ]]> <![CDATA[7.74×10 -4 ]]> <![CDATA[2.51×10 -5 ]]> 0.032 NiCo-MOF@UGT&SUSy <![CDATA[8.69×10 -4 ]]> <![CDATA[3.69×10 -4 ]]> <![CDATA[2.61×10 -5 ]]> 0.071
[0095] In addition, the kinetic parameters of free UGT&SUSy and NiCo-MOF@UGT&SUSy were studied by measuring the kinetic parameters of PPD conversion catalyzed by ginsenosides at different substrate concentrations. As shown in Table 2, the v max The K of the immobilized enzyme was higher than that of the free UGT&SUSy, indicating that the catalytic rate was improved after the immobilized enzyme. This improvement may be due to the fact that immobilization reduced the accumulation of enzyme-substrate complexes, thereby enhancing the effective substrate conversion. m The value is lower than that of the free enzyme, indicating that the affinity of the immobilized enzyme to the substrate is enhanced. This may be because immobilization changes the spatial conformation, thereby increasing the possibility of substrate-enzyme complex formation and providing more substrate binding sites. After immobilization, k cat / K m The increase in the value indicates that the enzyme has an enhanced ability to convert substrates into products. This enhancement may be due to the improvement of the microenvironment around the enzyme, maintaining its spatial structure. In addition, the improvement in conversion efficiency may be due to the fact that the distance between the enzyme molecules in the immobilized form is shorter than that of the free enzyme, which maintains the activity of the enzyme and speeds up the mass transfer efficiency, thereby making the substrate conversion ability stronger and the conversion rate higher.
[0096] Thermal deformation dynamic parameters
[0097] Table 3 Thermal denaturation kinetic parameters of free UGT&SUSy and NiCo-MOF@UGT&SUSy
[0098]
[0099] In order to further compare the temperature stability of immobilized enzyme and free enzyme, at 40-80 °C, Fig.12 Figures (a) and (d) show the deactivation kinetics of free enzyme and NiCo-MOF@UGT&SUSy. The relative activities of both samples decreased over time, but the relative activity of the immobilized enzyme decreased less than that of the free enzyme. Fig.12 Figure (b) and (e) show the lnA of free enzyme and NiCo-MOF@UGT&SUSy RA The linear relationship with t showed that both the free enzyme and the immobilized enzyme showed good linear fit with high correlation coefficient (R 2 >0.960). The corresponding k T The values are shown in Table 3. At the same temperature, the inactivation rate constants (k T ) increased with increasing temperature, but the inactivation rate constant of the immobilized enzyme was significantly lower than that of the free enzyme. T k T The value increases more slowly.
[0100] In addition, if Fig.12 In Figures (f) and (c), the deactivation energy of the immobilized enzyme (80.1 kJ / mol) is higher than that of the free enzyme (68.7 kJ / mol). For example, in Table 3, over the entire temperature range, the t 1 / 2 It is 1.68 to 3.12 times that of the free enzyme. 1 / 2 is 1307.8min, while the t 1 / 2 The temperature stability of the free enzyme was significantly improved by immobilized enzyme.
[0101] Molecular docking
[0102] Table 4 Relevant fitting parameters of recombinant UGT and recombinant SUSy and their respective template proteins
[0103]
[0104] Visualization by PyMOL, such as Fig.13 As shown in Figure 2, the His-tag is located at the end of the amino acid sequence of recombinant UGT and recombinant SUSy, far away from the substrate binding pocket. Ab initio calculation and PyMOL-align were used to simulate the structure of recombinant UGT and compare the homologous sequences, such as Fig.13As shown in Figure (a) and Table 4, the global structural similarity and global structural comparison values of the recombinant UGT and the UGT in the database are 0.86 and 0.91, respectively, which are highly similar. The root mean square deviation (RMSD) is 1.92, which is less than 2, indicating that the residue matching error of the two structures is small, similar to that of sucrose synthase (1.16), such as Fig.13 As shown in Figures (b) and (c), the overall structural similarity between the recombinant SUSy and the template protein is 89%, indicating that the structures of the recombinant glycosyltransferase and sucrose synthase remain basically unchanged. These results indicate that the his tag has no effect on the conformation of the enzyme.
[0105] In addition, the nitrogen in the six imidazole rings of the his tag is closely related to the Ni in NiCo-MOF. 2+ and Co 2+ Coordination, such as Fig.18 As shown, the activity of the enzyme is maintained while the enzyme is fixed to the material.
[0106] In order to simulate the structure of the immobilized enzyme, based on the fact that immobilization does not change the enzyme structure, we used the structure of the free enzyme to replace the structure of the immobilized enzyme, and used Autodock to perform docking analysis of UGT and substrates UDPG and PPD. Fig.14 and Fig.16 As shown in Figure 1, the binding sites of glycosyltransferases with PPD and UDPG substrates are located in the barrel region formed by the peptide chain helix and connected by hydrogen bonds. Fig.17 As shown in Figure 2, it further revealed that the key amino acids Lys248 and Glu247 of glycosyltransferase are connected to the small molecule substrate UDPG through 1 and 5 hydrogen bonds, respectively. The distances between the side chain carboxyl group of Glu247 and the glycoside O of UDPG are and In addition, the key amino acids Ala246 and Lys244 are connected to the small molecule substrate PPD through 1 and 2 hydrogen bonds, respectively, as Fig.15 The distances between these amino acids and PPD glycoside O are and In these regions, small molecules UDPG and PPD undergo deglycosylation and glycosylation reactions, respectively, and are continuously converted into the target product Rh2.
[0107] Structural stability analysis
[0108] The influence of temperature and pH is very important for enzymatic reactions. First, the present invention studies and compares the relative activity changes of free enzymes and three immobilized enzymes (Ni-MOF@UGT&SUSy in Comparative Example 1, Co-MOF@UGT&SUSy in Comparative Example 2, and NiCo-MOF@UGT&SUSy in Example 1) at pH 3-10. Fig.19 As shown in Figure (a), when the pH is 3 and 10, the relative activity of the free enzyme is 40.01% and 30.87%. However, at the same time, the relative activities of the three immobilized enzymes are higher than those of the free enzymes. Among them, when the pH is 3 and 10, the relative activity of NiCo-MOF@UGT&SUSy is higher than that of the other two materials, which are 65.15% and 65.46%, respectively. In addition, compared with the optimal pH of the free enzyme = 7, the optimal pH of the three immobilized enzymes has changed to 8, and the immobilized enzyme is less affected by pH changes than the free enzyme.
[0109] When the temperature is too high or too low, the relative activities of the free enzyme and the three immobilized enzymes will decrease, but the relative activity of the immobilized enzyme is less affected by temperature than that of the free enzyme. Fig.19 As shown in Figure (b) in Figure 2, the free enzyme and the three immobilized enzymes reached their optimum temperatures at 35°C and 40°C, respectively. When the temperature was 80°C, the activity of the free enzyme was 25.84%, but the three immobilized enzymes all maintained a relative activity of more than 40%, among which the relative activity of NiCo-MOF@UGT&SUSy was higher than that of the other two materials, at 49.69%. This shows that the temperature tolerance of the enzyme is improved after being immobilized.
[0110] Based on the high stability, enzyme loading and activity of NiCo-MOF@UGT&SUSy, we conducted the following research on its storage stability and reusability. Fig.19 As shown in Figure (c), with the extension of storage time, the activity of both free enzyme and immobilized enzyme will decrease, and the degree of activity loss of free enzyme is greater than that of immobilized enzyme. On the 30th day of storage, the free enzyme has only 49.7% relative activity, while the immobilized enzyme retains 77.6% relative activity.
[0111] The NiCo-MOF@UGT&SUSy was placed under optimal conditions for repeated transformation after separation, such as Fig.19 As shown in Figure (d), the relative activity of the immobilized enzyme will continue to decrease as the number of cycles increases. It is also possible that the immobilized enzyme will desorb from the material during the oscillation reaction. In addition, after the tenth reaction, the immobilized enzyme still has a relative activity of 68.97% and can still convert 65.87μg / mL of Rh2. This shows that the binding ability between the enzyme and the material is strong and the immobilized enzyme has good reusability.
[0112] In summary, the NiCo-MOF@UGT&SUSy provided by the present invention has better pH stability, thermal stability, superior reusability and storage stability. The NiCo-MOF prepared by the present invention has strong specific adsorption performance for UGT and SUSy with histidine tags. When the NiCo-MOF@UGT&SUSy prepared by the present invention is used as an enzyme biocatalyst to synthesize ginsenoside Rh2, a higher ginsenoside Rh2 conversion rate can be achieved, so it has great industrial application potential in enzyme purification and biocatalytic production of ginsenosides.
[0113] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A method for preparing NiCo-MOF co-immobilized glycosyltransferase and sucrose synthase, characterized in that: The following steps are involved: To soluble Ni 2+ Salt and soluble Co 2+ Add H3BTC and NaOH mixture to the mixed salt solution and stir at room temperature to make Ni 2+ and Co 2+ Coordinate reaction with H3BTC to obtain NiCo-MOF powder; The NiCo-MOF powder was dispersed in a phosphate buffer to obtain a dispersion, a mixed enzyme solution of glycosyltransferase and sucrose synthase was added to the dispersion, and the mixture was stirred at room temperature. 2+ and Co 2+ Specific adsorption of Ni to the histidine tag in glycosyltransferase and sucrose synthase 2+ and Co 2+ The glycosyltransferase and sucrose synthase are co-immobilized to obtain NiCo-MOF co-immobilized glycosyltransferase and sucrose synthase.
2. The preparation method according to claim 1, characterized in that: The soluble Ni 2+ The molar ratio of salt, H3BTC and NaOH is 1-3:1:3-3.
5.
3. The preparation method according to claim 1, characterized in that: The mixed salt solution is an ethanol aqueous solution of mixed salts, and the soluble Ni 2+ Salt and soluble Co 2+ The molar ratio of the salt is 0.5-1.5:0.5-1.
5.
4. The preparation method according to claim 1, characterized in that: The dosage ratio of the NiCo-MOF powder to the mixed enzyme solution of glycosyltransferase and sucrose synthase is 10 mg: 0.4-1.6 mL.
5. The preparation method according to claim 1, characterized in that: In the mixed enzyme solution of the glycosyltransferase and sucrose synthase, the concentrations of the glycosyltransferase and sucrose synthase are both 1.5 mg / mL, and the volume ratio is 1:1.2-1.
7.
6. The preparation method according to claim 1, characterized in that: The soluble Ni 2+ The salt is NiCl2·6H2O, the soluble Co 2+ The salt is CoCl2·6H2O.
7. The preparation method according to claim 1, characterized in that: The glycosyltransferase is a glycosyltransferase gene GE02773 mined from the genome of Bacillus subtilis SL-44, and a glycosyltransferase expression engineering bacterium BL21-GE02773-28a is constructed, and the bacterium is induced to express as a soluble protein glycosyltransferase; the sucrose synthase is a sucrose synthase gene mined from the genome of Vermifuge, and a sucrose synthase expression engineering bacterium pRSF-McSUSy-S31D is constructed, and the bacterium is induced to express as a soluble protein sucrose synthase.
8. A NiCo-MOF co-immobilized glycosyltransferase and sucrose synthase prepared by the preparation method according to any one of claims 1 to 7.
9. Use of the NiCo-MOF co-immobilized glycosyltransferase and sucrose synthase in the synthesis of ginsenoside Rh2 according to claim 8, characterized in that: The application is as follows: mixing protopanaxadiol, uridine diphosphate and NiCo-MOF co-immobilized glycosyltransferase and sucrose synthase in a phosphate buffer at pH = 7.4 according to a mass ratio of 1:1:8 to 12, shaking in a water bath at 35 to 40° C. for 2 to 4 hours, extracting with n-butanol, centrifuging, and freeze-drying to obtain ginsenoside Rh2.
Citation Information
Patent Citations
Novel catalytic system for preparing rare ginsenosides and application thereof
CN105087739A
Ultrasonic synthesis method and application of different single-metal and double-metal two-dimensional MOFs nano-enzymes
CN111330643A
Novel enzyme-metal organic framework composite material-cellulose membrane connected by DNA (Deoxyribonucleic Acid) as well as preparation method and application of novel enzyme-metal organic framework composite material-cellulose membrane
CN116656665A
Zn-NiMOF material immobilized glycosyl transferase as well as preparation method and application thereof
CN117511899A
Polyhedral cage-containing mesoporous metal-organic frameworks as platform for biocatalysis, methods of making these frameworks, and methods of using these frameworks
US20150087044A1