Photosensitive resin composition, photosensitive dry film and pattern forming method

By combining polymers containing silicon phenylene and polyether structures with photoacid generators, a photosensitive resin composition with cross-linked groups is formed, which solves the problem of peeling and cracking of the coating during thermal cycle tests. Achieves reliable adhesion and chemical resistance to substrates and electronic components, and is suitable for protective films and resist materials.

CN110501876BActive Publication Date: 2024-10-11SHIN ETSU CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201910405085.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-05-17
Filing Date
2019-05-16
Publication Date
2024-10-11
Estimated Expiration
2039-05-16

AI Technical Summary

Technical Problem

The cured coating of existing photosensitive silicone compositions is prone to peeling or cracking during thermal cycle tests, making it difficult to meet the requirements for reliable adhesion to the substrate and chemical resistance.

Method used

A polymer containing silicon phenylene and polyether structure is combined with a photoacid generator to form a photosensitive resin composition with cross-linking groups, and is prepared by combining a cross-linking agent, a solvent and a quencher. A photosensitive resin coating with improved film properties was developed.

Benefits of technology

Achieves improved adhesion, patterning ability and cracking resistance to substrates, electronic components and semiconductor devices, and is used as a reliable insulating protective film and resist material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002060965140000021
    Figure BDA0002060965140000021
  • Figure BDA0002060965140000031
    Figure BDA0002060965140000031
  • Figure BDA0002060965140000032
    Figure BDA0002060965140000032
Patent Text Reader

Abstract

The present invention is a photosensitive resin composition, a photosensitive dry film and a pattern forming method. A photosensitive resin composition comprising (A) a polymer containing a silicon phenylene group and a polyether structure and (B) a photoacid generator is applied to a substrate to form a photosensitive resin coating having improved adhesion to the substrate, pattern forming ability, crack resistance and reliability as a protective film.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This nonprovisional application claims priority under 35 U.S.C. 119(a) to Patent Application No. 2018-095370 filed in Japan on May 17, 2018, the entire contents of which are incorporated herein by reference. Technical Field

[0003] The invention relates to a photosensitive resin composition, a photosensitive dry film and a pattern forming method. Background Art

[0004] In the prior art, photosensitive protective films for semiconductor devices and photosensitive insulating films for multilayer printed circuit boards are formed from photosensitive polyimide compositions, photosensitive epoxy resin compositions, photosensitive silicone compositions, etc. As a photosensitive material applied to protect such substrates and circuits, a photosensitive silicone composition is disclosed in Patent Document 1. The photosensitive silicone composition can be cured at a low temperature and forms a coating that is completely reliable in terms of wet adhesion resistance and other properties, but is less resistant to chemicals such as photoresist strippers having a high solvent power, typically N-methyl-2-pyrrolidone (NMP).

[0005] In order to overcome this problem, Patent Document 2 proposes a photosensitive silicone composition based on a silicone polymer containing a silicon phenylene structure. This composition is improved in chemical resistance to photoresist strippers and the like, but still has a problem in which the cured coating peels off or cracks from the substrate in a thermal cycle test (a test of holding at -25°C for 10 minutes and at 125°C for 10 minutes repeated for 1,000 cycles). Further improvement in reliability is required.

[0006] Reference List

[0007] Patent Document 1: JP-A 2002-088158 (USP 6,590,010, EP 1186624)

[0008] Patent Document 2: JP-A 2008-184571 (USP 7,785,766, EP 1953183) Summary of the invention

[0009] An object of the present invention is to provide a photosensitive resin composition and a photosensitive dry film which produce a cured resin coating or resin layer, the cured resin coating or resin layer being capable of being processed into a thick film form defining a fine-sized pattern, having improved film properties including crack resistance and adhesion to a substrate for use in electronic components and semiconductor devices and a support for use in a circuit board, and thus being reliable as a protective film for electrical and electronic components. Another object is to provide a pattern forming method using the foregoing products.

[0010] The inventors have found that a polymer having a silicophenylene and polyether structure having a crosslinkable group or a reaction site sensitive to a crosslinking reaction in the molecule functions to provide sufficient film-forming ability; a composition containing the polymer is used to form a photosensitive resin coating having a wide range of thicknesses; and the photosensitive resin coating has improved adhesion to a substrate, electronic components, and semiconductor devices, pattern forming ability, crack resistance, electrical insulation, and reliability as an insulating protective film, and thus can be used as a protective film for electrical and electronic components and a resist material for plating.

[0011] In one aspect, the present invention provides a photosensitive resin composition comprising (A) a polymer having a silicophenylene and polyether structure containing repeating units of the following formulas (1) to (4), and (B) a photoacid generator.

[0012]

[0013] wherein X 1 is a divalent group having the following formula (X1), X 2 is a divalent group having the following formula (X2), X 3 is a divalent group having the following formula (X3), X 4 is a divalent group having the following formula (X4), and p, q, r, and s are numbers in the following ranges: 0 < p < 1, 0 ≤ q < 1, 0 ≤ r < 1, 0 ≤ s < 1, 0 < q + r + s < 1 and p + q + r + s = 1.

[0014]

[0015] wherein R 1 and R 2 are each independently hydrogen or a C1-C8 monovalent hydrocarbon group, R 3 and R 4 are each independently hydrogen or methyl, a 1 and a 2 are each independently an integer from 1 to 6, and n is an integer from 0 to 100.

[0016]

[0017] wherein Y1 is a single bond, a methylene group, a propane-2,2-diyl group, a 1,1,1,3,3,3-hexafluoropropane-2,2-diyl group or a fluorene-9,9-diyl group, R 11 and R 12 are each independently hydrogen or methyl, R 13 and R 14 Each independently is a C1-C4 alkyl or alkoxy group, b 1 and b 2 are each independently an integer from 0 to 7, and c 1 and c 2 Each independently represents an integer from 0 to 2.

[0018]

[0019] where Y 2 is a single bond, a methylene group, a propane-2,2-diyl group, a 1,1,1,3,3,3-hexafluoropropane-2,2-diyl group or a fluorene-9,9-diyl group, R 21 and R 22 are each independently hydrogen or methyl, R 23 and R 24 Each independently is a C1-C4 alkyl or alkoxy group, d 1 and d 2 are each independently an integer from 0 to 7, and e 1 and e 2 Each independently represents an integer from 0 to 2.

[0020]

[0021] Where R 31 and R 32 are each independently hydrogen or methyl, and f 1 and f 2 Each independently represents an integer from 0 to 7.

[0022] The photosensitive resin composition may further include (C) a crosslinking agent, (D) a solvent and / or (E) a quencher. The crosslinking agent is typically at least one compound selected from the group consisting of an amino condensate modified with formaldehyde or formaldehyde-alcohol, a phenol compound having an average of at least two hydroxymethyl or alkoxymethyl groups in the molecule, and an epoxy compound having an average of at least two epoxy groups in the molecule.

[0023] Typically, the photosensitive resin composition is to be formed into a coating for protecting electric and electronic parts, or used as a resist material in a step of forming copper interconnects by plating.

[0024] In another aspect, the present invention provides a photosensitive resin coating obtained from the photosensitive resin composition defined above.

[0025] In another aspect, the present invention provides a photosensitive dry film comprising a support and a photosensitive resin coating thereon.

[0026] In yet another aspect, the present invention provides a pattern forming method comprising the steps of: (i) applying the photosensitive resin composition defined above onto a substrate to form a photosensitive resin coating thereon, (ii) exposing the photosensitive resin coating to radiation to define exposed areas and unexposed areas, and (iii) developing the exposed resin coating with a developer to dissolve away the unexposed areas of the resin coating and form a pattern of the resin coating.

[0027] In a further aspect, the present invention provides a pattern forming method comprising the steps of: (i') using the photosensitive dry film defined above to form a photosensitive resin coating on a substrate, (ii) exposing the photosensitive resin coating to radiation to define exposed areas and unexposed areas, and (iii) developing the exposed resin coating with a developer to dissolve away the unexposed areas of the resin coating and form a pattern of the resin coating.

[0028] In any embodiment, the pattern forming method may further include the step of (iv) post-curing the patterned resin coating resulting from the developing step (iii) at a temperature of 100 to 250°C.

[0029] Beneficial effects of the present invention

[0030] The photosensitive resin composition and the photosensitive dry film have many advantages of photosensitive materials and can be easily processed in thick film form to define fine-sized patterns. The cured resin coating obtained from the photosensitive resin composition has improved film properties, including chemical resistance to photoresist strippers and plating baths, adhesion to substrates, electronic components, semiconductor devices, and circuit board supports, mechanical properties, and electrical insulation, and is therefore completely reliable as an insulating protective film. The cured resin coating also has crack resistance and can therefore be used as a forming material for protective films of electrical and electronic components (such as circuit boards, semiconductor devices, and display units) and a resist material for plating. DETAILED DESCRIPTION

[0031] As used herein, the notation (Cn-Cm) means a group containing n to m carbon atoms per group.

[0032] Photosensitive resin composition

[0033] One embodiment of the present invention is a photosensitive resin composition including (A) a polymer containing a silicon phenylene group and a polyether structure and (B) a photoacid generator.

[0034] (A) Polymers containing silicon phenylene and polyether structures

[0035] Component (A) is a polymer containing a silylphenylene structure and a polyether structure, and in particular, contains repeating units having the following formulae (1) to (4). For simplicity, the polymer is referred to as polymer A and the repeating units having the formulae (1) to (4) are referred to as repeating units (1) to (4), respectively. Polymer A has a crosslinking group such as an epoxy group and a hydroxyl group or a reactive site susceptible to a crosslinking reaction in the molecule.

[0036]

[0037] In formula (1), X 1 is a divalent group having the formula (X1).

[0038]

[0039] In formula (X1), R 1 and R 2 Each independently represents hydrogen or a C1-C8 monovalent hydrocarbon group, R 3 and R 4 are each independently hydrogen or methyl, a 1 and a 2 Each is independently an integer of 1 to 6, preferably an integer of 1 to 4, and more preferably an integer of 1 or 2, and n is an integer of 0 to 100, preferably an integer of 1 to 50, and more preferably an integer of 5 to 30.

[0040] The C1-C8 monovalent hydrocarbon group may be linear, branched or cyclic and includes, for example, monovalent aliphatic hydrocarbon groups such as C1-C8 alkyl groups and C2-C8 alkenyl groups and monovalent aromatic hydrocarbon groups such as C6-C8 aryl groups and C7 or C8 aralkyl groups.

[0041] Examples of C1-C8 alkyl groups include methyl, ethyl, n-propyl, isopropyl, cyclopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, cyclobutyl, n-pentyl, cyclopentyl, n-hexyl, cyclohexyl, n-heptyl and n-octyl. Examples of alkenyl groups include vinyl, propenyl, butenyl and pentenyl. Examples of aryl groups include phenyl, 2-methylphenyl, 3-methylphenyl, 4-methylphenyl, 2-ethylphenyl, 3-ethylphenyl, 4-ethylphenyl and dimethylphenyl. Examples of aralkyl groups include benzyl and phenethyl.

[0042] R 1 and R 2 Preferred is hydrogen or C1-C8 alkyl, more preferably hydrogen or methyl.

[0043] In formula (X1), the oxyalkylene units having the subscript n may be arranged randomly or alternately, or may be a plurality of blocks including the same oxyalkylene units.

[0044] In formula (2), X 2 is a divalent group having the formula (X2).

[0045]

[0046] In formula (X2), Y 1 is a single bond, a methylene group, a propane-2,2-diyl group, a 1,1,1,3,3,3-hexafluoropropane-2,2-diyl group or a fluorene-9,9-diyl group, R 11 and R 12 are each independently hydrogen or methyl, R 13 and R 14 Each independently is a C1-C4 alkyl or alkoxy group, b 1 and b 2 are each independently an integer from 0 to 7, and c 1 and c 2 Each independently represents an integer from 0 to 2.

[0047] The C1-C4 alkyl group may be linear, branched or cyclic, and examples thereof include methyl, ethyl, n-propyl, isopropyl, cyclopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl and cyclobutyl. The C1-C4 alkoxy group may be linear, branched or cyclic, and examples thereof include methoxy, ethoxy, n-propoxy, isopropoxy, cyclopropyloxy, n-butoxy, isobutoxy, sec-butoxy, tert-butoxy and cyclobutyloxy.

[0048] In formula (3), X 3 is a divalent group having the formula (X3).

[0049]

[0050] In formula (X3), Y 2 is a single bond, a methylene group, a propane-2,2-diyl group, a 1,1,1,3,3,3-hexafluoropropane-2,2-diyl group or a fluorene-9,9-diyl group, R 21 and R 22 are each independently hydrogen or methyl, R 23 and R 24 Each independently is a C1-C4 alkyl or alkoxy group, d 1 and d 2 are each independently an integer from 0 to 7, and e 1 and e 2An integer that is independently 0, 1, or 2 for each. Examples of C1-C4 alkyl or alkoxy are exemplified in the description of formula (X2).

[0051] In formula (4), X 4 is a divalent group having formula (X4).

[0052]

[0053] In formula (X4), R 31 and R 32 are each independently hydrogen or methyl, and f 1 and f 2 are each independently an integer from 0 to 7.

[0054] In formulas (1) to (4), p, q, r, and s respectively represent the contents (molar fractions) of the repeating units (1), (2), (3), and (4) in polymer A, and are numbers within the following ranges: 0 < p < 1, 0 ≤ q < 1, 0 ≤ r < 1, 0 ≤ s < 1, 0 < q + r + s < 1, and p + q + r + s = 1. For film-forming or processing considerations, p, q, r, and s are preferably numbers within the following ranges: 0.1 ≤ p ≤ 0.9, 0 ≤ q ≤ 0.9, 0 ≤ r ≤ 0.9, 0 ≤ s ≤ 0.9, and 0.1 ≤ q + r + s ≤ 0.9, more preferably 0.2 ≤ p ≤ 0.8, 0 ≤ q ≤ 0.8, 0 ≤ r ≤ 0.8, 0 ≤ s ≤ 0.8, and 0.2 ≤ q + r + s ≤ 0.8, provided that p + q + r + s = 1. The repeating units (1) to (4) can be arranged randomly or in blocks.

[0055] Polymer A preferably has a weight-average molecular weight (Mw) of 3,000 to 500,000, more preferably 5,000 to 200,000. Polymers having an Mw within the said range are completely soluble in the most common organic solvents. It should be noted throughout this disclosure that Mw is measured by gel permeation chromatography (GPC) using tetrahydrofuran as the eluent relative to polystyrene standards.

[0056] Polymer A can be composed of randomly or alternately arranged repeating units (1) to (4) or multiple blocks each composed of the same type of units.

[0057] Polymer A imparts sufficient film-forming function in the photosensitive resin composition. The photosensitive resin coating obtained from the composition containing polymer A has improved adhesiveness, pattern-forming ability, and crack resistance to substrates, electronic components, semiconductor devices, etc.

[0058] Preparation of Polymer A

[0059] Polymer A can be prepared by addition polymerization of a compound having formula (5), a compound having formula (X1') and at least one compound selected from a compound having formula (X2'), a compound having formula (X3') and a compound having formula (X4') in the presence of a metal catalyst as shown below.

[0060]

[0061] where Y 1 , Y 2 , R 1 To R 4 , R 11 To R 14 , R 21 To R 24 , R 31 , R 32 、a 1 、a 2 , b 1 , b 2 、c 1 、c 2 ,d 1 ,d 2 、e 1 、e 2 、f 1 、f 2 and n are as defined above.

[0062] Examples of the metal catalyst used herein include individual platinum group metals such as platinum (including platinum black), rhodium and palladium; platinum chlorides, chloroplatinic acid and chloroplatinates such as H2PtCl4·xH2O, H2PtCl6·xH2O, NaHPtCl6·xH2O, KHPtCl6·xH2O, Na2PtCl6·xH2O, K2PtCl4·xH2O, PtCl4·xH2O, PtCl2 and Na2HPtCl4·xH2O, wherein x is preferably an integer from 0 to 6, more preferably 0 or 6; alcohol-modified chloroplatinic acid as described in USP 3,220,972; as described in USP 3,159,601, USP 3,159,662 and USP 3,775,452; supported catalysts containing platinum group metals, such as palladium and platinum black on supports of alumina, silica and carbon; rhodium-olefin complexes; chlorotris(triphenylphosphine)rhodium (known as Wilkinson's catalyst); and complexes of platinum chloride, chloroplatinic acid and chloroplatinates with vinyl-containing siloxanes, particularly vinyl-containing cyclic siloxanes.

[0063] The catalyst is used in a catalytic amount, and the amount is preferably 0.001 to 0.1% by weight of a platinum group metal, based on the total weight of the reactants used for the polymerization reaction. In the polymerization reaction, a solvent can be used if necessary. Suitable solvents are hydrocarbon solvents, such as toluene and xylene. Regarding polymerization conditions, the polymerization temperature is preferably selected in the range of 40 to 150° C., more preferably 60 to 120° C., so that the catalyst can not be deactivated and the polymerization is completed in a short time. Although the polymerization time varies with the type and amount of the monomer, the polymerization reaction is preferably completed in about 0.5 to about 100 hours, more preferably about 0.5 to about 30 hours, to prevent moisture from entering the polymerization system. After the completion of the polymerization reaction, if there is a solvent, it is distilled off to obtain polymer A.

[0064] The reaction process is not particularly limited. A preferred process is to first mix a compound having formula (X1') with one or more compounds selected from a compound having formula (X2'), a compound having formula (X3') and a compound having formula (X4'), heat the mixture, add a metal catalyst to the mixture, and then dropwise add a compound having formula (5) over 0.1 to 5 hours.

[0065] The reactants are preferably combined in such amounts that the molar ratio of the hydrosilyl groups on the compound having formula (5) to the sum of the alkenyl groups on the compounds having formulae (X1'), (X2'), (X3') and (X4') may be in the range of 0.67 / 1 to 1.67 / 1, more preferably 0.83 / 1 to 1.25 / 1. The Mw of polymer A may be controlled using a molecular weight control agent such as a monoallyl compound (e.g., o-allylphenol), a monohydrogen silane (e.g., triethylhydrogen silane) or a monohydrogen siloxane.

[0066] (B) Photoacid generator

[0067] The photoacid generator (PAG) as component (B) is typically a compound that decomposes and produces acid when exposed to light with a wavelength of 190 to 500nm, and the acid produced serves as a curing catalyst. Because the photosensitive resin composition of the present invention is highly compatible with PAG, PAG can be selected from a variety of such compounds. Typical PAGs include onium salts, diazomethane derivatives, oxadioxime derivatives, β-ketosulfone derivatives, disulfone derivatives, nitrobenzyl sulfonate derivatives, sulfonate derivatives, imidosulfonate derivatives, sulfonic acid oxime ester derivatives, imidosulfonate derivatives and triazine derivatives.

[0068] From the viewpoint of photocuring, PAG (B) is preferably used in an amount of 0.05 to 20 parts by weight, and more preferably 0.05 to 5 parts by weight per 100 parts by weight of component (A). When the amount of PAG is at least 0.05 parts, it can generate a sufficient amount of acid for carrying out a crosslinking reaction. As long as the amount of PAG is at most 20 parts, any increase in light absorption due to the PAG itself is prevented and a decrease in transparency is avoided. PAG can be used alone or in combination of two or more.

[0069] (C) Cross-linking agent

[0070] Preferably, the photosensitive resin composition further comprises (C) a crosslinking agent. The function of the crosslinking agent is to promote pattern formation and increase the strength of the cured composition.

[0071] Preferably, the crosslinking agent is selected from amino condensates modified with formaldehyde or formaldehyde-alcohol, nitrogen-containing compounds such as melamine, guanamine, glycoluril and urea compounds having an average of at least two hydroxymethyl and / or alkoxymethyl groups in the molecule, phenol compounds having an average of at least two hydroxymethyl or alkoxymethyl groups in the molecule, and epoxy compounds having an average of at least two epoxy groups in the molecule. These compounds can be used alone or in combination.

[0072] Examples of the amino condensate modified with formaldehyde or formaldehyde-alcohol include melamine condensate modified with formaldehyde or formaldehyde-alcohol, and urea condensate modified with formaldehyde or formaldehyde-alcohol.

[0073] Suitable melamine compounds include hexamethylolmelamine, hexamethoxymethylmelamine, trimethoxymethylmonomethylolmelamine, dimethoxymethylmonomethylolmelamine, trimethylolmelamine and hexamethoxyethylmelamine. Suitable guanamine compounds include tetramethylolguanamine, tetramethoxymethylguanamine and tetramethoxyethylguanamine.

[0074] Suitable glycoluril compounds include tetramethylol glycoluril and tetramethoxymethyl glycoluril. Suitable urea compounds include tetramethylol urea, tetramethoxymethyl urea and tetramethoxyethyl urea.

[0075] Examples of the phenol compound having an average of at least two hydroxymethyl groups or alkoxymethyl groups in the molecule include (2-hydroxy-5-methyl)-1,3-benzenedimethanol and 2,2′,6,6′-tetramethoxymethylbisphenol A.

[0076] Examples of epoxy compounds having an average of at least two epoxy groups in the molecule include bisphenol epoxy resins such as bisphenol A epoxy resin and bisphenol F epoxy resin, novolac epoxy resins such as phenol novolac epoxy resin and cresol novolac epoxy resin, trisphenol alkane epoxy resin, biphenyl epoxy resin, dicyclopentadiene-modified phenol novolac epoxy resin, phenol aralkyl epoxy resin, biphenyl aralkyl epoxy resin, naphthalene ring-containing epoxy resin, glycidyl ester epoxy resin, alicyclic epoxy resin and heterocyclic epoxy resin.

[0077] The crosslinking agent (C) is preferably used in an amount of 0.5 to 50 parts by weight, and even more preferably 1 to 30 parts by weight per 100 parts by weight of component (A). At least 0.5 parts of component (C) ensures sufficient curing during exposure. As long as the amount of component (C) is at most 50 parts, the proportion of polymer A in the resin composition is not reduced, allowing the cured composition to fully exert its effect. The crosslinking agents can be used alone or in combination.

[0078] (D) Solvent

[0079] The photosensitive resin composition may further include a solvent as component (D). The solvent used herein is not particularly limited as long as the aforementioned components (A) to (C) and component (E) and additives to be described later are soluble.

[0080] Preferred are organic solvents in which the aforementioned components are completely dissolved. Illustrative, non-limiting examples of organic solvents include ketones such as cyclohexanone, cyclopentanone, and methyl-2-n-pentyl ketone; alcohols such as 3-methoxybutanol, 3-methyl-3-methoxybutanol, 1-methoxy-2-propanol, and 1-ethoxy-2-propanol; ethers such as propylene glycol monomethyl ether, ethylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, propylene glycol dimethyl ether, and diethylene glycol dimethyl ether; and esters such as propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monoethyl ether acetate, ethyl lactate, ethyl pyruvate, butyl acetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, tert-butyl acetate, tert-butyl propionate, propylene glycol monotert-butyl ether acetate, and γ-butyrolactone. These solvents can be used alone or in combination. Of these solvents, preferred are ethyl lactate, cyclohexanone, cyclopentanone, PGMEA, γ-butyrolactone and mixtures thereof, in which PAG is most soluble.

[0081] From the viewpoint of compatibility and viscosity of the resin composition, the amount of solvent (D) used is preferably 50 to 2,000 parts by weight, more preferably 50 to 1,000 parts by weight, and even more preferably 50 to 100 parts by weight per 100 parts by weight of components (A) and (B) combined.

[0082] (E) Quencher

[0083] The photosensitive resin composition may further contain a quencher as component (E). The quencher used herein is preferably a compound capable of inhibiting the diffusion rate when the acid generated by the PAG diffuses in the resin coating. The incorporation of the quencher improves resolution, inhibits changes in photosensitivity after exposure, reduces substrate and environmental dependence, and improves exposure margin and pattern profile.

[0084] Examples of the quencher include aliphatic primary, secondary and tertiary amines, mixed amines, aromatic amines, heterocyclic amines, nitrogen-containing compounds having a carboxyl group, nitrogen-containing compounds having a sulfonyl group, nitrogen-containing compounds having a hydroxyl group, nitrogen-containing compounds having a hydroxyphenyl group, alcoholic nitrogen-containing compounds, amide derivatives and imide derivatives.

[0085] From the viewpoint of photosensitivity, the amount of the quencher (E) is preferably 0 to 3 parts by weight, more preferably 0.01 to 1 part by weight, per 100 parts by weight of component (A).The quencher may be used alone or in admixture of two or more.

[0086] Other additives

[0087] In addition to the aforementioned components, the photosensitive resin composition may include optional additives. A typical additive is a surfactant generally used to improve coating properties.

[0088] Preferred surfactants are nonionic surfactants, such as fluorochemical surfactants, such as perfluoroalkyl polyoxyethylene ethanol, fluorinated alkyl esters, perfluoroalkyl amine oxides, and fluorinated organosiloxane compounds. These surfactants are commercially available. Illustrative examples include 3M's FC-430, from AGC SeimiChemical Co., Ltd. S-141 and S-145 from Daikin Industries Ltd. DS-401, DS-4031 and DS-451 from DIC Corp. F-8151, and X-70-093 from Shin-Etsu Chemical Co., Ltd. Preferred surfactants are Fluorad FC-430 and X-70-093.

[0089] The surfactant is preferably used in an amount of 0.01 to 5 parts by weight, more preferably 0.1 to 3 parts by weight, per 100 parts by weight of component (A). The surfactant may be used alone or in combination.

[0090] Another useful additive is a silane coupling agent, which is effective for further increasing the adhesion of the resin composition to the adherend. Suitable silane coupling agents include epoxy-containing silane coupling agents and aromatic-containing aminosilane coupling agents. The silane coupling agent can be used alone or in combination. Although the amount of the silane coupling agent used is not particularly limited, it is preferably 0.01 to 5 weight % of the resin composition.

[0091] The photosensitive resin composition of the present invention is prepared in any desired manner. For example, it can be prepared by stirring and mixing the aforementioned components and optionally passing the mixture through a filter to remove solids.

[0092] A resin coating layer having a wide range of thicknesses can be formed from the photosensitive resin composition. A pattern having fine feature size and verticality can be formed from the resin coating layer by a pattern forming method to be described below.

[0093] The photosensitive resin composition is advantageously used, for example, as a film-forming material for semiconductor device protection films, interconnect protection films, cover films, solder masks and TSV dielectric films, adhesives between substrates in three-dimensional laminates, and resist materials for plating.

[0094] Pattern forming method using photosensitive resin composition

[0095] Another embodiment of the present invention is a pattern forming method comprising the following steps:

[0096] (i) applying the photosensitive resin composition onto a substrate to form a photosensitive resin coating thereon,

[0097] (ii) exposing the photosensitive resin coating to radiation to define exposed areas and unexposed areas, and

[0098] (iii) The exposed resin coating is developed with a developer to dissolve away unexposed areas of the resin coating and form a pattern of the resin coating.

[0099] First, in step (i), a photosensitive resin composition is applied to a substrate to form a photosensitive resin coating thereon. Examples of the substrate include silicon wafers, TSV silicon wafers, silicon wafers thinned by backside polishing, plastic substrates, ceramic substrates, and substrates having a metal coating of Ni or Au completely or partially on the surface by ion sputtering or plating.

[0100] The coating technique may be any known technique, such as dip coating, spin coating, roller coating, etc. The coating weight may be appropriately selected for a particular purpose, preferably so as to form a photosensitive resin coating having a thickness of 1 to 400 μm, more preferably 5 to 200 μm.

[0101] The pre-wetting technique of dripping the solvent on the substrate before applying the resin composition can be used for the purpose of making the coating thickness on the substrate more uniform. The type and amount of the solvent to be dripped can be selected for a specific purpose. For example, alcohols such as isopropyl alcohol (IPA), ketones such as cyclohexanone and glycols such as propylene glycol monomethyl ether are preferred. Solvents used in photosensitive resin compositions can also be used.

[0102] At this time, if necessary, for efficient photocuring reaction, the coating material may be pre-baked to volatilize the solvent, etc. The pre-baking may be performed, for example, at 40 to 140° C. for 1 minute to about 1 hour.

[0103] Next in step (ii), the photosensitive resin coating is exposed to radiation to define exposed areas and unexposed areas. The exposure radiation generally has a wavelength of 1 to 600 nm, preferably 10 to 600 nm, more preferably 190 to 500 nm. Examples of radiation within the wavelength range include radiation of various wavelengths from a unit emitting radiation, particularly UV radiation, such as g-line, h-line or i-line and deep UV (248 nm, 193 nm). Among these, radiation of a wavelength of 248 to 436 nm is preferred. A suitable exposure dose is 10 to 10,000 mJ / cm 2 .

[0104] Exposure can be accomplished through a photomask. The photomask can be, for example, one that is perforated with a desired pattern. Although the material of the photomask is not particularly limited, it is preferably a material that can shield radiation within the above-mentioned wavelength range, typically chromium.

[0105] The next step may be post-exposure baking (PEB), which is effective for enhancing the developing sensitivity. PEB is preferably performed at 40 to 150° C. for 0.5 to 10 minutes. The exposed areas of the resin coating are cross-linked by PEB to form an insoluble pattern that is insoluble in a solvent as a developer.

[0106] Exposure or PEB is followed by a step (iii) of developing the exposed resin coating with a developer to dissolve away the unexposed areas of the resin coating and form a pattern of the resin coating. Preferred developers are organic solvents, including alcohols such as IPA, ketones such as cyclohexanone and glycols such as propylene glycol monomethyl ether. Solvents used in photosensitive resin compositions are also useful. Development is carried out in a conventional manner, for example by immersing the exposed coating in a developer. Development is followed by washing, rinsing and drying, if necessary, to obtain a resin coating having a desired pattern in this manner.

[0107] In step (iv), the patterned coating can be post-cured with an oven or hot plate at a temperature preferably of 100 to 250° C., more preferably 150 to 220° C. The photosensitive resin composition ensures that a resin coating with improved film properties is obtained from post-curing even at a relatively low temperature of about 200° C. Post-curing is effective for increasing the cross-linking density of the resin coating and removing any residual volatile substances. The resulting coating has increased adhesion to the substrate, heat resistance, mechanical strength, good electrical properties, bonding strength and reliability. Post-curing temperatures in the range of 100 to 250° C. are preferred for obtaining the above properties. The post-cured resin coating has a thickness of 1 to 400 μm, preferably 5 to 200 μm.

[0108] Although a patterning method has been described, sometimes it is not necessary to form a pattern. For example, when only a uniform film is desired, the same procedure as above can be followed, except that in step (ii), the resin coating is exposed directly, i.e. without a photomask, to radiation of a suitable wavelength.

[0109] Photosensitive dry film

[0110] Another embodiment of the present invention is a photosensitive dry film including a support and a photosensitive resin coating of a photosensitive resin composition thereon.

[0111] The photosensitive dry film (support + photosensitive resin coating) is solid, and the photosensitive resin coating does not contain solvent. This eliminates the risk of bubbles generated by the volatilization of the solvent remaining in the resin coating and between the resin coating and the uneven substrate surface. When considering the flatness and step coverage on the uneven substrate surface and the substrate lamination spacing, the resin coating has an appropriate thickness range. From the viewpoint of flatness, step coverage and substrate lamination spacing, it is preferred that the photosensitive resin coating has a thickness of 5 to 500 μm, more preferably 20 to 350 μm.

[0112] In addition, the viscosity and fluidity of the photosensitive resin coating are closely related. As long as the photosensitive resin coating has a viscosity in an appropriate range, it shows sufficient fluidity to fill deeply even in a narrow gap, or it softens to enhance adhesion to the substrate. Therefore, from the viewpoint of fluidity, the photosensitive resin coating should have a viscosity in the range of 10 to 5,000 Pa·s, more preferably 30 to 2,000 Pa·s, and even more preferably 50 to 300 Pa·s at a temperature of 80 to 120°C. It should be noted that the viscosity is measured by a rotational viscometer.

[0113] The photosensitive dry film has the advantage that when it is closely attached to a substrate having irregularities on its surface, a photosensitive resin coating is applied to follow the irregularities and achieve high flatness. In addition, if the photosensitive resin coating and the substrate are in close contact in a vacuum environment, the generation of a gap therebetween is effectively suppressed.

[0114] The photosensitive dry film can be manufactured by applying the photosensitive resin composition to a support and drying the resin composition to a resin coating. The equipment for manufacturing the photosensitive dry film can be a coating machine commonly used for manufacturing pressure-sensitive adhesive products. Suitable coating machines include, for example, notch wheel coaters, notch wheel reverse coaters, multi-purpose coaters (multiplecoater), die coaters, lip plate coaters, lip plate reverse coaters, gravure coaters, offset gravure coaters, three roll bottom reverse coaters (three roll bottom reverse coater) and four roll bottom reverse coaters (four rollbottom reverse coater).

[0115] The support (film) is unwound from the feed roller of the coating machine, conveyed through the head of the coating machine, where the photosensitive resin composition is applied to the support to a predetermined cumulative amount, and then moved through a hot air circulation oven at a predetermined temperature for a predetermined time, where the photosensitive resin coating is dried on the support. The support having the photosensitive resin coating thereon and the protective film unwound from another feed roller in the coating machine are then conveyed through a laminating roller at a predetermined pressure, thereby bonding the protective film to the photosensitive resin coating on the support, whereupon the laminate (photosensitive dry film with protective film) is wound on a pick-up shaft in the coating machine. Preferably, the oven temperature is 25 to 150° C., the conveying time is 1 to 100 minutes, and the bonding pressure is 0.01 to 5 MPa.

[0116] The support film used in the photosensitive dry film can be a single film or a multilayer film composed of multiple stacked polymer layers. Examples of film materials include synthetic resins such as polyethylene, polypropylene, polycarbonate and polyethylene terephthalate (PET), wherein PET films are preferred due to their suitable flexibility, mechanical strength and heat resistance. These films may have been pretreated, such as by corona treatment or coating with a release agent. Such films are commercially available, for example, from Toray Advanced Film Co., Ltd. WZ(RX) and BX8(R); E7302 and E7304 from Toyobo Co., Ltd.; G31 and G71T1; and PET38×1-A3, PET38×1-V8 and PET38×1-X08 from Nippa Co., Ltd.

[0117] The protective film used in the photosensitive dry film can be similar to the support film. In particular, PET and polyethylene films with appropriate flexibility are preferred. Such films are also commercially available. For example, PET films are as mentioned above, and polyethylene films include GF-8 from Tamapoly Co., Ltd. and O-type PE films from Nippa Co., Ltd.

[0118] Both the support and the protective film preferably have a thickness of 10 to 100 μm, more preferably 25 to 50 μm, in order to stably produce a photosensitive dry film and prevent winding and curling on a pickup roller.

[0119] Pattern forming method using photosensitive dry film

[0120] Another embodiment of the present invention is a pattern forming method comprising the following steps:

[0121] (i') using a photosensitive dry film to form a photosensitive resin coating on a substrate,

[0122] (ii) exposing the photosensitive resin coating to radiation to define exposed areas and unexposed areas,

[0123] (iii) The exposed resin coating is developed with a developer to dissolve away unexposed areas of the resin coating and form a pattern of the resin coating.

[0124] In step (i'), the photosensitive dry film is used to form a photosensitive resin coating on the substrate. Specifically, the photosensitive dry film is bonded to the substrate at its photosensitive resin coating to form a photosensitive resin coating on the substrate. When the photosensitive dry film is covered with a protective film, the dry film is bonded to the substrate at its photosensitive resin coating after the protective film is peeled off therefrom to form a photosensitive resin coating on the substrate. The dry film can be bonded using a film bonding device.

[0125] Examples of substrates include silicon wafers, TSV silicon wafers, silicon wafers that have been thinned by backside polishing, plastic substrates, ceramic substrates, and substrates having a metal coating of Ni or Au on the surface in whole or in part by ion sputtering or plating. Also useful are substrates having holes and / or grooves with an opening width of 10 to 100 μm and a depth of 10 to 120 μm.

[0126] The film laminating device is preferably a vacuum laminator. The photosensitive dry film is installed in the film laminating device, where the protective film is peeled off from the dry film. In a vacuum chamber maintained at a predetermined vacuum degree, on a workbench at a predetermined temperature, the exposed photosensitive resin coating of the dry film is tightly bonded to the substrate using a bonding roller under a predetermined pressure. Preferably, the temperature is 60 to 120°C, the pressure is 0 to 5.0MPa, and the vacuum degree is 50 to 500Pa.

[0127] If necessary, the lamination of the dry film may be repeated multiple times to obtain a photosensitive resin coating having a desired thickness. The lamination step is repeated 1 to 10 times, for example, then a photosensitive resin coating having a thickness of 10 to 1,000 μm, preferably 100 to 500 μm is obtained.

[0128] If necessary, the assembly of the photosensitive resin coating on the substrate may be prebaked to promote the photocuring reaction of the photosensitive resin coating or enhance the adhesion between the resin coating and the substrate. The prebaking may be performed, for example, at 40 to 140° C. for 1 minute to 1 hour.

[0129] As in the pattern forming method using a photosensitive resin composition, the photosensitive resin coating layer attached to the substrate can be subjected to the following steps: (ii) exposing the photosensitive resin coating layer to radiation, (iii) developing the exposed resin coating layer with a developer to dissolve away the unexposed areas of the resin coating layer and form a pattern of the resin coating layer, and optionally (iv) post-curing the patterned coating layer. It is to be noted that the support of the photosensitive dry film can be removed by mechanical stripping or the like before pre-baking or before PEB, depending on the specific process.

[0130] The resin coating obtained from the photosensitive resin composition or the photosensitive dry film has excellent properties, including flexibility, pattern forming ability, electrical insulation, reliability as a dielectric protective film, mechanical properties and substrate adhesion. The resin coating is therefore best suited as a protective film for electrical and electronic parts such as semiconductor devices and as a resist material for plating.

[0131] Example

[0132] Examples of the present invention are given below by way of illustration and not by way of limitation. The weight average molecular weight (Mw) was measured by gel permeation chromatography (GPC) relative to monodisperse polystyrene standards using a GPC column TSKgel Super HZM-H (Tosoh Corp.) under the following analytical conditions: flow rate 0.6 mL / min, tetrahydrofuran eluent and column temperature 40° C. All parts are by weight (pbw).

[0133] The compounds used in the synthesis of the polymers are shown below.

[0134]

[0135] [1] Synthesis of polymers

[0136] Example 1-1

[0137] Synthesis of Resin 1

[0138] Into a 3L flask equipped with a stirrer, a thermometer, a nitrogen purge line and a reflux condenser, 156.8g (0.40mol) of a compound having the formula (S-1), 53.9g (0.10mol) of a compound having the formula (S-3a) (UNIOX from NOF Corp.) and 2,000g of toluene were charged and heated at 70°C. Thereafter, 1.0g of a toluene solution of chloroplatinic acid (platinum concentration 0.5wt%) was added, and 97.0g (0.50mol) of a compound having the formula (S-5) was added dropwise over 1 hour. The ratio of the total number of moles of hydrosilyl groups to the total number of moles of alkenyl groups was 1 / 1. At the end of the addition, the reaction solution was heated and aged at 100°C for 6 hours. Toluene was distilled off from the reaction solution in a vacuum to produce resin 1. Resin 1 has an Mw of 43,000. Use 1 By H-NMR spectroscopy (Bruker Corp.), resin 1 was identified as a polymer containing repeating units (1) and (2).

[0139] Example 1-2

[0140] Synthesis of Resin 2

[0141] Into a 3L flask equipped with a stirrer, a thermometer, a nitrogen purge line and a reflux condenser, 172.0g (0.40mol) of a compound having the formula (S-7), 53.9g (0.10mol) of a compound having the formula (S-3a) and 2,000g of toluene were charged and heated at 70°C. Thereafter, 1.0g of a toluene solution of chloroplatinic acid (platinum concentration 0.5wt%) was added, and 97.0g (0.50mol) of a compound having the formula (S-5) was added dropwise over 1 hour. The ratio of the total number of moles of hydrosilyl groups to the total number of moles of alkenyl groups was 1 / 1. At the end of the addition, the reaction solution was heated and aged at 100°C for 6 hours. Toluene was distilled off from the reaction solution in a vacuum to produce resin 2. Resin 2 has an Mw of 25,000. Use 1 By H-NMR spectroscopy (Bruker Corp.), resin 2 was identified as a polymer containing repeating units (1) and (3).

[0142] Examples 1-3

[0143] Synthesis of Resin 3

[0144] Into a 3L flask equipped with a stirrer, a thermometer, a nitrogen purge line and a reflux condenser, 106.0g (0.40mol) of a compound having the formula (S-2), 53.9g (0.10mol) of a compound having the formula (S-3a) and 2,000g of toluene were charged and heated at 70°C. Thereafter, 1.0g of a toluene solution of chloroplatinic acid (platinum concentration 0.5wt%) was added, and 97.0g (0.50mol) of a compound having the formula (S-5) was added dropwise over 1 hour. The ratio of the total number of moles of hydrosilyl groups to the total number of moles of alkenyl groups was 1 / 1. At the end of the addition, the reaction solution was heated and aged at 100°C for 6 hours. Toluene was distilled off from the reaction solution in a vacuum to produce resin 3. Resin 3 has an Mw of 34,000. Use 1 By H-NMR spectroscopy (Bruker Corp.), resin 3 was identified as a polymer containing repeating units (1) and (4).

[0145] Examples 1-4

[0146] Synthesis of Resin 4

[0147] A 3L flask equipped with a stirrer, a thermometer, a nitrogen purge line and a reflux condenser was charged with 9.8 g (0.025 mol) of a compound having the formula (S-1), 10.8 g (0.025 mol) of a compound having the formula (S-7), 13.3 g (0.05 mol) of a compound having the formula (S-2) and 215.6 g (0.40 mol) of a compound having the formula (S-3a), and then charged with 2,000 g of toluene and heated at 70°C. 1.0 g of chloroplatinic acid toluene solution (platinum concentration 0.5 wt%) was then added, and 97.0 g (0.50 mol) of a compound having the formula (S-5) was added dropwise over 1 hour. The ratio of the total molar number of hydrosilyl groups to the total molar number of alkenyl groups was 1 / 1. At the end of the addition, the reaction solution was heated and aged at 100°C for 6 hours. Toluene was distilled off from the reaction solution in a vacuum to generate resin 4. Resin 4 has a Mw of 50,000. 1 By H-NMR spectroscopy (Bruker Corp.), resin 4 was identified as a polymer containing repeating units (1), (2), (3) and (4).

[0148] Examples 1-5

[0149] Synthesis of Resin 5

[0150] A 3L flask equipped with a stirrer, a thermometer, a nitrogen purge line and a reflux condenser was charged with 9.8 g (0.025 mol) of a compound having the formula (S-1), 10.8 g (0.025 mol) of a compound having the formula (S-7), 13.3 g (0.05 mol) of a compound having the formula (S-2) and 327.2 g (0.40 mol) of a compound having the formula (S-3b), and then charged with 2,000 g of toluene and heated at 70°C. 1.0 g of chloroplatinic acid toluene solution (platinum concentration 0.5 wt%) was then added, and 97.0 g (0.50 mol) of a compound having the formula (S-5) was added dropwise over 1 hour. The ratio of the total number of moles of hydrosilyl groups to the total number of moles of alkenyl groups was 1 / 1. At the end of the addition, the reaction solution was heated and aged at 100°C for 6 hours. Toluene was distilled off from the reaction solution in a vacuum to produce resin 5. Resin 5 has a Mw of 58,000. 1 By H-NMR spectroscopy (Bruker Corp.), resin 5 was identified as a polymer containing repeating units (1), (2), (3) and (4).

[0151] Comparative Example 1-1

[0152] Synthesis of Resin 6

[0153] A 3L flask equipped with a stirrer, a thermometer, a nitrogen purge line and a reflux condenser was charged with 196.0 g (0.50 mol) of a compound of formula (S-1), then charged with 2,000 g of toluene and heated at 70°C. 1.0 g of chloroplatinic acid toluene solution (platinum concentration 0.5 wt%) was then added, and 87.3 g (0.45 mol) of a compound of formula (S-5) and 79.3 g (0.05 mol) of a compound of formula (S-6) (wherein y=20) were added dropwise over 1 hour. The ratio of the total number of moles of hydrosilyl groups to the total number of moles of alkenyl groups was 1 / 1. At the end of the addition, the reaction solution was heated and aged at 100°C for 6 hours. Toluene was distilled off from the reaction solution in a vacuum to produce resin 6. Resin 6 had an Mw of 41,000.

[0154] Comparative Example 1-2

[0155] Synthesis of Resin 7

[0156] A 3L flask equipped with a stirrer, a thermometer, a nitrogen purge line and a reflux condenser was charged with 215.0 g (0.50 mol) of a compound of formula (S-7), then charged with 2,000 g of toluene and heated at 70°C. 1.0 g of chloroplatinic acid toluene solution (platinum concentration 0.5 wt%) was then added, and 48.5 g (0.25 mol) of a compound of formula (S-5) and 396.3 g (0.25 mol) of a compound of formula (S-6) (wherein y=20) were added dropwise over 1 hour. The ratio of the total molar number of hydrosilyl groups to the total molar number of alkenyl groups was 1 / 1. At the end of the addition, the reaction solution was heated and matured at 100°C for 6 hours. Toluene was distilled off from the reaction solution in a vacuum to produce resin 7. Resin 7 has an Mw of 31,000.

[0157] Comparative Examples 1-3

[0158] Synthesis of Resin 8

[0159] A 3L flask equipped with a stirrer, a thermometer, a nitrogen purge line and a reflux condenser was charged with 132.5 g (0.50 mol) of a compound of formula (S-2), then charged with 2,000 g of toluene and heated at 70°C. 1.0 g of chloroplatinic acid toluene solution (platinum concentration 0.5 wt%) was then added, and 77.6 g (0.40 mol) of a compound of formula (S-5) and 158.5 g (0.10 mol) of a compound of formula (S-6) (wherein y = 20) were added dropwise over 1 hour. The ratio of the total molar number of hydrosilyl groups to the total molar number of alkenyl groups was 1 / 1. At the end of the addition, the reaction solution was heated and matured at 100°C for 6 hours. Toluene was distilled off from the reaction solution in a vacuum to produce resin 8. Resin 8 has an Mw of 44,000.

[0160] Comparative Examples 1-4

[0161] Synthesis of Resin 9

[0162] A 3L flask equipped with a stirrer, a thermometer, a nitrogen purge line and a reflux condenser was charged with 9.8 g (0.025 mol) of a compound having the formula (S-1), 10.8 g (0.025 mol) of a compound having the formula (S-7), 13.3 g (0.05 mol) of a compound having the formula (S-2) and 74.4 g (0.40 mol) of a compound having the formula (S-4), and then charged with 2,000 g of toluene and heated at 70°C. 1.0 g of chloroplatinic acid toluene solution (platinum concentration 0.5 wt%) was then added, and 97.0 g (0.50 mol) of a compound having the formula (S-5) was added dropwise over 1 hour. The ratio of the total number of moles of hydrosilyl groups to the total number of moles of alkenyl groups was 1 / 1. At the end of the addition, the reaction solution was heated and aged at 100°C for 6 hours. Toluene was distilled off from the reaction solution in a vacuum to produce resin 9. Resin 9 had a Mw of 39,000.

[0163] Comparative Examples 1-5

[0164] Synthesis of Resin 10

[0165] A 3L flask equipped with a stirrer, a thermometer, a nitrogen purge line and a reflux condenser was charged with 78.4 g (0.20 mol) of a compound of formula (S-1), 43.0 g (0.10 mol) of a compound of formula (S-7) and 53.0 g (0.20 mol) of a compound of formula (S-2), and then charged with 2,000 g of toluene and heated at 70°C. 1.0 g of chloroplatinic acid toluene solution (platinum concentration 0.5 wt%) was then added, and 97.0 g (0.50 mol) of a compound of formula (S-5) was added dropwise over 1 hour. The ratio of the total number of moles of hydrosilyl groups to the total number of moles of alkenyl groups was 1 / 1. At the end of the addition, the reaction solution was heated and aged at 100°C for 6 hours. Toluene was distilled off from the reaction solution in a vacuum to produce resin 10. Resin 10 has an Mw of 29,000.

[0166] [2] Preparation and evaluation of photosensitive resin compositions

[0167] Examples 2-1 to 2-11 and Comparative Examples 2-1 to 2-10

[0168] The resins (resins 1 to 10), photoacid generators, crosslinking agents, solvents and quenchers were combined according to the formulations shown in Tables 1 and 2, stirred at room temperature until dissolved, and passed through a pore size of 1.0 μm. The obtained products were finely filtered to prepare photosensitive resin compositions of Examples 2-1 to 2-11 and Comparative Examples 2-1 to 2-10.

[0169] Table 1

[0170]

[0171] Table 2

[0172]

[0173] In Tables 1 and 2, the photoacid generator PAG-1, the crosslinkers CL-1 and CL-2, and the quencher AM-1 are identified as follows.

[0174]

[0175] (1) Pattern formation and evaluation

[0176] A die coater was used as a coating machine and a 38 μm thick polyethylene terephthalate (PET) was used as a support. Each of the photosensitive resin compositions of Examples 2-1 to 2-11 and Comparative Examples 2-1 to 2-10 was coated on a support. The coated support was passed through a hot air circulation oven (length 4 m) set at 100° C. for 5 minutes to dry and form a photosensitive resin coating on the support to generate a photosensitive dry film. A 50 μm thick polyethylene film as a protective film was bonded to the photosensitive resin coating at a pressure of 1 MPa using a laminating roller to generate a photosensitive dry film with a protective film. The thickness of each photosensitive resin coating is listed in Tables 3 and 4. The thickness of the resin coating was measured by an optical interference film thickness meter.

[0177] The protective film was peeled off from the photosensitive dry film with the protective film. The photosensitive resin coating on the support was tightly bonded to a silicon substrate on which copper sputtered to a thickness of 400 nm was deposited on its surface using a vacuum laminator TEAM-100RF (Takatori Corp.) with a vacuum chamber set at 80 Pa vacuum. The temperature was 110° C. After returning to atmospheric pressure, the substrate was taken out of the laminator and the support was peeled off. The photosensitive resin coating was then prebaked on a hot plate at 130° C. for 5 minutes to enhance adhesion to the substrate.

[0178] Next, the photosensitive resin coating was exposed to 405 nm radiation through a mask with a line-space pattern and a contact hole pattern using a contact lithography machine exposure tool. After exposure, the coated substrate was baked (PEB) on a hot plate at 120° C. for 5 minutes and cooled. This was followed by spray development in propylene glycol monomethyl ether acetate (PGMEA) for 300 seconds to form a pattern of the resin coating.

[0179] The patterned photosensitive resin coating on the substrate was post-cured in an oven at 180°C for 2 hours while the oven was purged with nitrogen. Under a scanning electron microscope (SEM), 300 μm, 200 μm, 100 μm, 80 μm and 60 μm contact hole patterns were observed in cross section, and the smallest hole pattern in which the hole extended down to the bottom of the film was reported as the maximum resolution. From the cross-sectional photograph, the verticality of the 80 μm contact hole pattern was evaluated, and the vertical pattern was rated as "Excellent (Exc.)", the slightly reverse tapered profile was rated as "Good", the reverse tapered profile was rated as "Fair" and the opening failure was rated as "Poor".

[0180] (2) Evaluation of electrical properties (dielectric breakdown strength)

[0181] In order to evaluate the dielectric breakdown strength of the photosensitive resin coating of the photosensitive resin composition, each of the photosensitive resin compositions of Examples 2-1 to 2-11 and Comparative Examples 2-1 to 2-10 was coated on a 13 cm × 15 cm × 0.7 mm (thick) steel plate by means of a bar coater and heated in an oven at 180° C. for 2 hours to form a photosensitive resin coating. The resin composition was applied so that the resulting coating had a thickness of 0.2 μm. The resin coating was tested by a breakdown tester TM-5031AM (TamaDensoku Co., Ltd.) to determine its dielectric breakdown strength.

[0182] (3) Evaluation of reliability (adhesion, crack resistance)

[0183] Each of the substrates with the photosensitive resin coating after pattern formation and post-curing in the test (1) was cut into 10 mm square samples using a dicing saw (DISCO Co.'s DAD685, spindle speed 40,000 rpm, cutting rate 20 mm / sec) with a dicing blade. Ten samples of each embodiment were examined by a thermal cycle test (a test of keeping at -25°C for 10 minutes and keeping at 125°C for 10 minutes, the test was repeated 1,000 cycles). After the test, it was observed whether the resin coating was peeled off from the substrate and whether the resin coating was cracked. The sample was rated as "good" when all samples were not peeled off or cracked, "peeled" when one or more samples were peeled off, and "cracked" when one or more samples were cracked.

[0184] The results are shown in Tables 3 and 4.

[0185] Table 3

[0186]

[0187] Table 4

[0188]

[0189] As can be seen from the test results, the photosensitive resin compositions of Examples 2-1 to 2-11 within the scope of the present invention experienced little film thickness loss, showing good resolution, i.e., sufficient properties as photosensitive materials. The cured resin coating obtained therefrom has improved electrical properties (e.g., dielectric breakdown strength) and improved adhesion and crack resistance after thermal cycle testing, and can therefore be used as a protective film for circuits and electronic components. Therefore, a photosensitive dry film with better reliability can be obtained.

[0190] (4) Evaluation of resist materials for plating

[0191] The photosensitive resin compositions of Examples 2-1 to 2-11 were examined for their performance as resist materials for plating.

[0192] The protective film was peeled off from the photosensitive dry film with a protective film prepared by the same procedure as in (1). Using a vacuum laminator TEAM-100RF (Takatori Corp.) with a vacuum chamber set at a vacuum of 80 Pa, the photosensitive resin coating on the support was tightly bonded to a silicon substrate on which copper was sputter-deposited to a thickness of 400 nm. The temperature was 110° C. After returning to atmospheric pressure, the substrate was taken out of the laminator and the support was peeled off. The photosensitive resin coating was then prebaked on a hot plate at 130° C. for 5 minutes to enhance adhesion to the substrate.

[0193] Next, using a contact lithography machine exposure tool, the photosensitive resin coating is exposed to 405nm radiation through a mask with a line-space pattern and a contact hole pattern. After exposure, the coated substrate is baked (PEB) on a hot plate at 120°C for 5 minutes and cooled. This is followed by spray development in PGMEA for 300 seconds to form a pattern of the resin coating. The patterned substrate is immersed in a copper plating bath (Microfab Cu200, Electroplating Engineers of Japan Ltd.), where copper is electroplated at a constant current. In Examples 2-1 to 2-11, Cu plating columns are correctly formed without stripping of the resin coating. It has been confirmed that the photosensitive resin composition can also be used as a resist material for plating.

[0194] Japanese Patent Application No. 2018-095370 is incorporated herein by reference.

[0195] While some preferred embodiments have been described, numerous modifications and variations are possible in light of the above teachings. It is therefore to be understood that the invention may be practiced otherwise than as specifically described without departing from the scope of the appended claims.

Claims

1. A photosensitive resin composition comprising (A) a polymer containing a silicon-containing phenylene group and a polyether structure and comprising repeating units having the following formulae (1) to (4), and (B) a photoacid generator, in, X 1 is a divalent group having the following formula (X1), X 2 is a divalent group having the following formula (X2), X 3 is a divalent group having the following formula (X3), X 4 is a divalent group having the following formula (X4), and p, q, r, and s are numbers within the following ranges: 0.1 ≤ p < 1, 0 ≤ q < 1, 0 ≤ r < 1, 0 ≤ s < 1, 0 < q + r + s < 1, and p + q + r + s = 1, Among them, R 1 and R 2 Each independently represents hydrogen or a C1-C8 monovalent hydrocarbon group, R 3 and R 4 are each independently hydrogen or methyl, a 1 and a 2 are each independently an integer from 1 to 6, and n is an integer from 0 to 100, Among them, Y 1 is a single bond, a methylene group, a propane-2,2-diyl group, a 1,1,1,3,3,3-hexafluoropropane-2,2-diyl group or a fluorene-9,9-diyl group, R 11 and R 12 are each independently hydrogen or methyl, R 13 and R 14 Each independently is a C1-C4 alkyl or alkoxy group, b 1 and b 2 are each independently an integer from 0 to 7, and c 1 and c 2 are each independently an integer from 0 to 2, Among them, Y 2 is a single bond, a methylene group, a propane-2,2-diyl group, a 1,1,1,3,3,3-hexafluoropropane-2,2-diyl group or a fluorene-9,9-diyl group, R 21 and R 22 are each independently hydrogen or methyl, R 23 and R 24 Each independently is a C1-C4 alkyl or alkoxy group, d 1 and d 2 are each independently an integer from 0 to 7, and e 1 and e 2 are each independently an integer from 0 to 2, Among them, R 31 and R 32 are each independently hydrogen or methyl, and f 1 and f 2 Each independently represents an integer from 0 to 7. 2 . The photosensitive resin composition according to claim 1 , further comprising (C) a crosslinking agent.

3. The photosensitive resin composition according to claim 2, wherein the crosslinking agent is at least one compound selected from the group consisting of an amino condensate modified with formaldehyde or formaldehyde-alcohol, a phenol compound having an average of at least two hydroxymethyl or alkoxymethyl groups in a molecule, and an epoxy compound having an average of at least two epoxy groups in a molecule. The photosensitive resin composition according to claim 1 , further comprising (D) a solvent. The photosensitive resin composition according to claim 1 , further comprising (E) a quencher. 6 . A photosensitive resin coating obtained from the photosensitive resin composition according to claim 1 .

7. A photosensitive dry film comprising a support and the photosensitive resin coating according to claim 6 thereon.

8. A pattern forming method comprising the following steps: (i) applying the photosensitive resin composition according to claim 1 onto a substrate to form a photosensitive resin coating thereon, (ii) exposing the photosensitive resin coating to radiation to define exposed areas and unexposed areas, and (iii) developing the exposed resin coating with a developer to dissolve away unexposed areas of the resin coating and form a pattern of the resin coating.

9. A pattern forming method comprising the following steps: (i') using the photosensitive dry film according to claim 7 to form a photosensitive resin coating on a substrate, (ii) exposing the photosensitive resin coating to radiation to define exposed areas and unexposed areas, and (iii) developing the exposed resin coating with a developer to dissolve away unexposed areas of the resin coating and form a pattern of the resin coating.

10. The pattern forming method according to claim 8, further comprising the step (iv) post-curing the patterned resin coating obtained from the developing step (iii) at a temperature of 100 to 250°C. 11 . The photosensitive resin composition according to claim 1 , which is used to form a coating for protecting electric and electronic parts.

12. The photosensitive resin composition according to claim 1, which is used as a resist material in a step of forming a copper interconnector by plating.