VO2-doped thin film sputtering method, spliced composite target material and thin film
The preparation of VO2 films by splicing composite targets and magnetron sputtering methods has solved the problems of complex processes and many impurities in the existing technology, and achieved efficient and safe preparation of doped films, satisfying the adjustable phase change of building energy-saving windows Temperature demand.
Patent Information
- Application Number
- CN202410974642.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-15
AI Technical Summary
The existing VO2 film preparation process is complex, with many impurities, high cost and low efficiency, and difficult to effectively control the doping amount and phase change temperature, which cannot meet the needs of building energy-saving windows.
Using splicing composite targets and magnetron sputtering methods, VO2 films are prepared through sputtering technology, and targets are mixed with pure VO2 and metal oxides (such as WO3 or MoO3) to achieve gradient changes in doping content in the film to avoid sudden occurrence V2O5, designed with adjustable phase transition temperature.
A one-step process is implemented to prepare VO2 films with multiple doping contents, which avoids the generation of highly toxic substances. The phase transition temperature can be designed to continuously adjust from room temperature to 60℃ according to the requirements, meeting the temperature control needs of different ambient temperatures, and improving the preparation Safety and efficiency.
Smart Images

Figure CN118957514A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of functional thin films, and in particular relates to a sputtering method of a doped VO2 thin film, a spliced composite target material and a thin film. Background Art
[0002] Building energy consumption has always accounted for a large proportion of the world's energy consumption. my country's annual building energy consumption can be converted into 1.1 billion tons of standard coal, accounting for 1 / 3 of the country's total energy consumption, and is increasing year by year. Therefore, research on reducing building energy consumption is of great significance. Among the many forms of building energy consumption, the heat loss of door and window glass accounts for more than 50% of the total building energy consumption, which is the most important part of building energy consumption. The main reason for the heat loss of door and window glass is the heat exchange between door and window glass and the external environment. Reducing heat loss is an effective way to reduce building energy consumption. The use of energy-saving glass can effectively reduce heat loss.
[0003] Vanadium oxides can achieve automatic adjustment of the transmittance and reflectance of infrared radiation in sunlight as the ambient temperature changes. Vanadium oxides have unique metal-semiconductor (Metal to Insulator Transfer, MIT) transition characteristics, that is, as the temperature rises, the material undergoes a phase change, from a semiconductor state to a metallic state. Among the various vanadium oxides, VO2 has attracted widespread attention because its phase change temperature is closest to room temperature. When vanadium oxides undergo a phase change, their optical properties in the visible light region do not change much, but important optical characteristics change in the infrared band, that is, as the temperature rises, the infrared band changes from high transmittance to high reflectivity. Therefore, this characteristic of the material can be used to achieve automatic adjustment of the transmittance and reflectance of infrared radiation in sunlight as the ambient temperature changes, so as to achieve the purpose of regulating the room temperature.
[0004] At present, the preparation technology of doped VO2 is complex. The existing technology cannot well control the gradient doping amount, and it is easy to generate toxic substances V2O5. At present, according to the reaction medium involved, it is divided into two categories: based on vapor deposition and based on solution deposition. Vapor deposition includes chemical vapor deposition (CVD) and physical vapor deposition (PVD). Solution deposition mainly includes sol-gel, electrochemical process, hydrothermal process and polymer-assisted deposition. CVD is a common industrial technology for depositing high-quality and high-performance films, but the equipment is expensive, the atmosphere control is strict, and the process is complicated. Common methods of PVD include vacuum evaporation, that is, heating V2O5 in a vacuum so that its atoms or molecules are vaporized from the surface of V2O5 and escape from the steam flow, which is incident on the substrate and condensed to form a solid V2O5 film. The V2O5 film is heated at a certain temperature in a vacuum reduction furnace to obtain a VO2 film. There is also a sputtering method, using a V target, in an O2 atmosphere, the sputtered V is oxidized into V oxide and deposited on the substrate. However, there is a problem that the purity of the film is not high and the highly toxic substance V2O5 will be generated. Solution deposition preparation methods, such as the sol-gel method, generally obtain V2O5 sol, and then repeat the coating-drying process to obtain a dry gel film by vacuum heat treatment. Although it has the advantages of low cost, easy doping, and large-area film formation, the vanadium raw material used has poor solubility and long aging time. In addition, the V2O5 sol is highly toxic and prone to the formation of impurities. Using the commonly used PVD, a trace amount of doping materials such as W, Mo or Nb is uniformly doped into a metal vanadium target to prepare a doped film through reactive sputtering. This requires precise control of the content of the reaction gas, has high process requirements, and can only prepare a film with a doping content and doping component, that is, a film with only one phase transition temperature, resulting in low target utilization and poor economic benefits.
[0005] The phase transition temperature of pure VO2 is 68°C, which is much higher than room temperature and cannot meet the requirements of temperature-controlled smart windows. Lowering the phase transition temperature of VO2 is the key to its application in building energy-saving windows. By doping and other methods, the phase transition temperature can be changed, high-valent ions (such as Nb 5+ , 5+ , W 6+ However, there are still difficulties in the method of doping VO2 thin films, and a stable doping process is urgently needed to achieve VO2 doping. Summary of the invention
[0006] The purpose of the present invention is to propose a new process method for doping VO2 thin films in view of the problems of complex preparation process of existing doped VO2 thin films, more impurities, high cost and low efficiency.
[0007] In order to achieve the above object, the present invention provides the following technical solution, providing a sputtering method for a doped VO2 thin film, the sputtering method comprising the following steps:
[0008] S1: cleaning substrate;
[0009] S2: Place the sample in the magnetron sputtering coating machine, move the baffle between the sample and the target, and evacuate the sample until the vacuum degree is less than 10 -5 Pa;
[0010] S3: introducing inert protective gas;
[0011] S4: empty sputtering to clean the target;
[0012] S5: bias cleaning substrate;
[0013] S6: Remove the baffle and perform sputtering deposition with a sputtering power of 100-200 W and a deposition time of 20-60 min.
[0014] The sputtering method provided by the present invention also has the following technical features: the target material is a spliced composite target material, which is composed of a pure VO2 target material and a mixed target material, and the mixed target material is a mixed target material of metal oxide and VO2.
[0015] The sputtering method provided by the present invention also has the following technical characteristics: the metal oxide is WO3 or MoO3.
[0016] The sputtering method provided by the present invention also has the following technical features: the substrate includes multiple substrates arranged under the target material, the multiple substrates have the same structure, and the multiple substrates are symmetrically placed along the splicing line.
[0017] The sputtering method provided by the present invention also has the following technical characteristics: the cleaning of the substrate includes ultrasonic cleaning in acetone for 15 minutes and ultrasonic cleaning in analytical grade isopropanol for 15 minutes.
[0018] The sputtering method provided by the present invention also has the following technical features: the sputtering power in S4 is 100-200W, the sputtering time is not less than 15min,
[0019] In S5, the bias cleaning voltage is 300-800V, the current is 0.05A, the duty cycle is 75%, and the time is 5-15min.
[0020] The sputtering method provided by the present invention also has the following technical characteristics: the S3 inert gas is argon gas with a purity of 99.99% and a gas pressure of 0.5-1Pa.
[0021] The second object of the present invention is to provide a spliced composite target material for use in any of the sputtering methods described above.
[0022] The spliced composite target material provided by the present invention also has the following technical characteristics: half of the spliced composite target material is a pure VO2 target material, and the other half is a mixed target material of VO2 and metal oxide, and the mass fraction of the metal oxide is 1%-30%.
[0023] The third object of the present invention is to provide a doped VO2 thin film, which is produced using the sputtering method as described in any of the above items.
[0024] Beneficial Effects
[0025] The sputtering method provided by the present invention can achieve a gradient change in the doping content in the film in a single preparation process by splicing composite target materials, thereby realizing a one-step preparation of VO2 films with various doping contents. The preparation process avoids the generation of highly toxic V2O5 in the process and is safe and reliable.
[0026] The spliced composite target material provided by the present invention can achieve a gradient change in the doping content of other metal components in the film during a single preparation process.
[0027] The doped VO2 film provided by the present invention has a gradient doping with other metal contents. Since films with different doping contents have different phase transition temperatures, films with different doping W / Mo contents can be used for temperature-controlled smart window films at different ambient temperatures. The phase transition temperature can be designed according to demand and can be continuously adjusted from room temperature to 60°C, which can meet the intelligent control of room temperature in different seasons and latitudes. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 A schematic diagram of the relative positions of a substrate and a spliced composite target material in a sputtering method provided in an embodiment of the present invention;
[0030] Figure 2 Schematic diagram of a magnetron sputtering device in an embodiment of the present invention;
[0031] Figure 3 is the mass fraction of W in the thin film obtained by the sputtering method provided in the embodiment of the present invention;
[0032] Figure 4 The infrared reflectivity of the thin film sample at 8-14 microns obtained by the sputtering method provided in the embodiment of the present invention;
[0033] Figure 5This is a refractive index influence diagram of a thin film sample obtained by the sputtering method provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0034] The present invention is further described in detail below in conjunction with examples, but it should be noted that these implementation modes are not limitations of the present invention, and any equivalent transformations or substitutions in functions, methods, or structures made by ordinary technicians in the field based on these implementation modes are all within the protection scope of the present invention.
[0035] The embodiment of the present invention provides a sputtering method for a doped VO2 thin film, wherein the device used is as follows: Figure 2 As shown, the sputtering method comprises the following steps:
[0036] S1: cleaning substrate;
[0037] S2: Place the sample in the magnetron sputtering coating machine, move the baffle between the sample and the target, and evacuate the sample until the vacuum degree is less than 10 -5 Pa, vacuum degree is less than 10 -5 Pa can prevent VO2 from being oxidized;
[0038] S3: introducing inert protective gas;
[0039] S4: To remove pollutants or oxides such as V2O3 and V2O5 on the target, the target is cleaned by empty sputtering;
[0040] S5: Bias cleaning of the substrate to remove contaminants on the substrate and to give the substrate surface a certain degree of roughness to increase the bonding strength with the film;
[0041] S6: Remove the baffle and perform sputtering deposition with a sputtering power of 100-200 W and a deposition time of 20-60 min.
[0042] In some embodiments, the target material is a spliced composite target material, which is composed of a pure VO2 target material and a mixed target material, and the mixed target material is a mixed target material of metal oxide and VO2.
[0043] In some embodiments, the metal oxide is WO3 or MoO3.
[0044] In some embodiments, the substrate includes a plurality of substrates disposed under the target material, the plurality of substrates have the same structure, and the plurality of substrates are symmetrically placed along a stitching line.
[0045] In some embodiments, the cleaning of the substrate includes ultrasonic cleaning in acetone for 15 minutes and ultrasonic cleaning in analytical grade isopropanol for 15 minutes. Since the cleanliness of the substrate will greatly affect the bonding strength between the substrate and the film, acetone can clean off organic matter such as grease on the substrate, but due to the limited purity of acetone and the large amount of impurities, analytical grade isopropanol is needed for cleaning afterwards.
[0046] In some embodiments, the sputtering power in S4 is 100-200 W, and the sputtering time is not less than 15 min.
[0047] In S5, the bias cleaning voltage is 300-800V, the current is 0.05A, the duty cycle is 75%, and the time is 5-15min.
[0048] In some embodiments, the S3 inert gas is argon with a purity of 99.99% and a gas pressure of 0.5-1Pa.
[0049] In some embodiments, a spliced composite target is provided for use in any of the sputtering methods described above.
[0050] In some embodiments, half of the spliced composite target is a pure VO2 target, and the other half is a mixed target of metal oxide and VO2, with the mass fraction of the metal oxide being 1%-30%.
[0051] In some embodiments, a doped VO2 thin film is provided, wherein the thin film is manufactured using any of the sputtering methods described above.
[0052] Embodiment 1
[0053] A spliced composite target with a purity of 99.9% is provided, wherein half of the spliced composite target is pure VO2 and the other half is a mixture of VO2 and WO3, wherein the mass fraction of WO3 is 20%. Figure 1 The substrate is coated, and the mass fractions of W in the films at positions 1-5 are 2-6%, 9-11%, 12-14%, 15-16% and 16-17% respectively. A gradient change of the doped W content is formed, as shown in Figure 3 .
[0054] like Figure 4 As shown in the figure, the infrared reflectivity at 8-14 μm indicates that the phase transition temperature of the W-doped film of this system is around 30°C. When W ion doping is performed on VO2, when the mass fraction of W exceeds 2%, the phase transition temperature decreases from 68°C to below 30°C.
[0055] The refractive index of the film at different positions is Figure 5As shown, as the coating position under the splicing target changes, the refractive index response changes, and as the W content increases, the refractive index of the film gradually increases. The refractive index of the film of this system is between 2.2-2.3, indicating that it has a certain transmittance.
[0056] Embodiment 2
[0057] A spliced composite target with a purity of 99.9% is provided, wherein half of the spliced target is pure VO2 and the other half is a mixture of VO2 and WO3, wherein the mass fraction of WO3 is 5%. Figure 1 The substrate is coated, wherein the mass fractions of W in the films corresponding to positions 1-5 are 0.5-1%, 1-1.5%, 1.5-2%, 2-3% and 3-4% respectively, forming a gradient change in the content of doped W. The phase transition temperatures of the films corresponding to positions 1-5 are approximately 40°C, 35°C, 30°C, 25°C and 20°C respectively.
[0058] Embodiment 3
[0059] A spliced composite target with a purity of 99.9% is provided, wherein half of the spliced target is pure VO2 and the other half is a mixture of VO2 and MoO3, wherein the mass fraction of MoO3 is 10%. Figure 1 The substrate is coated, and the mass fractions of Mo in the films corresponding to positions 1-5 are 1-2%, 2-4%, 4-5%, 5-7% and 7-8% respectively, forming a gradient change in the content of doped Mo. As the Mo content increases, the phase transition temperature decreases from 60°C to about 40°C.
[0060] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention shall be included in the protection scope of the present invention. The above description is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present invention. These improvements and variations should also be regarded as the protection scope of the present invention.
Claims
1. A sputtering method for a doped VO2 thin film, characterized in that: The sputtering method comprises the following steps: S1: cleaning substrate; S2: Place the sample in the magnetron sputtering coating machine, move the baffle between the sample and the target, and evacuate the sample until the vacuum degree is less than 10 - 5 Pa; S3: introducing inert protective gas; S4: empty sputtering to clean the target; S5: bias cleaning substrate; S6: Remove the baffle and perform sputtering deposition with a sputtering power of 100-200 W and a deposition time of 20-60 min.
2. The sputtering method according to claim 1, characterized in that: The target material is a spliced composite target material, which is formed by splicing a pure VO2 target material and a mixed target material, and the mixed target material is a mixed target material of metal oxide and VO2.
3. The sputtering method according to claim 2, characterized in that: The metal oxide is WO3 or MoO3.
4. The sputtering method according to claim 1, characterized in that: The substrate comprises a plurality of substrates arranged under the target material, the plurality of substrates have the same structure, and the plurality of substrates are symmetrically placed along a splicing line.
5. The sputtering method according to claim 1, characterized in that: The cleaning of the substrate includes ultrasonic cleaning in acetone for 15 minutes and ultrasonic cleaning in analytical grade isopropanol for 15 minutes.
6. The sputtering method according to claim 1, characterized in that: The sputtering power in S4 is 100-200W, and the sputtering time is not less than 15min. In S5, the bias cleaning voltage is 300-800V, the current is 0.05A, the duty cycle is 75%, and the time is 5-15min.
7. The sputtering method according to claim 3, characterized in that: The S3 inert gas is argon with a purity of 99.99% and a gas pressure of 0.5-1Pa.
8. A spliced composite target, characterized in that: Used in the sputtering method according to any one of claims 1 to 7.
9. The spliced composite target according to claim 8, characterized in that: Half of the spliced composite target material is a pure VO2 target material, and the other half is a mixed target material of metal oxide and VO2, with the mass fraction of the metal oxide being 1-30%.
10. A doped VO2 thin film, characterized in that: The thin film is prepared by the sputtering method according to any one of claims 1 to 7.
Citation Information
Patent Citations
Method for preparing vanadium dioxide film through magnetron sputtering at low temperature
CN108220897A
Preparation method of PFM film with transverse gradient
CN117431513A
Cited By
Copper-titanium co-doped amorphous carbon coating and high-throughput preparation method
CN120330676A
Copper and titanium co-doped amorphous carbon coating and high-throughput preparation method
CN120330676B
Method for preparing copper-titanium co-doped amorphous carbon coating at high flux
CN122610038A