Modified imidazoline and flower-like zinc oxide blended corrosion and hydrogen inhibitor and preparation method thereof

By blending imidazoline oleate with flower-like zinc oxide, combining surfactant to promote flower-like structure, the problem of poor hydrogen permeation and corrosion inhibition in oil and gas fields is solved, and efficient corrosion inhibition and hydrogen permeation inhibition is achieved, which significantly improves the The protective performance of oil and gas fields.

CN119020789APending Publication Date: 2024-11-26SOUTHWEST PETROLEUM UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411113570.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the prior art, corrosion inhibitors cannot effectively inhibit hydrogen penetration in oil and gas fields, resulting in hydrogen bubbles and hydrogen-induced stress cracking, and traditional coatings are costly to protect and easily damaged.

Method used

By blending the modified imidazoline oleate with flower-like zinc oxide, a P-π structure conjugation system is formed, which enhances the adsorption effect with metal materials, and combines dodecyldimethylbenzylammonium chloride to promote flower-like zinc oxide. The growth of the flower-like structure with a high specific surface area is formed, and hydrogen ion adsorption is inhibited.

Benefits of technology

It has achieved efficient corrosion inhibition and hydrogen permeability inhibition, significantly improved the protection performance of local corrosion and hydrogen-induced stress cracking in oil and gas fields, improved corrosion inhibition efficiency, and reached 46%, solving the problem of poor results in traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020789A_ABST
    Figure CN119020789A_ABST
Patent Text Reader

Abstract

The invention discloses a modified imidazoline and flower-like zinc oxide blended corrosion and hydrogen inhibitor and a preparation method thereof, and relates to the field of oil field corrosion and hydrogen inhibitors and preparation methods thereof, the modified imidazoline and flower-like zinc oxide blended corrosion and hydrogen inhibitor is prepared from the following raw materials: modified oleic acid imidazoline and flower-like zinc oxide, the modified oleic acid imidazoline is prepared from oleic acid imidazoline and benzyl chloride. The oleic acid imidazoline and the benzyl chloride are modified to obtain the modified oleic acid imidazoline, the modified oleic acid imidazoline is mixed with the flower-like zinc oxide to obtain the blended corrosion and hydrogen inhibitor, and the blended corrosion and hydrogen inhibitor has efficient corrosion inhibition effect and hydrogen permeation inhibition effect; the common phenomena of local corrosion and hydrogen-induced stress cracking in the field of oil and gas fields can be effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of oilfield corrosion and hydrogen inhibitors and a preparation method thereof, and in particular to a modified imidazoline and flower-shaped zinc oxide mixed corrosion and hydrogen inhibitor and a preparation method thereof. Background Art

[0002] Oleic acid imidazoline is a commonly used acidic oil and gas field corrosion inhibitor with good compatibility, no irritating odor, low toxicity and other advantages. The hydrophilic side chain of oleic acid imidazoline contains heteroatoms such as N and O, which can be stably adsorbed on the metal surface to form a monomolecular adsorption film layer, thereby inhibiting corrosion.

[0003] Zinc oxide is a polar crystal with a zinc-rich anode and an oxygen-rich cathode. The growth unit of zinc oxide particles prepared by hydrothermal method is Zn(OH)4 2- , dodecyl dimethyl benzyl ammonium chloride is a cationic surfactant, which will dissociate into positively charged ions in the solution. Positively charged cations and Zn(OH)4 2- There is an electrostatic attraction between them, which makes the crystal grow faster along the anode surface, restricting its growth on certain specific crystal planes and finally forming particles of different shapes.

[0004] In the service conditions of oil and gas fields, most of them are acidic and oxygen-free conditions. The cathode mainly undergoes hydrogen evolution reaction to produce a large number of hydrogen atoms. Under the driving force of the concentration gradient, the hydrogen atoms penetrate into the metal matrix, causing hydrogen bubbling and hydrogen-induced stress cracking, which seriously threatens production safety. The main method to inhibit hydrogen penetration in oil fields is to apply a coating, but the coating is easy to damage and has a high cost of use.

[0005] Chinese patent CN106319529A discloses a method for preparing a modified imidazoline corrosion inhibitor, which is mainly aimed at the corrosion protection of metal materials. The components and mass fractions of the modified imidazoline corrosion inhibitor are as follows: 250-350 parts of fatty acid, 120-200 parts of polyamine, wherein the fatty acid is one of rosin acid, tall oil fatty acid, lauric acid, linoleic acid, palmitic acid, caproic acid, and stearic acid, and the polyamine is one of diethylenetriamine, triethylenetetramine, tetraethylenepentamine, hydrogenated tallow amine, oil-based primary amine, and N-tallow-1,3-propylene diamine. The corrosion inhibitor is both water-soluble and oil-soluble, which expands the application conditions. However, the corrosion inhibitor does not show the effect of inhibiting hydrogen penetration.

[0006] Chinese patent CN107829095A discloses a method for preparing a modified imidazoline quaternary ammonium salt corrosion inhibitor, which is mainly aimed at corrosion and protection problems in the field of oil and gas fields. The components and mass ratio of the modified imidazoline quaternary ammonium salt corrosion inhibitor are as follows: oleic acid: diethylenetriamine: xylene: boric acid = 3.5:10:7:0.5, imidazoline intermediate: benzoic acid = 2:3. The preparation method of the corrosion inhibitor is simple, and a benzene ring and an O-containing polar group are introduced on the basis of the imidazoline structure, and the quaternary ammonium salt formed by quaternization of benzyl chloride is used to improve its water solubility. However, the corrosion inhibition effect of the corrosion inhibitor is poor, and the effect of inhibiting hydrogen penetration is not reflected.

[0007] In view of this, this application is filed. Summary of the invention

[0008] The purpose of the present invention is to provide a modified imidazoline and flower-shaped zinc oxide mixed corrosion inhibitor and a preparation method thereof, by modifying imidazoline and then mixing it with flower-shaped zinc oxide to solve the problem of poor corrosion inhibition effect and inability to inhibit hydrogen penetration in the prior art.

[0009] The present invention is achieved by the following technical scheme: a modified imidazoline and flower-shaped zinc oxide mixed corrosion inhibitor and hydrogen inhibitor, comprising the following raw materials:

[0010] Modified oleic acid imidazoline and flower-shaped zinc oxide. The raw materials for preparing the modified oleic acid imidazoline include oleic acid imidazoline and benzyl chloride.

[0011] Principle: In the embodiment of the present invention, the modified oleic acid imidazoline has a P-π structure conjugated system, which can enhance the adsorption effect with the metal material and further enhance the corrosion inhibition effect.

[0012] Preferably, the raw materials for preparing the flower-shaped zinc oxide include zinc acetate dihydrate, sodium hydroxide, a surfactant and a catalyst.

[0013] Preferably, the mass ratio of the modified oleic acid imidazoline to the flower-shaped zinc oxide is 8 to 12:1.

[0014] Preferably, the mass ratio of the oleic acid imidazoline to the benzyl chloride is 18-22:2.

[0015] Preferably, the mass ratio of zinc acetate dihydrate, sodium hydroxide, surfactant and catalyst is 8-12:1.5-2.5:3-5:1.

[0016] Preferably, the surfactant is dodecyldimethylbenzyl ammonium chloride, and the catalyst is anhydrous dimethyl sulfoxide.

[0017] In the embodiment of the present invention, dodecyldimethylbenzyl ammonium chloride is a cationic surfactant, which will dissociate into positively charged ions in the solution, causing the zinc oxide to grow faster along the anode surface during its formation, ultimately leading to a flower-like structure.

[0018] In order to better solve the problem of the embodiment of the present invention, a method for preparing a modified imidazoline and flower-shaped zinc oxide mixed corrosion inhibitor and hydrogen inhibitor is also provided, comprising the following steps:

[0019] S1: placing oleic acid imidazoline and benzyl chloride in a reaction device, heating and adding tetrabutylammonium bromide to react, and cooling after the reaction is completed to obtain modified oleic acid imidazoline;

[0020] S2: reacting zinc acetate dihydrate, sodium hydroxide, a surfactant and a catalyst, centrifuging and filtering in sequence after the reaction is completed, washing the filtered white powder with water, taking it out, centrifuging and filtering it again, and finally drying it to obtain flower-shaped zinc oxide;

[0021] S3: The modified oleic acid imidazoline is mixed with flower-shaped zinc oxide to obtain a blended corrosion inhibitor and hydrogen inhibitor.

[0022] Preferably, S1 includes placing oleic acid imidazoline and benzyl chloride in a three-necked flask, reflux with a condenser, adding tetrabutylammonium bromide when the temperature rises to 100-150° C., then heating to 180-240° C., reacting for 4-6 hours, and cooling to obtain modified oleic acid imidazoline.

[0023] Preferably, S2 comprises reacting zinc acetate dihydrate, sodium hydroxide, a surfactant and a catalyst at a constant temperature of 60 to 90° C. for 6 to 8 hours, centrifuging and filtering in sequence after cooling to room temperature, repeatedly washing the filtered white powder with deionized water, taking it out and centrifuging and filtering it again, and drying it at a temperature of 60 to 80° C. for 20 to 24 hours under a nitrogen atmosphere to obtain flower-shaped zinc oxide.

[0024] Preferably, the mass ratio of the tetrabutylammonium bromide to the oleic acid imidazoline is 1:18-22.

[0025] Compared with the prior art, the embodiments of the present invention have the following advantages and beneficial effects:

[0026] 1. In the embodiment of the present invention, oleic acid imidazoline and benzyl chloride are modified to obtain modified oleic acid imidazoline, which is then mixed with flower-shaped zinc oxide to obtain a blended corrosion inhibitor and hydrogen inhibitor. The blended corrosion inhibitor and hydrogen inhibitor has both efficient corrosion inhibition effect and hydrogen permeation inhibition effect, and can effectively solve the local corrosion and hydrogen-induced stress cracking phenomena that are common in oil and gas fields (in acidic environments).

[0027] 2. The blended corrosion inhibitor and hydrogen inhibitor provided and prepared by the present invention has higher corrosion inhibition efficiency than the traditional oleic acid imidazoline corrosion inhibitor.

[0028] 3. Dodecyl dimethyl benzyl ammonium chloride combines with the synthetic product through charge characteristics such as electrostatic adsorption, hydrogen bonding, and chemical bonding, thereby changing the physical and chemical properties of the synthetic product and improving its performance. Because dodecyl dimethyl benzyl ammonium chloride is a cationic surfactant, it will dissociate positively charged ions in the solution, which will make the zinc oxide grow faster along the anode surface during its formation, and eventually promote a flower-like structure.

[0029] 4. The zinc oxide particles prepared by the traditional method are elliptical. The flower-shaped zinc oxide particles have a larger specific surface area and can release more zinc ions during use. Zinc ions can be adsorbed on the surface of the corrosion inhibition film, making the corrosion inhibition film have positive properties. Since hydrogen ions also have positive charges, there is a repulsive force between them and the zinc ions adsorbed on the surface of the flower-shaped film layer, and hydrogen ions are not easily adsorbed on the metal surface. Therefore, the occurrence of hydrogen evolution reaction on the metal surface is suppressed, thereby suppressing the hydrogen permeation phenomenon.

[0030] 5. The embodiment of the present invention designs the ratio of each component so that when the blended corrosion inhibitor and hydrogen inhibitor is added at a dosage of 200 mg / L, the corrosion inhibition rate reaches 95% and the hydrogen inhibition rate reaches 46%. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the technical solutions of the exemplary embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present invention and should not be regarded as limiting the scope. For those of ordinary skill in the art, other relevant drawings can be obtained based on these drawings without creative work. In the drawings:

[0032] Figure 1 This is a SEM image of the flower-shaped zinc oxide prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0034] Therefore, the detailed description of the embodiments of the present invention provided below is not intended to limit the scope of the claimed invention, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] The embodiment of the present invention provides a method for preparing a modified imidazoline and flower-shaped zinc oxide mixed corrosion inhibitor and hydrogen inhibitor, comprising the following steps:

[0036] S1: placing oleic acid imidazoline and benzyl chloride in a three-necked flask, reflux with a condenser, and when the temperature rises to 100-150°C, adding tetrabutylammonium bromide, then heating to 180-240°C, reacting for 4-6 hours, and cooling to obtain modified oleic acid imidazoline;

[0037] S2: reacting zinc acetate dihydrate, sodium hydroxide, dodecyldimethylbenzyl ammonium chloride and anhydrous dimethyl sulfoxide at a constant temperature of 60 to 90° C. for 6 to 8 hours, centrifuging and filtering in sequence after cooling to room temperature, repeatedly washing the filtered white powder with deionized water, taking it out and centrifuging and filtering it again, and drying it at a temperature of 60 to 80° C. for 20 to 24 hours under a nitrogen atmosphere to obtain flower-like zinc oxide;

[0038] S3: The modified oleic acid imidazoline is mixed with flower-shaped zinc oxide to obtain a blended corrosion inhibitor and hydrogen inhibitor.

[0039] Example 1

[0040] This embodiment provides a method for preparing a modified imidazoline and flower-shaped zinc oxide mixed corrosion inhibitor and hydrogen inhibitor, comprising the following contents:

[0041] Take 20g of oleic acid imidazoline and 2g of benzyl chloride and put them in a three-necked flask. Use a condenser to reflux. When the temperature rises to 120°C, add 1g of tetrabutylammonium bromide, then quickly heat up to 200°C, react for 5h, and cool to obtain modified oleic acid imidazoline. 10g of zinc acetate dihydrate, 2g of sodium hydroxide, 4g of dodecyldimethylbenzyl ammonium chloride and 1g of anhydrous dimethyl sulfoxide are reacted at a constant temperature of 80°C for 6h. After cooling to room temperature, centrifuge and filter. The filtered white powder is repeatedly washed with deionized water, taken out and centrifuged and filtered again. Dry at 70°C for 22h under a nitrogen atmosphere to obtain flower-shaped zinc oxide. The modified oleic acid imidazoline and the flower-shaped zinc oxide are fully mixed in a mass ratio of 10:1 to obtain the target blended corrosion inhibitor and hydrogen inhibitor. The flower-shaped zinc oxide prepared in Example 1 is subjected to SEM scanning. The scanning results are as shown in FIG. Figure 1 As shown, the surface area is significantly increased.

[0042] Example 2

[0043] This embodiment provides a method for preparing a modified imidazoline and flower-shaped zinc oxide mixed corrosion inhibitor and hydrogen inhibitor, comprising the following contents:

[0044] Take 18g of oleic acid imidazoline and 2g of benzyl chloride and place them in a three-necked flask, reflux with a condenser, and when the temperature rises to 100°C, add 1g of tetrabutylammonium bromide, then quickly heat to 180°C, react for 4h, and cool to obtain modified oleic acid imidazoline. 8g of zinc acetate dihydrate, 1.5g of sodium hydroxide, 3g of dodecyl dimethyl benzyl ammonium chloride and 1g of anhydrous dimethyl sulfoxide are reacted at a constant temperature of 60°C for 6h, and after cooling to room temperature, centrifuged and filtered, the filtered white powder is repeatedly washed with deionized water, taken out and centrifuged and filtered again, and dried at 60°C for 20h under a nitrogen atmosphere to obtain flower-shaped zinc oxide. The modified oleic acid imidazoline and the flower-shaped zinc oxide are fully mixed in a mass ratio of 8:1 to obtain the target blended corrosion inhibitor and hydrogen inhibitor.

[0045] Example 3

[0046] Provided is a method for preparing a modified imidazoline and flower-shaped zinc oxide mixed corrosion inhibitor and hydrogen inhibitor, comprising the following contents:

[0047] Take 22g of oleic acid imidazoline and 2g of benzyl chloride and place them in a three-necked flask, reflux with a condenser, and when the temperature rises to 150°C, add 1g of tetrabutylammonium bromide, then quickly heat to 240°C, react for 6h, and cool to obtain modified oleic acid imidazoline. 12g of zinc acetate dihydrate, 2.5g of sodium hydroxide, 5g of dodecyl dimethyl benzyl ammonium chloride and 1g of anhydrous dimethyl sulfoxide are reacted at a constant temperature of 90°C for 8h, and after cooling to room temperature, centrifuged and filtered, the filtered white powder is repeatedly washed with deionized water, taken out and centrifuged and filtered again, and dried at 80°C for 24h under a nitrogen atmosphere to obtain flower-shaped zinc oxide. The modified oleic acid imidazoline and the flower-shaped zinc oxide are fully mixed in a mass ratio of 12:1 to obtain the target blended corrosion inhibitor and hydrogen inhibitor.

[0048] Example 4

[0049] Provided is a method for preparing a modified imidazoline and flower-shaped zinc oxide mixed corrosion inhibitor and hydrogen inhibitor, comprising the following contents:

[0050] Take 25g of oleic acid imidazoline and 1g of benzyl chloride and place them in a three-necked flask, reflux with a condenser, and when the temperature rises to 200°C, add 1g of tetrabutylammonium bromide, then quickly heat to 300°C, react for 8h, and cool to obtain modified oleic acid imidazoline. 15g of zinc acetate dihydrate, 5g of sodium hydroxide, 7g of dodecyl dimethyl benzyl ammonium chloride and 1g of anhydrous dimethyl sulfoxide are reacted at a constant temperature of 100°C for 10h, and after cooling to room temperature, centrifuged and filtered, the filtered white powder is repeatedly washed with deionized water, taken out and centrifuged and filtered again, and dried at 100°C for 30h under a nitrogen atmosphere to obtain flower-shaped zinc oxide. The modified oleic acid imidazoline and the flower-shaped zinc oxide are fully mixed in a mass ratio of 15:1 to obtain the target blended corrosion inhibitor and hydrogen inhibitor.

[0051] Example 5

[0052] Provided is a method for preparing a modified imidazoline and flower-shaped zinc oxide mixed corrosion inhibitor and hydrogen inhibitor, comprising the following contents:

[0053] Take 10g of oleic acid imidazoline and 2g of benzyl chloride and place them in a three-necked flask, reflux with a condenser, and when the temperature rises to 80°C, add 1g of tetrabutylammonium bromide, then quickly heat to 150°C, react for 3h, and cool to obtain modified oleic acid imidazoline. 5g of zinc acetate dihydrate, 0.5g of sodium hydroxide, 2g of dodecyl dimethyl benzyl ammonium chloride and 1g of anhydrous dimethyl sulfoxide are reacted at a constant temperature of 50°C for 8h, and after cooling to room temperature, centrifuged and filtered, the filtered white powder is repeatedly washed with deionized water, taken out and centrifuged and filtered again, and dried at 50°C for 15h under a nitrogen atmosphere to obtain flower-shaped zinc oxide. The modified oleic acid imidazoline and the flower-shaped zinc oxide are fully mixed in a mass ratio of 5:1 to obtain the target blended corrosion inhibitor and hydrogen inhibitor.

[0054] Comparative Example 1

[0055] Provided is a method for preparing an unmodified imidazoline and flower-shaped zinc oxide mixed corrosion and hydrogen inhibitor, comprising the following contents:

[0056] 10g zinc acetate dihydrate, 2g sodium hydroxide, 4g benzyl chloride and 1g anhydrous dimethyl sulfoxide were reacted at 60°C for 6h, cooled to room temperature, centrifuged and filtered, the filtered white powder was repeatedly washed with deionized water, taken out and centrifuged and filtered again, and dried at 60°C for 20h under nitrogen atmosphere to obtain flower-shaped zinc oxide. Oleic acid imidazoline and flower-shaped zinc oxide were fully mixed at a mass ratio of 10:1 to obtain a blended corrosion inhibitor and hydrogen inhibitor.

[0057] Comparative Example 2

[0058] A method for preparing a corrosion and hydrogen inhibitor mixed with imidazoline modified in another way and flower-shaped zinc oxide is provided, comprising the following contents:

[0059] Take 20g of oleic acid imidazoline and 2g of didecyl dimethyl ammonium chloride and place them in a three-necked flask, reflux with a condenser, and when the temperature rises to 100°C, then quickly heat it to 180°C, react for 4h, and cool it to obtain modified oleic acid imidazoline. 10g of zinc acetate dihydrate, 2g of sodium hydroxide, 4g of dodecyl dimethyl benzyl ammonium chloride and 1g of anhydrous dimethyl sulfoxide are reacted at a constant temperature of 60°C for 6h, and after cooling to room temperature, centrifuged and filtered, the filtered white powder is repeatedly washed with deionized water, taken out and centrifuged and filtered again, and dried at 60°C for 20h under a nitrogen atmosphere to obtain flower-shaped zinc oxide. The modified oleic acid imidazoline and the flower-shaped zinc oxide are fully mixed in a mass ratio of 10:1 to obtain the target blended corrosion inhibitor and hydrogen inhibitor.

[0060] Comparative Example 3

[0061] Provided is a method for preparing a modified imidazoline and granular zinc oxide mixed corrosion inhibitor and hydrogen inhibitor, comprising the following contents:

[0062] Take 20g of oleic acid imidazoline and 2g of benzyl chloride and place them in a three-necked flask, reflux with a condenser, and when the temperature rises to 100°C, add 1g of tetrabutylammonium bromide, then quickly heat to 180°C, react for 4h, and cool to obtain modified oleic acid imidazoline. 10g of zinc acetate dihydrate, 2g of sodium hydroxide, and 1g of anhydrous dimethyl sulfoxide are reacted at a constant temperature of 60°C for 6h, and after cooling to room temperature, centrifuged and filtered, the filtered white powder is repeatedly washed with deionized water, taken out and centrifuged and filtered again, and dried at 60°C for 20h under a nitrogen atmosphere to obtain granular zinc oxide. The modified oleic acid imidazoline and granular zinc oxide are fully mixed in a mass ratio of 10:1 to obtain the target blended corrosion inhibitor and hydrogen inhibitor.

[0063] Test results: The corrosion inhibition and hydrogen inhibition performance of the corrosion inhibitors prepared in Examples 1 to 5 and Comparative Examples 1 to 3 were tested:

[0064] (1) Corrosion inhibition performance test

[0065] The corrosive medium is 3.5wt.% NaCl solution, pH adjusted to 5.5, temperature 37°C, normal pressure. The N80 steel sample is made into a 30*15*3 hanging piece, placed in the corrosive solution, 3 pieces are placed in each bottle, different types of corrosion inhibitors are added respectively, and corroded for 14 days.

[0066] After the experiment, the sample was cleaned with a film removal solution (100 mL hydrochloric acid + 10 g hexamethylenetetramine + 900 ml deionized water), then dehydrated with ethanol and dried with N2. The static uniform corrosion inhibition rate determination method in the petroleum and natural gas industry standard SY / T 5273-2014 "Performance Indicators and Evaluation Methods for Corrosion Inhibitors for Oilfield Produced Water Treatment" was used for evaluation. The formula for uniform corrosion rate is as follows:

[0067]

[0068] Among them, in the formula,

[0069] r c —Uniform corrosion rate, in mm / a;

[0070] m—mass of the test piece before the test, in g;

[0071] m1—mass of the test piece after the test, in g;

[0072] S—total area of ​​the test piece, in cm 2 ;

[0073] ρ—density of the test piece material, in g / cm 3 ;

[0074] t—test time, in hours.

[0075] The formula for corrosion inhibition efficiency is as follows:

[0076]

[0077] In the formula,

[0078] η w —Corrosion inhibition efficiency, in %;

[0079] r0—Corrosion rate of blank test piece, in mm / a;

[0080] r1—Corrosion rate of the specimen after adding the slow-release hydrogen inhibitor, in mm / a.

[0081] (2) Hydrogen barrier performance test experiment:

[0082] The hydrogen permeation curve was tested with reference to the test method provided in the national standard GB / T 30074-2013 "Method for measuring hydrogen permeation (absorption and migration) in metals by electrochemical techniques", and the hydrogen concentration was calculated by the calculation method provided therein.

[0083] Formula 1:

[0084]

[0085] In the formula,

[0086] J ss —The hydrogen atom permeation flux on the oxidation surface of the sample when the steady state is reached, in mol / m 2 s 1 ;

[0087] I ss —Steady-state hydrogen atom penetration current, unit is A / m 2 ;

[0088] A—Exposed area of ​​the sample in the oxidation cell, in m 2 ;

[0089] F—Faraday constant (F=96485), unit is C / mol 1 ;

[0090] D1—lattice diffusion coefficient of hydrogen atoms, unit is m 2 / s 1 ;

[0091] C0—subsurface hydrogen atom concentration on the hydrogen-filled side of the experiment, in mol / m 3 ;

[0092] L—sample thickness, in m.

[0093] Formula 2:

[0094]

[0095] In the formula,

[0096] η h —Hydrogen suppression efficiency, in %;

[0097] C0—Hydrogen concentration of blank test piece, in ppm;

[0098] C1—Hydrogen concentration of the test piece after adding the slow-release hydrogen inhibitor, in ppm.

[0099] Conclusion: The blended corrosion and hydrogen inhibitors prepared in Examples 1-5 and Comparative Examples 1-3 were subjected to corrosion inhibition and hydrogen barrier performance tests. The results are shown in Table 1 below:

[0100] Table 1: Comparison of sustained release effect and hydrogen barrier effect

[0101]

[0102] From the results of the comparison between Comparative Example 1 and Examples 1-3 in the above 1, it can be seen that the modified oleic acid imidazoline in the embodiment of the present invention has a P-π structure conjugated system, which can enhance the adsorption effect with the metal material, thereby enhancing the corrosion inhibition effect. From the comparison between Comparative Example 2 and Examples 1-3, it can be seen that the oleic acid imidazoline can also improve the corrosion inhibition efficiency by using other modifiers, but since the P-π structure conjugated system in the embodiment of the present invention is not formed, the corrosion inhibition efficiency is not as obvious as that in the embodiment of the present invention. By comparing Comparative Example 3 with Comparative Example 2 and Examples 1-3, it can be seen that the addition of dodecyl dimethyl benzyl ammonium chloride can promote the flower-like structure of zinc oxide, thereby significantly improving the hydrogen inhibition efficiency of the corrosion inhibitor and hydrogen inhibitor. By comparing Examples 4-5 with Examples 1-3, it can be seen that when the mass ratio of modified oleic acid imidazoline and flower-like zinc oxide is in the range of 8 to 12:1, the mass ratio of oleic acid imidazoline and benzyl chloride is in the range of 18 to 22:2, and the mass ratio of zinc acetate dihydrate, sodium hydroxide, surfactant and catalyst is in the range of 8 to 12:1.5 to 2.5:3 to 5:1, the corrosion inhibitor and hydrogen inhibitor have better performance.

[0103] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A modified imidazoline and flower-shaped zinc oxide blended corrosion inhibitor, characterized in that: The modified oleic acid imidazoline comprises the following raw materials: modified oleic acid imidazoline and flower-shaped zinc oxide. The raw materials for preparing the modified oleic acid imidazoline comprise oleic acid imidazoline and benzyl chloride.

2. The modified imidazoline and flower-shaped zinc oxide blended corrosion inhibitor according to claim 1, characterized in that: The raw materials for preparing the flower-shaped zinc oxide include zinc acetate dihydrate, sodium hydroxide, a surfactant and a catalyst.

3. The modified imidazoline and flower-shaped zinc oxide blended corrosion inhibitor according to claim 1, characterized in that: The mass ratio of the modified oleic acid imidazoline to the flower-shaped zinc oxide is 8 to 12:

1.

4. The modified imidazoline and flower-shaped zinc oxide blended corrosion inhibitor and hydrogen inhibitor according to claim 1, characterized in that: The mass ratio of the oleic acid imidazoline to the benzyl chloride is 18-22:

2.

5. The modified imidazoline and flower-shaped zinc oxide blended corrosion inhibitor and hydrogen inhibitor according to claim 2, characterized in that: The mass ratio of the zinc acetate dihydrate, sodium hydroxide, surfactant and catalyst is 8-12:1.5-2.5:3-5:

1.

6. A modified imidazoline and flower-shaped zinc oxide blended corrosion inhibitor and hydrogen inhibitor according to claim 2 or 5, wherein the surfactant is dodecyldimethylbenzylammonium chloride and the catalyst is anhydrous dimethyl sulfoxide.

7. A method for preparing a modified imidazoline and flower-shaped zinc oxide mixed corrosion inhibitor and hydrogen inhibitor, characterized in that: The following steps are involved: S1: placing oleic acid imidazoline and benzyl chloride in a reaction device, heating and adding tetrabutylammonium bromide to react, and cooling after the reaction is completed to obtain modified oleic acid imidazoline; S2: reacting zinc acetate dihydrate, sodium hydroxide, a surfactant and a catalyst, centrifuging and filtering in sequence after the reaction is completed, washing the filtered white powder with water, taking it out, centrifuging and filtering it again, and finally drying it to obtain flower-shaped zinc oxide; S3: The modified oleic acid imidazoline is mixed with flower-shaped zinc oxide to obtain a blended corrosion inhibitor and hydrogen inhibitor.

8. The method for preparing a modified imidazoline and flower-shaped zinc oxide blended corrosion inhibitor and hydrogen inhibitor according to claim 7, characterized in that: S1 includes placing oleic acid imidazoline and benzyl chloride in a three-necked flask, reflux with a condenser, adding tetrabutylammonium bromide when the temperature rises to 100-150° C., then heating to 180-240° C., reacting for 4-6 hours, and cooling to obtain modified oleic acid imidazoline.

9. The method for preparing a modified imidazoline and flower-shaped zinc oxide blended corrosion inhibitor and hydrogen inhibitor according to claim 7, characterized in that: S2 includes reacting zinc acetate dihydrate, sodium hydroxide, a surfactant and a catalyst at a constant temperature of 60 to 90° C. for 6 to 8 hours, centrifuging and filtering in sequence after cooling to room temperature, repeatedly washing the filtered white powder with deionized water, taking it out and centrifuging and filtering it again, and drying it at a temperature of 60 to 80° C. for 20 to 24 hours in a nitrogen atmosphere to obtain flower-like zinc oxide.

10. The method for preparing a modified imidazoline and flower-shaped zinc oxide blended corrosion inhibitor and hydrogen inhibitor according to claim 7, characterized in that: The mass ratio of the tetrabutylammonium bromide to the oleic acid imidazoline is 1:18-22.