Reinforced recycled aggregate, preparation method thereof and application of reinforced recycled aggregate in solid waste stabilized macadam base

Through mechanically strengthening ball milling-heating shaping and solid waste gelling material slurry treatment, the mechanical properties of recycled aggregates are improved, and the lack of performance in the road base is solved. Through the use of solid waste gelling materials, the mechanical properties of recycled aggregates are improved, and the problem of insufficient performance in the road base is solved. Production costs and environmental pollution have promoted the large-scale application of solid waste in road projects.

CN118993598AActive Publication Date: 2024-11-22SHANDONG TRAFFIC PLANNING DESIGN INST +1

Patent Information

Application Number
CN202411101712.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

The existing recycled aggregate has low mechanical properties in road stable gravel bases, and the production process of solid waste gelling materials requires external reinforcement of alkaline reagents, resulting in environmental pollution and high production costs, which limits its large-scale use.

Method used

Use mechanical reinforced ball mill-heating and shaping to regenerate aggregates, activate regenerated micro powders, and slurry through solid waste gelling material to form a dense slurry layer to improve the mechanical properties of the aggregates. At the same time, use solid waste gelling material as cement Reduce dependence on natural materials.

Benefits of technology

It significantly improves the porosity, water absorption and mechanical properties of recycled aggregates, reduces production costs, reduces environmental pollution, and promotes the large-scale application of solid waste and the development of green transportation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004989536810000161
    Figure BDA0004989536810000161
  • Figure BDA0004989536810000171
    Figure BDA0004989536810000171
  • Figure BDA0004989536810000172
    Figure BDA0004989536810000172
Patent Text Reader

Abstract

The invention discloses a reinforced recycled aggregate, a preparation method thereof and application of the reinforced recycled aggregate in a solid waste stabilized macadam base, and belongs to the technical field of building materials. Carrying out ball milling, heating and shaping on the recycled aggregate to obtain shaped recycled aggregate and recycled micro powder; mixing the regenerated micro powder with a nano material and a filling material, and then carrying out ball milling treatment to obtain activated regenerated micro powder; mixing an alkaline solid waste activator, a precursor material and the activated and regenerated micro powder, and performing ball milling to obtain a solid waste cementing material; and mixing the solid waste cementing material with water to obtain solid waste cementing material mixed slurry, and coating the reshaped recycled aggregate with the slurry to obtain the reinforced recycled aggregate for preparing the stable macadam base. Through ball milling shaping and slurry wrapping treatment, old mortar attached to the surface of the recycled aggregate is effectively removed, the number of edges and corners is reduced, the porosity is reduced, the problems of high porosity, high water absorption, low apparent density and the like of the recycled aggregate are solved, and the mechanical property of the recycled aggregate is improved, so that the recycled aggregate can be used for preparing a stable macadam base.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and in particular relates to a reinforced recycled aggregate and a preparation method thereof and an application thereof in a solid waste stabilized crushed stone base. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] With the continuous advancement of industrialization and urbanization, the demand for building materials and the generation of construction waste and bulk industrial solid waste have increased significantly, and the consumption of resources and the damage to the ecological environment have become increasingly serious. Using bulk solid waste as stable gravel base material for roads after optimized treatment can not only solve the environmental pollution problems caused by the storage and burial of bulk solid waste, but also reduce the over-exploitation of natural resources, which is in line with the core concept of green development of the comprehensive resource utilization industry.

[0004] Recycled aggregate refers to the aggregate obtained by sorting, crushing and screening construction waste such as waste concrete. The surface of recycled coarse aggregate made from waste concrete is adhered to old mortar, with a rough surface and many angular particles. It is damaged during the crushing process and forms a large number of micro cracks inside, resulting in high porosity, high water absorption, low apparent density, high crushing index and high Ca(OH) 2 There are outstanding problems such as crystal content. If recycled aggregate is simply used to replace natural aggregate to prepare a stable gravel base for roads, there is often a problem of low mechanical properties, which seriously limits the promotion and application of recycled aggregate in road engineering construction. When physical strengthening, chemical strengthening or biological strengthening are used to strengthen recycled aggregates, such as CN116143437 N, CN 115215572A, CN114716211A, etc., the strengthening effect is insufficient, the water absorption rate and crushing value indicators are still too large, and there is still a big difference with the performance of natural aggregates, and it cannot be used in large quantities. In addition, most of the current solid waste cementitious materials use bulk solid waste materials with high "silicon aluminum" content. After physical excitation, chemical excitation or composite excitation, it has gelling properties and is expected to become a potential substitute for cement, which provides an effective solution to reduce the high carbon emissions of cement manufacturing and the problem of bulk solid waste storage. However, at present, solid waste cementitious materials need to be activated by adding strong alkaline reagents from the outside, and the hardened specimens are severely alkali-rich, causing secondary pollution to the environment. In addition, the added strong alkaline reagent also increases the production cost of solid waste cementitious materials, limiting their large-scale use. Summary of the invention

[0005] In order to solve the shortcomings of the prior art, the purpose of the present invention is to provide a reinforced recycled aggregate and a preparation method thereof and an application in a solid waste stabilized gravel base. The present invention uses recycled aggregate and other solid waste cementitious materials to prepare a stable gravel base with high mechanical strength to solve the problem that solid waste such as construction waste is difficult to utilize.

[0006] In order to achieve the above object, the technical solution of the present invention is:

[0007] The first aspect of the present invention provides a method for preparing reinforced recycled aggregate, comprising the following steps:

[0008] The recycled aggregate is ball-milled and shaped, and heated during the ball-milling process; after the ball-milling process is completed, shaped recycled aggregate and recycled micro-powder are obtained;

[0009] The regenerated micropowder is mixed with nanomaterials and fillers and then ball-milled to obtain activated regenerated micropowder; an alkaline solid waste activator, a precursor material and the activated regenerated micropowder are mixed and then ball-milled to obtain a solid waste gelling material; the solid waste gelling material is mixed with water to obtain a solid waste gelling material mixed slurry;

[0010] The shaped recycled aggregate is immersed in the solid waste cementitious material mixed slurry, and after the immersion is completed, the shaped recycled aggregate is taken out and subjected to standard curing to obtain reinforced recycled aggregate.

[0011] In some embodiments of the present invention, the ball milling shaping time is 5 to 10 minutes, and the rotation speed is 20 to 40 r / min.

[0012] In some embodiments of the present invention, the heating temperature is 450-550°C.

[0013] In some embodiments of the present invention, the nanomaterial includes nano silicon dioxide and / or nano calcium oxide, and the filler includes Bayer red mud and / or desulfurized gypsum;

[0014] The mass ratio of the recycled micro powder, nano material and filler is (90-95):(0.5-1):(4-9.5).

[0015] In some embodiments of the present invention, the alkaline solid waste activator includes Bayer red mud, desulfurized gypsum and carbide slag, and the mass ratio of Bayer red mud, desulfurized gypsum and carbide slag is (5-6): (2-4): (0.5-1);

[0016] The precursor material includes at least one of blast furnace slag, coal gangue powder, waste glass powder and fly ash;

[0017] The mass ratio of the alkaline solid waste activator, the precursor material and the activated regenerated micropowder is: (1-3): (5-8): (0.5-2).

[0018] In some embodiments of the present invention, the mass ratio of water to solid waste gelling material is (1-5):1.

[0019] In some embodiments of the present invention, the shaped recycled aggregate is washed and dried and then immersed in the mixed slurry of solid waste cementitious material, and intermittent vibration immersion is adopted, the vibration immersion is 5 to 10 minutes, and then the static immersion is 30 to 60 minutes, and the vibration immersion and static immersion are performed alternately, and the total immersion time is 5 to 6 hours.

[0020] The second aspect of the present invention provides a reinforced recycled aggregate, which is prepared by the above-mentioned preparation method.

[0021] In some embodiments of the present invention, the particle size composition of the reinforced recycled aggregate is as follows:

[0022] 0.075-2.36 mm accounts for 10-30 wt%;

[0023] 2.36-4.75mm accounts for 15-25wt%;

[0024] 4.75-9.5mm accounts for 20-35wt%;

[0025] 9.5-19.0 mm accounts for 25-40 wt%;

[0026] 19.0~31.5mm accounts for 10~20wt%.

[0027] The third aspect of the present invention provides a use of the above-mentioned reinforced recycled aggregate in a solid waste stabilized gravel base.

[0028] A fourth aspect of the present invention provides a solid waste stabilized gravel base, wherein the raw materials of the solid waste stabilized gravel base include, by weight: 3 to 6 parts of solid waste cementitious material, 100 to 120 parts of the above-mentioned reinforced recycled aggregate, and 8 to 10 parts of water;

[0029] The solid waste gelling material comprises, by mass percentage, 10-30% of alkaline solid waste activator, 60-80% of precursor material and 10-20% of activated regenerated micro powder.

[0030] The fifth aspect of the present invention provides a method for preparing the above-mentioned solid waste stabilized gravel base, comprising the following steps: mixing solid waste cementitious material, reinforced recycled aggregate and water in proportion, and after paving, rolling and curing, a solid waste stabilized gravel base is obtained.

[0031] The beneficial effects of the present invention are:

[0032] The invention adopts a mechanically enhanced ball milling-heating shaping method to treat the recycled aggregate, which can effectively reduce the content of old mortar attached to the recycled aggregate, effectively reduce the number of edges and corners, remove impurities, and provide a relatively clean surface environment for further enhanced treatment. Then, the recycled aggregate is coated with a slurry prepared from a solid waste gelling material made of activated recycled micropowder, an alkaline solid waste activator, and a precursor material to reduce the porosity of the recycled aggregate and the edges and corners on the surface of the recycled aggregate, thereby obtaining a reinforced recycled aggregate, solving the problems of high porosity, high water absorption, low apparent density, high pressure crushing index and high Ca(OH) 2 The crystal content and other issues are solved, and its mechanical properties are improved, so that it can be promoted and applied in road engineering construction. Among them, the present invention uses solid waste gelling materials to coat the recycled aggregate. On the one hand, the gel formed by the solid waste gelling materials through alkali excitation can fill the pores or microcracks of the recycled aggregate and effectively wrap the surface of the recycled aggregate to form a slurry layer with a dense microstructure. On the other hand, the activator reacts with the silicon-aluminum substances attached to the pores or microcracks of the recycled aggregate to generate more CASH gel, which further exerts the filling effect and reduces the porosity of the recycled aggregate. In addition, the use of solid waste gelling materials as strengthening liquid can fully absorb large amounts of solid waste, which is beneficial to environmental protection.

[0033] The present invention conducts multi-stage strengthening treatment on the recycled aggregate, and prepares a stable crushed stone base with other various solid waste materials, abandoning the traditional preparation method's reliance on high-energy cement and natural sand and stone, adopts solid waste cementitious materials prepared from bulk solid waste as a binder, activates recycled micropowder as an auxiliary binder, and strengthens the recycled aggregate as aggregate, thus promoting the full utilization of recycled aggregate in construction, promoting the large-scale application of bulk solid waste in road engineering construction, and conforming to the concept of green transportation and sustainable development. DETAILED DESCRIPTION

[0034] Terminology explanation:

[0035] Stabilized gravel base, also known as cement stabilized gravel base, is a road base made by mixing cement as a cementitious material with aggregates, fly ash, etc. Compared with traditional rigid and flexible bases, cement stabilized gravel base has the following characteristics:

[0036] 1. Higher bearing capacity: Cement stabilized gravel base has higher strength and stability, can withstand larger loads, and is suitable for all types of roads.

[0037] 2. Better anti-seepage and anti-cracking performance: The cement in the cement-stabilized gravel base can effectively prevent moisture penetration and avoid road cracks, potholes and other diseases.

[0038] 3. Environmental protection and sustainability: Compared with traditional rigid base, cement-stabilized crushed stone base uses less cement, which reduces the impact on the environment. At the same time, the crushed stone can be recycled and has better sustainability.

[0039] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.

[0040] The present invention provides a reinforced recycled aggregate obtained by mechanically strengthening and ball milling solid waste, activating recycled micropowder and coating with solid waste cementitious materials. The obtained reinforced recycled aggregate has low porosity, low water absorption, high apparent density and high mechanical properties, and can be used for the preparation of a stable crushed stone base.

[0041] A first typical embodiment of the present invention provides a method for preparing reinforced recycled aggregate, comprising the following steps:

[0042] The recycled aggregate is ball-milled and shaped, and heated during the ball-milling process; after the ball-milling process is completed, shaped recycled aggregate and recycled micro-powder are obtained;

[0043] The regenerated micropowder is mixed with nanomaterials and fillers and then ball-milled to obtain activated regenerated micropowder; an alkaline solid waste activator, a precursor material and the activated regenerated micropowder are mixed and then ball-milled to obtain a solid waste gelling material; the solid waste gelling material is mixed with water to obtain a solid waste gelling material mixed slurry;

[0044] The shaped recycled aggregate is immersed in the solid waste cementitious material mixed slurry, and after the immersion is completed, the shaped recycled aggregate is taken out and subjected to standard curing to obtain reinforced recycled aggregate.

[0045] The present invention proposes a "three-step method" for strengthening recycled aggregates, namely, mechanically strengthened ball milling-heating shaping treatment, activation of recycled micropowders, and slurry coating treatment with solid waste cementitious materials. Mechanically strengthened ball milling-heating shaping treatment can reduce the content of old mortar attached to the recycled aggregate, effectively reduce the number of edges and corners, remove impurities, and provide a relatively clean surface environment for further strengthening treatment. In addition, the filler material will also fill the cracks and pores of the recycled aggregate through physical adsorption during the ball milling process. The activation of the recycled micropowder is to fully mix the nanomaterials and fillers with the recycled micropowder (obtained during the mechanically strengthened ball milling-heating shaping process) by physical ball milling method, so as to increase the specific surface area and silicon-aluminum content of the recycled micropowder, and firmly attach the stimulating filler to the surface of the recycled micropowder. The present invention performs slurry coating on solid waste gelling materials. On the one hand, the gel formed by the solid waste gelling materials through alkali excitation can fill the pores or microcracks of the recycled aggregate and effectively wrap the surface of the recycled aggregate to form a slurry layer with a dense microstructure. On the other hand, the activator reacts with the silicon-aluminum substances attached to the pores or microcracks of the recycled aggregate to generate more CASH gel, further exerting the filling effect and reducing the porosity of the recycled aggregate. In addition, the use of solid waste gelling materials as strengthening liquid can fully absorb large amounts of solid waste, which is beneficial to environmental protection. The method has the characteristics of being simple, convenient, and highly operable for strengthening recycled aggregates.

[0046] In some embodiments of the present invention, the heating temperature is 450-550°C, and can be specifically 450°C, 451°C, 460°C, 470°C, 480°C, 490°C, 500°C, 510°C, 520°C, 530°C, 540°C, 549°C or 550°C, etc.

[0047] In some embodiments of the present invention, the ball milling shaping time is 5 to 10 minutes, specifically 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes or 10 minutes, etc. The ball milling shaping can be performed in an abrasion tester, and the rotation speed of the abrasion tester can be 20 to 40 r / min, specifically 20 r / min, 21 r / min, 23 r / min, 25 r / min, 27 r / min, 29 r / min, 30 r / min, 31 r / min, 33 r / min, 35 r / min, 37 r / min, 39 r / min or 40 r / min, etc.

[0048] In some embodiments of the present invention, the regenerated micropowder is mixed with nanomaterials and fillers and then ball-milled for 5 to 10 minutes, specifically 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes or 10 minutes.

[0049] In some embodiments of the present invention, the nanomaterial includes nano silicon dioxide and / or nano calcium oxide, and the filler includes Bayer red mud and / or desulfurized gypsum;

[0050] The mass ratio of the recycled micro powder, nano material and filler is (90-95):(0.5-1):(4-9.5).

[0051] In some embodiments of the present invention, the alkaline solid waste activator includes Bayer red mud, desulfurized gypsum and carbide slag, and the mass ratio of Bayer red mud, desulfurized gypsum and carbide slag is (5-6): (2-4): (0.5-1);

[0052] The precursor material includes at least one of blast furnace slag, coal gangue powder, waste glass powder and fly ash;

[0053] The mass ratio of the alkaline solid waste activator, the precursor material and the activated regenerated micropowder is: (1-3): (5-8): (0.5-2).

[0054] In some embodiments of the present invention, the mass ratio of water to solid waste gelling material is (1-5):1.

[0055] In some embodiments of the present invention, the alkaline solid waste activator, the precursor material, and the activated regenerated micropowder are mixed and ball-milled for 3 to 5 minutes, specifically 3 minutes, 3.5 minutes, 4 minutes, 4.5 minutes or 5 minutes, etc.; a ball mill can be used for ball milling, and the rotation speed during ball milling is 400 to 500 r / min, specifically 400 r / min, 410 r / minn, 420 r / min, 430 r / min, 440 r / min, 450 r / min, 460 r / min, 470 r / min, 480 r / min, 490 r / min or 500 r / min, etc.

[0056] In some embodiments of the present invention, the shaped recycled aggregate is washed and dried (free water is fully removed) and then immersed in the solid waste cementitious material mixed slurry, and intermittent vibration immersion is adopted, the vibration immersion is 5 to 10 minutes, specifically 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes or 10 minutes, etc.; then static immersion is carried out for 30 to 60 minutes, specifically 30 minutes, 31 minutes, 35 minutes, 39 minutes, 40 minutes, 41 minutes, 45 minutes, 49 minutes, 50 minutes, 51 minutes, 55 minutes, 59 minutes or 60 minutes, etc.; vibration immersion and static immersion are carried out alternately, and the total immersion time is 5 to 6 hours, specifically 5 hours, 5.1 hours, 5.2 hours, 5.3 hours, 5.4 hours, 5.5 hours, 5.6 hours, 5.7 hours, 5.8 hours, 5.9 hours or 6 hours, etc.

[0057] The second aspect of the present invention provides a reinforced recycled aggregate, which is prepared by the above-mentioned preparation method.

[0058] In some embodiments of the present invention, the particle size composition of the reinforced recycled aggregate is as follows:

[0059] 0.075-2.36 mm accounts for 10-30wt%, specifically 10wt%, 11wt%, 13wt%, 15wt%, 17wt%, 19wt%, 20wt%, 21wt%, 23wt%, 25wt%, 27wt%, 29wt% or 30wt%, etc.;

[0060] 2.36-4.75mm accounts for 15-25wt%, which can be 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt%, 21wt%, 22wt%, 23wt%, 24wt% or 25wt% etc.;

[0061] 4.75-9.5 mm accounts for 20-35wt%, which can be 20wt%, 21wt%, 23wt%, 25wt%, 27wt%, 29wt%, 30wt%, 31wt%, 33wt%, 34wt% or 35wt% etc.;

[0062] 9.5-19.0 mm accounts for 25-40wt%, which can be 25wt%, 26wt%, 27wt%, 29wt%, 30wt%, 31wt%, 33wt%, 35wt%, 37wt%, 39wt% or 40wt% etc.;

[0063] 19.0~31.5mm accounts for 10~20wt%, and can be specifically selected as 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt% or 20wt%, etc.

[0064] The third aspect of the present invention provides a use of the above-mentioned reinforced recycled aggregate in a solid waste stabilized gravel base.

[0065] A fourth aspect of the present invention provides a solid waste stabilized gravel base layer, wherein the raw materials of the solid waste stabilized gravel base layer include, by weight:

[0066] 3 to 6 parts of solid waste cementitious materials, specifically 3 parts, 3.1 parts, 3.5 parts, 3.9 parts, 4 parts, 4.1 parts, 4.5 parts, 4.9 parts, 5 parts, 5.1 parts, 5.5 parts, 5.6 parts or 6 parts;

[0067] 100-120 parts of the above-mentioned reinforced recycled aggregate, specifically 100 parts, 101 parts, 103 parts, 105 parts, 107 parts, 109 parts, 110 parts, 111 parts, 113 parts, 115 parts, 117 parts, 119 parts or 120 parts;

[0068] 8 to 10 parts of water, specifically 8 parts, 8.1 parts, 8.3 parts, 8.5 parts, 8.7 parts, 8.9 parts, 9 parts, 9.1 parts, 9.3 parts, 9.5 parts, 9.7 parts, 9.9 parts or 10 parts;

[0069] The solid waste gelling material comprises, by mass percentage, 10-30% (e.g., 10%, 11%, 13%, 15%, 17%, 19%, 20%, 21%, 23%, 25%, 27%, 29% or 30%) of alkaline solid waste activator, 60-80% (e.g., 60%, 61%, 63%, 65%, 67%, 69%, 70%, 71%, 73%, 75%, 77%, 79% or 80%) of precursor material and 10-20% (e.g., 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20%) of activated regenerated micropowder.

[0070] The fifth aspect of the present invention provides a method for preparing the above-mentioned solid waste stabilized gravel base, comprising the following steps: mixing solid waste cementitious material, reinforced recycled aggregate and water in proportion, and after paving, rolling and curing, a solid waste stabilized gravel base is obtained.

[0071] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.

[0072] Unless otherwise specified, the raw materials used in the following examples are conventional commercial products that can be purchased, such as nano silicon dioxide with a purity of 99.5%, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; nano calcium oxide with a particle size of <160 nm accounting for 98%, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.

[0073] Example 1

[0074] This embodiment provides a reinforced recycled aggregate, and the preparation method thereof is as follows:

[0075] S1. The construction waste is initially crushed and sieved to obtain recycled aggregate, which is then placed in an abrasion tester for ball milling and shaping. The shaping time is 5 minutes, the rotation rate of the abrasion tester is 40r / min, and the ball milling is heated at a heating temperature of 450°C. After the ball milling, recycled micro powder and shaped recycled aggregate are obtained.

[0076] S2, the regenerated micro powder obtained in step S1 is mixed with the nano material and the filler in a mass ratio of 90:0.5:9.5, and then ball milled for 5 minutes to obtain activated regenerated micro powder. In which, by mass percentage, the nano material contains 30% nano silicon dioxide and 70% nano calcium oxide; the filler contains 60% Bayer red mud and 40% desulfurized gypsum.

[0077] S3. The solid waste gelling material composed of alkaline solid waste activator, precursor material and activated regenerated micropowder is mixed and ball milled for 3 minutes at a speed of 500r / min to obtain a solid waste gelling material; the solid waste gelling material is mixed with water to prepare a solid waste gelling material mixed slurry. In terms of mass percentage, the solid waste gelling material includes 30% slag, 35% fly ash, 14.3% Bayer red mud, 9.5% desulfurized gypsum, 1.2% carbide slag, and 10% activated regenerated micropowder, and the solid waste gelling material: water = 1:1, mass ratio.

[0078] S4, drying the free water in the shaped recycled aggregate prepared in step S1, and soaking it in the mixed slurry of solid waste cementitious materials obtained in step S3, intermittently vibrating it during soaking, and resting it for 60 minutes after each vibration for 5 minutes, and the total soaking time is 6 hours. After soaking, take out the soaked shaped recycled aggregate and perform standard curing (curing for 28 days at a temperature of 20±2°C and a humidity greater than 95%) to obtain reinforced recycled aggregate.

[0079] Example 2

[0080] This embodiment provides a reinforced recycled aggregate, and the preparation method thereof is as follows:

[0081] S1. The construction waste is initially crushed and sieved to obtain recycled aggregate, which is then placed in an abrasion tester for ball milling and shaping. The shaping time is adjusted to 10 minutes, the rotation rate of the abrasion tester is adjusted to 20 r / min, and heating is performed during ball milling. The heating temperature is adjusted to 500°C. After the ball milling, recycled micro powder and shaped recycled aggregate are obtained.

[0082] S2, the regenerated micro powder obtained in step S1 is mixed with the nano material and the filler in a mass ratio of 95:1:4, and then ball milled for 5 minutes to obtain activated regenerated micro powder. In which, by mass percentage, the nano material contains 50% nano silicon dioxide and 50% nano calcium oxide; the filler contains 70% Bayer red mud and 30% desulfurized gypsum.

[0083] S3. After mixing the solid waste gelling material composed of the alkaline solid waste activator, the precursor material, and the activated regenerated micropowder, the ball milling time is 4 minutes and the rotation speed is 400r / min to obtain the solid waste gelling material; the solid waste gelling material is mixed with water to prepare a solid waste gelling material mixed slurry. Among them, by mass percentage, the solid waste gelling material includes 30% slag, 20% fly ash, 20% Bayer red mud, 8% desulfurized gypsum, 2% carbide slag, and 20% activated regenerated micropowder, and the solid waste gelling material: water = 1:3, mass ratio.

[0084] S4, drying the free water in the shaped recycled aggregate prepared in step S1, and soaking it in the mixed slurry of solid waste cementitious materials obtained in step S3, intermittently vibrating it during soaking, and resting it for 30 minutes after each vibration of 10 minutes, and the total soaking time is 5 hours. After soaking, take out the soaked shaped recycled aggregate and perform standard curing (curing for 28 days at a temperature of 20±2°C and a humidity greater than 95%) to obtain reinforced recycled aggregate.

[0085] Example 3

[0086] This embodiment provides a reinforced recycled aggregate, and the preparation method thereof is as follows:

[0087] S1. The construction waste is initially crushed and sieved to obtain recycled aggregate, which is then placed in an abrasion tester for ball milling and shaping. The shaping time is adjusted to 8 minutes, the rotation rate of the abrasion tester is adjusted to 30r / min, and heating is performed during ball milling. The heating temperature is adjusted to 480°C. After the ball milling, recycled micro powder and shaped recycled aggregate are obtained.

[0088] S2, the regenerated micro powder obtained in step S1 is mixed with the nano material and the filler in a mass ratio of 93:1:6, and then ball milled for 5 minutes to obtain the activated regenerated micro powder. In which, by mass percentage, the nano material contains 40% nano silicon dioxide and 60% nano calcium oxide; the filler contains 50% Bayer red mud and 50% desulfurized gypsum.

[0089] S3. The solid waste gelling material composed of alkaline solid waste activator, precursor material and activated regenerated micropowder is mixed and ball milled for 3.5 minutes at a speed of 450r / min to obtain a solid waste gelling material; the solid waste gelling material is mixed with water to prepare a solid waste gelling material mixed slurry. In terms of mass percentage, the solid waste gelling material includes 35% slag, 35% fly ash, 12.5% ​​Bayer red mud, 5% desulfurized gypsum, 2.5% carbide slag, and 10% activated regenerated micropowder, and the solid waste gelling material: water = 1:5, mass ratio.

[0090] S4, drying the free water in the shaped recycled aggregate prepared in step S1, and soaking it in the mixed slurry of solid waste cementitious materials obtained in S3, intermittently vibrating it during soaking, and resting it for 40 minutes after each vibration for 8 minutes, and the total soaking time is 5.5 hours. After soaking, take out the soaked shaped recycled aggregate and perform standard curing (curing for 28 days at a temperature of 20±2°C and a humidity greater than 95%) to obtain reinforced recycled aggregate.

[0091] Example 4

[0092] This embodiment provides a reinforced recycled aggregate, and the preparation method thereof is as follows:

[0093] S1. The construction waste is initially crushed and sieved to obtain recycled aggregate, which is then placed in an abrasion tester for ball milling and shaping. The shaping time is adjusted to 7 minutes, and the rotation rate of the abrasion tester is adjusted to 35r / min. The ball milling is heated and the heating temperature is adjusted to 500°C. After the ball milling, recycled micro powder and shaped recycled aggregate are obtained.

[0094] S2, the regenerated micro powder obtained in step S1 is mixed with the nano material and the filler in a mass ratio of 92:1:7, and then ball milled for 7 minutes to obtain activated regenerated micro powder. In which, by mass percentage, the nano material contains 8% nano silicon dioxide and 20% nano calcium oxide; the filler contains 90% Bayer red mud and 10% desulfurized gypsum.

[0095] S3. After mixing the solid waste gelling material composed of the alkaline solid waste activator, the precursor material, and the activated regenerated micropowder, the ball milling time is 5 minutes and the rotation speed is 400r / min to obtain the solid waste gelling material; the solid waste gelling material is mixed with water to prepare a solid waste gelling material mixed slurry. Among them, by mass percentage, the solid waste gelling material includes 40% slag, 30% fly ash, 6.25% Bayer red mud, 2.5% desulfurized gypsum, 1.25% carbide slag, and 20% activated regenerated micropowder, and the solid waste gelling material: water = 1:4, mass ratio.

[0096] S4, drying the free water in the shaped recycled aggregate prepared in step S1, and soaking it in a mixed slurry of solid waste cementitious materials, performing intermittent vibration during soaking, and resting for 50 minutes after each vibration for 8 minutes, and the total soaking time is 5 hours. After soaking, take out the soaked shaped recycled aggregate and perform standard curing (curing for 28 days at a temperature of 20±2°C and a humidity greater than 95%) to obtain reinforced recycled aggregate.

[0097] Example 5

[0098] This embodiment provides a reinforced recycled aggregate, and the preparation method thereof is as follows:

[0099] S1. The construction waste is initially crushed and sieved to obtain recycled aggregate, which is then placed in an abrasion tester for ball milling and shaping. The shaping time is adjusted to 8 minutes, the abrasion tester rotation rate is adjusted to 40r / min, and heating is performed during ball milling. The heating temperature is adjusted to 490°C. After the ball milling, recycled micro powder and shaped recycled aggregate are obtained.

[0100] S2, the regenerated micro powder obtained in step S1 is mixed with the nano material and the filler in a mass ratio of 91:0.8:8.2, and then ball milled for 7 minutes to obtain activated regenerated micro powder. In which, by mass percentage, the nano material contains 70% nano silicon dioxide and 30% nano calcium oxide; the filler contains 80% Bayer red mud and 20% desulfurized gypsum.

[0101] S3. The solid waste gelling material composed of alkaline solid waste activator, precursor material and activated regenerated micropowder is mixed and ball milled for 4 minutes at a speed of 480r / min to obtain a solid waste gelling material; the solid waste gelling material is mixed with water to prepare a solid waste gelling material mixed slurry. In terms of mass percentage, the solid waste gelling material includes 40% slag, 40% fly ash, 10% Bayer red mud, 4% desulfurized gypsum, 1% carbide slag, and 5% activated regenerated micropowder, and the solid waste gelling material: water = 1:2, mass ratio.

[0102] S4, drying the free water in the shaped recycled aggregate prepared in step S1, and soaking it in the mixed slurry of solid waste cementitious materials obtained in step S3, intermittently vibrating it during soaking, and resting it for 40 minutes after each vibration of 10 minutes, and the total soaking time is 6 hours. After soaking, take out the soaked shaped recycled aggregate and perform standard curing (curing for 28 days at a temperature of 20±2°C and a humidity greater than 95%) to obtain reinforced recycled aggregate.

[0103] Example 6

[0104] This embodiment provides a stable crushed stone base, which includes 100 parts of reinforced recycled aggregate, 3 parts of solid waste cementitious material and 8 parts of water, by weight, wherein the reinforced recycled aggregate and the solid waste cementitious material are the same as those in Example 1, and the gradation of the reinforced recycled aggregate is shown in Table 1 below:

[0105] Table 1 Grading of reinforced recycled aggregate in Example 6

[0106]

[0107] The above-mentioned raw materials of the stable crushed stone base were used to make test pieces in the laboratory for testing mechanical properties. The specific steps are as follows:

[0108] Pour the solid waste cementitious material, the reinforced recycled aggregate and water into a mixer and mix them evenly to obtain a mixture;

[0109] The stirred mixture is placed in a molding machine for compression molding to obtain a test piece;

[0110] Place the pressed specimens in a curing room with a temperature of 20±2℃ and a humidity greater than 75% for curing.

[0111] Example 7

[0112] This embodiment provides a stable crushed stone base, which includes 100 parts of reinforced recycled aggregate, 6 parts of solid waste cementitious material and 8 parts of water, by weight, wherein the reinforced recycled aggregate and the solid waste cementitious material are the same as those in Example 2, and the gradation of the reinforced recycled aggregate is shown in Table 2 below:

[0113] Table 2 Grading of reinforced recycled aggregate in Example 7

[0114]

[0115] The raw materials of the above-mentioned stable crushed stone base layer were used to make test pieces in the laboratory for testing mechanical properties. The specific steps refer to Example 6.

[0116] Example 8

[0117] This embodiment provides a stable crushed stone base, which includes 120 parts of reinforced recycled aggregate, 5 parts of solid waste cementitious material and 10 parts of water, by weight, wherein the reinforced recycled aggregate and the solid waste cementitious material are the same as those in Example 3, and the gradation of the reinforced recycled aggregate is shown in Table 3 below:

[0118] Table 3 Grading of reinforced recycled aggregate in Example 8

[0119]

[0120] The raw materials of the above-mentioned stable crushed stone base layer were used to make test pieces in the laboratory for testing mechanical properties. The specific steps refer to Example 6.

[0121] Example 9

[0122] This embodiment provides a stable crushed stone base, which includes 110 parts of reinforced recycled aggregate, 6 parts of solid waste cementitious material and 9 parts of water, by weight, wherein the reinforced recycled aggregate and the solid waste cementitious material are the same as those in Example 4, and the gradation of the reinforced recycled aggregate is shown in Table 3 below:

[0123] Table 4 Reinforced recycled aggregate gradation in Example 9

[0124]

[0125] The raw materials of the above-mentioned stable crushed stone base layer were used to make test pieces in the laboratory for testing mechanical properties. The specific steps refer to Example 6.

[0126] Example 10

[0127] This embodiment provides a stable crushed stone base layer, which includes 100 parts of reinforced recycled aggregate, 5 parts of solid waste cementitious material and 8 parts of water, by weight, wherein the reinforced recycled aggregate and the solid waste cementitious material are the same as those in Example 5.

[0128] Table 5 Grading of reinforced recycled aggregate in Example 10

[0129]

[0130] The raw materials of the above-mentioned stable crushed stone base layer were used to make test pieces in the laboratory for testing mechanical properties. The specific steps refer to Example 6.

[0131] Comparative Example 1

[0132] This comparative example provides a stable crushed stone base, which is different from Example 6 in that the reinforced recycled aggregate mixed slurry uses commercially available P·O 42.5 ordinary Portland cement, and other methods and steps are the same as Example 6, which will not be repeated here.

[0133] Comparative Example 2

[0134] This comparative example provides a stable crushed stone base, which is different from Example 6 in that the reinforced recycled aggregate used is not subjected to mechanical reinforcement ball milling-heating shaping treatment, and other methods and steps are the same as Example 6, which will not be repeated here.

[0135] Comparative Example 3

[0136] This comparative example provides a stable crushed stone base, which is different from Example 6 in that the reinforced recycled aggregate used is only subjected to mechanical reinforcement ball milling and shaping treatment, and is not subjected to heating treatment. Other methods and steps are the same as those in Example 6 and will not be repeated here.

[0137] Comparative Example 4

[0138] This comparative example provides a stable gravel base layer, which is different from Example 6 in that the regenerated micropowder used is not subjected to activation treatment, and other methods and steps are the same as those in Example 6, which will not be repeated here.

[0139] Comparative Example 5

[0140] This comparative example provides a stable gravel base, which is different from Example 6 in that the reinforced recycled aggregate used is not treated with solid waste cementitious material slurry coating, and other methods and steps are the same as Example 6, which will not be repeated here.

[0141] Comparative Example 6

[0142] This comparative example provides a stable gravel base layer, which differs from Example 6 in that the reinforced recycled aggregate used is not subjected to intermittent vibration immersion when it is coated with solid waste cementitious materials. Other methods and steps are the same as those in Example 6 and will not be repeated here.

[0143] Comparative Example 7

[0144] This comparative example provides a stable gravel base, which differs from Example 6 in that the reinforced recycled aggregate used is coated with solid waste cementitious materials and no standard curing is adopted. Other methods and steps are the same as Example 6 and will not be repeated here.

[0145] Comparative Example 8

[0146] This comparative example provides a stable gravel base layer, which differs from Example 6 in that the reinforced recycled aggregate used has not been subjected to mechanical strengthening ball milling and shaping treatment, the recycled micropowder in the solid waste cementitious material has not been activated, and the solid waste cementitious material has not been subjected to slurry coating treatment. Other methods and steps are the same as those in Example 6 and will not be repeated here.

[0147] Performance Test:

[0148] The stable crushed stone base obtained in Examples 6 to 10 and Comparative Examples 1 to 8 was tested. The performance indicators of the reinforced recycled aggregates and the prepared stable crushed stone base used in Examples 6 to 10 and Comparative Examples 1 to 8 are shown in Table 6 below:

[0149] Table 6 Performance test results of stable crushed stone base obtained from Examples 6 to 10 and Comparative Examples 1 to 8

[0150]

[0151]

[0152] As shown in Table 6, the strengthening combination of recycled aggregates significantly improves the various properties of the strengthened recycled aggregates. The strengthened recycled aggregates used in Examples 6 to 10, i.e., the strengthened recycled aggregates prepared in Examples 1 to 5, are significantly better than those in Comparative Examples 1 to 8 in terms of water absorption, crushing index, and needle-like content. In Comparative Example 8, the recycled aggregates that have not been treated with mechanically strengthened ball milling, activated recycled micropowder, and slurry coated with solid waste cementitious materials are further deteriorated in terms of water absorption, crushing index, and needle-like content compared to other comparative examples, indicating that mechanically strengthened ball milling, activated recycled micropowder, and solid waste cementitious materials have significant effects on reducing the water absorption, crushing index, and needle-like content of the recycled aggregates. On the one hand, the solid waste cementitious materials are treated with alkali activation to form a cementitious material, which not only has excellent filling performance, but also can accurately fill the pores and tiny cracks in the recycled aggregates, and it can also tightly wrap around the surface of the recycled aggregates to construct a dense slurry layer. This slurry layer not only improves the microstructure of the recycled aggregate, enhances its overall density, but also improves its mechanical properties and durability. At the same time, the alkali activator reacts chemically with the silicon and aluminum substances in the pores or microcracks of the recycled aggregate during the reaction process to generate more CASH gel. The generation of CASH gel further strengthens the filling effect. It is like a microscopic "adhesive" that tightly connects the particles inside the recycled aggregate, further reduces the porosity of the recycled aggregate, and enhances the density and strength of the recycled aggregate.

[0153] Comparing the 7d unconfined compressive strength of the stable crushed stone base in Table 6, it can be seen that the 7d unconfined compressive strength of the stable crushed stone base provided by Examples 6 to 10 is close to or higher than 5.0 MPa, while the stable crushed stone bases provided by Comparative Examples 2 to 8 are all lower than the 4.0 MPa required by the specification, and most of them are around 3.0 MPa. Only the strength provided by Comparative Example 1 just reaches 4.0 MPa, and the 7d unconfined compressive strength of the stable crushed stone base prepared by Comparative Example 8 using recycled aggregates that have not been treated with any strengthening measures is only 1.9 MPa, which is far below the specification requirements.

[0154] In summary, the present invention strengthens the recycled aggregate by adopting treatment methods such as mechanical strengthening ball milling, regenerated micropowder activation, and solid waste cementitious material slurry coating, and then uses the strengthened recycled aggregate, activated regenerated micropowder and solid waste cementitious material to prepare a stable crushed stone base. The 7d unconfined compressive strength of the stable crushed stone base is around 5.0MPa, has high mechanical properties, and can meet construction requirements.

[0155] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing reinforced recycled aggregate, characterized in that: The steps include: The recycled aggregate is ball-milled and shaped, and heated during the ball-milling process; after the ball-milling process is completed, shaped recycled aggregate and recycled micro-powder are obtained; The regenerated micropowder is mixed with nanomaterials and fillers and then ball-milled to obtain activated regenerated micropowder; an alkaline solid waste activator, a precursor material and the activated regenerated micropowder are mixed and then ball-milled to obtain a solid waste gelling material; the solid waste gelling material is mixed with water to obtain a solid waste gelling material mixed slurry; The shaped recycled aggregate is immersed in the solid waste cementitious material mixed slurry, and after the immersion is completed, the shaped recycled aggregate is taken out and subjected to standard curing to obtain reinforced recycled aggregate.

2. The method for preparing a reinforced recycled aggregate according to claim 1, characterized in that: The ball milling shaping time is 5 to 10 minutes, and the rotation speed is 20 to 40 r / min; Preferably, the heating temperature is 450-550°C.

3. The method for preparing a reinforced recycled aggregate according to claim 1, characterized in that: The nano material includes nano silicon dioxide and / or nano calcium oxide, and the filler includes Bayer red mud and / or desulfurized gypsum; The mass ratio of the recycled micro powder, nano material and filler is (90-95):(0.5-1):(4-9.5).

4. The method for preparing a reinforced recycled aggregate according to claim 1, characterized in that: The alkaline solid waste activator comprises Bayer red mud, desulfurized gypsum and carbide slag, and the mass ratio of Bayer red mud, desulfurized gypsum and carbide slag is (5-6):(2-4):(0.5-1); Preferably, the precursor material includes at least one of blast furnace slag, coal gangue powder, waste glass powder and fly ash; Preferably, the mass ratio of the alkaline solid waste activator, the precursor material and the activated regenerated micropowder is (1-3):(5-8):(0.5-2).

5. The method for preparing a reinforced recycled aggregate according to claim 1, characterized in that: The mass ratio of water to solid waste gelling material is (1-5):

1.

6. A reinforced recycled aggregate, characterized in that: The reinforced recycled aggregate is prepared by the preparation method according to any one of claims 1 to 5.

7. The reinforced recycled aggregate according to claim 6, characterized in that: The particle size composition of the reinforced recycled aggregate is as follows: 0.075-2.36 mm accounts for 10-30 wt%; 2.36-4.75mm accounts for 15-25wt%; 4.75-9.5mm accounts for 20-35wt%; 9.5-19.0 mm accounts for 25-40 wt%; 19.0~31.5mm accounts for 10~20wt%.

8. Use of the reinforced recycled aggregate according to claim 6 or 7 in a solid waste stabilized crushed stone base.

9. A solid waste stabilized gravel base, characterized in that: The raw materials of the solid waste stabilized crushed stone base layer include, by weight: 3 to 6 parts of solid waste cementitious materials, 100 to 120 parts of the reinforced recycled aggregate according to claim 6 or 7, and 8 to 10 parts of water; The solid waste gelling material comprises, by mass percentage, 10-30% of alkaline solid waste activator, 60-80% of precursor material and 10-20% of activated regenerated micro powder.

10. A method for preparing a solid waste stabilized gravel base layer according to claim 9, characterized in that: The method comprises the following steps: mixing solid waste cementitious materials, reinforced recycled aggregate and water in a proportion as specified in the claim, and obtaining a solid waste stabilized crushed stone base after spreading, rolling and curing.

Citation Information

Patent Citations

  • Recycled concrete prepared through waste concrete and preparation method of recycled concrete

    CN109970402A

  • Regenerated aggregate concrete and preparation method thereof

    CN110845184A

  • Regenerated geopolymer mortar as well as preparation method and application thereof

    CN112408875A

  • Performance-adjustable solid waste-based composite cementing material as well as preparation method and application thereof

    CN116969698A

  • All-solid-waste base material for roads and construction process of all-solid-waste base material

    CN117383897A

Cited By

  • Solid-waste-based expansive recycled aggregate interface enhancer as well as slurry coating method and application of solid-waste-based expansive recycled aggregate interface enhancer

    CN120483658A

  • Solid waste-based expansion type recycled aggregate interface strengthening agent and its grouting method and application

    CN120483658B