Method for extracting lithium from lithium-containing solution in one step through small-pore zeolite
Through ion exchange technology of small pore zeolite under low temperature conditions, the problems of large energy consumption and low selectivity of lithium resource extraction in the existing technology are solved, and efficient and environmentally friendly one-step extraction and separation and recovery of lithium ions are achieved, suitable for lithium-ion batteries Various environments such as leaching liquid, seawater and brine.
Patent Information
- Application Number
- CN202411007473.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-25
AI Technical Summary
The prior art has problems such as large energy consumption, complex operation and low lithium selectivity when extracting lithium resources from lithium-containing solutions, making it difficult to effectively separate lithium ions, especially in mixed solutions of multiple metal ions.
The small pore zeolite is ion exchange technology to perform high selective lithium extraction under low temperature conditions. By controlling the pore size, temperature and time of the zeolite, one-step extraction of more than 95% of lithium ions is achieved, and high efficiency is maintained through backexchange and recycling.
It has achieved high selectivity for lithium ions. The selectivity of lithium ions is as high as 100, and the adsorption of other metal ions is less. It can effectively separate and recover lithium resources in various environments. It has simple operation and no secondary pollution. The zeolite can be recycled. use.
Smart Images

Figure CN118957260A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of zeolite molecular sieve ion exchange, and in particular to a method for extracting lithium from a lithium-containing solution in one step by using small-pore zeolite. Background Art
[0002] In response to the requirements of low-carbon development, the call for the evolution of energy structure is getting louder and louder. Improving the utilization rate of renewable energy, conversion, automobile electrification, etc., all involve the most promising energy material at present - lithium-ion batteries (LIBs). However, with its continued development momentum, the resource and environmental problems brought about by waste lithium-ion batteries should not be ignored. Secondly, the rapid development of the lithium battery industry will inevitably lead to a shortage of raw materials, and continuing to develop new resources on the earth is not conducive to its sustainable development.
[0003] Among them, lithium, as an important strategic resource and the main raw material of lithium-ion batteries, is often called "white oil". With the rapid development of lithium-ion batteries, the consumption of lithium resources has increased sharply, and there was a shortage. If there is no subsequent resource replenishment, it will be detrimental to the sustainable development of the industry. Therefore, the separation and recovery of lithium resources in waste lithium-ion batteries not only has the purpose of resource recycling, but also effectively solves the environmental problems caused. Secondly, the lithium resources on the earth are widely distributed in the ocean, such as seawater, salt lakes, brine, etc. If they can be effectively utilized, they can be used as an effective supplement to lithium resources. However, it is not an easy task to extract lithium from waste lithium-ion battery leachate and the ocean in one step. It involves the efficient separation of multiple metal ions in the solution.
[0004] At present, the industry generally uses extraction, evaporation, co-precipitation and other methods to extract and recover lithium resources. However, due to their high energy consumption, complex operation, and low lithium selectivity, new recovery methods are urgently needed to separate and recover lithium resources. As a promising green recovery method, adsorption has the advantages of simplicity, high recovery rate, and large processing capacity. It is widely used to separate different metal ions in liquids. Its principle is to use adsorbents to selectively adsorb metal ions, release ions after elution treatment, and then achieve the selective separation of specific metal ions in the solution.
[0005] The core of the adsorption method is the selection of adsorbents. Among them, manganese-based, aluminum-based, and titanium-based ion sieve adsorbents are research hotspots for extracting lithium ions. They are all based on the difference in the diameter of metal ions to achieve the purpose of selectively separating lithium. Zeolite molecular sieve adsorbents have been widely used in the water treatment industry due to their advantages such as simple preparation and easy scale-up. They achieve metal separation and extraction through the difference in the adsorption coefficient of the metal ion complex to be collected by zeolites with cation exchange capacity. It is an ion exchange method. Therefore, based on different separation methods and utilizing the characteristics of zeolite ion exchange, the present invention designs for the first time a new method for extracting lithium from a lithium-containing solution in one step using small-pore zeolites. Summary of the invention
[0006] The present invention aims at the problem of extracting lithium resources from lithium-containing solutions and their sustainable recycling, and provides a method for extracting lithium from lithium-containing solutions in one step by using small-pore zeolites. Due to differences in metal ion charge, size, etc., most zeolites have higher selectivity for high-valent metal ions than for low-valent metal ions. 2+ >M + , so for Ni 2+ / Co 2+ / Mn 2+ / Mg 2+ / Ca 2+ / Li + / Na + / K + Li in mixed solution of various elements + One-step extraction is quite difficult. + The lightest mass and the largest displacement speed, by controlling the pore size, temperature and time of zeolite, the displacement of Li + Therefore, the present invention provides a new method for high-selectivity one-step lithium extraction at low temperature and in a short time by simulating the ratio of metal ions in waste lithium-ion battery leachate, seawater, salt water and brine. This method achieves one-step extraction of more than 95% of lithium ions in the solution at low temperature ≤25°C and ≤4h ion exchange by adding small-pore zeolites EDI, SOD and GIS (pore size ≤0.35nm), with less adsorption of other metal ions, and high selectivity for lithium Li + / M 2+ (M=Ni 2+ / Co 2+ / Mn 2+ / Mg 2+ ) is as high as 100 or more, through zeolite Li + Desorption and recycling can maintain the original effect for more than 5 cycles.
[0007] The present invention is achieved through the following technical scheme: a method for extracting lithium from a lithium-containing solution in one step by using a small-pore zeolite, comprising the following steps:
[0008] (1) cooling the lithium-containing solution to below room temperature;
[0009] (2) Adding small-pore zeolite K-EDI, Na-SOD or Na-GIS to the lithium-containing solution of step (1), stirring is continued under heat preservation conditions to perform ion exchange, and highly selectively adsorb Li + ;
[0010] (3) Based on step (2), the small-pore zeolite after ion exchange is filtered and dried, and then reverse exchange is performed in NaCl or KCl solution to remove Li + , and only Li + -Na + / K + Solution.
[0011] As a further improvement of the technical solution of the present invention, after lithium removal in step (3), filtering and drying are continued to obtain reduced zeolite, and the reduced zeolite is repeatedly subjected to steps (1), (2), and (3) in a reciprocating cycle.
[0012] As a further improvement of the technical solution of the present invention, the lithium-containing solution is a lithium-containing multi-metal ion mixed solution.
[0013] As a further improvement of the technical solution of the present invention, the lithium-containing multi-metal ion mixed solution is + In addition, Ni 2+ 、Co 2+ , Mn 2+ , Li + Mg 2+ , Ca 2+ 、Na + , K + Any one or more metal ions.
[0014] As a further improvement of the technical solution of the present invention, the lithium-containing multi-metal ion mixed solution is Li + -Ni 2+ -Co 2+ -Mn 2+ or Li + -Mg 2+ -Ca 2+ -Na + -K + Mix the solution.
[0015] As a further improvement of the technical solution of the present invention, the Li + -Ni 2+ -Co2+ -Mn 2+ The molar concentration ratio of each ion in the mixed solution is 3-10:1-8:1-2:1-3; the Li + -Mg 2+ -Ca 2+ -Na + -K + The molar concentration ratio of each ion in the mixed solution is 1:1-100:0-0.1:1-19:1-6.
[0016] As a further improvement of the technical solution of the present invention, in step (2), the stirring time is 1-4h.
[0017] As a further improvement of the technical solution of the present invention, in step (3), reverse exchange is performed to remove Li + The temperature is 25-60℃ and the time is 1-4h.
[0018] As a further improvement of the technical solution of the present invention, the silicon-aluminum element ratios of the small-pore zeolites K-EDI, Na-SOD and Na-GIS are 2.0, 1.9 and 3.3 respectively.
[0019] The method for extracting lithium from a lithium-containing solution in one step by using a small-pore zeolite provided by the present invention has the following advantages compared with the prior art:
[0020] 1) The present invention provides a method for highly selectively extracting and separating lithium resources from a lithium-containing solution in one step, and achieves the effect of preferentially adsorbing lithium under ion exchange kinetics and thermodynamic conditions through small-pore zeolite ion exchange. Secondly, the one-step extraction of lithium resources from a solution by zeolite ion exchange is a different mechanism from other methods, and is the first time that it is achieved with high selectivity through small-pore zeolite.
[0021] 2) By selecting small-pore zeolites, the rate at which metal ions enter the zeolite pores is reduced, thereby effectively amplifying the Li + The fastest displacement rate achieves the purpose of kinetic priority selection.
[0022] 3) By lowering the exchange temperature, the diffusion rate of metal ions is further reduced, and the Li + The kinetic difference with other metals effectively inhibits the exchange of zeolite for divalent metals and improves the selectivity for lithium ions.
[0023] 4) The effect of small-pore zeolite ion exchange is obvious, such as: EDI zeolite can adsorb more than 95% of Li in the solution + , other metal ions adsorption <14%, for Li +The selectivity is as high as 100 or more, and it can be recycled for more than 5 times with basically unchanged adsorption efficiency. GIS zeolite can also effectively realize the preferential extraction of lithium under low temperature conditions by controlling the ion exchange kinetics and thermodynamics, and other ions are hardly adsorbed. SOD zeolite can achieve the effect of one-step extraction of lithium from high Mg / Li ratio (1, 10, 100) solution at room temperature, and it can also achieve the effect of one-step extraction of lithium from multi-ion Li + -Mg 2+ -Ca 2+ -Na + -K + In the presence of, lithium is still extracted in one step.
[0024] 5) The present invention can be applied to lithium-ion battery leachate, seawater, salt water, brine and other ions or different concentration ratios for one-step separation and recovery and effective extraction of lithium resources. Compared with the industrial method of recovering lithium or other adsorbents, the SOD zeolite used in the present invention is the most common zeolite, which can be synthesized on a large scale and is simple to synthesize. Secondly, the zeolite ion exchange process is simple and convenient to operate, without secondary pollution, and the zeolite can be recycled. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0027] Figure 1 In Example 1, Li + :Ni 2+ :Co 2+ :Mn 2+ Schematic diagram of the adsorption efficiency of K-EDI zeolite for four metal ions at a concentration ratio of 3:1:1:1. It shows that at 5°C, K-EDI zeolite can effectively adsorb 95% of Li in the solution. + , to you 2+ ,Co 2+ , Mn 2+ Ion adsorption <14%, achieving Li + Highly selective extraction.
[0028] Figure 2 In Example 1, Li + :Ni 2+ :Co 2+ :Mn 2+Schematic diagram of the selectivity of K-EDI zeolite for four ions at a concentration ratio of 3:1:1:1 and low temperature. It shows that K-EDI zeolite has a higher Li + adsorption, and still has lithium selectivity under low concentration conditions, so Li + Selectivity coefficient K d Second, K-EDI zeolite has a high selectivity for lithium. Showing excellent Li + Selective.
[0029] Figure 3 The step (3) in Example 1 is repeated for the steps (1) and (2), and after each cycle, Li + Schematic diagram of adsorption efficiency. It shows that after 5 ion exchange cycles, K-EDI zeolite still has more than 90% Li + Adsorption efficiency and performance remain basically unchanged.
[0030] Figure 4 The XRD diffraction pattern of K-EDI zeolite after repeated cycles in Example 1 shows that the structure of K-EDI zeolite is intact before and after the cycles and is not damaged.
[0031] Figure 5 In Example 2, Li + :Ni 2+ :Co 2+ :Mn 2+ Schematic diagram of the adsorption of four ions by Na-GIS zeolite at a concentration ratio of 3:1:1:1. It shows that at 0°C, Na-GIS can adsorb 0.6 mmol / L of Li + , but for you 2+ 、Co 2+ , Mn 2+ Almost no adsorption, showing high Li + Selectivity, achieving Li + One-step extraction.
[0032] Figure 6 In Example 3, Li + :Mg 2+ :Ca 2+ :Na + :K + Schematic diagram of the adsorption of metal ions in mixed solution by Na-SOD zeolite when the concentration ratio is 1:1:0.1:1:1. It shows that in the presence of various ions, Na-SOD zeolite has a strong adsorption capacity for Li + The adsorption capacity of the metal ions is the highest, which is 1.0mmol / L, which is more than 5 times that of other metal ions (<0.2mmol / L).+ Selective.
[0033] Figure 7 In Example 3, Li + :Mg 2+ :Ca 2+ :Na + :K + Schematic diagram of the adsorption of metal ions in mixed solution by Na-SOD zeolite when the concentration ratio is 1:10:0.1:1:1. 2+ The concentration is increased by 10 times, and it still has high Li + Adsorption capacity and selectivity, suitable for high concentration Mg 2+ / Li + Li in salt water + One-step extraction.
[0034] Figure 8 In Example 3, Li + :Mg 2+ :Ca 2+ :Na + :K + Schematic diagram of the adsorption of metal ions in mixed solution by Na-SOD zeolite when the concentration ratio is 1:100:0.1:1:1. 2+ The concentration is increased by 100 times, and it still has the highest Li + Adsorption capacity can achieve higher concentration of Mg 2+ / Li + Li in salt water + One-step extraction.
[0035] Fig. 9 In Example 4, Li + :Mg 2+ :Na + :K + Schematic diagram of the adsorption efficiency of K-EDI zeolite for metal ions in a mixed solution at a concentration ratio of 1:30:19:6 and low temperature. It shows that K-EDI zeolite has excellent Li + The adsorption capacity is high, and the adsorption efficiency is over 90%, and Mg is hardly adsorbed. 2+ , with high concentration of Mg 2+ / Li + The ability to extract lithium resources from seawater in one step.
[0036] Fig.10 In Example 5, Li + :Ni 2+ :Co 2+ :Mn 2+Schematic diagram of the adsorption efficiency of K-EDI zeolite for four metal ions when the solution temperature rises to 30°C under the condition of a concentration ratio of 3:1:1:1. It shows that as the temperature rises, the adsorption efficiency of zeolite for Ni 2+ 、Co 2+ , Mn 2 The adsorption efficiency of metal ions increases rapidly, and for Li + The efficiency is reduced for Li + Therefore, low temperature conditions are used as zeolite to absorb Li with high selectivity. + The importance of.
[0037] Fig.11 In Example 5, Li + :Ni 2+ :Co 2+ :Mn 2+ Schematic diagram of the adsorption efficiency of Na-GIS zeolite for four metal ions when the solution temperature rises to 30°C under the condition of a concentration ratio of 3:1:1:1. It shows that as the temperature rises, the adsorption efficiency of Na-GIS zeolite for divalent metal Co 2+ , Mn 2+ The adsorption efficiency of Li + was replaced by it, the adsorption efficiency decreased, showing that Mn 2+ Therefore, under high temperature conditions, zeolite does not have the ability to selectively absorb Li. 2+ , reflecting the importance of low temperature. DETAILED DESCRIPTION
[0038] In order to more clearly understand the above-mentioned objectives, features and advantages of the present invention, the scheme of the present invention will be further described below. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
[0039] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein; it is obvious that the embodiments in the specification are only part of the embodiments of the present invention, rather than all of the embodiments.
[0040] The present invention provides a specific embodiment of a method for extracting lithium from a lithium-containing solution in one step by using a small-pore zeolite, comprising the following steps:
[0041] (1) cooling the lithium-containing solution to below room temperature;
[0042] (2) Adding small-pore zeolite K-EDI, Na-SOD or Na-GIS to the lithium-containing solution of step (1), stirring is continued under heat preservation conditions to perform ion exchange and highly selectively adsorb Li + ;
[0043] (3) Based on step (2), the small-pore zeolite after ion exchange is filtered and dried, and then reverse exchange is performed in NaCl or KCl solution to remove Li + , and only Li + -Na + / K + Solution.
[0044] In step (1), the lithium-containing solution is a lithium-containing multi-metal ion mixed solution. Specifically, the lithium-containing multi-metal ion mixed solution contains Li + In addition, Ni 2+ 、Co 2+ , Mn 2+ , Li + Mg 2+ , Ca 2+ 、Na + , K + Any one or more metal ions in the lithium-containing multi-metal ion mixed solution. + The concentration is 0.01-0.1mol / L.
[0045] In one embodiment provided by the present invention, the lithium-containing multi-metal ion mixed solution is Li + -Ni 2+ -Co 2+ -Mn 2+ or Li + -Mg 2+ -Ca 2+ -Na + -K + Mixed solution. + -Ni 2+ -Co 2+ -Mn 2+ The molar concentration ratio of each ion in the mixed solution is 3-10:1-8:1-2:1-3; the Li + -Mg 2+ -Ca 2+ -Na + -K + The molar concentration ratio of each ion in the mixed solution is 1: 1 to 100: 0 to 0.1: 1 to 19: 1 to 6. In the above molar concentration ratio, 0 in 0 to 0.1 means that the concentration of the ion in the mixed solution is 0.
[0046] Specifically, Li + -Ni 2+ -Co 2+ -Mn 2+The molar concentration ratio of each ion in the mixed solution is 3:1:1:1 or 10:5:2:3 or 10:6:2:2 or 10:8:1:1. The aforementioned mixed solution is used to simulate the leaching solution rich in lithium, cobalt, manganese and nickel metal ions obtained by hydrometallurgy in different types of ternary battery industries.
[0047] Li + -Mg 2+ -Ca 2+ -Na + -K + The molar concentration ratio of each ion in the mixed solution is 1:1:0.1:1:1 or 1:10:0.1:1:1 or 1:100:0.1:1:1. The aforementioned mixed solution is used to simulate the ratio of metal ions in salt lake water.
[0048] Li + -Mg 2+ -Ca 2+ -Na + -K + The molar concentration ratio of each ion in the mixed solution is 1:30:0:19:6. The aforementioned mixed solution is used to simulate the ratio of metal ions in real seawater.
[0049] The various mixed solutions provided by the present invention are only for simulating the proportions of metal ions under various environments, and the method of the present invention is not limited to the above-mentioned mixed solutions.
[0050] Wherein below room temperature is specifically 0-25°C. In different embodiments, the lithium-containing solution can be cooled by placing it in an ice water bath. In different embodiments, the lithium-containing solution can be cooled to 0°C, 5°C, 10°C, 15°C, 20°C, 25°C, or at a temperature within any two defined ranges.
[0051] In step (2), the stirring speed after adding the small-pore zeolite is 300-700r / min, and the stirring time is 1-4h. In different embodiments, the stirring speed can be 300r / min, 400r / min, 500r / min, 600r / min, 700r / min, or carried out at a stirring speed within any two limited ranges. In different embodiments, the stirring time can be 0h, 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, or carried out at a stirring time within any two limited ranges.
[0052] The silicon-aluminum element ratios of the small-pore zeolites K-EDI, Na-SOD and Na-GIS are 2.0, 1.9 and 3.3 respectively.
[0053] In step (3), the small-pore zeolite after ion exchange is filtered and dried at a temperature of 60-100° C. Then, reverse exchange is performed in a NaCl or KCl solution to remove Li + The concentration of the NaCl or KCl solution used is 1-2 mol / L. The purpose of the reverse exchange is to convert the Li + is released into the solution, while Na + or K + Supplement Li in zeolite + position occupied, thereby reducing the zeolite.
[0054] Back exchange Li removal + The temperature is 25-60°C and the time is 1-4h. + The temperature during the reaction is 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, or at a temperature within any two defined ranges. In different embodiments, the reaction time can be 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, or at a time within any two defined ranges.
[0055] After the lithium removal in step (3), the zeolite is filtered and dried to obtain the reduced zeolite. The reduced zeolite is subjected to the repetitive cycle of steps (1), (2) and (3). Preferably, the drying temperature is 60-100°C.
[0056] The specific embodiments of the present invention are described in detail below.
[0057] Embodiment 1:
[0058] ① Prepare LiCl with an initial molar concentration ratio of 3:1:1:1 (or 10:5:2:3 or 10:6:2:2 or 10:8:1:1) by adding lithium chloride, cobalt chloride, manganese chloride and nickel chloride samples. + -Ni 2+ -Co 2+ -Mn 2+ Mixed solution, in which Li + The concentration is 0.015mol / L. When the solution temperature is cooled to 5°C, K-EDI zeolite is added to 50mL of the mixed solution. The K-EDI zeolite concentration in the solution is 14g / L. The solution is stirred for 4 hours at a stirring rate of 500r / min for ion exchange and lithium extraction. Finally, the residual metal ion content in the solution is tested by ICP. The adsorption amount of each metal ion in the mixed solution by K-EDI zeolite is shown in the following table.
[0059] ② Filter the step ① to obtain lithium-containing zeolite (LiK-EDI), and dry it at 80°C for 24h. Then add the dried lithium-containing zeolite to 50ml KCl solution with a concentration of 1.5mol / L and a zeolite concentration of 20g / L, and stir at 40°C for 2h to obtain Li + -K + solution, and reducing the zeolite.
[0060] ③ Wash and filter the product from step ② to obtain reduced K-EDI zeolite, and repeat steps ① and ② for 5 cycles.
[0061] Table 1
[0062]
[0063] It can be seen from the table above that under the simulated concentrations of different types of lithium-ion battery leachates, when the solution temperature is cooled to 5°C, K-EDI all maintains a high Li + The adsorption capacity is more than 30 times that of other metal ions, and it has the ability to highly selectively separate and recover Li from four metal ions in one step. + ability.
[0064] Embodiment 2:
[0065] LiCl was prepared by adding LiCl, CoCl, MnCl, and NiCl samples with an initial molar concentration ratio of 3:1:1:1. + -Ni 2+ -Co 2+ -Mn 2+ Mixed solution, in which Li + The concentration is 0.015 mol / L. When the solution temperature is cooled to 0°C, Na-GIS zeolite is added to 50 mL of the mixed solution, the Na-GIS zeolite concentration in the solution is 10 g / L, and stirred for 4 hours at a stirring rate of 400 r / min to perform ion exchange and lithium extraction, and finally the residual metal ion content in the solution is tested by ICP.
[0066] ② Filter the step ① to obtain lithium-containing zeolite (LiNa-GIS), and dry it at 80°C for 24h. Then add the dried lithium-containing zeolite to 50ml NaCl solution with a concentration of 2mol / L and a zeolite concentration of 20g / L, and stir at 60°C for 2h to obtain Li + -Na + solution, and reducing the zeolite.
[0067] Embodiment 3:
[0068] ① Prepare LiCl with an initial molar concentration ratio of 1:1:0.1:1:1 (or 1:10:0.1:1:1 or 1:100:0.1:1:1) by adding lithium chloride, magnesium chloride, sodium chloride, potassium chloride and calcium chloride samples. + -Mg 2+ -Ca 2+ -Na + -K + Mixed solution, in which Li + The concentration is 0.015 mol / L. At 25°C, Na-SOD zeolite was added to 50 mL of the mixed solution, the Na-SOD zeolite concentration in the solution was 4 g / L, and stirred for 4 hours at a stirring rate of 600 r / min to perform ion exchange and lithium extraction, and finally the residual metal ion content in the solution was tested by ICP.
[0069] ② Filter the step ① to obtain lithium-containing zeolite (LiNa-SOD), and dry it at 80°C for 24h. Then add the dried lithium-containing zeolite to 50ml NaCl solution with a concentration of 1mol / L, and the zeolite concentration is 10g / L, and stir at 25°C for 4h to obtain Li + -Na + solution, and reducing the zeolite.
[0070] Embodiment 4:
[0071] LiCl was prepared by adding LiCl, MgCl, NaCl, and KCl samples with an initial molar concentration ratio of 1:30:19:6. + -Mg 2+ -Na + -K + Mixed solution, in which Li + The concentration is 0.015 mol / L. When the solution temperature is cooled to 0°C, K-EDI zeolite is added to 50 mL of the mixed solution, the K-EDI zeolite concentration in the solution is 14 g / L, and stirred for 4 hours at a stirring rate of 500 r / min to perform ion exchange and lithium extraction, and finally the residual metal ion content in the solution is tested by ICP.
[0072] Embodiment 5:
[0073] Prepare LiCl with an initial molar concentration ratio of 3:1:1:1 by adding LiCl, CoCl, MnCl, and NiCl samples. + -Ni 2+ -Co 2+ -Mn 2+Mixed solution. Increase the solution temperature to 30°C, add K-EDI or Na-GIS zeolite to 50 mL of the mixed solution, the concentration of K-EDI zeolite in the solution is 14 g / L, the concentration of Na-GIS zeolite in the solution is 10 g / L, stir for 4 hours, stirring speed is 400 r / min, and finally test the residual metal ion content in the solution by ICP.
[0074] The above is only a specific implementation of the present invention, which enables those skilled in the art to understand or implement the present invention. Although detailed descriptions are given with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments, and they should all be covered by the protection scope of the claims.
Claims
1. A method for extracting lithium from a lithium-containing solution in one step by using a small-pore zeolite, characterized in that: The steps include: (1) Cooling the lithium-containing solution to below room temperature; (2) Add small-pore zeolite K-EDI, Na-SOD or Na-GIS to the lithium-containing solution in step (1), continue stirring under heat preservation conditions, and perform ion exchange to selectively adsorb Li + ; (3) Based on step (2), the small-pore zeolite after ion exchange is filtered and dried, and then reverse exchange is performed in NaCl or KCl solution to remove Li + , and only Li + -Na + / K + Solution.
2. The method for extracting lithium from a lithium-containing solution in one step by using a small-pore zeolite according to claim 1, characterized in that: After lithium removal in step (3), filtering and drying are continued to obtain the reduced zeolite. The reduced zeolite is subjected to the repetitive cycle of (1), (2) and (3).
3. The method for extracting lithium from a lithium-containing solution in one step by using a small-pore zeolite according to claim 1, characterized in that: The lithium-containing solution is a lithium-containing multi-metal ion mixed solution.
4. The method for extracting lithium from a lithium-containing solution in one step by using a small-pore zeolite according to claim 3, characterized in that: The lithium-containing multi-metal ion mixed solution removes Li + In addition, Ni 2+ 、Co 2+ , Mn 2+ , Li + Mg 2+ , Ca 2+ 、 + , K + Any one or more metal ions.
5. The method for extracting lithium from a lithium-containing solution in one step by using a small-pore zeolite according to claim 4, characterized in that: The lithium-containing multi-metal ion mixed solution is Li + -Ni 2+ -Co 2+ -Mn 2+ or Li + -Mg 2+ -Ca 2+ -Na + -K + Mix the solution.
6. The method for extracting lithium from a lithium-containing solution in one step by using a small-pore zeolite according to claim 5, characterized in that: The Li + -Ni 2+ -Co 2+ -Mn 2+ The molar concentration ratio of each ion in the mixed solution is 3-10:1-8:1-2:1-3; the Li + -Mg 2+ -Ca 2+ -Na + -K + The molar concentration ratio of each ion in the mixed solution is 1:1-100:0-0.1:1-19:1-6.
7. The method for extracting lithium from a lithium-containing solution in one step by using a small-pore zeolite according to claim 1, characterized in that: In step (2), the stirring time is 1-4 hours.
8. The method for extracting lithium from a lithium-containing solution in one step by using a small-pore zeolite according to claim 1, characterized in that: In step (3), reverse exchange is performed to remove Li + The temperature is 25-60℃ and the time is 1-4h.
9. The method for extracting lithium from a lithium-containing solution in one step by using a small-pore zeolite according to claim 1, characterized in that: The silicon-aluminum element ratios of the small-pore zeolites K-EDI, Na-SOD and Na-GIS are 2.0, 1.9 and 3.3 respectively.
Citation Information
Patent Citations
Low-silica-alumina-ratio X-type zeolite molecular sieve [(Li,Ca)-LSX] preparation method
CN103539150A
GIS-type zeolite, adsorbent material, and separation method
CN118019710A
Method for producing X zeolite particle exchanged with metal cation
CN1250025A
Method for producing lithium-type zeolite
JP2009227484A
GIS-type zeolite formed body, adsorption apparatus, separation method, and GIS-type zeolite
US20240216888A1
Cited By
Manganese-based lithium ion sieve and preparation method and application thereof
CN120420936A
Method for extracting lithium from spodumene by low-temperature calcination
CN122879521A