Toner for electrostatic image development, electrostatic image developer, toner cartridge

By adjusting the viscosity characteristics of the toner used in electrostatic imaging development and the aspect ratio of the release agent, the problem of white spots in images under low temperature and high humidity conditions was solved, and the effective penetration and peeling of toner into the recording medium was achieved, thus improving image quality.

CN110908258BActive Publication Date: 2024-11-22FUJIFILM BUSINESS INNOVATION CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN201910167872.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-09-14
Filing Date
2019-03-06
Publication Date
2024-11-22
Estimated Expiration
2039-06-15

AI Technical Summary

Technical Problem

Existing electrostatic toners for imaging are prone to causing white spots in images under low temperature and high humidity conditions, and may not fully penetrate the recording medium or be effectively peeled off during the fixing process, resulting in a decline in image quality.

Method used

By adjusting the viscosity characteristics of the toner, the natural logarithmic viscosity ratio at 60℃, 90℃ and 130℃ is made to meet specific conditions, and the aspect ratio and maximum endothermic peak temperature of the release agent are controlled, thus optimizing the viscosity characteristics of the toner to improve the image development effect.

Benefits of technology

Reduce white spots in images under low temperature and high humidity conditions, ensure that toner fully penetrates the recording medium and is effectively peeled off, and improve image quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110908258B_ABST
    Figure CN110908258B_ABST
Patent Text Reader

Abstract

The present invention provides a toner for electrostatic charge image development, an electrostatic charge image developer, and a toner box. The present invention provides a toner for electrostatic charge image development with fewer white spots in the obtained image. The toner for electrostatic charge image development, when the viscosity η of the toner at T1=60°C is set to η(T1), the viscosity η of the toner at T2=90°C is set to η(T2), and the viscosity η of the toner at T3=130°C is set to η(T3), (lnη(T1)-lnη(T2)) / (T1-T2) is less than -0.14, (lnη(T2)-lnη(T3)) / (T2-T3) is greater than -0.15, and (lnη(T2)-lnη(T3)) / (T2-T3) is a value greater than (lnη(T1)-lnη(T2)) / (T1-T2).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a toner for developing an electrostatic charge image, an electrostatic charge image developer, a toner box, a processing box, an image forming device, and an image forming method. Background Art

[0002] Methods such as electrophotography that visualize image information via electrostatic charge images are currently used in various fields.

[0003] In the past, in electronic photography, a method generally used to make it visible is to use the following multiple steps: various components are used to form an electrostatic latent image on a photoreceptor or an electrostatic recording body, and charge-detecting particles called toner are attached to the electrostatic latent image to develop the electrostatic latent image (toner image), transfer it to the surface of the transfer body, and fix it by heating or the like.

[0004] Patent Document 1 discloses a heat fixing method, which is a method of using a capsule toner formed by coating the surface of a core particle mainly composed of a binder resin, a release agent, and a colorant with a resin, and heat fixing the developed image of the toner on a recording material, wherein: a) capsule toner is used, wherein the binder resin contains a polyester resin obtained by co-condensation of (1) an etherified bisphenol and (2) a divalent or higher carboxylic acid or its anhydride or its lower alkyl ester, and the polyester resin has the following characteristics: The melt viscosity η' obtained at the 50% outflow point is 103 poise to 105 poise, and the absolute value of the slope of the graph when the natural logarithm (Inη') of the melt viscosity is plotted against the temperature is less than 1.0In (poise) / °C, b) using a fixedly supported heating body and a heating component that makes the recording material close to the heating body, the developed image of the toner is heated and fixed on the recording material, and the film is peeled off from the toner fixing surface at a temperature that is 30°C higher than the maximum value of the endothermic peak of the toner measured by DSC.

[0005] Patent document 2 describes a heating fixing method, which is a heating fixing method for heating and fixing a developed image of a toner on a recording medium, wherein: a) a toner is used, and the toner is a toner containing a polyester resin obtained by co-condensing an etherified bisphenol and a carboxylic acid selected from the group consisting of a divalent or higher carboxylic acid, anhydride thereof and a lower alkyl ester thereof, and a release agent, wherein (i) the polyester resin has the following physical properties: the melt viscosity η' obtained by a heat rise flow tester is 103P (poise) to 106P (poise) at any temperature in the temperature range of 80°C to 120°C, and the absolute value of the inclination of the graph when the natural logarithm (Inη') of the melt viscosity at 80°C and 120°C is plotted against the temperature is The invention relates to a method for preparing the toner according to the present invention, wherein the toner has a melting point of 1 cp (centipoise) to 250 cp (centipoise) at 160°C and a release agent which is a polyolefin grafted with an aromatic vinyl monomer and an unsaturated resin acid or an unsaturated fatty acid ester and has a melt viscosity of 1 cp (centipoise) to 250 cp (centipoise) at 160°C and contains 0.1 wt % to 20 wt % relative to the total binder resin; b) a developing image of the toner is heat-fixed on the recording body by a heating body which is fixedly supported and a pressing member which is pressed against the heating body and makes the recording body close to the heating body via a fixing film; and c) the fixing film is peeled off from the fixing surface of the toner at a temperature higher than the maximum value of the endothermic peak of the toner measured by DSC.

[0006] Patent Document 3 describes an electrophotographic toner, which is an electrophotographic toner comprising a binder resin and a colorant, wherein: as the binder resin, the following resin is used: a resin having a glass transition temperature (Tg) to a loss elastic coefficient (G") of G" = 1 × 10 4 The minimum value of tan δ of the binder resin exists between the temperatures of Pa, the minimum value of tan δ is less than 1.2, and the storage elastic coefficient (G') at the temperature where tan δ is minimum is G'=5×10 5 Pa or above, and reach G" = 1 × 10 4 The value of tan δ at a temperature of Pa is 3.0 or more.

[0007] [Prior art literature]

[0008] [Patent Document]

[0009] [Patent Document 1] Japanese Patent Publication No. 8-12456

[0010] [Patent Document 2] Japanese Patent Publication No. 8-16804

[0011] [Patent Document 3] Japanese Patent Application Laid-Open No. 11-194542 Summary of the invention

[0012] [Problems to be solved by the invention]

[0013] The problem to be solved by the present invention is to provide a toner for electrostatic charge image development, wherein when the viscosity η of the toner at T1=60°C is set to η(T1), the viscosity η of the toner at T2=90°C is set to η(T2), and the viscosity η of the toner at T3=130°C is set to η(T3), (lnη(T1)-lnη(T2)) / (T1-T2) exceeds -0.14, or (lnη(T2)-lnη(T3)) / (T2-T3) is less than -0.15, or the value of (lnη(T1)-lnη(T2)) / (T1-T2) is less than the value of (lnη(T2)-lnη(T3)) / (T2-T3), the image obtained has fewer white spots than when the viscosity η of the toner at T1=60°C is set to η(T1), the viscosity η of the toner at T2=90°C is set to η(T2), and the viscosity η of the toner at T3=130°C is set to η(T3), the image obtained has fewer white spots than when the viscosity η of the toner at T1=60°C is set to η(T1), the viscosity η of the toner at T2=90°C is set to η(T2), and the viscosity η of the toner at T3=130°C is set to η(T3).

[0014] [Technical means to solve the problem]

[0015] Specific means for solving the above-mentioned problems include the following embodiments.

[0016] <1> A toner for developing electrostatic images, wherein, when the viscosity η of the toner at T1=60°C is η(T1), the viscosity η of the toner at T2=90°C is η(T2), and the viscosity η of the toner at T3=130°C is η(T3), (lnη(T1)-lnη(T2)) / (T1-T2) is -0.14 or less, (lnη(T2)-lnη(T3)) / (T2-T3) is -0.15 or more, and (lnη(T2)-lnη(T3)) / (T2-T3) is a value larger than (lnη(T1)-lnη(T2)) / (T1-T2).

[0017] <2> The electrostatic image developing toner according to <1>, wherein (lnη(T1)-lnη(T2)) / (T1-T2) is -0.16 or less.

[0018] <3> The electrostatic image developing toner according to <1> or <2>, wherein (lnη(T2)-lnη(T3)) / (T2-T3) is -0.13 or more.

[0019] <4> The electrostatic image developing toner according to <2>, wherein, when a is the number of releasing agents in the toner having an aspect ratio of 5 or more and b is the number of releasing agents having an aspect ratio of 5 or less, 1.0<a / b<8.0.

[0020] <5> The electrostatic image developing toner according to <3>, wherein, when c is an area of ​​the releasing agent in the toner having an aspect ratio of 5 or more and d is an area of ​​the releasing agent having an aspect ratio of 5 or less, 1.0<c / d<4.0.

[0021] <6> The electrostatic charge image developing toner according to any one of <1> to <5>, wherein the toner has a maximum endothermic peak temperature of 70° C. or more and 100° C. or less.

[0022] <7> The electrostatic charge image developing toner according to <6>, wherein the toner has a maximum endothermic peak temperature of 75° C. or higher and 95° C. or lower.

[0023] <8> The electrostatic charge image developing toner according to any one of <1> to <7>, comprising a styrene acrylic resin as a binder resin.

[0024] <9> The electrostatic charge image developing toner according to any one of <1> to <7>, comprising a non-crystalline polyester resin as a binder resin.

[0025] <10> The electrostatic image developing toner according to <9>, wherein the toner particles have an infrared absorption spectrum of 1,500 cm -1 The absorbance relative to the wavelength of 720cm -1 The absorbance ratio is less than 0.6, and the wavelength is 820cm -1 The absorbance relative to the wavelength of 720cm -1 The absorbance ratio is less than 0.4.

[0026] <11> The electrostatic image developing toner according to <10>, wherein the toner particles have an infrared absorption spectrum of 1,500 cm -1 The absorbance relative to the wavelength of 720cm -1 The absorbance ratio is below 0.4, and the wavelength is 820cm -1 The absorbance relative to the wavelength of 720cm -1 The absorbance ratio is less than 0.2.

[0027] <12> An electrostatic image developer comprising the electrostatic image developing toner according to any one of <1> to <11>.

[0028] <13> A toner cartridge that houses the electrostatic image developing toner according to any one of <1> to <11> and is detachably disposed in an image forming apparatus.

[0029] <14> A processing box that can be detachably arranged in an image forming device, the processing box includes a developing component, the developing component stores the electrostatic charge image developer according to <12>, and uses the electrostatic charge image developer to develop the electrostatic charge image formed on the surface of the image retaining body into a toner image.

[0030] <15> An image forming device, comprising: an image retaining body; a charging component for charging the surface of the image retaining body; an electrostatic charge image forming component for forming an electrostatic charge image on the charged surface of the image retaining body; a developing component for storing the electrostatic charge image developer according to <12> and developing the electrostatic charge image formed on the surface of the image retaining body into a toner image using the electrostatic charge image developer; a transferring component for transferring the toner image formed on the surface of the image retaining body to the surface of a recording medium; and a fixing component for fixing the toner image transferred to the surface of the recording medium.

[0031] <16> An image forming method, comprising: a charging step for charging the surface of an image retaining body; an electrostatic charge image forming step for forming an electrostatic charge image on the charged surface of the image retaining body; a developing step for developing the electrostatic charge image formed on the surface of the image retaining body into a toner image using the electrostatic charge image developer according to <12>; a transferring step for transferring the toner image formed on the surface of the image retaining body to the surface of a recording medium; and a fixing step for fixing the toner image transferred to the surface of the recording medium.

[0032] [Effects of the Invention]

[0033] According to the invention of <1>, <8> or <9>, the following electrostatic charge image developing toner can be provided: when the viscosity η of the toner at T1=60°C is set to η(T1), the viscosity η of the toner at T2=90°C is set to η(T2), and the viscosity η of the toner at T3=130°C is set to η(T3), (lnη(T1)-lnη(T2)) / (T1-T2) exceeds -0.14, or (lnη(T2)-lnη(T3)) / (T2-T3) is less than -0.15, or the value of (lnη(T1)-lnη(T2)) / (T1-T2) is less than the value of (lnη(T2)-lnη(T3)) / (T2-T3), the image obtained has fewer white spots than when the viscosity η of the toner at T1=60°C is set to η(T1), the viscosity η of the toner at T2=90°C is set to η(T2), and the viscosity η of the toner at T3=130°C is set to η(T3), the image obtained has fewer white spots.

[0034] According to the invention of <2>, it is possible to provide an electrostatic image developing toner that can produce an image with fewer white spots than when (lnη(T1)-lnη(T2)) / (T1-T2) exceeds -0.16.

[0035] According to the invention of <3>, it is possible to provide an electrostatic image developing toner that can produce an image with fewer white spots than when (lnη(T2)-lnη(T3)) / (T2-T3) is less than -0.13.

[0036] According to the invention of <4>, it is possible to provide an electrostatic image developing toner which can obtain an image with fewer white spots than when the a / b is 1.0 or less or 8.0 or more.

[0037] According to the invention of <5>, it is possible to provide an electrostatic image developing toner which can obtain an image with fewer white spots than when the c / d is 1.0 or less or 4.0 or more.

[0038] According to the invention of <6>, it is possible to provide an electrostatic image developing toner having fewer white spots in an image obtained compared with a toner having a maximum endothermic peak temperature of less than 70°C or exceeding 100°C.

[0039] According to the invention of <7>, it is possible to provide an electrostatic image developing toner having fewer white spots in an image obtained compared with a toner having a maximum endothermic peak temperature of less than 75°C or exceeding 95°C.

[0040] According to the invention of <10>, there is provided a toner for electrostatic image development: -1 The absorbance relative to the wavelength of 720cm -1 The absorbance ratio is greater than 0.6, or the wavelength is 820cm -1 The absorbance relative to the wavelength of 720cm -1 Compared with the case where the absorbance ratio exceeds 0.4, the obtained image has fewer white spots.

[0041] According to the invention of <11>, the following electrostatic image developing toner can be provided: -1 The absorbance relative to the wavelength of 720cm -1 The absorbance ratio is greater than 0.4, or the wavelength is 820cm -1 The absorbance relative to the wavelength of 720cm -1 Compared with the case where the absorbance ratio exceeds 0.2, the obtained image has fewer white spots.

[0042] According to the inventions of <12> to <16>, it is possible to provide an electrostatic charge image developer, a toner cartridge, a processing cartridge, an image forming apparatus or an image forming method having fewer white spots in an image obtained compared to a case where (lnη(T1)-lnη(T2)) / (T1-T2) exceeds -0.14, or (lnη(T2)-lnη(T3)) / (T2-T3) is less than -0.15, or the value of (lnη(T1)-lnη(T2)) / (T1-T2) is less than the value of (lnη(T2)-lnη(T3)) / (T2-T3). BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 It is a diagram schematically showing the configuration of the image forming apparatus according to the present embodiment.

[0044] Figure 2 It is a diagram schematically showing the configuration of a process cartridge according to the present embodiment.

[0045] Explanation of symbols

[0046] 1Y, 1M, 1C, 1K: Photoreceptor (an example of an image holding body)

[0047] 2Y, 2M, 2C, 2K: Charging roller (an example of a charging member)

[0048] 3: Exposure device (an example of electrostatic charge image forming member)

[0049] 3Y, 3M, 3C, 3K: Laser light

[0050] 4Y, 4M, 4C, 4K: Development device (an example of a development unit)

[0051] 5Y, 5M, 5C, 5K: primary transfer rollers (an example of primary transfer members)

[0052] 6Y, 6M, 6C, 6K: Photosensitive body cleaning device (an example of an image holding body cleaning member)

[0053] 8Y, 8M, 8C, 8K: Toner cartridge

[0054] 10Y, 10M, 10C, 10K: Image forming unit

[0055] 20: Intermediate transfer belt (an example of an intermediate transfer body)

[0056] 22: Driving roller

[0057] 24: Support roller

[0058] 26: Secondary transfer roller (an example of a secondary transfer member)

[0059] 28: Fixing device (an example of a fixing part)

[0060] 30: Intermediate transfer belt cleaning device (an example of an intermediate transfer body cleaning component)

[0061] P: Recording paper (an example of recording medium)

[0062] 107: Photoreceptor (an example of an image holding member)

[0063] 108: Charging roller (an example of a charging component)

[0064] 109: Exposure device (an example of electrostatic charge image forming member)

[0065] 111: Development device (an example of a development unit)

[0066] 112: Transfer device (an example of a transfer member)

[0067] 113: Photosensitive body cleaning device (an example of a photosensitive body cleaning member)

[0068] 115: Fixing device (an example of a fixing member)

[0069] 116: Install the rails

[0070] 117: Frame

[0071] 118: Opening for exposure

[0072] 200: Processing box

[0073] 300: Recording paper (an example of recording medium) DETAILED DESCRIPTION

[0074] In the present specification, when the amount of each component in the composition is mentioned, and when a plurality of substances corresponding to each component are present in the composition, unless otherwise specified, the amount refers to the total amount of the plurality of substances present in the composition.

[0075] In this specification, “toner for developing electrostatic charge image” is also simply referred to as “toner”, and “electrostatic charge image developer” is also simply referred to as “developer”.

[0076] Hereinafter, an embodiment as an example of the present invention will be described.

[0077] <Toner for electrostatic image development>

[0078] Regarding the toner for electrostatic charge image development of the present embodiment, when the viscosity η of the toner at T1=60°C is set to η(T1), the viscosity η of the toner at T2=90°C is set to η(T2), and the viscosity η of the toner at T3=130°C is set to η(T3), (lnη(T1)-lnη(T2)) / (T1-T2) is less than -0.14, (lnη(T2)-lnη(T3)) / (T2-T3) is greater than -0.15, and (lnη(T2)-lnη(T3)) / (T2-T3) is a value greater than (lnη(T1)-lnη(T2)) / (T1-T2).

[0079] In previous toners, in a low temperature and high humidity environment (10°C and 80% RH), when, for example, an image was fixed on a recording medium with a large surface irregularity (for example, rough paper such as Leathac), there was a situation where white spots were produced in the image due to factors such as insufficient penetration into the recording medium and failure of the image to be peeled off from the fixing member.

[0080] It is estimated that the temperature of the interface between the fixing member and the unfixed toner in the fixing device increases from 90°C to 130°C, and the temperature of the interface between the unfixed toner and the recording medium increases from 60°C to 90°C.

[0081] The electrostatic image developing toner of the present embodiment can obtain an image with few image defects by the above-mentioned configuration. The reason for this is not clear, but it is estimated as shown below.

[0082] It is believed that if (lnη(T1)-lnη(T2)) / (T1-T2) is less than -0.14, the viscosity of the toner surface on the fixing member side is high, and the toner image is easily peeled off from the fixing member. In addition, if (lnη(T2)-lnη(T3)) / (T2-T3) is greater than -0.15 and is a value greater than (lnη(T1)-lnη(T2)) / (T1-T2), the toner interface on the recording medium side is easily melted, and the toner is easily and fully penetrated into the recording medium. These synergistic effects can obtain a toner for electrostatic charge image development with less white spots in the image.

[0083] Hereinafter, the electrostatic image developing toner according to the present embodiment will be described in detail.

[0084] (Characteristic values ​​of toner temperature and viscosity)

[0085] Regarding the electrostatic charge image developing toner of the present embodiment, when the viscosity η of the toner at T1 = 60° C. is denoted as η(T1), the viscosity η of the toner at T2 = 90° C. is denoted as η(T2), and the viscosity η of the toner at T3 = 130° C. is denoted as η(T3),

[0086] (lnη(T1)-lnη(T2)) / (T1-T2) is less than -0.14,

[0087] (lnη(T2)-lnη(T3)) / (T2-T3) is -0.15 or more,

[0088] (lnη(T2)-lnη(T3)) / (T2-T3) is a value larger than (lnη(T1)-lnη(T2)) / (T1-T2).

[0089] In the present disclosure, "lnη(T1)" is a value of the natural logarithm of the viscosity η of the toner at T1 = 60° C. Alternatively, it may be expressed as ln(η(T1)).

[0090] In addition, unless otherwise specified, the unit of the viscosity of the toner in the present embodiment is Pa·s.

[0091] The viscosity of the toner at each temperature in the present embodiment refers to a value measured by the following method.

[0092] The loss elastic coefficient of the color powder in this embodiment is as follows: using a rotating flat plate rheometer (manufactured by Rheometrics: RDA2, RHIOS system ver.4.3), using parallel plates with a diameter of 8 mm, applying a frequency of 1 Hz and a strain of less than 20%, and measuring the temperature between about 40°C and 150°C at a heating rate of 1°C / min. and a sample weight of about 0.3 g.

[0093] (lnη(T1)-lnη(T2)) / (T1-T2), which is one of the characteristic values ​​of the present embodiment, is less than -0.14. From the viewpoint of suppressing white spots in the obtained image, it is preferably less than -0.16, more preferably greater than -0.30 and less than -0.18, and particularly preferably greater than -0.25 and less than -0.20.

[0094] In addition, (lnη(T2)-lnη(T3)) / (T2-T3), which is one of the characteristic values ​​of the present embodiment, is greater than -0.15. From the viewpoint of suppressing white spots in the obtained image, it is preferably greater than -0.14, more preferably greater than -0.13, further preferably greater than -0.12 and less than -0.03, and particularly preferably greater than -0.11 and less than -0.05.

[0095] Furthermore, in the electrostatic charge image developing toner of the present embodiment, (lnη(T2)-lnη(T3)) / (T2-T3) is a value greater than (lnη(T1)-lnη(T2)) / (T1-T2), and from the viewpoint of suppressing white spots in the obtained image, the value of {(lnη(T2)-lnη(T3)) / (T2-T3)}-{(lnη(T1)-lnη(T2)) / (T1-T2)} is preferably greater than 0.01, more preferably greater than 0.05 and less than 0.5, and particularly preferably greater than 0.08 and less than 0.2.

[0096] (Maximum endothermic peak temperature of toner)

[0097] From the viewpoint of suppressing white spots in the obtained image and fixing properties, the maximum endothermic peak temperature of the electrostatic charge image developing toner of the present embodiment is preferably 70°C to 100°C, more preferably 75°C to 95°C, and particularly preferably 83°C to 93°C.

[0098] The maximum endothermic peak temperature of the toner in the present embodiment is a temperature that provides a maximum endothermic peak in an endothermic curve that includes at least a range of -30°C to 150°C in differential scanning calorimetry.

[0099] A method for measuring the maximum endothermic peak temperature of the toner in this embodiment is described below.

[0100] A differential scanning calorimeter DSC-7 manufactured by Perkin Elmer was used. The melting points of indium and zinc were used for temperature correction of the detection part of the device, and the heat of fusion of indium was used for heat correction. An aluminum pan was used for sample use, and an empty pan for reference was set. The temperature was raised from room temperature to 150°C at a heating rate of 10°C / min, and then lowered from 150°C to -30°C at a rate of 10°C / min, and then raised from -30°C to 150°C at a rate of 10°C / min. The temperature of the maximum endothermic peak during the second heating was set as the maximum endothermic peak temperature.

[0101] (Infrared absorption spectrum of toner particles)

[0102] When the electrostatic image developing toner of the present embodiment contains the non-crystalline polyester resin described later as a binder resin, the electrostatic image developing toner of the present embodiment preferably has a wavelength of 1,500 cm in infrared absorption spectrum analysis of toner particles from the viewpoint of suppressing white spots in the obtained image. -1 The absorbance relative to the wavelength of 720cm -1 The absorbance ratio (wavelength 1,500cm -1 Absorbance / wavelength 720cm -1 The absorbance is below 0.6 and the wavelength is 820cm -1 The absorbance relative to the wavelength of 720cm -1 The absorbance ratio (wavelength 820cm -1 Absorbance / wavelength 720cm -1 The absorbance of the toner particles is preferably 0.4 or less, and more preferably 1,500 cm in wavelength in infrared absorption spectrum analysis of the toner particles. -1 The absorbance relative to the wavelength of 720cm -1 The absorbance ratio is less than 0.4 and the wavelength is 820cm -1 The absorbance relative to the wavelength of 720cm -1The absorbance ratio of the toner particles is preferably 0.2 or less, and particularly preferably 1,500 cm in wavelength in infrared absorption spectrum analysis of the toner particles. -1 The absorbance relative to the wavelength of 720cm -1 The absorbance ratio is 0.2 or more and 0.4 or less, and the wavelength is 820cm -1 The absorbance relative to the wavelength of 720cm -1 The absorbance ratio is 0.05 or more and 0.2 or less.

[0103] The absorbance at each wavelength in the infrared absorption spectrum analysis in this embodiment is measured by the method shown below. First, for the toner particles to be measured (the toner particles are obtained by removing external additives as necessary), a measurement sample is prepared by the KBr tablet method. Then, an infrared spectrophotometer (manufactured by JASCO Corporation: FT-IR-410) is used with respect to the measurement sample at a cumulative count of 300 and a resolution of 4 cm. -1 The wave number was measured at 500 cm -1 Over 4,000cm -1 Then, a baseline correction is performed on the shifted portion where no light is absorbed, and the absorbance at each wavelength is obtained.

[0104] In addition, in the electrostatic image developing toner of the present embodiment, from the viewpoint of suppressing white spots in the obtained image, the toner particles have an infrared absorption spectrum of 1,500 cm -1 The absorbance relative to the wavelength of 720cm -1 The absorbance ratio of is preferably 0.6 or less, more preferably 0.4 or less, further preferably 0.2 or more and 0.4 or less, particularly preferably 0.3 or more and 0.4 or less.

[0105] Furthermore, in the electrostatic image developing toner of the present embodiment, from the viewpoint of suppressing white spots in the obtained image, the toner particles have an infrared absorption spectrum of 820 cm -1 The absorbance relative to the wavelength of 720cm -1 The absorbance ratio of is preferably 0.4 or less, more preferably 0.2 or less, further preferably 0.05 or more and 0.2 or less, particularly preferably 0.08 or more and 0.2 or less.

[0106] The toner of the present embodiment includes toner particles (also referred to as “toner mother particles”) and, if necessary, external additives.

[0107] (Toner particles)

[0108] The toner particles contain, for example, a binder resin, a colorant as needed, a release agent, and other additives, and preferably contain a binder resin and a release agent.

[0109] In the present embodiment, the toner particles may be, in addition to yellow toner, magenta toner, cyan toner, black toner and other toner particles, white toner particles, transparent toner particles, photoluminescent toner particles and the like, without particular limitation.

[0110] -Bonding resin-

[0111] Examples of the binder resin include homopolymers of monomers such as styrenes (e.g., styrene, p-chlorostyrene, α-methylstyrene, etc.), (meth)acrylates (e.g., methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, lauryl methacrylate, 2-ethylhexyl methacrylate, etc.), ethylenically unsaturated nitriles (e.g., acrylonitrile, methacrylonitrile, etc.), vinyl ethers (e.g., vinyl methyl ether, vinyl isobutyl ether, etc.), vinyl ketones (e.g., vinyl methyl ketone, vinyl ethyl ketone, vinyl isopropenyl ketone, etc.), olefins (e.g., ethylene, propylene, butadiene, etc.), or copolymers of two or more of these monomers.

[0112] Examples of the binder resin include epoxy resins, polyester resins, polyurethane resins, polyamide resins, cellulose resins, polyether resins, modified rosins and other non-vinyl resins, mixtures of these with the vinyl resins, or graft polymers obtained by polymerizing vinyl monomers in the presence of these.

[0113] These binder resins may be used alone or in combination of two or more.

[0114] Among them, from the viewpoint of suppressing white spots in the obtained image, the binder resin preferably comprises at least one selected from the group consisting of styrene acrylic resin and non-crystalline (amorphous) polyester resin, more preferably comprises styrene acrylic resin or non-crystalline polyester resin, further preferably comprises 50% by mass or more of styrene acrylic resin or non-crystalline polyester resin relative to the total mass of the binder resin contained in the color powder, and particularly preferably comprises 80% by mass or more of styrene acrylic resin or non-crystalline polyester resin relative to the total mass of the binder resin contained in the color powder.

[0115] From the viewpoint of toner strength and storage stability, the electrostatic image developing toner of the present embodiment preferably contains a styrene acrylic resin as a binder resin.

[0116] In addition, from the viewpoint of low-temperature fixing property, the electrostatic image developing toner of the present embodiment preferably contains a non-crystalline polyester resin as a binder resin.

[0117] Furthermore, as the non-crystalline polyester resin, from the viewpoint of suppressing white spots of the obtained image and improving the fixing property, a non-crystalline polyester resin having no bisphenol structure is preferred.

[0118] As the binder resin, styrene acrylic resin is preferred.

[0119] Styrene acrylic resin is a copolymer obtained by copolymerizing at least a styrene monomer (a monomer having a styrene skeleton) and a (meth) acrylic monomer (a monomer having a (meth) acryloyl group, preferably a monomer having a (meth) acryloyloxy group). Styrene acrylic resin includes, for example, a copolymer of a styrene monomer and the above-mentioned (meth) acrylate monomer.

[0120] The acrylic resin part in the styrene acrylic resin is a partial structure formed by polymerizing either an acrylic monomer or a methacrylic monomer. In addition, the term "(meth)acrylic acid" includes both "acrylic acid" and "methacrylic acid".

[0121] Specific examples of styrene monomers include styrene, alkyl-substituted styrene (e.g., α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-ethylstyrene, 3-ethylstyrene, 4-ethylstyrene, etc.), halogen-substituted styrene (e.g., 2-chlorostyrene, 3-chlorostyrene, 4-chlorostyrene, etc.), vinylnaphthalene, etc. The styrene monomers may be used alone or in combination of two or more.

[0122] Among these, as the styrene-based monomer, styrene is preferred from the viewpoint of easiness of reaction, easiness of reaction control, and further availability.

[0123] As the (meth)acrylic monomer, for example, (meth)acrylic acid and (meth)acrylic acid esters can be specifically mentioned. As the (meth)acrylic acid esters, for example, (meth)acrylic acid alkyl esters (for example, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, n-lauryl (meth)acrylate, n-tetradecyl (meth)acrylate, n-hexadecyl (meth)acrylate, n-octadecyl (meth)acrylate, isopropyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, isopentyl (meth)acrylate, pentyl (meth)acrylate) , neopentyl (meth)acrylate, isohexyl (meth)acrylate, isoheptyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, tert-butylcyclohexyl (meth)acrylate, etc.), aryl (meth)acrylate (for example, phenyl (meth)acrylate, biphenyl (meth)acrylate, diphenylethyl (meth)acrylate, tert-butylphenyl (meth)acrylate, terphenyl (meth)acrylate, etc.), dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, methoxyethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, β-carboxyethyl (meth)acrylate, (meth)acrylamide, etc. The (meth)acrylic monomer may be used alone or in combination of two or more.

[0124] Among the (meth)acrylic monomers, (meth)acrylates having an alkyl group with 2 to 14 carbon atoms (preferably 2 to 10 carbon atoms, more preferably 3 to 8 carbon atoms) are preferred in terms of fixability.

[0125] Among them, n-butyl (meth)acrylate is preferred, and n-butyl acrylate is particularly preferred.

[0126] The copolymerization ratio of the styrene-based monomer to the (meth)acrylic-based monomer (based on mass, styrene-based monomer / (meth)acrylic-based monomer) is not particularly limited, but is preferably 85 / 15 to 70 / 30.

[0127] From the viewpoint of suppressing white spots in the obtained image, the styrene acrylic resin preferably has a crosslinked structure. Preferred examples of the styrene acrylic resin having a crosslinked structure include a styrene acrylic resin obtained by copolymerizing at least a styrene monomer, a (meth)acrylic monomer, and a crosslinking monomer.

[0128] Examples of the crosslinkable monomer include bifunctional or higher-functional crosslinking agents.

[0129] Examples of the bifunctional crosslinking agent include divinylbenzene, divinylnaphthalene, di(meth)acrylate compounds (e.g., diethylene glycol di(meth)acrylate, methylenebis(meth)acrylamide, decanediol diacrylate, glycidyl(meth)acrylate, etc.), polyester di(meth)acrylate, and 2-([1'-methylpropyleneamino]carboxyamino)ethyl methacrylate.

[0130] Examples of the polyfunctional crosslinking agent include tri(meth)acrylate compounds (e.g., pentaerythritol tri(meth)acrylate, trimethylolethane tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, etc.), tetra(meth)acrylate compounds (e.g., pentaerythritol tetra(meth)acrylate, oligoester (meth)acrylate, etc.), 2,2-bis(4-methacryloyloxy, polyethoxyphenyl)propane, diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, diaryl chlorendate, and the like.

[0131] Among them, as the crosslinking monomer, from the viewpoint of suppressing white spots of the obtained image and fixing property, a difunctional or higher (meth)acrylate compound is preferred, a difunctional (meth)acrylate compound is more preferred, a difunctional (meth)acrylate compound having an alkylene group having 6 to 20 carbon atoms is further preferred, and a difunctional (meth)acrylate compound having a linear alkylene group having 6 to 20 carbon atoms is particularly preferred.

[0132] The copolymerization ratio of the crosslinkable monomer to the total monomers (weight basis, crosslinkable monomer / total monomers) is not particularly limited, but is preferably 2 / 1,000 to 20 / 1,000.

[0133] The glass transition temperature (Tg) of the styrene acrylic resin is preferably 40° C. or higher and 75° C. or lower, and more preferably 50° C. or higher and 65° C. or lower, from the viewpoint of fixability.

[0134] The glass transition temperature is determined based on a DSC curve obtained by differential scanning calorimetry (DSC), and more specifically, based on the “extrapolated glass transition initiation temperature” described in the method for determining the glass transition temperature of Japanese Industrial Standards (JIS) K 7121-1987 “Method for determining transition temperatures of plastics”.

[0135] From the viewpoint of storage stability, the weight average molecular weight of the styrene acrylic resin is preferably 5,000 or more and 200,000 or less, more preferably 10,000 or more and 100,000 or less, and particularly preferably 20,000 or more and 80,000 or less.

[0136] The method for preparing the styrene acrylic resin is not particularly limited, and various polymerization methods (e.g., solution polymerization, precipitation polymerization, suspension polymerization, bulk polymerization, emulsion polymerization, etc.) can be applied. In addition, the polymerization reaction can be applied to a known operation (e.g., batch, semi-continuous, continuous, etc.).

[0137] The binder resin is preferably a polyester resin. Examples of the polyester resin include polycondensates of polycarboxylic acids and polyols.

[0138] Examples of the polycarboxylic acid include aliphatic dicarboxylic acids (e.g., oxalic acid, malonic acid, maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, succinic acid, alkenylsuccinic acid, adipic acid, sebacic acid, etc.), alicyclic dicarboxylic acids (e.g., cyclohexanedicarboxylic acid, etc.), aromatic dicarboxylic acids (e.g., terephthalic acid, isophthalic acid, phthalic acid, naphthalene dicarboxylic acid, etc.), anhydrides thereof, or lower (e.g., carbon number 1 to 5) alkyl esters thereof. Among these, it is preferred to use at least an aliphatic dicarboxylic acid, an anhydride thereof, or a lower alkyl ester thereof as the polycarboxylic acid, and it is more preferred to use an aliphatic dicarboxylic acid, an anhydride thereof, or a lower alkyl ester thereof and an aromatic dicarboxylic acid, an anhydride thereof, or a lower alkyl ester thereof.

[0139] As the polycarboxylic acid, a trivalent or higher carboxylic acid that can be used together with a dicarboxylic acid to obtain a crosslinked structure or a branched structure can be used. Examples of the trivalent or higher carboxylic acid include trimellitic acid, pyromellitic acid, anhydrides thereof, or lower (e.g., carbon number 1 to 5) alkyl esters thereof.

[0140] The polyvalent carboxylic acid may be used alone or in combination of two or more.

[0141] Examples of the polyol include aliphatic diols (e.g., ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, butanediol, hexanediol, neopentyl glycol, etc.), alicyclic diols (e.g., cyclohexanediol, cyclohexanedimethanol, hydrogenated bisphenol A, etc.), and aromatic diols (e.g., ethylene oxide adducts of bisphenol A, propylene oxide adducts of bisphenol A, etc.). Among these, the polyol is preferably an aliphatic diol or an alicyclic diol, and more preferably an aliphatic diol.

[0142] As the polyol, a trivalent or higher polyol that can obtain a crosslinked structure or a branched structure can be used together with a diol. Examples of the trivalent or higher polyol include glycerin, trimethylolpropane, and pentaerythritol.

[0143] The polyols may be used alone or in combination of two or more.

[0144] The glass transition temperature (Tg) of the polyester resin is preferably 50°C or higher and 80°C or lower, and more preferably 50°C or higher and 65°C or lower.

[0145] The glass transition temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC), and more specifically, is determined according to the “extrapolated glass transition initiation temperature” described in the method for determining the glass transition temperature in JIS K7121-1987 “Methods for determining transition temperatures of plastics”.

[0146] The weight average molecular weight (Mw) of the polyester resin is preferably 5000 or more and 1000000 or less, and more preferably 7000 or more and 500000 or less. The number average molecular weight (Mn) of the polyester resin is preferably 2000 or more and 100000 or less. The molecular weight distribution Mw / Mn of the polyester resin is preferably 1.5 or more and 100 or less, and more preferably 2 or more and 60 or less.

[0147] The weight average molecular weight and number average molecular weight of the binder resin are measured by gel permeation chromatography (GPC). The molecular weight determination by GPC is performed using a GPC HLC-8120GPC manufactured by Tosoh as a measuring device and a column TSKgel SuperHM-M (15 cm) manufactured by Tosoh in a THF solvent. The weight average molecular weight and number average molecular weight are calculated based on the measurement results and using a molecular weight calibration curve made from a monodisperse polystyrene standard sample.

[0148] The polyester resin can be obtained by a known production method. Specifically, for example, the polyester resin can be obtained by a method in which the polymerization temperature is set to 180° C. to 230° C., and the pressure in the reaction system is reduced as necessary to remove water or alcohol generated during condensation and then react.

[0149] In the case where the monomer of the raw material is insoluble or incompatible at the reaction temperature, a high boiling point solvent may be added as a dissolution aid to dissolve it. In such a case, the dissolution aid is distilled off and the polycondensation reaction is carried out. In the case where there are monomers with poor compatibility, the monomers with poor compatibility may be condensed in advance with the acid or alcohol to be polycondensed with the monomer and then polycondensed with the main component.

[0150] The content of the binder resin is preferably 40% by mass or more and 95% by mass or less, more preferably 50% by mass or more and 90% by mass or less, and still more preferably 60% by mass or more and 85% by mass or less, based on the entire toner particles.

[0151] The content of the binder resin when the toner particles are white toner particles is preferably 30% by mass or more and 85% by mass or less, and more preferably 40% by mass or more and 60% by mass or less, relative to the entire white toner particles.

[0152] -Release agent-

[0153] Examples of the release agent include hydrocarbon waxes, natural waxes such as carnauba wax, rice wax, and candelilla wax, synthetic or mineral / petroleum waxes such as montan wax, and ester waxes such as fatty acid esters and montanic acid esters. The release agent is not limited thereto.

[0154] From the viewpoint of suppressing white spots in the obtained image, the melting temperature of the release agent is preferably 50°C to 110°C, more preferably 70°C to 100°C, further preferably 75°C to 95°C, particularly preferably 83°C to 93°C.

[0155] The melting temperature of the release agent is determined from a DSC curve obtained by differential scanning calorimetry (DSC) according to the “melting peak temperature” described in the method for determining the melting temperature in JIS K7121-1987 “Methods for determining transition temperatures of plastics”.

[0156] Regarding the toner particles of the electrostatic charge image developing toner of the present embodiment, from the viewpoint of suppressing white spots in the obtained image, when the number of release agents in the toner having an aspect ratio of 5 or more is set to a and the number of release agents in the toner having an aspect ratio of less than 5 is set to b, it is preferably 1.0<a / b<8.0, more preferably 2.0<a / b<7.0, and particularly preferably 3.0<a / b<6.0.

[0157] In addition, with respect to the toner particles of the electrostatic charge image developing toner of the present embodiment, from the viewpoint of suppressing white spots in the obtained image, when the area in which the aspect ratio of the release agent in the toner is greater than 5 is set to c and the area less than 5 is set to d, it is preferably 1.0<c / d<4.0, more preferably 1.5<c / d<3.5, and particularly preferably 2.0<c / d<3.0.

[0158] The aspect ratio of the release agent in the toner is measured by the following method.

[0159] The toner is mixed with the epoxy resin and the epoxy resin is cured. The obtained cured product is cut using an ultrathin slicer device (Ultracut UCT manufactured by Leica) to produce a thin sheet sample with a thickness of more than 80nm and less than 130nm. Secondly, the thin sheet sample is dyed with ruthenium tetroxide in a desiccator at 30°C for 3 hours. Then, an SEM image of the dyed thin sheet sample is obtained using an ultra-high resolution field emission scanning electron microscope (FE-SEM) (for example, S-4800 manufactured by Hitachi High-technologies (Hitachi High-technologies) (stock). In general, the release agent is more easily stained with ruthenium tetroxide than the adhesive resin, so the release agent is identified by the shade caused by the degree of dyeing. In the case where it is difficult to distinguish the shade according to the state of the sample, the dyeing time is adjusted. Furthermore, in the cross section of a toner particle, the colorant region is generally smaller than the release agent region, and thus the two can be distinguished based on their size.

[0160] The SEM images include toner particle cross sections of various sizes, and toner particle cross sections having a diameter of 85% or more of the volume average particle diameter of the toner particles are selected, and 100 toner particle cross sections are randomly selected from the cross sections and observed. Here, the diameter of the toner particle cross section refers to the maximum length (so-called major diameter) drawn between any two points on the contour line of the toner particle cross section.

[0161] In the SEM image, image analysis was performed at 0.010000 μm / pixel using image analysis software (WinROOF manufactured by Mitani Shoji Co., Ltd.) for each of the 100 toner particle cross sections selected in the above manner. The image analysis can be used to observe the image of the cross section of the toner particle based on the brightness difference (contrast) between the epoxy resin used for embedding and the binder resin of the toner particle. The length of the release agent region in the toner particle in the major axis direction, the ratio (length in the major axis direction / length in the minor axis direction), and the area can be obtained based on the observed image.

[0162] As a method for adjusting the aspect ratio of the release agent in the color powder, the aspect ratio can be adjusted by maintaining the temperature around the solidification point of the release agent for a certain period of time during cooling to allow crystal growth. By using two or more release agents with different melting points to promote crystal growth during cooling, the aspect ratio can be adjusted.

[0163] The content of the releasing agent is preferably 1% by mass or more and 20% by mass or less, and more preferably 5% by mass or more and 15% by mass or less, based on the entire toner particles.

[0164] -Colorants-

[0165] Examples of the colorant include carbon black, chrome yellow, Hansa yellow, benzidine yellow, threne yellow, quinoline yellow, pigment yellow, permanent orange GTR, pyrazolone orange, vulcan orange, watchung red, permanent red, brilliant carmine 3B, brilliant carmine 6B, Dupont Oil Red, pyrazolone red, lithotripter red, rhodamine B lake, lake red C, pigment red, rose bengal, aniline blue, ultramarine blue, calco oil blue, and chromatin. oilblue), methylene blue chloride, phthalocyanine blue, pigment blue, phthalocyanine green, malachite green oxalate, titanium oxide, zinc oxide, calcium carbonate, basic lead carbonate, zinc sulfide-barium sulfate mixture, zinc sulfide, silicon dioxide, aluminum oxide and other pigments; acridine series, xanthene series, azo series, benzoquinone series, azine series, anthraquinone series, thioindigo series, dioxazine series, thiazine series, azomethine series, indigo series, phthalocyanine series, aniline black series, polymethine series, triphenylmethane series, diphenylmethane series, thiazole series and other dyes.

[0166] When the toner particles are white toner particles, a white pigment may be used as a colorant.

[0167] As the white pigment, titanium oxide and zinc oxide are preferred, and titanium oxide is more preferred.

[0168] The coloring agent may be used alone or in combination of two or more.

[0169] The colorant may be a surface-treated colorant as required, or may be used together with a dispersant.

[0170] The content of the colorant is preferably 1% by mass or more and 30% by mass or less, and more preferably 3% by mass or more and 15% by mass or less, based on the entire toner particles.

[0171] The content of the white pigment when the toner particles are white toner particles is preferably 15% by mass or more and 70% by mass or less, and more preferably 20% by mass or more and 60% by mass or less, relative to the entire white toner particles.

[0172] -Other additives-

[0173] Examples of other additives include known additives such as magnetic materials, charge control agents, and inorganic powders. These additives are contained in toner particles as internal additives.

[0174] -Characteristics of toner particles, etc.-

[0175] The toner particles may be monolayer toner particles or so-called core-shell toner particles including a core (core particle) and a coating layer (shell layer) covering the core. The core-shell toner particles include, for example, a core containing a binder resin and, if necessary, a colorant and a release agent, and a coating layer containing a binder resin.

[0176] The volume average particle size (D50v) of the toner particles is preferably 2 μm or more and 10 μm or less, and more preferably 4 μm or more and 8 μm or less.

[0177] The volume average particle size of the toner particles was measured using a Coulter Multisizer II (manufactured by Beckman-Coulter) and the electrolyte was measured using an ISOTON-II (manufactured by Beckman-Coulter).

[0178] During the measurement, 0.5 mg to 50 mg of the measurement sample is added to 2 ml of a 5 mass % aqueous solution of a surfactant (preferably sodium alkylbenzene sulfonate) as a dispersant, and then added to 100 ml to 150 ml of the electrolyte.

[0179] The electrolyte in which the sample was suspended was dispersed by an ultrasonic disperser for 1 minute, and the particle size of each particle in the range of 2 μm to 60 μm was measured by a Coulter Counter II using an aperture of 100 μm. The number of particles sampled was 50,000.

[0180] The measured particle sizes were cumulatively distributed based on volume from the smaller diameter side, and the particle size at which the cumulative distribution reached 50% was defined as the volume average particle size D50v.

[0181] In this embodiment, the average circularity of the toner particles is not particularly limited, but is preferably 0.91 to 0.98, more preferably 0.94 to 0.98, and even more preferably 0.95 to 0.97 from the viewpoint of optimizing the cleanliness of the toner of the image holder.

[0182] In this embodiment, the circularity of the toner particles is (the circumference of a circle having the same area as the particle projection image) ÷ (the circumference of the particle projection image), and the average circularity of the toner particles is the circularity that reaches 50% from the smallest side in the circularity distribution. The average circularity of the toner particles is obtained by analyzing at least 3,000 toner particles using a flow-type particle image analyzer.

[0183] For example, when toner particles are produced by the aggregation and unification method, the average circularity of the toner particles can be controlled by adjusting the stirring speed of the dispersion, the temperature of the dispersion, or the holding time in the fusion and unification step.

[0184] (External additives)

[0185] Examples of the external additives include inorganic particles, such as SiO2, TiO2, Al2O3, CuO, ZnO, SnO2, CeO2, Fe2O3, MgO, BaO, CaO, K2O, Na2O, ZrO2, CaO·SiO2, K2O·(TiO2)n, Al2O3·2SiO2, CaCO3, MgCO3, BaSO4, and MgSO4.

[0186] The surface of the inorganic particles as an external additive may be subjected to a hydrophobic treatment. The hydrophobic treatment is performed, for example, by immersing the inorganic particles in a hydrophobic treatment agent. The hydrophobic treatment agent is not particularly limited, and examples thereof include: a silane coupling agent, silicone oil, a titanate coupling agent, an aluminum coupling agent, etc. These may be used alone or in combination of two or more.

[0187] The amount of the hydrophobizing agent is preferably 1 part by mass or more and 10 parts by mass or less relative to 100 parts by mass of the inorganic particles.

[0188] Examples of external additives include resin particles (polystyrene, polymethylmethacrylate (PMMA), melamine resin, etc.), cleaning activators (for example, metal salts of higher fatty acids represented by zinc stearate, and particles of fluorine-based high molecular weight bodies), and the like.

[0189] The amount of the external additive added is, for example, preferably 0.01% by mass or more and 10% by mass or less, and more preferably 0.01% by mass or more and 6% by mass or less, based on the toner particles.

[0190] [Method for producing toner]

[0191] Next, a method for producing toner according to the present embodiment will be described.

[0192] The toner of this embodiment is obtained by manufacturing toner particles and then adding an external additive to the toner particles.

[0193] The toner particles can be produced by any of dry methods (e.g., kneading and pulverization methods) and wet methods (e.g., agglomeration, suspension polymerization, dissolution suspension methods, etc.). These methods are not particularly limited, and known methods can be used. Among these, the toner particles can also be obtained by agglomeration.

[0194] Specifically, for example, when the toner particles are manufactured by the agglomeration method, the toner particles are manufactured through the following steps:

[0195] A step of preparing a resin particle dispersion in which resin particles serving as a binding resin are dispersed (resin particle dispersion preparation step); a step of agglomerating resin particles (and other particles as necessary) in the resin particle dispersion (a dispersion obtained by mixing other particle dispersions as necessary) to form agglomerated particles (agglomerated particle formation step); and a step of heating the agglomerated particle dispersion in which agglomerated particles are dispersed to fuse and unify the agglomerated particles to form color powder particles (fusion and unification step).

[0196] The following describes the details of each step.

[0197] In the following description, a method for obtaining toner particles containing a colorant and a release agent is described, but the colorant and the release agent are used as needed. Of course, other additives besides the colorant and the release agent may also be used.

[0198] - Resin particle dispersion preparation step -

[0199] A resin particle dispersion in which resin particles serving as a binder resin are dispersed, a colorant particle dispersion in which colorant particles are dispersed, and a release agent particle dispersion in which release agent particles are dispersed are prepared.

[0200] The resin particle dispersion is prepared by dispersing the resin particles in a dispersion medium using a surfactant, for example.

[0201] Examples of the dispersion medium used in the resin particle dispersion include aqueous media.

[0202] Examples of the aqueous medium include water such as distilled water and ion-exchanged water, and alcohols, etc. These may be used alone or in combination of two or more.

[0203] Examples of surfactants include anionic surfactants such as sulfate ester salts, sulfonates, phosphates, and soaps; cationic surfactants such as amine salts and quaternary ammonium salts; and nonionic surfactants such as polyethylene glycols, alkylphenol ethylene oxide adducts, and polyols. Among these, anionic surfactants and cationic surfactants are particularly useful. Nonionic surfactants can be used in combination with anionic surfactants or cationic surfactants.

[0204] The surfactant may be used alone or in combination of two or more.

[0205] In the resin particle dispersion, as a method for dispersing the resin particles in the dispersion medium, for example, general dispersion methods such as a rotary shearing homogenizer, or a ball mill, a sand mill, and a dyno mill with a medium can be cited. In addition, the resin particles can be dispersed in the dispersion medium by using a phase inversion emulsification method depending on the type of resin particles. The so-called phase inversion emulsification method is the following method: the resin to be dispersed is dissolved in a hydrophobic organic solvent in which the resin is soluble, a base is added to the organic continuous phase (O phase) and neutralized, and then an aqueous medium (W phase) is added, thereby performing a phase inversion from W / O to O / W, thereby dispersing the resin in the aqueous medium in the form of particles.

[0206] The volume average particle size of the resin particles dispersed in the resin particle dispersion is, for example, preferably 0.01 μm or more and 1 μm or less, more preferably 0.08 μm or more and 0.8 μm or less, and still more preferably 0.1 μm or more and 0.6 μm or less.

[0207] The volume average particle size of the resin particles is a particle size distribution obtained by measurement using a laser diffraction particle size distribution measuring device (e.g., LA-700 manufactured by Horiba, Ltd.), and a cumulative distribution is drawn from the small particle size side for the volume relative to the divided particle size range (channel), and the particle size that accumulates to 50% relative to the total particles is measured as the volume average particle size D50v. The volume average particle size of particles in other dispersions is also measured in the same manner.

[0208] The content of the resin particles contained in the resin particle dispersion is preferably 5% by mass or more and 50% by mass or less, and more preferably 10% by mass or more and 40% by mass or less.

[0209] Similar to the resin particle dispersion, for example, a colorant particle dispersion and a release agent particle dispersion are also prepared. That is, the volume average particle size of the particles in the resin particle dispersion, the dispersion medium, the dispersion method, and the content of the particles are the same for the colorant particles dispersed in the colorant particle dispersion and the release agent particles dispersed in the release agent particle dispersion.

[0210] - Agglomerated Particle Formation Steps -

[0211] Next, a resin particle dispersion, a colorant particle dispersion, and a release agent particle dispersion are mixed, and then the resin particles, the colorant particles, and the release agent particles are heterogeneously aggregated in the mixed dispersion to form aggregated particles having a diameter close to the target toner particle diameter and including the resin particles, the colorant particles, and the release agent particles.

[0212] Specifically, for example, a coagulant is added to the mixed dispersion, and the pH value of the mixed dispersion is adjusted to be acidic (for example, a pH value of not less than 2 and not more than 5), and after a dispersion stabilizer is added as needed, it is heated at a temperature close to the glass transition temperature of the resin particles (specifically, for example, the glass transition temperature of the resin particles is not less than -30°C and not more than -10°C), so that the particles dispersed in the mixed dispersion are agglomerated to form agglomerated particles.

[0213] In the step of forming aggregated particles, for example, a coagulant can be added to the mixed dispersion using a rotary shearing homogenizer under stirring at room temperature (e.g., 25° C.), the pH of the mixed dispersion can be adjusted to an acidic state (e.g., a pH of 2 or more and 5 or less), a dispersion stabilizer can be added as needed, and then the mixture can be heated.

[0214] Examples of the coagulant include a surfactant having a polarity opposite to that of the surfactant contained in the mixed dispersion, an inorganic metal salt, and a divalent or higher metal complex. When a metal complex is used as the coagulant, the amount of the surfactant used can be reduced, and the charging characteristics are improved.

[0215] If necessary, an additive that forms a complex with the metal ion of the coagulant or a similar bond may be used together with the coagulant. As the additive, a chelating agent may be preferably used.

[0216] Examples of the inorganic metal salt include metal salts such as calcium chloride, calcium nitrate, barium chloride, magnesium chloride, zinc chloride, aluminum chloride, and aluminum sulfate; and inorganic metal salt polymers such as polyaluminum chloride, polyaluminum hydroxide, and calcium polysulfide.

[0217] As the chelating agent, a water-soluble chelating agent can be used. Examples of the chelating agent include hydroxycarboxylic acids such as tartaric acid, citric acid, and gluconic acid; and aminocarboxylic acids such as iminodiacetic acid (IDA), nitrilotriacetic acid (NTA), and ethylenediaminetetraacetic acid (EDTA).

[0218] The amount of the coagulant added is preferably 0.01 parts by mass or more and 5.0 parts by mass or less, and more preferably 0.1 parts by mass or more and less than 3.0 parts by mass, relative to 100 parts by mass of the resin particles.

[0219] -Fusion and unification steps-

[0220] Secondly, the agglomerated particle dispersion containing the agglomerated particles is heated to a temperature, for example, above the glass transition temperature of the resin particles (for example, a temperature 30°C to 50°C higher than the glass transition temperature of the resin particles) and above the melting temperature of the release agent to allow the agglomerated particles to fuse and merge, thereby forming toner particles.

[0221] In the fusion and unification step, the resin and the release agent are in a fused state at a temperature above the glass transition temperature of the resin particles and above the melting temperature of the release agent. Thereafter, the mixture is cooled to obtain toner particles.

[0222] As a method for adjusting the aspect ratio of the release agent in the color powder, the aspect ratio can be adjusted by maintaining the temperature around the solidification point of the release agent for a certain period of time during cooling to allow crystal growth. By using two or more release agents with different melting points to promote crystal growth during cooling, the aspect ratio can be adjusted.

[0223] The toner particles are obtained through the above steps.

[0224] The color powder particles can also be manufactured through the following steps: after obtaining a coagulated particle dispersion in which coagulated particles are dispersed, the coagulated particle dispersion is further mixed with a resin particle dispersion in which resin particles are dispersed, so as to agglomerate the resin particles by attaching them to the surface of the coagulated particles to form a second coagulated particle; and the second coagulated particle dispersion in which the second coagulated particles are dispersed is heated to fuse and unify the second coagulated particles to form a color powder particle with a core-shell structure.

[0225] After the fusion and unification step is completed, the color powder particles formed in the dispersion are subjected to a known washing step, a solid-liquid separation step, and a drying step to obtain the color powder particles in a dry state. From the perspective of chargeability, the washing step can be fully carried out by replacement washing using ion exchange water. From the perspective of productivity, the solid-liquid separation step can be carried out by suction filtration, pressure filtration, etc. From the perspective of productivity, the drying step can be carried out by freeze drying, air flow drying, fluidized drying, vibration-type fluidized drying, etc.

[0226] The toner of the present embodiment can be produced, for example, by adding an external additive to the obtained dry toner particles and mixing them. The mixing can be performed, for example, using a V-type blender, a Henschel mixer, a Loedige mixer, etc. Furthermore, if necessary, a vibration sieving machine, a wind sieving machine, etc. can be used to remove coarse particles of the toner.

[0227] <Electrostatic image developer>

[0228] The electrostatic charge image developer of this embodiment includes at least the toner of this embodiment. The electrostatic charge image developer of this embodiment may be a single-component developer including only the toner of this embodiment, or a two-component developer including the toner and a carrier.

[0229] The carrier is not particularly limited, and known carriers can be cited. Examples of the carrier include: a coated carrier in which a core material containing magnetic powder is coated with a resin; a magnetic powder dispersion carrier in which magnetic powder is dispersed in a matrix resin and formulated; a resin impregnated carrier in which a porous magnetic powder is impregnated with a resin, etc. The magnetic powder dispersion carrier and the resin impregnated carrier may be a carrier in which the constituent particles of the carrier are set as a core material and the surface thereof is coated with a resin.

[0230] Examples of the magnetic powder include magnetic metals such as iron, nickel, and cobalt; and magnetic oxides such as ferrite and magnetite.

[0231] Examples of the coating resin and matrix resin include polyethylene, polypropylene, polystyrene, polyvinyl acetate, polyvinyl alcohol, polyvinyl butyral, polyvinyl chloride, polyvinyl ether, polyvinyl ketone, vinyl chloride-vinyl acetate copolymer, styrene-acrylate copolymer, pure silicone resin or modified products thereof containing organic siloxane bonds, fluororesins, polyesters, polycarbonates, phenol resins, epoxy resins, etc. The coating resin and matrix resin may also contain additives such as conductive particles. Examples of conductive particles include metals such as gold, silver, and copper, carbon black, titanium oxide, zinc oxide, tin oxide, barium sulfate, aluminum borate, and potassium titanate.

[0232] When the surface of the core material is coated with a resin, a coating layer forming solution prepared by dissolving a coating resin and various additives (used as needed) in an appropriate solvent can be used for coating. The solvent is not particularly limited, and can be selected by considering the type of resin used or coating adaptability. Specific resin coating methods include: an immersion method in which the core material is immersed in a coating layer forming solution; a spray method in which the coating layer forming solution is sprayed on the surface of the core material; a fluidized bed method in which the coating layer forming solution is sprayed while the core material is suspended by flowing air; a kneading coater method in which the core material of the carrier is mixed with the coating layer forming solution in a kneading coater and then the solvent is removed.

[0233] The mixing ratio (mass ratio) of the toner and the carrier in the two-component developer is preferably toner:carrier=1:100 to 30:100, more preferably 3:100 to 20:100.

[0234] <Image forming apparatus, image forming method>

[0235] The image forming apparatus and image forming method according to the present embodiment will be described.

[0236] The image forming device of the present embodiment includes: an image holder; a charging member for charging the surface of the image holder; an electrostatic charge image forming member for forming an electrostatic charge image on the surface of the charged image holder; a developing member for storing an electrostatic charge image developer and developing the electrostatic charge image formed on the surface of the image holder into a toner image using the electrostatic charge image developer; a transfer member for transferring the toner image formed on the surface of the image holder to the surface of a recording medium; and a fixing member for fixing the toner image transferred to the surface of the recording medium. Furthermore, as the electrostatic charge image developer, the electrostatic charge image developer of the present embodiment can be applied.

[0237] In the image forming device of the present embodiment, an image forming method (the image forming method of the present embodiment) is implemented, and the image forming method includes: a charging step of charging the surface of an image retaining body; an electrostatic charge image forming step of forming an electrostatic charge image on the surface of the charged image retaining body; a developing step of developing the electrostatic charge image formed on the surface of the image retaining body into a toner image using the electrostatic charge image developer of the present embodiment; a transfer step of transferring the toner image formed on the surface of the image retaining body to the surface of a recording medium; and a fixing step of fixing the toner image transferred to the surface of the recording medium.

[0238] The image forming device of this embodiment can apply the following well-known image forming devices: a device using a direct transfer method for directly transferring a toner image formed on the surface of an image retaining body to a recording medium; a device using an intermediate transfer method for transferring a toner image formed on the surface of an image retaining body to the surface of an intermediate transfer body for the first time, and for a second time transferring the toner image transferred to the surface of the intermediate transfer body to the surface of a recording medium; a device including a cleaning component for cleaning the surface of the image retaining body before charging after the transfer of the toner image; a device including a static eliminating component for eliminating static by irradiating the surface of the image retaining body with static eliminating light after the transfer of the toner image and before charging, etc.

[0239] In the case where the image forming device of the present embodiment is an intermediate transfer type device, the transfer component can, for example, be applied with the following structure, which comprises an intermediate transfer body for transferring the toner image to the surface, a primary transfer component for transferring the toner image formed on the surface of the image retaining body to the surface of the intermediate transfer body for the first time, and a secondary transfer component for secondarily transferring the toner image transferred to the surface of the intermediate transfer body to the surface of the recording medium.

[0240] In the image forming apparatus of the present embodiment, for example, the portion including the developing component may be a box structure (processing box) that is detachably arranged relative to the image forming apparatus. As the processing box, for example, a processing box including a developing component that accommodates the electrostatic charge image developer of the present embodiment may be preferably used.

[0241] Hereinafter, an example of the image forming apparatus according to the present embodiment will be described, but the present invention is not limited thereto. In the following description, the main parts shown in the drawings will be described, and the description of other parts will be omitted.

[0242] Figure 1 It is a diagram schematically showing the configuration of the image forming apparatus according to the present embodiment.

[0243] Figure 1 The image forming apparatus shown includes first to fourth image forming units 10Y, 10M, 10C, and 10K (image forming means) of an electrophotographic method for outputting images of respective colors of yellow (Y), magenta (M), cyan (C), and black (K) based on color-decomposed image data. These image forming units (hereinafter, also referred to as "units") 10Y, 10M, 10C, and 10K are arranged side by side at a predetermined distance from each other in the horizontal direction. These units 10Y, 10M, 10C, and 10K may be process cartridges that are detachably disposed with respect to the image forming apparatus.

[0244] An intermediate transfer belt (an example of an intermediate transfer body) 20 is extended above each unit 10Y, 10M, 10C, and 10K through each unit. The intermediate transfer belt 20 is wound around a driving roller 22 and a supporting roller 24 that are in contact with the inner surface of the intermediate transfer belt 20, and moves in the direction from the first unit 10Y to the fourth unit 10K. A force is applied to the supporting roller 24 in a direction away from the driving roller 22 by a spring (not shown), so that tension is applied to the intermediate transfer belt 20 wound around the two. An intermediate transfer belt cleaning device 30 is provided on the image holding surface side of the intermediate transfer belt 20 facing the driving roller 22.

[0245] The developing devices (an example of developing means) 4Y, 4M, 4C, 4K of the respective units 10Y, 10M, 10C, 10K are supplied with yellow, magenta, cyan, and black toners contained in toner boxes 8Y, 8M, 8C, 8K.

[0246] The first to fourth units 10Y, 10M, 10C, and 10K have the same configuration and operation, and therefore the first unit 10Y disposed on the upstream side in the intermediate transfer belt moving direction and forming a yellow image will be representatively described here.

[0247] The first unit 10Y has a photosensitive body 1Y that functions as an image holder. The following are arranged in order around the photosensitive body 1Y: a charging roller (an example of a charging member) 2Y that charges the surface of the photosensitive body 1Y to a predetermined potential; an exposure device (an example of an electrostatic charge image forming member) 3 that forms an electrostatic charge image by exposing the charged surface to a laser beam 3Y based on a color-decomposed image signal; a developing device (an example of a developing member) 4Y that supplies charged toner to the electrostatic charge image and develops the electrostatic charge image; a primary transfer roller (an example of a primary transfer member) 5Y that transfers the developed toner image to the intermediate transfer belt 20; and a photosensitive body cleaning device (an example of an image holder cleaning member) 6Y that removes the toner remaining on the surface of the photosensitive body 1Y after the primary transfer.

[0248] The primary transfer roller 5Y is arranged inside the intermediate transfer belt 20 and is provided at a position facing the photoreceptor 1Y. A bias power supply (not shown) for applying a primary transfer bias is connected to each of the primary transfer rollers 5Y, 5M, 5C, and 5K of each unit. Each bias power supply changes the value of the transfer bias applied to each primary transfer roller by control of a control unit (not shown).

[0249] Next, the operation of forming a yellow image in the first unit 10Y will be described.

[0250] First, before the operation, the surface of the photoreceptor 1Y is charged to a potential of -600 V to -800 V by the charging roller 2Y.

[0251] The photoreceptor 1Y is conductive (for example, the volume resistivity at 20° C. is 1×10 -6 The photosensitive layer is formed by laminating a photosensitive layer on a substrate with a resistance of 100 Ωcm or less. The photosensitive layer is usually high in resistance (resistance of a general resin), and has a property that the resistivity of the portion irradiated with the laser light changes when irradiated with laser light. Therefore, according to the image data for yellow sent from the control unit (not shown), the surface of the charged photoreceptor 1Y is irradiated with laser light 3Y from the exposure device 3. As a result, an electrostatic charge image of a yellow image pattern is formed on the surface of the photoreceptor 1Y.

[0252] The so-called electrostatic charge image is an image formed on the surface of the photoreceptor 1Y by charging, and is a so-called negative latent image formed by utilizing the laser light 3Y to reduce the resistivity of the irradiated portion of the photosensitive layer, causing the charged charge on the surface of the photoreceptor 1Y to flow, while the charge on the portion not irradiated by the laser light 3Y remains.

[0253] The electrostatic charge image formed on the photoreceptor 1Y rotates to a predetermined development position as the photoreceptor 1Y moves. Then, at the development position, the electrostatic charge image on the photoreceptor 1Y is developed into a toner image by the developing device 4Y and made visible.

[0254] The developing device 4Y contains, for example, an electrostatic charge image developer containing at least yellow toner and a carrier. The yellow toner is stirred and frictionally charged inside the developing device 4Y, and has a charge of the same polarity (negative polarity) as the charge on the photoreceptor 1Y, and is retained on a developer roller (an example of a developer retainer). Then, the surface of the photoreceptor 1Y is difficult to pass through the developing device 4Y, so that the yellow toner is electrostatically attached to the de-charged latent image portion on the surface of the photoreceptor 1Y, and the latent image is developed using the yellow toner. The photoreceptor 1Y formed with the yellow toner image then moves at a predetermined speed, and the toner image developed on the photoreceptor 1Y is transported to a predetermined primary transfer position.

[0255] When the yellow toner image on the photoreceptor 1Y is conveyed to the primary transfer position, a primary transfer bias is applied to the primary transfer roller 5Y, and the electrostatic force from the photoreceptor 1Y to the primary transfer roller 5Y acts on the toner image, thereby transferring the toner image on the photoreceptor 1Y to the intermediate transfer belt 20. The transfer bias applied at this time is a polarity (+) opposite to the polarity (-) of the toner, and is controlled to, for example, +10 μA by a control unit (not shown) in the first unit 10Y. The toner remaining on the photoreceptor 1Y is removed and recovered by the photoreceptor cleaning device 6Y.

[0256] The primary transfer bias applied to the primary transfer rollers 5M, 5C, and 5K after the second unit 10M is also controlled by the first unit.

[0257] In this way, the intermediate transfer belt 20 to which the yellow toner image has been transferred in the first unit 10Y is sequentially conveyed through the second to fourth units 10M, 10C, and 10K, and toner images of respective colors are superimposed to perform multi-transfer.

[0258] The intermediate transfer belt 20 to which the toner images of four colors are multi-transferred through the first to fourth units arrives at a secondary transfer section including the intermediate transfer belt 20, a support roller 24 in contact with the inner surface of the intermediate transfer belt, and a secondary transfer roller (an example of a secondary transfer member) 26 disposed on the image holding surface side of the intermediate transfer belt 20. On the other hand, a recording paper (an example of a recording medium) P is supplied to the gap between the secondary transfer roller 26 and the intermediate transfer belt 20 at a predetermined time point via a supply mechanism, and a secondary transfer bias is applied to the support roller 24. The transfer bias applied at this time has the same polarity (-) as the polarity (-) of the toner, and the electrostatic force from the intermediate transfer belt 20 to the recording paper P acts on the toner image, thereby transferring the toner image on the intermediate transfer belt 20 to the recording paper P. The secondary transfer bias at this time is determined based on the resistance detected by the resistance detection member (not shown) that detects the resistance of the secondary transfer section, and the voltage is controlled.

[0259] The recording paper P to which the toner image is transferred is fed into the pressure contact portion (nip portion) of a pair of fixing rollers in the fixing device (an example of a fixing member) 28, and the toner image is fixed on the recording paper P, thereby forming a fixed image. The recording paper P to which the color image has been fixed is discharged toward the discharge portion, and a series of color image forming operations are completed.

[0260] As the recording paper P to transfer the toner image, for example, ordinary paper used in electrophotographic copiers, printers, etc. can be cited. As the recording medium, in addition to the recording paper P, OHP sheets can also be cited. In order to further improve the smoothness of the image surface after fixing, it is preferred that the surface of the recording paper P is also smooth, for example, coated paper obtained by coating the surface of ordinary paper with a resin or the like, coated paper for printing, etc. can be preferably used.

[0261] <Process cartridge, toner cartridge>

[0262] The processing box of this embodiment is a processing box that can be detachably configured in an image forming device: it includes a developing component that accommodates the electrostatic charge image developer of this embodiment and uses the electrostatic charge image developer to develop the electrostatic charge image formed on the surface of the image retaining body into a toner image.

[0263] The process cartridge of this embodiment may be configured to include a developing member and, if necessary, at least one member selected from other members such as an image holding member, a charging member, an electrostatic charge image forming member, and a transfer member.

[0264] An example of the process cartridge of the present embodiment is shown below, but the present invention is not limited thereto. In the following description, the main parts shown in the drawings are described, and the description of other parts is omitted.

[0265] Figure 2 It is a schematic structural diagram showing an example of the process cartridge according to the present embodiment.

[0266] Figure 2 The processing box 200 shown, for example, utilizes a frame 117 including a mounting guide 116 and an opening 118 for exposure, and combines and holds a photosensitive body 107 (an example of an image retaining body), a charging roller 108 (an example of a charging component) disposed around the photosensitive body 107, a developing device 111 (an example of a developing component), and a photosensitive body cleaning device 113 (an example of a cleaning component) in an integral manner, thereby being boxed.

[0267] Figure 2 109 denotes an exposure device (an example of an electrostatic charge image forming member), 112 denotes a transfer device (an example of a transfer member), 115 denotes a fixing device (an example of a fixing member), and 300 denotes recording paper (an example of a recording medium).

[0268] Next, the toner cartridge according to the present embodiment will be described.

[0269] The toner cartridge of the present embodiment is a toner cartridge that stores the toner of the present embodiment and is detachably disposed in an image forming apparatus. The toner cartridge stores replenishment toner to be supplied to a developing unit provided in the image forming apparatus.

[0270] Figure 1 The image forming apparatus shown is an image forming apparatus having a toner supply box 8Y, 8M, 8C, 8K which is detachably arranged, and the developing devices 4Y, 4M, 4C, 4K are connected to the toner boxes corresponding to the respective colors by toner supply pipes not shown. When the toner stored in the toner box becomes low, the toner box is replaced.

[0271] [Example]

[0272] Hereinafter, examples of the present invention will be described, but the present invention is not limited to the following examples. In the following description, "parts" and "%" are based on mass unless otherwise specified.

[0273] In addition, the viscosity, maximum endothermic peak temperature, and absorbance at each wavelength of the toner were measured by the above-mentioned method.

[0274] (Example 1 to Example 13, and Comparative Example 1 and Comparative Example 2)

[0275] <Preparation of resin particle dispersion (1)>

[0276] Styrene: 200 parts

[0277] n-Butyl acrylate: 50 parts

[0278] Acrylic acid: 1 part

[0279] β-Carboxyethyl acrylate: 3 parts

[0280] Propylene glycol diacrylate: 1 part

[0281] 2-Hydroxyethyl acrylate: 0.5 parts

[0282] Dodecanethiol: 1 part

[0283] A solution prepared by dissolving 4 parts of anionic surfactant (Dowfax manufactured by Dow Chemical) in 550 parts of ion exchange water was placed in a flask, and the mixed solution mixed with the raw materials was placed therein for emulsification. The emulsion was slowly stirred for 10 minutes and 50 parts of ion exchange water in which 6 parts of ammonium persulfate were dissolved was added. Then, nitrogen replacement was fully performed in the system, and the system was heated in an oil bath until the temperature reached 75°C, and polymerization was carried out for 30 minutes.

[0284] Secondly,

[0285] Styrene: 110 parts

[0286] n-Butyl acrylate: 50 parts

[0287] β-Carboxyethyl acrylate: 5 parts

[0288] 1,10-Decanediol diacrylate: 2.5 parts

[0289] Dodecanethiol: 2 parts

[0290] The mixed solution mixed with the raw materials was added and emulsified, and the emulsion was added to the flask over 120 minutes, and the emulsion polymerization was continued for 4 hours in the above state. Thus, a resin particle dispersion in which resin particles having a weight average molecular weight of 32,000, a glass transition temperature of 53° C., and a volume average particle size of 240 nm were dispersed was obtained. Ion exchange water was added to the resin particle dispersion, and the solid content was adjusted to 20% by mass, thereby preparing a resin particle dispersion (1).

[0291] <Preparation of Resin Particle Dispersion (2)>

[0292] Styrene: 200 parts

[0293] n-Butyl acrylate: 50 parts

[0294] Acrylic acid: 1 part

[0295] β-Carboxyethyl acrylate: 3 parts

[0296] Propylene glycol diacrylate: 1 part

[0297] 2-Hydroxyethyl acrylate: 0.5 parts

[0298] Dodecanethiol: 1.5 parts

[0299] A solution prepared by dissolving 4 parts of anionic surfactant (Dowfax manufactured by Dow Chemical) in 550 parts of ion exchange water was placed in a flask, and the mixed solution mixed with the raw materials was placed therein for emulsification. The emulsion was slowly stirred for 10 minutes and 50 parts of ion exchange water in which 6 parts of ammonium persulfate were dissolved was added. Then, nitrogen replacement was fully performed in the system, and the system was heated in an oil bath until the temperature reached 75°C, and polymerization was carried out for 30 minutes.

[0300] Secondly,

[0301] Styrene: 110 parts

[0302] n-Butyl acrylate: 50 parts

[0303] β-Carboxyethyl acrylate: 5 parts

[0304] 1,10-Decanediol diacrylate: 2.5 parts

[0305] Dodecanethiol: 2.5 parts

[0306] The mixed solution mixed with the raw materials was added and emulsified, and the emulsion was added to the flask over 120 minutes, and the emulsion polymerization was continued for 4 hours in the above state. Thus, a resin particle dispersion in which resin particles having a weight average molecular weight of 30,000, a glass transition temperature of 53° C., and a volume average particle size of 220 nm were dispersed was obtained. Ion exchange water was added to the resin particle dispersion, and the solid content was adjusted to 20% by mass, thereby preparing a resin particle dispersion (2).

[0307] <Preparation of Resin Particle Dispersion (3)>

[0308] Styrene: 200 parts

[0309] n-Butyl acrylate: 50 parts

[0310] Acrylic acid: 1 part

[0311] β-Carboxyethyl acrylate: 3 parts

[0312] Propylene glycol diacrylate: 1 part

[0313] 2-Hydroxyethyl acrylate: 0.5 parts

[0314] Dodecanethiol: 1.5 parts

[0315] A solution prepared by dissolving 4 parts of anionic surfactant (Dowfax manufactured by Dow Chemical) in 550 parts of ion exchange water was placed in a flask, and the mixed solution mixed with the raw materials was placed therein for emulsification. The emulsion was slowly stirred for 10 minutes and 50 parts of ion exchange water in which 7 parts of ammonium persulfate were dissolved was added. Then, nitrogen substitution was fully performed in the system, and the system was heated in an oil bath until the temperature reached 80°C, and polymerization was carried out for 30 minutes.

[0316] Secondly,

[0317] Styrene: 110 parts

[0318] n-Butyl acrylate: 50 parts

[0319] β-Carboxyethyl acrylate: 5 parts

[0320] 1,10-Decanediol diacrylate: 2.5 parts

[0321] Dodecanethiol: 3.0 parts

[0322] The mixed solution mixed with the raw materials was added and emulsified, and the emulsion was added to the flask over 120 minutes, and the emulsion polymerization was continued for 4 hours in the above state. Thus, a resin particle dispersion in which resin particles having a weight average molecular weight of 28,000, a glass transition temperature of 53° C., and a volume average particle size of 230 nm were dispersed was obtained. Ion exchange water was added to the resin particle dispersion, and the solid content was adjusted to 20% by mass, thereby preparing a resin particle dispersion (3).

[0323] <Preparation of Resin Particle Dispersion (4)>

[0324] Styrene: 200 parts

[0325] n-Butyl acrylate: 50 parts

[0326] Acrylic acid: 1 part

[0327] β-Carboxyethyl acrylate: 3 parts

[0328] Propylene glycol diacrylate: 1 part

[0329] 2-Hydroxyethyl acrylate: 0.5 parts

[0330] Dodecanethiol: 2.0 parts

[0331] A solution prepared by dissolving 4 parts of anionic surfactant (Dowfax manufactured by Dow Chemical) in 550 parts of ion exchange water was placed in a flask, and the mixed solution mixed with the raw materials was placed therein for emulsification. The emulsion was slowly stirred for 10 minutes and 50 parts of ion exchange water in which 7.2 parts of ammonium persulfate were dissolved was added. Then, nitrogen substitution was fully performed in the system, and the system was heated in an oil bath until the temperature reached 85°C, and polymerization was carried out for 30 minutes.

[0332] Secondly,

[0333] Styrene: 110 parts

[0334] n-Butyl acrylate: 50 parts

[0335] β-Carboxyethyl acrylate: 5 parts

[0336] 1,10-Decanediol diacrylate: 2.5 parts

[0337] Dodecanethiol: 3.5 parts

[0338] The mixed solution mixed with the raw materials was added and emulsified, and the emulsion was added to the flask over 120 minutes, and the emulsion polymerization was continued for 4 hours in the above state. Thus, a resin particle dispersion in which resin particles having a weight average molecular weight of 26,500, a glass transition temperature of 53° C., and a volume average particle size of 210 nm were dispersed was obtained. Ion exchange water was added to the resin particle dispersion, and the solid content was adjusted to 20% by mass, thereby preparing a resin particle dispersion (4).

[0339] <Preparation of magenta colored particle dispersion>

[0340] CI Pigment Red 122: 50 parts

[0341] Ionic surfactant Neogen RK (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.): 5 parts

[0342] Ion exchange water: 220 parts

[0343] The above components were mixed and treated at 240 MPa for 10 minutes using an ultimixer (manufactured by Sugino Machine Co., Ltd.) to prepare a magenta colored particle dispersion (solid content concentration: 20%).

[0344] <Preparation of Release Agent Particle Dispersion (1)>

[0345] · Ester wax (WEP-2 manufactured by NOF Corporation): 100 parts

[0346] Anionic surfactant (produced by Daiichi Kogyo Seiyaku Co., Ltd., Neogen RK): 2.5 parts

[0347] Ion exchange water: 250 parts

[0348] The materials were mixed and heated to 120°C, dispersed using a homogenizer (Ultraturrax T50 manufactured by IKA), and then dispersed using a Manton Gaulin high-pressure homogenizer (manufactured by Gaulin) to obtain a release agent particle dispersion (1) (solid content 29.1%) in which release agent particles having a volume average particle size of 330 nm were dispersed.

[0349] <Preparation of Release Agent Particle Dispersion (2)>

[0350] Fischer-Tropsch wax (HNP-9 manufactured by Nippon Seiwa Co., Ltd.): 100 parts

[0351] Anionic surfactant (produced by Daiichi Kogyo Seiyaku Co., Ltd., Neogen RK): 2.5 parts

[0352] Ion exchange water: 250 parts

[0353] The materials are mixed and heated to 120°C, dispersed using a homogenizer (Ultraturrax T50 manufactured by IKA), and then dispersed using a Menton Gaulin high pressure homogenizer (manufactured by Gaulin) to obtain a release agent particle dispersion (2) (solid content 29.2%) in which release agent particles having a volume average particle size of 340 nm are dispersed.

[0354] <Preparation of Release Agent Particle Dispersion (3)>

[0355] Paraffin wax (FNP0090 manufactured by Nippon Seiwa Co., Ltd.): 100 parts

[0356] Anionic surfactant (produced by Daiichi Kogyo Seiyaku Co., Ltd., Neogen RK): 2.5 parts

[0357] Ion exchange water: 250 parts

[0358] The materials are mixed and heated to 120°C, dispersed using a homogenizer (Ultraturrax T50 manufactured by IKA), and then dispersed using a Menton Gaulin high pressure homogenizer (manufactured by Gaulin) to obtain a release agent particle dispersion (3) (solid content 29.0%) in which release agent particles having a volume average particle size of 360 nm are dispersed.

[0359] <Preparation of Release Agent Particle Dispersion (4)>

[0360] Polyethylene wax (Polywax 725 manufactured by Toyo Petrolite Co., Ltd.): 100 parts

[0361] Anionic surfactant (produced by Daiichi Kogyo Seiyaku Co., Ltd., Neogen RK): 2.5 parts

[0362] Ion exchange water: 250 parts

[0363] The materials are mixed and heated to 100°C, dispersed using a homogenizer (Ultraturrax T50 manufactured by IKA), and then dispersed using a Menton Gaulin high pressure homogenizer (manufactured by Gaulin) to obtain a release agent particle dispersion (4) (solid content 29.3%) in which release agent particles having a volume average particle size of 370 nm are dispersed.

[0364] <How to make toner>

[0365] Ion exchange water: 400 parts

[0366] Resin particle dispersion (1): 200 parts

[0367] Magenta colored particle dispersion: 40 parts

[0368] Release agent particle dispersion (2): 12 parts

[0369] Release agent particle dispersion (3): 24 parts

[0370] The above components were placed in a reaction container equipped with a thermometer, a pH meter, and a stirrer, and the temperature was controlled from the outside using a mantle heater. The temperature was maintained at 30° C. and a stirring speed of 150 rpm for 30 minutes.

[0371] The mixture was dispersed using a homogenizer (Ultraturrax T50 manufactured by IKA Japan Co., Ltd.), and a polyaluminum chloride (PAC, manufactured by Oji Paper Co., Ltd.: 30% powder) aqueous solution was added, wherein 2.1 parts of PAC was dissolved in 100 parts of ion exchange water. The mixture was then heated to 50° C., and the particle size was measured using a Coulter particle counter II (aperture: 50 μm, manufactured by Coulter Co., Ltd.), and the volume average particle size was set to 5.0 μm. Thereafter, 115 parts of the resin particle dispersion (1) was added, and the resin particles were attached to the surface of the aggregated particles (shell structure).

[0372] Then, 20 parts of a 10% by mass aqueous solution of nitrilotriacetic acid (NTA) metal salt (Chelest 70: manufactured by Chelist (Co., Ltd.)) were added, and the pH value was set to 9.0 using a 1N aqueous sodium hydroxide solution. Thereafter, the temperature was raised to 91°C at a rate of 0.05°C / min, and after being kept at 91°C for 3 hours, the obtained toner slurry was cooled to 85°C and kept for 1 hour. Thereafter, it was cooled to 25°C to obtain a magenta powder. It was further redispersed in ion exchange water and filtered, and the above operation was repeated. After washing until the conductivity of the filtrate became less than 20μS / cm, it was vacuum dried in an oven at 40°C for 5 hours to obtain toner particles.

[0373] 1.5 parts by mass of hydrophobic silica (RY50, manufactured by Aerosil Co., Ltd.) and 1.0 parts by mass of hydrophobic titanium oxide (T805, manufactured by Aerosil Co., Ltd.) were mixed and blended with 100 parts by mass of the obtained toner particles using a sample mill at 10,000 rpm for 30 seconds. Thereafter, the mixture was sieved using a vibrating sieve with a mesh size of 45 μm to prepare the toner (toner for electrostatic image development) of Example 1. The volume average particle size of the obtained toner was 5.7 μm.

[0374] -Production of electrostatic charge image developer-

[0375] The developer (electrostatic charge image developer) of Example 1 was prepared by mixing 8 parts of the toner of Example 1 and 92 parts of the carrier using a V-type blender.

[0376] The resin particle dispersion, release agent particle dispersion, agglomeration amount, unification temperature, holding temperature, and holding time used were as shown in Table 1 to obtain magenta powders of Examples 2 to 13 and Comparative Examples 1 and 2, respectively.

[0377] In addition, electrostatic charge image developers of Examples 2 to 13 and Comparative Examples 1 and 2 were prepared by the same method as that of Example 1.

[0378] The following evaluations were performed using the obtained electrostatic image developing toners and electrostatic image developers of Examples 1 to 13 and Comparative Examples 1 and 2. The evaluation results are summarized in Table 1.

[0379] 〔evaluate〕

[0380] <Image defect evaluation>

[0381] The obtained electrostatic charge image developer was filled into the developer of a commercially available electrophotographic copier (DocuCentre Color 450, manufactured by Fuji Xerox Co., Ltd.), and the Japan Society of Image Science test chart No. 5-2 was output for loss tone color white (weight per unit area 256 gsm), and image defect evaluation (white spot degree evaluation) of the high TMA portion was implemented.

[0382] A: No white spots were observed visually or with a magnifying glass.

[0383] B: White spots were not confirmed by visual observation, but slight shedding was confirmed at less than 3 sites within one field of view by observation with a magnifying glass.

[0384] C: No white spots were observed visually, but slight shedding was observed at 3 or more sites and less than 5 sites within one field of view under a magnifying glass.

[0385] D: White spots were not confirmed by visual observation, but slight shedding was confirmed at 5 or more and less than 10 sites within one field of view by observation with a magnifying glass.

[0386] E: White spots were slightly observed visually.

[0387] F: White spots were observed. This is an unacceptable level.

[0388]

[0389] "a / b" in Table 1 means "a / b when the number of release agents in the color powder with an aspect ratio of 5 or more is set to a and the number of release agents with an aspect ratio of less than 5 is set to b", and "c / d" means "c / d when the area of ​​the release agents in the color powder with an aspect ratio of 5 or more is set to c and the area of ​​less than 5 is set to d".

[0390] From the results shown in Table 1, it can be seen that the image obtained by the electrostatic image developing toner of this example has fewer white spots than the electrostatic image developing toner of the comparative example.

[0391] <Preparation of amorphous polyester resin particle dispersion>

[0392] -Preparation of Resin Particle Dispersion (5)-

[0393] In a three-necked flask with a dry interior, 60 parts by mass of dimethyl terephthalate, 74 parts by mass of dimethyl fumarate, 30 parts by mass of dodecenyl succinic anhydride, 22 parts by mass of trimellitic acid, 138 parts by mass of propylene glycol, and 0.3 parts by mass of dibutyltin oxide were added, and water generated by the reaction was removed to the outside of the system under a nitrogen atmosphere, and the reaction was carried out at 185° C. for 3 hours, and then the pressure was gradually reduced and the temperature was raised to 240° C., and the reaction was further carried out for 4 hours, followed by cooling. In this way, an amorphous polyester resin (A5) having a weight average molecular weight of 39,000 was prepared.

[0394] Next, 200 parts by mass of the amorphous polyester resin (AA5) after removing the insoluble components, 100 parts by mass of methyl ethyl ketone, 35 parts by mass of isopropyl alcohol, and 7.0 parts by mass of a 10% by mass ammonia solution were placed in a separable flask, and after being fully mixed and dissolved, ion exchange water was added dropwise at a liquid delivery rate of 8 g / min using a liquid delivery pump while heating and stirring at 40°C. After the solution became uniformly turbid, the liquid delivery rate was increased to 15 g / min and the phase was inverted, and the dropwise addition was stopped when the liquid delivery amount reached 580 parts by mass. Thereafter, the solvent was removed under reduced pressure to obtain an amorphous polyester resin particle dispersion (5) (resin particle dispersion (5)). The volume average particle size of the obtained polyester resin particles was 170 nm, and the solid content concentration of the resin particles was 35%.

[0395] - Preparation of Resin Particle Dispersion Liquids (6) to (8) -

[0396] Resin particle dispersions (6) to (8) were obtained in the same manner as in the amorphous polyester resin particle dispersion (1) except that the conditions were changed to those shown in Table 2.

[0397] [Table 2]

[0398]

[0399] (Example 14)

[0400] <How to make toner>

[0401] Ion exchange water: 400 parts

[0402] Amorphous polyester resin particle dispersion (5): 200 parts

[0403] Magenta colored particle dispersion: 40 parts

[0404] Release agent particle dispersion (2): 12 parts

[0405] Release agent particle dispersion (3): 24 parts

[0406] The above components were placed in a reaction container equipped with a thermometer, a pH meter, and a stirrer, and the temperature was controlled from the outside with a mantle heater, and the temperature was maintained at 30° C. and a stirring speed of 150 rpm for 30 minutes.

[0407] The mixture was dispersed using a homogenizer (Ultraturrax T50 manufactured by IKA Japan Co., Ltd.), and a polyaluminum chloride (PAC, manufactured by Oji Paper Co., Ltd.: 30% powder) aqueous solution was added, wherein 2.1 parts of PAC was dissolved in 100 parts of ion exchange water. The mixture was then heated to 50° C., and the particle size was measured using a Coulter particle counter II (aperture: 50 μm, manufactured by Coulter Co., Ltd.), and the volume average particle size was 4.9 μm. Thereafter, 115 parts of the resin particle dispersion (1) was added, and the resin particles were attached to the surface of the aggregated particles (shell structure).

[0408] Then, 20 parts of a 10% by mass aqueous solution of nitrilotriacetic acid (NTA) metal salt (Chelest 70: manufactured by Chelist (Co., Ltd.)) were added, and the pH value was set to 9.0 using a 1N aqueous sodium hydroxide solution. Thereafter, the temperature was raised to 91°C at a rate of 0.05°C / min, and after being kept at 91°C for 3 hours, the obtained toner slurry was cooled to 85°C and kept for 1 hour. Thereafter, it was cooled to 25°C to obtain a magenta powder. It was further redispersed in ion exchange water and filtered, and the above operation was repeated. After washing until the conductivity of the filtrate became less than 20μS / cm, it was vacuum dried in an oven at 40°C for 5 hours to obtain toner particles.

[0409] 1.5 parts by mass of hydrophobic silica (RY50, manufactured by Aerosil Co., Ltd.) and 1.0 parts by mass of hydrophobic titanium oxide (T805, manufactured by Aerosil Co., Ltd.) were mixed and blended with 100 parts by mass of the obtained toner particles using a sample mill at 10,000 rpm for 30 seconds. Thereafter, the mixture was sieved using a vibrating sieve with a mesh size of 45 μm to prepare a toner (toner for electrostatic image development) of Example 14. The volume average particle size of the obtained toner was 5.8 μm.

[0410] -Production of electrostatic charge image developer-

[0411] The developer (electrostatic charge image developer) of Example 14 was prepared by mixing 8 parts of the toner of Example 14 and 92 parts of the carrier using a V-type blender.

[0412] (Example 15 to Example 26, and Comparative Example 3 and Comparative Example 4)

[0413] The resin particle dispersion, release agent particle dispersion, agglomeration amount, unification temperature, holding temperature, and holding time used are as shown in Table 3 to obtain magenta powders of Examples 15 to 26 and Comparative Examples 3 and 4, respectively.

[0414] In addition, electrostatic charge image developers of Examples 15 to 26 and Comparative Examples 3 and 4 were prepared by the same method as that of Example 14.

[0415] The same evaluation as in Example 1 was performed using the electrostatic image developing toners and electrostatic image developers obtained in Examples 14 to 26 and Comparative Examples 3 and 4. Table 3 summarizes the evaluation results.

[0416]

[0417] In Table 3, "a / b" means "a / b when the number of release agents in the toner with an aspect ratio of 5 or more is a and the number of release agents with an aspect ratio of 5 or less is b", "c / d" means "c / d when the area of ​​the release agents in the toner with an aspect ratio of 5 or more is c and the area of ​​the release agents with an aspect ratio of 5 or less is d", and "1,500 cm -1 / 720cm -1 " is the wavelength of 1,500 cm in the infrared absorption spectrum analysis of the toner particles in the toner -1 The absorbance relative to the wavelength of 720cm -1 The absorbance ratio of "820cm -1 / 720cm -1 " is the wavelength of 820cm in the infrared absorption spectrum analysis of the toner particles in the toner -1 The absorbance relative to the wavelength of 720cm -1 The value of the ratio of absorbance.

[0418] From the results shown in Table 3, it can be seen that the image obtained by the electrostatic image developing toner of this example has fewer white spots than the electrostatic image developing toner of the comparative example.

Claims

1. A toner for developing electrostatic images, Features: The invention has toner particles, wherein the toner particles contain a binder resin and two kinds of release agents. and comprising styrene acrylic resin as the binding resin, The release agent is selected from ester wax, Fischer-Tropsch wax, paraffin wax and polyethylene wax, When the viscosity η of the toner at T1 = 60°C is defined as η(T1), The viscosity η of the toner at T2 = 90°C is η(T2), When the viscosity η of the toner at T3 = 130°C is denoted as η(T3), (lnη(T1)-lnη(T2)) / (T1-T2) is less than -0.14, (lnη(T2)-lnη(T3)) / (T2-T3) is -0.15 or more, (lnη(T2)-lnη(T3)) / (T2-T3) is a value greater than (lnη(T1)-lnη(T2)) / (T1-T2), When the number of releasing agents in the toner having an aspect ratio of 5 or more is defined as a and the number of releasing agents having an aspect ratio of 5 or less is defined as b, 1.0<a / b<8.

0.

2. The electrostatic charge image developing toner according to claim 1, Features: (lnη(T1)-lnη(T2)) / (T1-T2) is less than -0.

16.

3. The electrostatic charge image developing toner according to claim 1, Features: (lnη(T2)-lnη(T3)) / (T2-T3) is greater than or equal to -0.

13.

4. The electrostatic charge image developing toner according to claim 3, Features: When the area of ​​the release agent in the toner having an aspect ratio of 5 or more is defined as c and the area of ​​5 or less is defined as d, 1.0<c / d<4.

0.

5. The electrostatic charge image developing toner according to claim 1, Features: The toner has a maximum endothermic peak temperature of 70° C. or higher and 100° C. or lower.

6. The electrostatic charge image developing toner according to claim 5, Features: The toner has a maximum endothermic peak temperature of 83° C. or higher and 93° C. or lower.

7. The electrostatic charge image developing toner according to claim 1, Features: The copolymerization ratio of the styrene-based monomer to the (meth)acrylic-based monomer in the styrene acrylic resin is 85 / 15 to 70 / 30.

8. A toner for developing electrostatic images, Features: The invention has toner particles, wherein the toner particles contain a binder resin and two kinds of release agents. and comprising a non-crystalline polyester resin as the binder resin, The release agent is selected from ester wax, Fischer-Tropsch wax, paraffin wax and polyethylene wax, When the viscosity η of the toner at T1 = 60°C is defined as η(T1), The viscosity η of the toner at T2 = 90°C is η(T2), When the viscosity η of the toner at T3 = 130°C is denoted as η(T3), (lnη(T1)-lnη(T2)) / (T1-T2) is less than -0.14, (lnη(T2)-lnη(T3)) / (T2-T3) is -0.15 or more, (lnη(T2)-lnη(T3)) / (T2-T3) is a value greater than (lnη(T1)-lnη(T2)) / (T1-T2), When the number of releasing agents in the toner having an aspect ratio of 5 or more is defined as a and the number of releasing agents having an aspect ratio of 5 or less is defined as b, 1.0<a / b<8.

0.

9. The electrostatic charge image developing toner according to claim 8, Features: In the toner, the wavelength of the toner particles in the infrared absorption spectrum analysis is 1,500 cm -1 The absorbance relative to the wavelength of 720cm -1 The absorbance ratio is 0.6 or less, Wavelength 820cm -1 The absorbance relative to the wavelength of 720cm -1 The absorbance ratio is less than 0.

4.

10. The electrostatic charge image developing toner according to claim 8, Features: In the toner, the wavelength of the toner particles in the infrared absorption spectrum analysis is 1,500 cm -1 The absorbance relative to the wavelength of 720cm -1 The absorbance ratio is 0.4 or less, Wavelength 820cm -1 The absorbance relative to the wavelength of 720cm -1 The absorbance ratio is less than 0.

2.

11. An electrostatic charge image developer, Features: The invention comprises the electrostatic charge image developing toner as claimed in claim 1.

12. A toner cartridge, Features: The electrostatic image developing toner according to claim 1 is stored and is detachably arranged in an image forming apparatus.

Citation Information

Patent Citations

  • Toner for electrophotography, developer for electrophotography, and image forming method

    JP1999194542A

  • Image forming toner, and developer and process cartridge using the toner

    CN101446781A

  • Electrostatic Charge Image Developing Toner, Electrostatic Charge Image Developer, Toner Cartridge, And Process Cartridge

    CN104932215A

  • Toner For Developing Electrostatically Charged Images

    CN106066583A

  • Electrostatic charge image developing toner

    CN106249557A