Ultrahigh-toughness engineering material mixture and preparation method thereof
By using a mill without grinding medium in the factory dry premix method to perform self-crumbing and self-graining, combined with dispersant, the problem of uneven material dispersion in traditional ultra-high toughness engineering materials is solved, and the mixing is improved The quality performance and transportation convenience of materials.
Patent Information
- Application Number
- CN202411159879.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-22
AI Technical Summary
Traditional ultra-high toughness engineering material mixtures cannot introduce coarse aggregates in factory dry pre-mixing methods, resulting in uneven dispersion of materials and uneven distribution, and the quality performance of the mixture fluctuates greatly and is difficult to control.
A grinding medium-free mill is used to perform self-crumbing and self-graining. Combined with the use of dispersant, particle refinement and grading optimization are achieved, and particles of different sizes are synchronized to improve dispersion and uniformity.
The problems of uneven dispersion and uneven distribution of materials were solved, the quality performance of the mixture was significantly improved, the particle shape was more rounded and the distribution uniformity was greatly improved, the batching process was simplified, and the difficulty of transportation and use was reduced.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fiber-reinforced cement-based composite materials, and in particular to an ultra-high toughness engineering material mixture and a preparation method thereof. Background Art
[0002] Ultra-high toughness engineering materials are a type of fiber-reinforced cement-based composite material and a type of ultra-high performance concrete. Compared with conventional concrete, they have higher load-bearing capacity, toughness and durability, and their deformation behavior is closer to that of steel bars. Therefore, they are considered to be the most promising engineering materials for future high-performance, long-life structures and major infrastructure. The design of ultra-high toughness engineering materials is based on the principle of the closest packing of particles and the fiber reinforcement mechanism. The particles and the stacking gaps are bonded and filled with cementitious material slurry, and the fibers play a role in composite reinforcement, stress transfer and bridging.
[0003] The preparation method of traditional ultra-high toughness engineering materials mainly uses finely formulated continuous graded quartz sand and quartz powder as the supporting skeleton phase, high-dosage cement, high-fineness fly ash and silica fume as the cementing phase and filling phase, steel fiber as the reinforcing phase, high-performance water reducer and low-dosage mixing water as the dispersed phase, and forms a slurry through efficient mixing and mixing, and then pours and maintains it to form a cast-in-place structure or prefabricated parts. With the development of modern infrastructure engineering structures to remote and environmentally harsh areas with inconvenient transportation, the demand for ultra-high toughness engineering materials is also increasing. Despite this, mixing ultra-high toughness engineering material slurry in traditional mixing plants, then transporting it to the construction site for pouring and construction, or making ultra-high toughness engineering materials into large prefabricated parts, etc., has high requirements for transportation, and slurry mixers or large prefabricated parts in remote and environmentally harsh areas are difficult to transport to the site. Based on this, industry practitioners began to focus on the development of ultra-high toughness engineering material mixtures, which are dry premixed in the factory, then shipped to the project site in bags, and then mixed with water and water reducers on site for use.
[0004] An ideal mixture of ultra-high toughness engineering materials requires that the particles of each component raw material be nearly spherical, small in size and well-graded, and the fibers be ultra-evenly dispersed. However, the factory dry premixing method requires good raw material quality, multiple raw material warehouses, complex ingredients, and difficulty in material metering and mixing. As a result, the prepared ultra-high toughness engineering material mixture generally has the problems of being unable to introduce coarse aggregate, poor dispersion of each component material, and uneven distribution, resulting in large fluctuations in the quality and performance of the mixture. Summary of the invention
[0005] The present invention aims to solve the problems that the ultra-high toughness engineering material mixture prepared by the current factory dry premixing method generally has the inability to introduce coarse aggregate, the poor dispersion and uneven distribution of the component materials, etc., which result in the difficulty in controlling the quality of the mixture during use and large fluctuations. An ultra-high toughness engineering material mixture and a preparation method thereof are proposed.
[0006] In order to achieve the above technical objectives, the technical solution provided by the present invention is:
[0007] A mixture of ultra-high toughness engineering materials comprises the following raw materials in percentage by dry basis weight: 40% to 50% of high-titanium heavy slag crushed stone, 25% to 35% of high-titanium heavy slag sand, 15% to 20% of silicate cement clinker powder, 3% to 4% of lithium slag powder, 3.5% to 4.0% of silica fume and 1.5% to 2.0% of chopped fibers.
[0008] Furthermore, all particles of the ultra-high toughness engineering material mixture are below 10 mm, of which 5mm-10mm particles account for 20%-25%, particles smaller than 0.045mm account for 30%-40%, and the remaining particles are larger than 0.045mm and smaller than 5mm, and the uniformity of the mixture is greater than 90%.
[0009] Furthermore, after the ultra-high toughness engineering material mixture is mixed with 6% to 8% water by mass of the mixture, the slump of the formed slurry is 250 to 280 mm, the expansion is greater than 600 to 650 mm, and the compressive strength of the hardened body after curing for 28 days is 120 to 140 MPa and the flexural strength is 15 to 20 MPa.
[0010] Furthermore, the particle size of the high-titanium heavy slag crushed stone is 10 mm to 20 mm, and the mass percentage of TiO2 in its chemical composition is ≥20%.
[0011] Furthermore, the particle size of the high-titanium heavy slag sand is less than 5 mm, of which the mass percentage of particles less than 0.045 mm is not less than 10%; and the mass percentage of TiO2 in its chemical composition is ≥20%.
[0012] Furthermore, the mass percentage of particles below 0.045 mm in the Portland cement clinker powder is greater than 80%.
[0013] Furthermore, the SO3 content in the chemical composition of the lithium slag powder is not less than 15%, and the dihydrate gypsum content in the mineral composition is not less than 30%.
[0014] Furthermore, the silica fume is SF90 silica fume.
[0015] Furthermore, the chopped fibers are any one of chopped basalt fibers, chopped carbon fibers, chopped polypropylene fibers, and chopped polyethylene glycol fibers, or a mixture of two or more thereof.
[0016] The present invention also provides a method for preparing an ultra-high toughness engineering material mixture, which comprises mixing high-titanium heavy slag crushed stone, high-titanium heavy slag sand, silicate cement clinker powder, lithium slag powder, silica fume and chopped fibers in a certain proportion and placing the mixture in a mill without grinding media for self-crushing and self-grinding, and spraying a dispersant to obtain an ultra-high toughness engineering material mixture.
[0017] Furthermore, the dispersant accounts for 6‰ of the raw material mass entering the mill.
[0018] Furthermore, the dispersant is a mixture of high-performance polycarboxylate water-reducing agent, triethanolamine, diethanol monoisopropanolamine, triisopropanolamine, and graphene oxide dispersion, wherein the mass percentage of the high-performance polycarboxylate water-reducing agent is not less than 90%.
[0019] The present invention has the following beneficial effects:
[0020] 1. The present invention changes the previous process of manufacturing ultra-high toughness engineering material mixtures, which only relies on the mixing action of a dry mixer. It can not only introduce coarse aggregates, but also crush and grind coarse particles during the mixture manufacturing process, so that particles of different sizes of materials are synchronously shaped, the particles are refined and the grading is optimized, thereby solving the problem of poor dispersion and uneven distribution of the component materials, which leads to large fluctuations in the quality and performance of the mixture.
[0021] 2. The ultra-high toughness engineering material mixture provided by the present invention has all raw materials other than silicate cement clinker powder and chopped fibers that are solid waste, with a solid waste content of up to 88%, so it has green, low-carbon and environmentally friendly properties.
[0022] 3. The preparation method of the ultra-high toughness engineering material mixture provided by the present invention uses a mill without grinding media, so that in addition to the mixing process, the preparation process also introduces self-crushing and self-grinding processes, which greatly reduces the requirements for the particle size and gradation of each raw material particle of the mixture, greatly simplifies the ingredients and processing processes, and the dispersion of the prepared mixture material particles, particle distribution and uniformity of the distribution of each raw material particle are greatly improved.
[0023] 4. In the preparation method of the ultra-high toughness engineering material mixture provided by the present invention, no grinding media is used in the mill during the preparation process, and high-titanium heavy slag crushed stone and high-titanium heavy slag sand are used as self-crushing and self-grinding media: first, the particles directly rub against each other, making the particle shape more rounded, and the sphericity and roundness of the particles better; second, during the self-crushing and grinding process, the particle grading of the mixture is further optimized; third, the dispersion and distribution uniformity of various materials are greatly improved.
[0024] 5. The ultra-high toughness engineering material mixture provided by the present invention can be directly transported to the construction site in bags for use. During use, only mixing water needs to be added according to the mass percentage of the material. It is convenient to transport and simple to use.
[0025] 6. The ultra-high toughness engineering material mixture provided by the present invention also contains lithium slag. The lithium slag contains a large amount of dihydrate gypsum, which can stimulate the hydration of cement clinker. At the same time, the lithium slag participates in the hydration to form expansive hydration products, thereby effectively reducing the self-shrinkage of the ultra-high toughness engineering material. DETAILED DESCRIPTION
[0026] The technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] In the description of the present invention, it should be noted that the directions or positional relationships indicated by "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc. are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance.
[0028] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0029] A mixture of ultra-high toughness engineering materials comprises the following raw materials in percentage by dry basis weight: 40% to 50% of high-titanium heavy slag crushed stone, 25% to 35% of high-titanium heavy slag sand, 15% to 20% of silicate cement clinker powder, 3% to 4% of lithium slag powder, 3.5% to 4.0% of silica fume and 1.5% to 2.0% of chopped fibers.
[0030] The coarse aggregate of the present invention can be selected from natural rocks such as quartz, basalt, granite, etc. with good wear resistance and toughness, as well as industrial solid waste aggregates such as steel slag and alloy slag, but it is preferably high-titanium heavy slag. First, high-titanium slag is industrial waste slag, low cost, and conducive to comprehensive resource utilization; second, high-titanium slag has better wear resistance and toughness than the above-mentioned natural ores, and has better chemical stability than the above-mentioned waste slag, and will not leach harmful substances or cause harmful aggregate expansion reactions. In addition, the lithium slag powder of the present invention is a preferred component: first, it contains active aluminum silicate volcanic ash components, and the filling and hydration effects are very significant, which can further reduce the cement clinker content; second, the development time of the volcanic ash activity reaction of lithium slag is relatively slow, which can reduce the hydration heat during the coagulation and hardening process of ultra-high toughness materials, thereby reducing the internal and external temperature difference, reducing internal temperature stress and microcracks; third, lithium slag also contains dihydrate gypsum, and the calcium sulfonate generated by dihydrate gypsum participating in cement hydration has an expansion type, which can offset the cement hydration self-shrinkage, thereby improving the volume stability of the material. Portland cement clinker powder and chopped fibers are necessary. Portland cement clinker powder is the main cementitious material, which provides the main strength of the engineering material after hydration and hardening, while the chopped fibers are for providing toughness.
[0031] Specifically, all particles of the ultra-high toughness engineering material mixture are below 10 mm, of which 5mm-10mm particles account for 20%-25%, particles less than 0.045mm account for 30%-40%, and the remaining particles are larger than 0.045mm and smaller than 5mm, and the uniformity of the mixture is greater than 90%; after the ultra-high toughness engineering material mixture is mixed with water accounting for 6%-8% of the mixture mass percentage, the formed slurry has a slump of 250-280mm and an expansion of more than 600-650mm. The hardened body after curing for 28 days has a compressive strength of 120-140MPa and a flexural strength of 15-20MPa.
[0032] Specifically, the high-titanium heavy slag crushed stone particles are molten slag produced during the smelting of vanadium-titanium magnetite in a blast furnace, which is naturally cooled by hot pouring and then crushed and screened. The size is 10mm~20mm, and the mass percentage of TiO2 in its chemical composition is ≥20%. The high-titanium heavy slag with a mass percentage of TiO2 ≥20% has a stable chemical structure and is suitable as an aggregate. The crushed stone with a particle size of 10mm~20mm has heavy weight and good toughness, and can be used as a grinding medium in the self-grinding process.
[0033] Specifically, the high-titanium heavy slag sand is the molten slag produced when smelting vanadium-titanium magnetite in a blast furnace, which is naturally cooled by hot pouring and then crushed and screened. The particle size is less than 5 mm, of which the mass percentage of particles less than 0.045 mm is not less than 10%; the mass percentage of TiO2 in its chemical composition is ≥20%. The high-titanium heavy slag with a mass percentage of TiO2 ≥20% has a stable chemical structure and low activity. The smaller the particle size, the higher the activity, which is conducive to the formation of high strength in the later stage. Therefore, the mass percentage of particles less than 0.045 mm is limited.
[0034] Specifically, the silicate cement clinker powder is a powder material prepared by grinding silicate cement clinker in a ball mill to meet the requirements of GB / T21372 "Silicate Cement Clinker", and the mass percentage of particles below 0.045 mm is greater than 80%.
[0035] Specifically, the lithium slag powder is obtained by drying the mud produced in the process of lithium extraction from spodumene by sulfuric acid method in a dryer at about 65°C. The SO3 content in the chemical composition is not less than 15%, and the dihydrate gypsum content in the mineral composition is not less than 30%. The SO3 in the lithium slag powder can stimulate the activity of high-titanium slag fine powder on the one hand, and compensate for the shrinkage produced during cement hydration on the other hand.
[0036] Specifically, the silica fume is SF90 silica fume that meets the requirements of GB / T 27690 "Silica fume for mortar and concrete".
[0037] Specifically, the chopped fibers are any one of chopped basalt fibers, chopped carbon fibers, chopped polypropylene fibers, and chopped polyethylene glycol fibers, or a mixture of two or more thereof.
[0038] The present invention also provides a method for preparing an ultra-high toughness engineering material mixture, which comprises mixing high-titanium heavy slag crushed stone, high-titanium heavy slag sand, silicate cement clinker powder, lithium slag powder, silica fume and chopped fibers in a certain proportion and placing the mixture in a mill without grinding media for self-crushing and self-grinding. The particles are self-crushed and self-grinded by mutual impact and friction, and a dispersant is sprayed in to obtain an ultra-high toughness engineering material mixture.
[0039] Specifically, the dispersant accounts for 6‰ of the mass of the raw material entering the mill.
[0040] Specifically, the dispersant is a mixture of high-performance polycarboxylate water-reducing agent, triethanolamine, diethanol monoisopropanolamine, triisopropanolamine, and graphene oxide dispersion, wherein the mass percentage of the high-performance polycarboxylate water-reducing agent is not less than 90%.
[0041] Example 1
[0042] A method for preparing an ultra-high toughness engineering material mixture comprises the following steps: 40% high-titanium heavy slag crushed stone, 35% high-titanium heavy slag sand, 15% silicate cement clinker powder, 4% lithium slag powder, 4.0% silica fume and 2.0% chopped basalt fiber are mixed and placed in a mill without grinding media for self-crushing and self-grinding. The self-crushing and self-grinding are carried out by mutual impact and friction between particles, and a dispersant accounting for 6‰ of the mass of the raw materials in the mill is sprayed into the mixture to obtain an ultra-high toughness engineering material mixture.
[0043] Specifically, the particles of the prepared ultra-high toughness engineering material mixture are all below 10 mm, of which 5mm-10mm particles account for 20%, particles less than 0.045mm account for 35%, and the uniformity of the mixture is 94%; after mixing with water accounting for 7% of the mass percentage of the mixture, the formed slurry has a slump of 250mm and an expansion of 620mm. The hardened body after curing for 28 days has a compressive strength of 135.8MPa and a flexural strength of 15.2MPa.
[0044] Specifically, the dispersant is a mixture of high-performance polycarboxylate water-reducing agent, triethanolamine, diethanol monoisopropanolamine, triisopropanolamine, and graphene oxide dispersion, wherein the mass percentage of the high-performance polycarboxylate water-reducing agent is not less than 90%.
[0045] Example 2
[0046] A method for preparing an ultra-high toughness engineering material mixture comprises the following steps: 40% high-titanium heavy slag crushed stone, 32% high-titanium heavy slag sand, 18% silicate cement clinker powder, 4% lithium slag powder, 4.0% silica fume and 2.0% chopped carbon fiber are mixed and placed in a mill without grinding media for self-crushing and self-grinding. The self-crushing and self-grinding are carried out by mutual impact and friction between particles, and a dispersant accounting for 6‰ of the mass of the raw materials entering the mill is sprayed into the mixture to obtain an ultra-high toughness engineering material mixture.
[0047] Specifically, the particles of the prepared ultra-high toughness engineering material mixture are all below 10 mm, of which 5mm-10mm particles account for 21%, particles less than 0.045mm account for 38%, and the uniformity of the mixture is 96%; after mixing with water accounting for 8% of the mass percentage of the mixture, the formed slurry has a slump of 275mm and an expansion of 650mm. The hardened body after curing for 28 days has a compressive strength of 139.2MPa and a flexural strength of 16.9MPa.
[0048] Specifically, the dispersant is a mixture of high-performance polycarboxylate water-reducing agent, triethanolamine, diethanol monoisopropanolamine, triisopropanolamine, and graphene oxide dispersion, wherein the mass percentage of the high-performance polycarboxylate water-reducing agent is not less than 90%.
[0049] Example 3
[0050] A method for preparing an ultra-high toughness engineering material mixture comprises the following steps: 40% high-titanium heavy slag crushed stone, 30% high-titanium heavy slag sand, 20% silicate cement clinker powder, 4% lithium slag powder, 4.0% silica fume and 2.0% chopped polypropylene fiber are mixed and placed in a mill without grinding media for self-crushing and self-grinding. The self-crushing and self-grinding are carried out by mutual impact and friction between particles, and a dispersant accounting for 6‰ of the mass of the raw materials entering the mill is sprayed into the mixture to obtain an ultra-high toughness engineering material mixture.
[0051] Specifically, the particles of the prepared ultra-high toughness engineering material mixture are all below 10 mm, of which 5mm-10mm particles account for 22%, particles less than 0.045mm account for 40%, and the uniformity of the mixture is 97%; after mixing with water accounting for 8% of the mass percentage of the mixture, the formed slurry has a slump of 280mm and an expansion of 650mm. The hardened body after curing for 28 days has a compressive strength of 138.9MPa and a flexural strength of 19.8MPa.
[0052] Specifically, the dispersant is a mixture of high-performance polycarboxylate water-reducing agent, triethanolamine, diethanol monoisopropanolamine, triisopropanolamine, and graphene oxide dispersion, wherein the mass percentage of the high-performance polycarboxylate water-reducing agent is not less than 90%.
[0053] Example 4
[0054] A method for preparing an ultra-high toughness engineering material mixture comprises the following steps: 45% high-titanium heavy slag crushed stone, 32% high-titanium heavy slag sand, 15% silicate cement clinker powder, 3% lithium slag powder, 3.5% silica fume and 1.5% chopped polyethylene glycol fiber are mixed and placed in a mill without grinding media for self-crushing and self-grinding. The self-crushing and self-grinding are carried out by mutual impact and friction between particles, and a dispersant accounting for 6‰ of the mass of the raw materials entering the mill is sprayed into the mixture to obtain an ultra-high toughness engineering material mixture.
[0055] Specifically, the particles of the prepared ultra-high toughness engineering material mixture are all below 10 mm, of which 5mm-10mm particles account for 22%, particles less than 0.045mm account for 33%, and the uniformity of the mixture is 94%; after mixing with water accounting for 6% of the mass percentage of the mixture, the formed slurry has a slump of 270mm and an expansion of 630mm. The hardened body after curing for 28 days has a compressive strength of 129.5MPa and a flexural strength of 15.4MPa.
[0056] Specifically, the dispersant is a mixture of high-performance polycarboxylate water-reducing agent, triethanolamine, diethanol monoisopropanolamine, triisopropanolamine, and graphene oxide dispersion, wherein the mass percentage of the high-performance polycarboxylate water-reducing agent is not less than 90%.
[0057] Example 5
[0058] A method for preparing an ultra-high toughness engineering material mixture comprises the following steps: 45% high-titanium heavy slag crushed stone, 28% high-titanium heavy slag sand, 18% silicate cement clinker powder, 3.5% lithium slag powder, 4.0% silica fume and 1.5% chopped basalt fiber are mixed and placed in a mill without grinding media for self-crushing and self-grinding. The self-crushing and self-grinding are carried out by mutual impact and friction between particles, and a dispersant accounting for 6‰ of the mass of the raw materials in the mill is sprayed into the mixture to obtain an ultra-high toughness engineering material mixture.
[0059] Specifically, the particles of the prepared ultra-high toughness engineering material mixture are all below 10 mm, of which 5mm-10mm particles account for 23%, particles less than 0.045mm account for 36%, and the uniformity of the mixture is 95%; after mixing with water accounting for 7% of the mixture mass, the formed slurry has a slump of 270mm and an expansion of 630mm. The hardened body after curing for 28 days has a compressive strength of 134.6MPa and a flexural strength of 17.4MPa.
[0060] Specifically, the dispersant is a mixture of high-performance polycarboxylate water-reducing agent, triethanolamine, diethanol monoisopropanolamine, triisopropanolamine, and graphene oxide dispersion, wherein the mass percentage of the high-performance polycarboxylate water-reducing agent is not less than 90%.
[0061] Example 6
[0062] A method for preparing an ultra-high toughness engineering material mixture comprises the following steps: 45% high-titanium heavy slag crushed stone, 25% high-titanium heavy slag sand, 20% silicate cement clinker powder, 4% lithium slag powder, 4.0% silica fume and 2.0% chopped carbon fiber are mixed and placed in a mill without grinding media for self-crushing and self-grinding. The self-crushing and self-grinding are carried out by mutual impact and friction between particles, and a dispersant accounting for 6‰ of the mass of the raw materials entering the mill is sprayed into the mixture to obtain the ultra-high toughness engineering material mixture.
[0063] Specifically, the particles of the prepared ultra-high toughness engineering material mixture are all below 10 mm, of which 5mm-10mm particles account for 24%, particles less than 0.045mm account for 37%, and the uniformity of the mixture is 95%; after mixing with water accounting for 8% of the mass percentage of the mixture, the formed slurry has a slump of 265mm and an expansion of 630mm. The hardened body after curing for 28 days has a compressive strength of 133.6MPa and a flexural strength of 18.2MPa.
[0064] Specifically, the dispersant is a mixture of high-performance polycarboxylate water-reducing agent, triethanolamine, diethanol monoisopropanolamine, triisopropanolamine, and graphene oxide dispersion, wherein the mass percentage of the high-performance polycarboxylate water-reducing agent is not less than 90%.
[0065] Example 7
[0066] A method for preparing an ultra-high toughness engineering material mixture comprises the following steps: mixing 50% high-titanium heavy slag crushed stone, 26% high-titanium heavy slag sand, 15% silicate cement clinker powder, 3% lithium slag powder, 4.0% silica fume and 2.0% short-cut polypropylene fiber, and placing the mixture in a mill without grinding media for self-crushing and self-grinding. The mixture is self-crushed and self-grinded by mutual impact and friction between particles, and a dispersant accounting for 6‰ of the mass of the raw materials entering the mill is sprayed into the mixture to obtain an ultra-high toughness engineering material mixture.
[0067] Specifically, the particles of the prepared ultra-high toughness engineering material mixture are all below 10 mm, of which 5mm-10mm particles account for 24%, particles less than 0.045mm account for 30%, and the uniformity of the mixture is 92%; after mixing with water accounting for 6% of the mass percentage of the mixture, the formed slurry has a slump of 265mm and an expansion of 610mm. The hardened body after curing for 28 days has a compressive strength of 121.3MPa and a flexural strength of 16.1MPa.
[0068] Specifically, the dispersant is a mixture of high-performance polycarboxylate water-reducing agent, triethanolamine, diethanol monoisopropanolamine, triisopropanolamine, and graphene oxide dispersion, wherein the mass percentage of the high-performance polycarboxylate water-reducing agent is not less than 90%.
[0069] Example 8
[0070] A method for preparing an ultra-high toughness engineering material mixture comprises the following steps: mixing 50% high-titanium heavy slag crushed stone, 27% high-titanium heavy slag sand, 15% silicate cement clinker powder, 3% lithium slag powder, 3.5% silica fume and 1.5% short-cut polyethylene glycol fiber, and placing the mixture in a mill without grinding media for self-crushing and self-grinding. The mixture is self-crushed and self-grinded by mutual impact and friction between particles, and a dispersant accounting for 6‰ of the mass of the raw materials entering the mill is sprayed into the mixture to obtain an ultra-high toughness engineering material mixture.
[0071] Specifically, the particles of the prepared ultra-high toughness engineering material mixture are all below 10 mm, of which 5mm-10mm particles account for 23%, particles less than 0.045mm account for 32%, and the uniformity of the mixture is greater than 91%; after mixing with water accounting for 8% of the mass percentage of the mixture, the formed slurry has a slump of 250mm and an expansion of 600mm. The hardened body after curing for 28 days has a compressive strength of 125.1MPa and a flexural strength of 18.3MPa.
[0072] Specifically, the dispersant is a mixture of high-performance polycarboxylate water-reducing agent, triethanolamine, diethanol monoisopropanolamine, triisopropanolamine, and graphene oxide dispersion, wherein the mass percentage of the high-performance polycarboxylate water-reducing agent is not less than 90%.
[0073] Example 9
[0074] A method for preparing an ultra-high toughness engineering material mixture comprises the following steps: mixing 50% high-titanium heavy slag crushed stone, 25% high-titanium heavy slag sand, 16% silicate cement clinker powder, 3% lithium slag powder, 4.0% silica fume and 2.0% short-cut polyethylene glycol fiber, and placing the mixture in a mill without grinding media for self-crushing and self-grinding. The mixture is self-crushed and self-grinded by mutual impact and friction between particles, and a dispersant accounting for 6‰ of the mass of the raw materials entering the mill is sprayed into the mixture to obtain an ultra-high toughness engineering material mixture.
[0075] Specifically, the particles of the prepared ultra-high toughness engineering material mixture are all below 10 mm, of which 5mm-10mm particles account for 25%, particles less than 0.045mm account for 34%, and the uniformity of the mixture is 94%; after mixing with water accounting for 8% of the mass percentage of the mixture, the formed slurry has a slump of 280mm and an expansion of 620mm. The hardened body after curing for 28 days has a compressive strength of 124.3MPa and a flexural strength of 17.5MPa.
[0076] Specifically, the dispersant is a mixture of high-performance polycarboxylate water-reducing agent, triethanolamine, diethanol monoisopropanolamine, triisopropanolamine, and graphene oxide dispersion, wherein the mass percentage of the high-performance polycarboxylate water-reducing agent is not less than 90%.
[0077] Comparative Example 1
[0078] A method for preparing an engineering material mixture is provided. According to the raw material component ratio of Example 2, each raw material is weighed and mixed, and then placed in a conventional mixer for mixing, and a dispersant accounting for 6‰ of the mass of the milled raw material is sprayed into it to obtain a comparative mixture.
[0079] Specifically, the prepared comparison mixture has 62% particles below 10 mm, 2% particles between 5 mm and 10 mm, 29% particles less than 0.045 mm, and 84% uniformity of the mixture; after mixing with 8% water by mass of the mixture, the formed slurries are dry and hard, with a slump and expansion of 0 mm, and the hardened body after curing for 28 days has a compressive strength of 65.8 MPa and a flexural strength of 7.8 MPa.
[0080] Specifically, the dispersant is a mixture of high-performance polycarboxylate water-reducing agent, triethanolamine, diethanol monoisopropanolamine, triisopropanolamine, and graphene oxide dispersion, wherein the mass percentage of the high-performance polycarboxylate water-reducing agent is not less than 90%.
[0081] Comparative Example 2
[0082] A method for preparing an engineering material mixture is provided. The raw materials are weighed according to the raw material component ratio of Example 5, mixed, and placed in a conventional mixer for mixing. A dispersant accounting for 6‰ of the mass of the milled raw materials is sprayed into the mixture to obtain a comparative mixture.
[0083] Specifically, the prepared comparison mixture has 58% particles below 10 mm, 2.5% particles between 5 mm and 10 mm, 28% particles less than 0.045 mm, and 80% uniformity of the mixture; after mixing with 8% water by mass of the mixture, the formed slurries are dry and hard, with a slump and expansion of 0 mm, and the hardened body after curing for 28 days has a compressive strength of 53.2 MPa and a flexural strength of 6.4 MPa.
[0084] Specifically, the dispersant is a mixture of high-performance polycarboxylate water-reducing agent, triethanolamine, diethanol monoisopropanolamine, triisopropanolamine, and graphene oxide dispersion, wherein the mass percentage of the high-performance polycarboxylate water-reducing agent is not less than 90%.
[0085] Comparative Example 3
[0086] A method for preparing an engineering material mixture is provided. The raw materials are weighed according to the raw material component ratio of Example 8, mixed, and placed in a conventional mixer for mixing, and a dispersant accounting for 6‰ of the mass of the milled raw materials is sprayed into the mixture to obtain a comparative mixture.
[0087] Specifically, the prepared comparison mixture has 53% particles below 10 mm, 2.9% particles between 5 mm and 10 mm, 22% particles less than 0.045 mm, and a mixture uniformity of 75%. After mixing with 8% water by mass of the mixture, the formed slurries are dry and hard, with a slump and expansion of 0 mm. The hardened body after curing for 28 days has a compressive strength of 43.9 MPa and a flexural strength of 5.2 MPa.
[0088] Specifically, the dispersant is a mixture of high-performance polycarboxylate water-reducing agent, triethanolamine, diethanol monoisopropanolamine, triisopropanolamine, and graphene oxide dispersion, wherein the mass percentage of the high-performance polycarboxylate water-reducing agent is not less than 90%.
[0089] Table 1 Mixture ratio design
[0090]
[0091] Table 2 Particle distribution of mixed materials
[0092]
[0093]
[0094] Table 3 Mixture performance
[0095]
[0096]
[0097] It can be seen from the data in Table 2 that the ultra-high toughness engineering material mixture prepared by the example of the present invention adopts a synchronous process of mixing, self-crushing and self-grinding, so all particles in the mixture are below 10 mm, the particle dispersion and distribution uniformity are good, and the mixture uniformity is above 90%; while the comparative example only undergoes a conventional mixing process, the proportion of particles above 10 mm is high, the particles are distributed in a discontinuous gradation state, and the uniformity is below 85%.
[0098] From the data in Table 3, it can be seen that after the ultra-high toughness engineering material mixture prepared by the example of the present invention is directly mixed with an appropriate amount of water, the slurry has good workability, the slump of the slurry is 250mm-280mm, and the expansion is 600mm-650mm; the hardened body has extremely high bearing capacity and toughness, that is, it has extremely high compressive strength and flexural strength. The mixture of the comparative example has only undergone a conventional mixing process, with a high proportion of particles larger than 10mm, and the particles are in a state of discontinuous gradation distribution, and the uniformity is below 85%. Therefore, after being directly mixed with an appropriate amount of water, the slurry is in a dry and hard state, and the compressive strength and flexural strength of the hardened body can only meet the requirements of conventional high-grade concrete or high-strength concrete, but cannot meet the mechanical performance requirements of ultra-high toughness engineering materials.
[0099] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
[0100] The above specific implementation methods are detailed descriptions of the present invention. It cannot be determined that the specific implementation methods of the present invention are limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions and substitutions can be made without departing from the concept of the present invention, which should be regarded as belonging to the protection scope of the present invention.
Claims
1. A mixture of ultra-high toughness engineering materials, characterized in that: The invention comprises the following raw materials in percentage by dry weight: 40% to 50% of high-titanium heavy slag crushed stone, 25% to 35% of high-titanium heavy slag sand, 15% to 20% of silicate cement clinker powder, 3% to 4% of lithium slag powder, 3.5% to 4.0% of silica fume and 1.5% to 2.0% of chopped fibers.
2. The ultra-high toughness engineering material mixture according to claim 1, characterized in that: All particles of the ultra-high toughness engineering material mixture are below 10 mm, of which 5mm-10mm particles account for 20%-25%, particles smaller than 0.045mm account for 30%-40%, and the remaining particles are larger than 0.045mm and smaller than 5mm, and the uniformity of the mixture is greater than 90%.
3. The ultra-high toughness engineering material mixture according to claim 1, characterized in that: After the ultra-high toughness engineering material mixture is mixed with 6% to 8% water by mass of the mixture, the slump of the formed slurry is 250 to 280 mm, the expansion is greater than 600 to 650 mm, and the compressive strength of the hardened body after curing for 28 days is 120 to 140 MPa and the flexural strength is 15 to 20 MPa.
4. The ultra-high toughness engineering material mixture according to claim 1, characterized in that: The high-titanium heavy slag crushed stone particles have a size of 10 mm to 20 mm, and the mass percentage of TiO2 in the chemical composition thereof is ≥20%.
5. The ultra-high toughness engineering material mixture according to claim 1, characterized in that: The particle size of the high-titanium heavy slag sand is less than 5 mm, of which the mass percentage of particles less than 0.045 mm is not less than 10%; the mass percentage of TiO2 in its chemical composition is ≥20%.
6. The ultra-high toughness engineering material mixture according to claim 1, characterized in that: The mass percentage of particles of the silicate cement clinker powder with a size of less than 0.045 mm is greater than 80%.
7. The ultra-high toughness engineering material mixture according to claim 1, characterized in that: The SO3 content in the chemical composition of the lithium slag powder is not less than 15%, and the dihydrate gypsum content in the mineral composition is not less than 30%.
8. The ultra-high toughness engineering material mixture according to claim 1, characterized in that: The silica fume is SF90 silica fume.
9. The ultra-high toughness engineering material mixture according to claim 1, characterized in that: The chopped fibers are any one of chopped basalt fibers, chopped carbon fibers, chopped polypropylene fibers, and chopped polyethylene glycol fibers, or a mixture of two or more thereof.
10. A method for preparing a mixture of ultra-high toughness engineering materials according to any one of claims 1 to 9, characterized in that: High-titanium heavy slag crushed stone, high-titanium heavy slag sand, silicate cement clinker powder, lithium slag powder, silica fume and chopped fibers are mixed in a certain proportion and placed in a mill without grinding media for self-crushing and self-grinding, and a dispersant is sprayed in to obtain an ultra-high toughness engineering material mixture.
11. The method for preparing a mixture of ultra-high toughness engineering materials according to claim 10, characterized in that: The dispersant accounts for 6‰ of the mass of the raw materials entering the mill.
12. The method for preparing a mixture of ultra-high toughness engineering materials according to claim 10, characterized in that: The dispersant is a mixture of high-performance polycarboxylate water reducer, triethanolamine, diethanol monoisopropanolamine, triisopropanolamine, and graphene oxide dispersion, wherein the mass percentage of the high-performance polycarboxylate water reducer is not less than 90%.
Citation Information
Patent Citations
High titanium slag light aggregate reactive powder concrete and preparation method thereof
CN109400061A
High titanium heavy slag sand superhigh-performance concrete and preparation method thereof
CN110698133A
High-titanium slag sand reactive powder concrete and preparation method thereof
CN111348871A
Graphene oxide ultra-high performance concrete with low cement consumption and preparation method thereof
CN111377687A
Low-shrinkage ultra-high performance concrete and preparation method thereof
CN115893953A