Preparation method and application of Mn-based perovskite illuminant glue

By preparing Mn-based perovskite luminescent in situ on the chip surface, the problem of lead-based and cadmium-based materials is solved, and the light efficiency improvement of non-toxic, anti-oxidant and water-resistant is achieved, and it is suitable for LED light conversion applications.

CN119039965APending Publication Date: 2024-11-29WENZHOU XINXIN TAIJING TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411151067.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing lead-based and cadmium-based perovskite materials limit their widespread use in chip surface packaging and applications due to their contamination and bioaccumulation, and require the development of non-toxic alternative materials.

Method used

The Mn-based perovskite precursor was used to combine with solvent and glue, heated under vacuum stirring to prepare the Mn-based perovskite luminescent in situ, and the light diffusion effect was improved by embedding the light diffusion agent to form a light emitting composite structure.

Benefits of technology

The preparation of lead-free and cadmium-free Mn-based perovskite luminescents has been realized, which improves its anti-oxidation and water resistance and light effect. It can be directly used for LED chip surface curing or base film surface coating to form a light conversion coating or film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039965A_ABST
    Figure CN119039965A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of Mn-based perovskite luminophor glue, which comprises the following steps: dissolving an Mn-based perovskite precursor in a solvent A, and stirring until the Mn-based perovskite precursor is completely dissolved to obtain a precursor solution; and then respectively adding the precursor solution and a light diffusion agent into glue, mixing, and heating under vacuum stirring to remove the solvent A, thereby preparing the Mn-based perovskite illuminant in situ in the glue, the solvent A and the glue are immiscible; the Mn-based perovskite precursor is composed of an organic halide and a manganese halide. The invention aims to develop the Mn-based perovskite luminous body glue so as to develop packaging and application of a non-toxic perovskite material on the surface of a chip.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of Mn-based luminophore synthesis, and in particular relates to a preparation method of Mn-based perovskite luminophore glue and application thereof. Background Art

[0002] Metal halide perovskite luminescent materials have attracted widespread attention due to their special crystal structure, high fluorescence quantum efficiency, narrow emission peak, adjustable band gap and other excellent optoelectronic properties. They have important application prospects in lighting, display, solar energy, laser, anti-counterfeiting and other fields, and have developed rapidly in a relatively short period of time.

[0003] However, the perovskite materials with excellent photoelectric properties reported so far are all based on lead-based organic-inorganic hybrid perovskites, or lead-based all-inorganic perovskite materials, or cadmium-based perovskite materials. Cadmium and lead are extremely polluting and easily accumulate in organisms, posing a great threat to the ecological environment and human health, and are not conducive to the large-scale use and promotion of perovskite materials. Therefore, it is crucial to develop new non-lead and non-cadmium perovskite materials.

[0004] Mn-based perovskite materials are a type of metal halide crystal material with a perovskite-like structure. They do not contain heavy metals such as lead and cadmium. Mn ions serve as luminescent centers. Their unique dd transitions allow them to have tunable crystal field luminescence, large Stokes shifts, strong absorption bands in the ultraviolet and blue regions, and resistance to thermal quenching of fluorescence. These unique properties make Mn-based perovskites suitable for future chip-based luminescent color conversion materials. Therefore, the development of a Mn-based perovskite luminescent body glue is crucial to the development of non-toxic perovskite materials for chip surface packaging and application. Summary of the invention

[0005] The purpose of the present invention is to provide a preparation method of a Mn-based perovskite luminescent glue and its application. The method aims to develop a Mn-based perovskite luminescent glue to develop non-toxic perovskite materials for packaging and application on chip surfaces.

[0006] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing a Mn-based perovskite luminescent glue, comprising the following steps:

[0007] The Mn-based perovskite precursor is dissolved in solvent A and stirred until completely dissolved to obtain a precursor solution; then the precursor solution and the light diffuser are added to the glue respectively and mixed, and heated under vacuum stirring to remove the solvent A, thereby in-situ preparing the Mn-based perovskite luminescent body in the glue;

[0008] The solvent A and the glue are insoluble in each other;

[0009] The Mn-based perovskite precursor consists of organic halide and manganese halide.

[0010] Further, the organic halide comprises one or a combination of tetraethylammonium halide, N-butyl-N-methylpiperidinium halide, 1-ethyl-2,3-dimethylimidazolium halide, and 1,2-dimethyl-3-ethylimidazolium halide;

[0011] In the above, the halogenation includes bromine, chlorine, iodine and combinations thereof.

[0012] Furthermore, the manganese halide comprises one or a combination of manganese bromide, manganese iodide and manganese chloride.

[0013] Furthermore, the solvent A includes one of water, ethanol, and N,N-dimethylformamide or a combination thereof.

[0014] Furthermore, the glue includes one or a combination of epoxy resin, organic silicone, and UV glue.

[0015] Furthermore, the light diffuser is one of nano silicon oxide, nano aluminum oxide, nano titanium oxide or a combination thereof; the particle size of the light diffuser is in the range of 30-1000 nm.

[0016] Furthermore, the molar ratio of the organic halide to the manganese halide is in the range of 0.1-5.

[0017] Furthermore, the molar ratio of the light diffuser to the manganese halide is in the range of 1:(1-10).

[0018] Furthermore, the volume ratio of the solvent A to the glue is 1:(1-20); the precursor solution is added to the glue by dropwise addition; and the heating and stirring temperature range is 30-80°C.

[0019] An application of a Mn-based perovskite luminescent glue, wherein the Mn-based luminescent glue can be directly cured on the surface of an LED chip to form a light conversion coating, thereby realizing LED light conversion applications;

[0020] or,

[0021] The Mn-based luminescent body glue is coated on the surface of the base film and heated and cured to form a light conversion film;

[0022] The Mn-based luminescent body glue is prepared by the above-mentioned preparation method.

[0023] The beneficial effects of the present invention are mainly reflected in:

[0024] 1. The Mn-based perovskite luminescent body of the present invention does not contain heavy metal elements such as lead and cadmium and is environmentally friendly.

[0025] 2. The present invention prepares an organic-inorganic hybrid Mn luminophore in situ in glue, which is beneficial to improving the antioxidant and water resistance of the luminophore. The in-situ preparation process in the glue is as follows: a Mn-based perovskite precursor is dissolved in solvent A to form a precursor solution, because solvent A and glue are immiscible. Therefore, when the precursor solution is added to the glue, the precursor solution will be dispersed in the glue to form droplets. At this time, while heating and removing solvent A under vacuum stirring, the Mn-based perovskite precursor will also prepare a Mn-based perovskite luminophore in situ in the glue. The Mn-based perovskite luminophore prepared in situ in the glue can be coated with glue to block water and oxygen after the preparation is completed, thereby improving the antioxidant and water resistance of the luminophore.

[0026] 3. The surface of the Mn-based perovskite luminescent body prepared by the present invention is embedded with a plurality of light diffusing agents to form a light-emitting composite structure, thereby improving the light diffusion effect of the Mn-based perovskite luminescent body and the light efficiency of the glue. At the same time, the Mn-based luminescent body glue of the present invention can be directly applied to the light conversion coating and light conversion film on the chip surface. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a scanning electron microscope image of the sample of Example 2 of the present invention;

[0028] Figure 2 The LED emission spectrum of the synthetic sample of Example 2 of the present invention;

[0029] Figure 3 PL spectra of the samples synthesized in various embodiments of the present invention;

[0030] Figure 4 PL spectra of the samples synthesized in Example 2 of the present invention and the samples synthesized in Comparative Example 2;

[0031] Figure 5 This is a picture of the synthetic sample of Example 2 of the present invention used to make a light conversion film. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific implementation methods described herein are only used to explain the present invention and are not used to limit the present invention.

[0033] Embodiment 1:

[0034] Step 1: Dissolve 512 mg of tetraethylammonium iodide and 572 mg of MnBr2·4H2O in 4 mL of water and stir until fully dissolved to obtain a clear and transparent solution (precursor solution).

[0035] Step 2: Pipette 0.4 mL of the precursor solution obtained in step 1 and drop it into 8 mL of organic silica gel; then add 120 mg of nano-silica gel, heat and stir at 80°C for 3 hours under negative pressure, so as to prepare the Mn-based perovskite luminescent body in situ in the glue.

[0036] Embodiment 2:

[0037] Step 1: Dissolve 1.024 g of tetraethylammonium iodide and 572 mg of MnBr2·4H2O in 4 mL of water and stir until fully dissolved to obtain a clear and transparent solution (precursor solution).

[0038] Step 2: Pipette 0.4 mL of the precursor solution obtained in step 1 and drop it into 8 mL of organic silica gel; then add 120 mg of nano-silica gel, heat and stir at 80°C for 3 hours under negative pressure, so as to prepare the Mn-based perovskite luminescent body in situ in the glue.

[0039] Experimental analysis: Figure 1 The figure shows the scanning electron microscope test image of the sample in Example 2. Figure 1 It can be seen that nano-silicon oxide is embedded on the surface of the Mn-based perovskite luminescent body to form a luminescent composite structure, thereby improving the light diffusion effect of the Mn-based perovskite luminescent body.

[0040] like Figure 2 As shown, the sample of Example 2 is drop-coated on an LED lamp bead and heated and cured in situ to form a light conversion coating, thereby realizing an LED emission spectrum formed by an LED light conversion application.

[0041] Embodiment 3:

[0042] Step 1: Dissolve 512 mg of tetraethylammonium iodide and 1.144 g of MnBr2·4H2O in 4 mL of water and stir until fully dissolved to obtain a clear and transparent solution (precursor solution).

[0043] Step 2: Pipette 0.4 mL of the precursor solution obtained in step 1 and drop it into 8 mL of organic silica gel; then add 120 mg of nano-silica gel, heat and stir at 80°C for 3 hours under negative pressure, so as to prepare the Mn-based perovskite luminescent body in situ in the glue.

[0044] Embodiment 4:

[0045] Step 1: Dissolve 512 mg of tetraethylammonium iodide and 572 mg of MnBr2·4H2O in 3 mL of water and stir until fully dissolved to obtain a clear and transparent solution (precursor solution).

[0046] Step 2: Pipette 0.4 mL of the precursor solution obtained in step 1 and drop it into 8 mL of organic silica gel; then add 120 mg of nano-silica gel, heat and stir at 80°C for 3 hours under negative pressure, so as to prepare the Mn-based perovskite luminescent body in situ in the glue.

[0047] Embodiment 5:

[0048] Step 1: Dissolve 512 mg of tetraethylammonium iodide and 572 mg of MnBr2·4H2O in 5 mL of water and stir until fully dissolved to obtain a clear and transparent solution (precursor solution).

[0049] Step 2: Pipette 0.4 mL of the precursor solution obtained in step 1 and drop it into 8 mL of organic silica gel; then add 120 mg of nano-silica gel, heat and stir at 80°C for 3 hours under negative pressure, so as to prepare the Mn-based perovskite luminescent body in situ in the glue.

[0050] Comparative Example 1:

[0051] The difference from Example 3 is that there is no glue.

[0052] Step 1: Dissolve 512 mg of tetraethylammonium iodide and 1.144 g of MnBr2·4H2O in 4 mL of water and stir until fully dissolved to obtain a clear and transparent solution (precursor solution).

[0053] Step 2: Anneal the precursor solution obtained in step 1 at 80° C. to prepare a Mn-based perovskite light emitter.

[0054] Experimental analysis: The product obtained in comparative example 1, the sample obtained by direct annealing without adding glue, glows in the air, but is easily deliquescent. After a few minutes, the luminescence weakens until it stops glowing.

[0055] Comparative Example 2:

[0056] Step 1: Dissolve 1.024 g of tetraethylammonium iodide and 572 mg of MnBr2·4H2O in 4 mL of water and stir until fully dissolved to obtain a clear and transparent solution (precursor solution).

[0057] Step 2: Pipette 0.4 mL of the precursor solution obtained in step 1 and add it to 8 mL of organic silica gel; heat and stir at 80° C. for 3 h under negative pressure to prepare a Mn-based perovskite luminescent body in situ in the glue.

[0058] The final products were prepared from the above examples. The emission wavelengths of the products under 450nm blue laser are shown in Table 1.

[0059] Table 1: Emission wavelengths of samples from different embodiments

[0060] Example Emission wavelength Example 1 532nm Example 2 533nm Example 3 532nm Example 4 532nm Example 5 534nm Comparative Example 2 533nm

[0061] Application examples:

[0062] The Mn-based luminescent glue prepared in Example 2 is coated on the surface of the base film and heated and cured to form a light conversion film. Figure 5 As shown, the film surface is smooth and the color is uniform, showing a uniform green color.

[0063] The present invention illustrates the detailed preparation method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed preparation method, that is, it does not mean that the present invention must rely on the above-mentioned products and detailed preparation methods to be implemented. It should be clear to those skilled in the art that any improvement of the present invention, the combination or equivalent replacement of the raw materials of the product of the present invention, all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a Mn-based perovskite luminescent body glue, characterized in that: The steps include: The Mn-based perovskite precursor is dissolved in solvent A and stirred until completely dissolved to obtain a precursor solution; then the precursor solution and the light diffuser are added to the glue respectively and mixed, and heated under vacuum stirring to remove the solvent A, thereby in-situ preparing the Mn-based perovskite luminescent body in the glue; The solvent A and the glue are insoluble in each other; The Mn-based perovskite precursor consists of organic halide and manganese halide.

2. The method for preparing a Mn-based perovskite luminescent body glue according to claim 1, characterized in that: The organic halide comprises one of tetraethylammonium halide, N-butyl-N-methylpiperidinium halide, 1-ethyl-2,3-dimethylimidazolium halide, 1,2-dimethyl-3-ethylimidazolium halide or a combination thereof; In the above, the halogenation includes bromine, chlorine, iodine and combinations thereof.

3. The method for preparing a Mn-based perovskite luminescent body glue according to claim 1, characterized in that: The manganese halide includes one of manganese bromide, manganese iodide, and manganese chloride, or a combination thereof.

4. The method for preparing a Mn-based perovskite luminescent body glue according to claim 1, characterized in that: The solvent A includes one of water, ethanol, and N,N-dimethylformamide or a combination thereof.

5. The method for preparing a Mn-based perovskite luminescent body glue according to claim 1, characterized in that: The glue includes one of epoxy resin, organic silica gel, UV glue or a combination thereof.

6. The method for preparing a Mn-based perovskite luminescent body glue according to claim 1, characterized in that: The light diffuser is one of nano silicon oxide, nano aluminum oxide, nano titanium oxide or a combination thereof; the particle size of the light diffuser is in the range of 30-1000 nm.

7. The method for preparing a Mn-based perovskite luminescent glue according to claim 1, characterized in that: The molar ratio of the organic halide to the manganese halide is in the range of 0.1-5.

8. The method for preparing a Mn-based perovskite luminescent body glue according to claim 1, characterized in that: The molar ratio of the light diffuser to the manganese halide is in the range of 1:(1-10).

9. The method for preparing a Mn-based perovskite luminescent body glue according to claim 1, characterized in that: The volume ratio of the solvent A to the glue is 1:(1-20); the heating and stirring temperature range is 30-80°C.

10. An application of a Mn-based perovskite luminescent glue, characterized in that: The Mn-based luminophore glue can be directly cured on the surface of the LED chip to form a light conversion coating to achieve LED light conversion applications; or, The Mn-based luminescent body glue is coated on the surface of the base film and heated and cured to form a light conversion film; The Mn-based luminophore glue is prepared using the preparation method described in claims 1-9.

Citation Information

Cited By