Toner and method for producing toner

By optimizing the binder resin structure of the toner particles, the low-temperature fixability and development durability are achieved in a long-life development system, the fogging and development stripes are solved, and the development performance is improved.

CN111929998BActive Publication Date: 2024-12-03CANON KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010400207.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-05-13
Filing Date
2020-05-13
Publication Date
2024-12-03
Estimated Expiration
2040-05-13

AI Technical Summary

Technical Problem

The prior art is difficult to achieve a toner with both development durability and low temperature fixability under low temperature conditions, resulting in image defects in fogging and developing stripes prone to long-life development systems.

Method used

A toner is developed that contains toner particles having an energy storage elastic modulus of 0.10 MPa to 3.00 MPa in dynamic viscoelastic determination and a load of 25°C, 150 μN in nanoindentation determination The surface energy storage elastic modulus under the surface is between 2.80 GPa and 4.50 GPa, and the performance of the toner is optimized by controlling the type and composition of the binder resin.

Benefits of technology

The low-temperature fixability is maintained in a long-life development system, while suppressing image defects in fogging and developing stripes, improving development performance and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002489096310000231
    Figure BDA0002489096310000231
  • Figure BDA0002489096310000241
    Figure BDA0002489096310000241
  • Figure BDA0002489096310000242
    Figure BDA0002489096310000242
Patent Text Reader

Abstract

The present invention relates to a toner and a method for producing the toner. A toner comprising toner particles, the toner particles including a binder resin, wherein in a dynamic viscoelasticity measurement of the toner, the storage elastic modulus of the toner at 70°C is 0.10 MPa to 3.00 MPa, and in a nanoindentation measurement of the toner, the surface storage elastic modulus of the toner at 25°C and 150 μN load is 2.80 GPa to 4.50 GPa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a toner for developing electrostatic images and a method for producing the same. Background Art

[0002] In recent years, methods such as an electrophotographic method for developing image data from an electrostatic latent image have been used in various fields, and in addition to high image quality and high speed, copy machines and printers are now required to be compact, energy-efficient, and have a long life.

[0003] In particular, it is necessary to reduce the running cost of copiers and printers. For this purpose, there is a need for machines with excellent energy saving performance and a long life that allows long-term printing with a single cartridge. In particular, for energy saving performance, toners with excellent low-temperature fixability are required to save electricity during heating and fixing.

[0004] In a long-life developing system, heat within the developing device or mechanical stress from components including a developing roller and a developing blade affects the toner for a long time. The toner deforms under such heat and stress, and as a result, it may crack or break. When the cracked or broken toner adheres to other components, a proper charge cannot be applied to the toner from components such as a developing blade, and the toner is transferred to a non-image portion of a printed image, resulting in an image defect called fogging.

[0005] In addition, if the toner further adheres and accumulates on a substance already attached to other members, vertical streaks called development streaks may be caused in the paper output direction on the halftone portion of the printed image. In such a long-life development system, a toner having excellent development durability is required that does not cause image defects such as fogging and development streaks over a long period of time.

[0006] In order to achieve both low temperature fixability and development durability, the viscoelasticity and melt viscosity of the toner are of concern. The toner is subjected to thermal and mechanical stresses in the development device, resulting in toner cracking and breaking. Increasing the viscoelasticity and melt viscosity of the toner is useful for improving development durability because it makes the toner resistant to deformation caused by external heat and stress.

[0007] On the other hand, in the fixing step, reducing the viscoelasticity and melt viscosity of the toner is useful for improving low-temperature fixability because the toner can be fixed on paper at a lower temperature. Therefore, low-temperature fixability and development durability are contradictory characteristics, and a lot of research has been conducted in the past on methods to satisfy both.

[0008] Japanese Patent Application Laid-Open No. 2014-164274 proposes a toner in which the surface hardness and displacement measured by a nanoindentation method are within specific ranges.

[0009] Japanese Patent Application Laid-Open No. 2015-64449 proposes toner particles comprising a specific amorphous polyester resin, a crystalline polyester, and an aluminum element, wherein a surface layer contains an amorphous polyester having an ethylenically unsaturated double bond. Summary of the invention

[0010] Through these technologies, it has become possible to improve development durability while maintaining low temperature fixability. However, it has become difficult to meet the recent greater demands for further energy saving and longer service life. There is room for further improvement to achieve energy saving and longer service life.

[0011] The present invention provides a toner that solves the above-mentioned problems of the prior art. That is, the present invention provides a toner having satisfactory developing performance, thereby suppressing image defects such as fogging and development streaks while maintaining low-temperature fixability in a long-life developing system.

[0012] A toner comprising toner particles, the toner particles including a binder resin, wherein in a dynamic viscoelasticity measurement of the toner, the storage elastic modulus of the toner at 70° C. is 0.10 MPa to 3.00 MPa, and

[0013] In nanoindentation measurement of the toner, the surface storage elastic modulus of the toner at 25° C. and a load of 150 μN is 2.80 GPa to 4.50 GPa.

[0014] The present invention can provide a toner having satisfactory developing performance, whereby image defects such as fogging and development streaks can be suppressed while maintaining low-temperature fixability in a long-life developing system.

[0015] Further features of the present invention will become apparent from the following description of exemplary embodiments. DETAILED DESCRIPTION

[0016] Unless otherwise specified, the expression "from XX to YY" or "XX to YY" expressing a numerical range means a numerical range including the lower limit and the upper limit as endpoints.

[0017] The present invention is explained in detail below.

[0018] Since the toner of the present invention has a high storage elastic modulus of the toner surface, it is unlikely to deform even when subjected to long-term stress from the developing roller and the developing blade during development. Therefore, the demand for high toner developing performance can be met while maintaining low-temperature fixability in a long-life developing system.

[0019] The inventors believe that the exact reason why these effects are obtained is as follows.

[0020] In the toner fixing step, heat and pressure are applied from a member such as a fixing roller to fix the toner on paper. Conventionally, there is a debate about the correlation between the fixing temperature and the storage elastic modulus value of the toner obtained by dynamic viscoelasticity measurement of the toner. In the past, the storage elastic modulus at 100°C was generally used, but recently the fixing temperature has tended to be lowered due to the demand for energy saving.

[0021] In this case, the inventors' research has shown that the storage elastic modulus at 70° C. has a higher correlation with the fixing temperature than the storage elastic modulus at 100° C. That is, in the dynamic viscoelasticity measurement of the toner, the storage elastic modulus at 70° C. of the toner must be within the range of 0.10 MPa to 3.00 MPa.

[0022] If the storage elastic modulus of the toner at 70°C is 3.00 MPa or less, the toner has excellent low-temperature fixability. On the other hand, the storage elastic modulus at 70°C is 0.10 MPa or more, because the toner has an appropriate storage elastic modulus, the toner has excellent development durability and resists thermal deformation.

[0023] The storage elastic modulus at 70° C. of the toner is more preferably in the range of 0.20 MPa to 2.50 MPa. Within this range, the requirements for both development durability and low-temperature fixability can be met at a higher level. The storage elastic modulus at 70° C. can be controlled by controlling the kind of the binder resin or the kind or ratio of the monomers constituting the binder resin.

[0024] Furthermore, in the nanoindentation measurement of the toner, the surface storage elastic modulus of the toner at 25° C. and 150 μN load must be in the range of 2.80 GPa to 4.50 GPa. The surface storage elastic modulus here means the storage elastic modulus of the portion very close to the toner surface, and the inventors' research has shown that this is correlated with the development durability.

[0025] As described above, when the toner is subjected to repeated stress from components such as a developing roller and a developing blade during development, toner cracking and breaking occur. If the surface storage elastic modulus is 2.80 GPa or more, the toner resists deformation even when subjected to repeated stress in a long-life developing system, and image defects such as fogging and development streaks can be suppressed.

[0026] For the purpose of charging assistance and fluidity improvement, inorganic or organic particles called external additives are also externally added to the toner particle surface as needed. This means that if the surface storage elastic modulus is 4.50 GPa or less, the resulting toner has excellent development durability because the external additive can be appropriately fixed to the toner particle surface and can be effectively used as an external additive for a long time.

[0027] The surface storage elastic modulus is more preferably in the range of 3.00 GPa to 4.50 GPa. Within this range, the toner has even better development durability. The surface storage elastic modulus under a load of 150 μN can be controlled by the Tg and acid value of the resin on the surface of the toner particles and the amount of metal ions on the surface.

[0028] Furthermore, in nanoindentation measurement of toner particles, the surface storage elastic modulus of the toner at 25° C. and under a load of 30 μN is preferably in the range of 3.50 GPa to 8.00 GPa, or more preferably in the range of 4.50 GPa to 6.50 GPa.

[0029] The nanoindentation measurement under a load of 30 μN measures the viscoelasticity of a portion closer to the surface of the toner particle than the measurement under a load of 150 μN. Therefore, the nanoindentation measurement under a load of 30 μN is used for toner particles that have not been covered with an external additive.

[0030] If the surface storage elastic modulus of the toner particles under a load of 30 μN is within this range, only the outermost surface of the toner particles has a high storage elastic modulus, resulting in the toner having excellent low-temperature fixability with little hindrance to fixation, while also having high developing performance. The surface storage elastic modulus under a load of 30 μN can be controlled by the Tg and acid value of the resin on the surface of the toner particles and the amount of metal ions on the surface.

[0031] Furthermore, in the nanoindentation measurement of the toner particles, the surface loss modulus of the toner at 25° C. and 30 μN load is preferably in the range of 0.25 GPa to 1.20 GPa, or more preferably in the range of 0.30 GPa to 1.20 GPa.

[0032] In the range of 1.00GPa.

[0033] The surface loss modulus represents the viscosity term of the viscoelasticity of the toner particle surface. If the surface loss modulus of the toner particle is low, the toner is similar to an elastomer and resists deformation caused by repeated stress applied from the outside. On the other hand, if the surface loss modulus is high, the toner is similar to a viscous body and is less likely to break because it dissipates excessive instantaneous external force or in other words, impact force.

[0034] That is, if the surface loss modulus is within the above range, the toner has appropriate elasticity and viscosity, is less likely to be damaged by external force, and resists breakage because it dissipates excessive impact force.

[0035] As a result, the toner has high development durability.The surface loss modulus under a load of 30 μN can be controlled by the Tg and acid value of the resin on the surface of the toner particles and the amount of metal ions on the surface.

[0036] Furthermore, the sum of the peak intensities of Mg, Al, Ca and Fe obtained by time-of-flight secondary ion mass spectrometry (TOF-SIMS) of the toner particles is taken as P(M), and the peak intensity of C obtained by TOF-SIMS of the toner particles is taken as P(C), preferably satisfying the following formula (1):

[0037] 2.0≤P(M) / P(C)≤30.0 (1)

[0038] or more preferably:

[0039] 2.5≤P(M) / P(C)≤25.0.

[0040] It is believed that in the toner particles satisfying this formula, the outermost surface is crosslinked by polyvalent metal (Mg, Al, Ca and / or Fe) ions. If P(M) / P(C) is 2.0 or more, it means that the toner particle surface is sufficiently crosslinked, is less likely to deform in response to external stress, and can be suppressed from breaking.

[0041] On the other hand, if P(M) / P(C) is 30.0 or less, it means that the toner has an appropriate viscosity due to moderate cross-linking and thus resists breakage due to the dissipation of impact force.

[0042] P(M) / P(C) can be controlled by the amount of polyvalent metal ions added.

[0043] It is also preferred that the toner particles contain a polar resin A on their surface, the polar resin A having an acid value Av, and the acid value Av is in the range of 2 mg KOH / g to 30 mg KOH / g. The polar resin A is also preferably crosslinked by a polyvalent metal. The acid value is more preferably in the range of 5 mg KOH / g to 25 mg KOH / g.

[0044] It is believed that when toner particles are produced by a method of granulation in an aqueous medium, the polar resin having an affinity for water is arranged at the interface with water, and the polar groups are oriented on the outermost surface. When a divalent or higher valent water-soluble metal salt with a polar group is added to this orientation, the water-soluble metal salt dissolves in the aqueous medium to generate divalent or higher valent metal ions. It is believed that these divalent or higher valent metal ions coordinate with the polar groups, crosslinking the polar resin and forming a hard toner particle surface.

[0045] If the acid value of the polar resin A is 2 mg KOH / g or more, more crosslinks are present on the surface of the toner particles, making deformation in response to external stress less likely and suppressing cracking. If the acid value is 30 mg KOH / g or less, the resulting toner has a certain viscosity due to moderate crosslinking, and thus resists cracking due to impact force dissipation.

[0046] The content (addition amount) of the polar resin A is preferably 1 to 20 parts by mass, or more preferably 2 to 10 parts by mass, relative to 100 parts by mass of the binder resin or the polymerizable monomer for producing the binder resin.

[0047] The polyvalent metal is preferably at least one selected from the group consisting of Al, Ca, Mg and Fe. One or more of these metals may be used alone in combination. These metals are divalent or higher metals that strongly crosslink with the polar resin A on the surface of the toner particles. This produces a toner that is resistant to cracking and chipping. Preferably, the metal is selected from the group consisting of trivalent metals Al and Fe, and more preferably Al.

[0048] For trivalent metal salts, the toner is more resistant to cracking and breaking due to having more crosslinking points with the polar resin A. In addition, Al has a smaller ionic radius than Fe and more strongly attracts the polar groups of the resin, resulting in stronger crosslinking and a toner that is more resistant to cracking and breaking.

[0049] Polar resin A preferably contains polyester resin, more preferably polyester resin. Since polyester resin has strong adhesion to paper, it adheres to paper when the toner melts and is not easy to fall off. Therefore, it has good low-temperature fixability compared with other resins.

[0050] The method for producing the toner particles is not particularly limited, but preferably includes a step of adding a water-soluble metal salt to an aqueous medium containing the toner particles having a binder resin, and a step of maintaining the pH of the aqueous medium at pH 7.5 to 10.

[0051] Preferably, the method for producing a toner has a granulation step in which particles of a polymerizable monomer composition containing a polar resin A and particles of a polymerizable monomer for producing a binder resin are formed in an aqueous medium; followed by a polymerization step in which the polymerizable monomer contained in the particles of the polymerizable monomer composition is polymerized to produce resin particles, wherein

[0052] The polymerization step includes a step of adding a water-soluble metal salt to an aqueous medium, and a step of maintaining the aqueous medium containing the obtained resin particles at a pH of 7.5 to 10.0,

[0053] The polar resin A has an acid group, the acid dissociation constant pKa of the polar resin A is 7.5 or less, and

[0054] The water-soluble metal salt is a salt of a metal having a valence of two or more.

[0055] As described above, it is believed that when toner particles are produced by a method of granulation in an aqueous medium, the polar resin having a high affinity for water is arranged at the interface with water, and the polar groups are oriented on the surface of the outermost layer. When a water-soluble metal salt having a valence of two or more is added as a polar group in this orientation, the polar resin is cross-linked to form a hard toner particle surface.

[0056] It is known that when crosslinking occurs by divalent or higher-valent metal ions in a low pH state, the divalent or higher-valent metal ions are attached to the polar groups of the outermost layer, and the polar groups are not sufficiently dissociated. This is one of the reasons why the durability of the toner is low.

[0057] This is why the polymerization step for producing the resin particles includes a step of adding a salt of a divalent or higher metal and then maintaining the pH of the aqueous medium containing the obtained resin particles in the range of 7.5 to 10.0 (maintaining step). These steps cause the polar groups on the surface of the resin particles to dissociate and coordinate the divalent or higher metal ions with the ionized polar groups. As a result, the toner particle surface is thoroughly cross-linked, and a toner having excellent development durability can be manufactured. The pH in the maintaining step is preferably in the range of 8.0 to 9.0.

[0058] The temperature in the maintaining step is preferably in the range of 70 to 95° C., or more preferably in the range of 75 to 90° C. The time is preferably in the range of about 5 to 120 minutes, or more preferably in the range of about 10 to 90 minutes.

[0059] Preferably, the polar resin A has an acid group, and the acid dissociation constant pKa of the polar resin is 7.5 or less. If the pKa is 7.5 or less, the metal ions with a valence of two or more can achieve strong crosslinking. The pKa is more preferably in the range of 5.0 to 7.0.

[0060] In this range, the step of maintaining the pH in the range of 7.5 to 10.0 can easily cause the polar groups on the resin particle surfaces to dissociate and the coordination between the divalent or higher metal ions and the ionized polar groups. Thus, a toner having excellent development durability in which the toner particle surfaces are strongly cross-linked can be manufactured.

[0061] The water-soluble metal salt is preferably a salt of a divalent or higher metal. The divalent or higher metal salt is more strongly cross-linked with the polar resin A to obtain a hard toner particle surface. Therefore, a toner having stronger durability and suppressing image defects during development can be produced.

[0062] The water-soluble metal salt is more preferably a trivalent metal salt. If the water-soluble metal salt is trivalent, it is more easily cross-linked with the polar resin, thereby producing a toner that is more durable and suppresses image defects during development.

[0063] A salt of at least one metal selected from the group consisting of Al, Ca, Mg and Fe is preferred. A salt of at least one metal selected from the group consisting of Al and Fe is more preferred, and a salt of Al is still more preferred.

[0064] The type of the salt is not particularly limited, but preferably a chloride salt, a hydroxide salt, a phosphate salt or the like can be used, and a chloride salt is more preferred.

[0065] In the adding step, the polymer conversion rate of the polymerizable monomer is preferably in the range of 50% to 100%. As the polymerization of the polymerizable monomer proceeds, polymer shrinkage occurs. If the polymer conversion rate is 50% or more, since the surface is cross-linked by metal ions, the hard surface layer is more likely to follow the shrinkage caused by polymerization, resulting in good adhesion between the surface layer and the polymer. Therefore, a toner with strong development durability can be manufactured in which the polar resin and the metal ions are thoroughly cross-linked.

[0066] More preferably, the adding step is performed with the polymer conversion rate of the polymerizable monomer in the range of 75% to 100%. As a result, the adhesion between the surface layer and the polymer is further improved, and a highly durable toner can be produced in which the polar resin and the metal ions are more thoroughly cross-linked.

[0067] The adding step is preferably performed before the step (maintaining step) of maintaining the pH of the aqueous medium under the condition of pH in the range of 7.5 to 10.0. The maintaining step is performed after the adding step for completely dissociating the acid groups of the polar resin A. Therefore, the crosslinking between the metal ions and the acid groups can be further promoted, and a toner having strong development durability can be manufactured.

[0068] The pH of the aqueous medium when adding the water-soluble metal salt (the pH of the aqueous medium immediately before the adding step) is not particularly limited, but is preferably about 4.0 to 9.0, more preferably about 4.0 to 8.7.

[0069] Likewise, the polymerizable monomer is preferably at least one selected from the group consisting of styrene monomers and (meth)acrylate monomers. The use of such a monomer makes the composition of the toner particles uniform. As a result, cracks are less likely to start from the inside of the toner particles in response to external stress, and the development durability is excellent.

[0070] More preferably, the polymerizable monomer is styrene and at least one selected from the group consisting of (meth)acrylate monomers. Styrene-based monomers and (meth)acrylate monomers are discussed below.

[0071] The concentration of the water-soluble metal salt in the aqueous medium in the adding step is preferably in the range of 0.2 mmol / L to 40.0 mmol / L, or more preferably in the range of 0.5 mmol / L to 20.0 mmol / L.

[0072] If the concentration of the water-soluble metal salt is 0.2 mmol / L or more, it can be sufficiently cross-linked with the polar resin, so that a toner having high durability and suppressing image defects during development can be produced. A concentration of 40.0 mmol / L or less can produce an appropriate degree of cross-linking between the polar resin and the metal ion, so that a toner resistant to cracking can be produced.

[0073] Next, the method for producing toner particles is explained in detail using examples of steps and usable materials, but these examples are not limitative.

[0074] The method for producing the toner particles is not particularly limited. A production method using suspension polymerization is described below.

[0075] <Method for producing toner particles>

[0076] The production method using suspension polymerization preferably includes the following production steps, but is not limited to the following method.

[0077] Preparation step, preparing a dispersion containing poorly water-soluble inorganic fine particles

[0078] • A granulation step of adding a polymerizable monomer composition containing a polymerizable monomer for producing a binder resin, a polar resin A, and, as required, a colorant, a release agent, and other additives to the dispersion liquid, and forming particles of the polymerizable monomer composition in the dispersion liquid.

[0079] A polymerization step (suspension polymerization step) of polymerizing the polymerizable monomer contained in the polymerizable monomer composition to produce toner particles

[0080] An adding step of adding a water-soluble metal salt to the aqueous medium during or after the polymerization step

[0081] A maintenance step (alkali treatment step) to maintain the pH of the aqueous medium in the range of 7.5 to 10.0 after the addition step

[0082] For example, the following composition preparation step may be included before the granulation step.

[0083] A composition preparation step of mixing a polymerizable monomer for producing a binder resin, a polar resin A, and, as required, a colorant, a release agent, and other additives together to prepare a polymerizable monomer composition.

[0084] The toner particles obtained by the polymerization step (polymerization reaction solution containing toner particles) may also be subjected to the following distillation step and washing, filtering and drying steps. The toner particles obtained by these steps may also be subjected to the following external addition step.

[0085] A distillation step of distilling the obtained polymerization reaction solution containing toner particles

[0086] A washing, filtering and drying step of washing, filtering and drying the obtained toner particles (or a dispersion containing the toner particles)

[0087] External addition step of adding external additives (e.g., inorganic fine powder) to the obtained toner particles

[0088] That is, the method for producing toner particles preferably includes a dispersion preparation step, a composition preparation step, a granulation step, a polymerization step (including a temperature increase step during polymerization), an addition step, a distillation step, a holding step, a washing, filtering and drying step, and an external addition step, preferably performed in sequence.

[0089] Each step is described in detail below.

[0090] [Dispersion Preparation Step]

[0091] First, a dispersion liquid containing poorly water-soluble inorganic fine particles as a dispersant is prepared.

[0092] (Dispersion liquid)

[0093] The dispersion containing the sparingly water-soluble inorganic fine particles may be a dispersion containing the sparingly water-soluble inorganic fine particles and water (aqueous dispersion). The dispersion may also contain counter ions generated during the production of the sparingly water-soluble inorganic fine particles, or the addition of an acid (e.g., hydrochloric acid or sulfuric acid) or an alkali (e.g., sodium hydroxide or sodium carbonate) to adjust the pH, etc. However, the dispersion may also consist only of the sparingly water-soluble inorganic fine particles and water.

[0094] ·water

[0095] For example, ion exchange water can be used as water (dispersion medium) in the dispersion. Preferably, 100 parts by mass or more of water is used to prepare the dispersion per 100 parts by mass of the polymerizable monomer. If the amount of water is 100 parts by mass or more, oil droplets (polymerizable monomer composition particles) can be easily formed without causing oil-water reversal.

[0096] Poorly water-soluble inorganic fine particles

[0097] The poorly water-soluble inorganic fine particles are used as a dispersion stabilizer for the polymerizable monomer composition in the dispersion in the granulation step. Here, the poorly water-soluble fine particles refer to fine particles having an average volume particle size of 1.0 μm or less and a solubility (at a measurement temperature of 60° C.) of 10 or less (indicating the mass (g) of the solute that can be dissolved in 100 g of water at a specific pH (e.g., a pH in the range of 4.0 to 10.0)).

[0098] Both inorganic and organic dispersion stabilizers are known as dispersion stabilizers for suspension polymerization, but inorganic dispersion stabilizers are preferred. Organic dispersion stabilizers such as surfactants may also be used in combination with the poorly water-soluble inorganic fine particles.

[0099] Examples of the poorly water-soluble inorganic fine particles include inorganic dispersion stabilizers (poorly water-soluble inorganic dispersion stabilizers) such as calcium phosphate, magnesium phosphate, aluminum phosphate, zinc phosphate, magnesium carbonate, calcium carbonate, calcium hydroxide, magnesium hydroxide, aluminum hydroxide, calcium metasilicate, calcium sulfate, barium sulfate, bentonite, silicon dioxide, alumina, and the like.

[0100] Among them, calcium phosphate is preferred as the sparingly water-soluble inorganic fine particles to facilitate particle size control. One type of sparingly water-soluble inorganic fine particles or a combination of multiple types may be used.

[0101] Preparation method of dispersion

[0102] When preparing the dispersion of dispersed sparingly water-soluble inorganic fine particles, commercially available dispersion stabilizers can be used as they are or dispersed in water as sparingly water-soluble inorganic fine particles. However, in order to obtain sparingly water-soluble inorganic fine particles (dispersion stabilizer fine particles) having a uniform fine particle size, it is preferred to produce and prepare sparingly water-soluble inorganic fine particles under high-speed stirring in water.

[0103] For example, when calcium phosphate is used as the sparingly water-soluble inorganic fine particles, it can be prepared as follows: That is, the sparingly water-soluble inorganic fine particles can be obtained by mixing a sodium phosphate aqueous solution and a calcium chloride aqueous solution under high-speed stirring at a low temperature range of 60° C. or less to form fine particles of calcium phosphate in water.

[0104] [Granulation step]

[0105] A polymerizable monomer composition containing a polymerizable monomer, a polar resin A, and, if necessary, a colorant, a release agent, and other additives is dispersed in a dispersion containing sparingly water-soluble inorganic fine particles, and the particles of the polymerizable monomer composition are granulated. That is, through the granulation step, a dispersion (dispersion liquid) containing the polymerizable monomer composition particles and sparingly water-soluble inorganic fine particles as a dispersion stabilizer can be obtained.

[0106] All of the polymerizable monomer composition added to the dispersion liquid does not necessarily constitute the polymerizable monomer composition particles, and a part of the added polymerizable monomer composition (eg, polymerization initiator) may also be contained in the dispersion medium.

[0107] Therefore, the relative usage amounts of the poorly water-soluble inorganic fine particles and the components of the polymerizable monomer composition with respect to the polymerizable monomer and the polymerizable monomer composition are based on the input amounts of the polymerizable monomer and the polymerizable monomer composition.

[0108] In addition, as described above, the polymerizable monomer, the polar resin A, and, if necessary, the colorant, the release agent, and other additives may be mixed in advance to prepare a polymerizable monomer composition (composition preparation step), and then the prepared polymerizable monomer composition may be dispersed in a dispersion to prepare particles of the polymerizable monomer composition.

[0109] The particles of the polymerizable monomer composition can be granulated using a stirring device such as a TK mixer (product name, Tokushu Kika Kogyo Co., Ltd.) or the like.

[0110] (Polymerizable Monomer Composition)

[0111] The polymerizable monomer composition may contain, in addition to the polymerizable monomer, a polar resin A and additives such as a polymerization initiator, a charge control agent, a chain transfer agent, a polymerization inhibitor, and a crosslinking agent. The polymerizable monomer composition may be obtained by mixing the polymerizable monomer and the additive.

[0112] Polymerizable monomers

[0113] The polymerizable monomer may be appropriately selected according to the toner particles to be produced, but for example, a radical polymerizable vinyl-based polymerizable monomer may be used.

[0114] A monofunctional polymerizable monomer or a polyfunctional polymerizable monomer may be used as the vinyl-based polymerizable monomer.

[0115] Examples of the monofunctional polymerizable monomer include the following: styrene-based monomers such as styrene and styrene derivatives such as α-methylstyrene, α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, p-n-butylstyrene, p-tert-butylstyrene, p-n-hexylstyrene, p-n-octylstyrene, p-n-nonylstyrene, p-n-decylstyrene, p-n-dodecylstyrene, p-methoxystyrene and p-phenylstyrene;

[0116] (Meth)acrylate monomers include, for example, acrylic polymerizable monomers such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, n-pentyl acrylate, n-hexyl acrylate, 2-ethylhexyl acrylate, n-octyl acrylate, n-nonyl acrylate, cyclohexyl acrylate, benzyl acrylate, dimethyl phosphate ethyl acrylate, diethyl phosphate ethyl acrylate, dibutyl phosphate ethyl acrylate, and 2-benzoyloxyethyl acrylate; and methacrylic polymerizable monomers such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, tert-butyl methacrylate, n-pentyl methacrylate, n-hexyl methacrylate, 2-ethylhexyl methacrylate, n-octyl methacrylate, n-nonyl methacrylate, diethyl phosphate ethyl methacrylate, and dibutyl phosphate ethyl methacrylate; and

[0117] Methylene aliphatic monocarboxylic acid esters; vinyl esters such as vinyl acetate, vinyl propionate, vinyl butyrate, vinyl benzoate and vinyl formate; vinyl ethers such as vinyl methyl ether, vinyl ethyl ether and vinyl isobutyl ether; and vinyl ketones such as vinyl methyl ketone, vinyl hexyl ketone and vinyl isopropyl ketone.

[0118] Examples of the multifunctional polymerizable monomer include the following: diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, polyethylene glycol diacrylate, 1,6-hexanediol diacrylate, neopentyl glycol diacrylate, tripropylene glycol diacrylate, polypropylene glycol diacrylate, 2,2'-bis(4-(acryloyloxy-diethoxy)phenyl)propane, trimethylolpropane triacrylate, tetramethylolmethane tetraacrylate, ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, Tetraethylene glycol dimethacrylate, polyethylene glycol dimethacrylate, 1,3-butanediol dimethacrylate, 1,6-hexanediol dimethacrylate, neopentyl glycol dimethacrylate, polypropylene glycol dimethacrylate, 2,2'-bis(4-methacryloyloxy-diethoxy)phenyl)propane, 2,2'-bis(4-(methacryloyloxy-polyethoxy)phenyl)propane, trimethylolpropane trimethacrylate, tetramethylolmethane tetramethacrylate, divinylbenzene, divinylnaphthalene and divinyl ether, etc.

[0119] A single polymerizable monomer or a combination of multiple ones may be used.

[0120] From the viewpoint of fixing, the amount of the polymerizable monomer used is preferably 50% by mass or more of the total polymerizable monomer composition.

[0121] Polar resin

[0122] As the polar resin, polyester resin, polycarbonate resin, phenol resin, epoxy resin, polyamide resin, cellulose resin, styrene acrylic resin, etc. can be used. A single polar resin or a mixture of plural kinds can be used.

[0123] The polar resin preferably includes a polyester resin. The polyester resin is preferably amorphous. Amorphous resins can impart heat-resistant storage properties. The presence or absence of a melting point determined by DSC can be used to determine whether the resin is amorphous.

[0124] The polyester resin is preferably a polycondensate of a polyol and a polycarboxylic acid.

[0125] Examples of the polyol component include ethylene glycol, propylene glycol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, diethylene glycol, triethylene glycol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, 2-ethyl-1,3-hexanediol, cyclohexanedimethanol, butene glycol, octenyl glycol, cyclohexanedimethanol, hydrogenated bisphenol A, bisphenol A ethylene oxide adduct, and bisphenol A propylene oxide adduct.

[0126] Examples of the polycarboxylic acid include benzene dicarboxylic acids and anhydrides thereof, such as phthalic acid, terephthalic acid, isophthalic acid and phthalic anhydride; and alkyl dicarboxylic acids and anhydrides thereof, such as succinic acid, adipic acid, sebacic acid and azelaic acid.

[0127] Polymerization initiator

[0128] When polymerizing the polymerizable monomer, either or both of an oil-soluble initiator and a water-soluble initiator may be used as a polymerization initiator.

[0129] Examples of oil-soluble initiators include nitrile initiators such as 2,2′-azobisisobutyronitrile, 2,2′-azobis-2,4-dimethylvaleronitrile, 1,1′-azobis(cyclohexane-1-carbonitrile) and 2,2′-azobis-4-methoxy-2,4-dimethylvaleronitrile; and peroxide initiators such as acetylcyclohexylsulfonyl peroxide, diisopropyl peroxycarbonate, decanonyl peroxide, lauroyl peroxide, stearoyl peroxide, propionyl peroxide, acetyl peroxide, tert-butyl peroxy-2-ethylhexanoate, benzoyl peroxide, tert-butyl peroxypivalate, tert-butyl peroxyisobutyrate, cyclohexanone peroxide, methyl ethyl ketone peroxide, dicumyl peroxide, tert-butyl hydroperoxide, di-tert-butyl peroxide and cumene hydroperoxide.

[0130] Examples of the water-soluble initiator include ammonium persulfate, potassium persulfate, 2,2'-azobis(N,N'-dimethyleneisobutyroamidine) hydrochloride, 2,2'-azobis(2-aminodinopropane) hydrochloride, azobis(isobutylamidine) hydrochloride, sodium 2,2'-azobisisobutyronitrile sulfonate, ferrous sulfate, and hydrogen peroxide.

[0131] From the viewpoint of polymerization efficiency and safety, the amount of these polymerization initiators is preferably in the range of 0.1 to 20 parts by mass, or more preferably in the range of 0.1 to 15 parts by mass relative to 100 parts by mass of the polymerizable monomer. After a half-life of 10 hours is referred to, a single polymerization initiator or a mixture of two or more can be used.

[0132] Cross-linking agent

[0133] When polymerizing the polymerizable monomer, a cross-linking agent may be used to increase the stress resistance of the toner particles and control the molecular weight of constituent molecules of the toner particles.

[0134] Compounds having two or more polymerizable double bonds can be used as crosslinking agents. Specific examples include aromatic divinyl compounds such as divinylbenzene and divinylnaphthalene; and carboxylates having two double bonds such as ethylene glycol diacrylate, ethylene glycol dimethacrylate, and 1,3-butanediol dimethacrylate; divinyl compounds such as divinylaniline, divinyl ether, divinyl sulfide, and divinyl sulfone; and compounds having three or more vinyl groups. One of these crosslinking agents may be used alone or as a mixture of two or more.

[0135] The amount of these crosslinking agents used is preferably 0.05 to 10 parts by mass, or more preferably 0.10 to 5 parts by mass, relative to 100 parts by mass of the polymerizable monomer, in view of the fixing performance and offset resistance of the toner.

[0136] Colorants

[0137] The colorant can be appropriately selected from known colorants in the toner field after considering hue angle, chroma, brightness, weather resistance, OHT transparency, dispersibility in toner, etc. Specific examples include black, yellow, magenta and cyan pigments described below, and other colorants such as dyes as needed.

[0138] A single colorant or a mixture of multiple colorants may be used. The colorant may also be used in the form of a solid solution.

[0139] The content (addition amount) of the colorant is preferably 1 to 20 parts by mass relative to 100 parts by mass of the binder resin or the polymerizable monomer used to produce the binder resin. If 1 part by mass or more of the colorant is added, tinting strength is easily obtained, while if 20 parts by mass or less is added, a clearer particle size distribution can be obtained. In order to disperse the pigment or other colorant in the toner particles, the colorant can be first dispersed in a solvent, and a polymerizable monomer (e.g., styrene) can be used as the solvent.

[0140] Black colorant

[0141] A black colorant known in the toner field can be used as the black colorant. Specific examples of the black colorant include carbon black and black obtained by mixing the following yellow, magenta, and cyan colorants.

[0142] The carbon black is not particularly limited, and for example, carbon black obtained by a manufacturing method such as a thermal method, an acetylene method, a tank method, a furnace method, or a lamp black method can be used. A single carbon black or a mixture of two or more carbon blacks can be used. The carbon black can be a crude pigment or a prepared pigment composition, as long as the effect of the pigment dispersant is not significantly inhibited.

[0143] The average particle size of the primary particles of carbon black is preferably in the range of 14 nm to 80 nm, or more preferably in the range of 25 nm to 50 nm. If the average particle size is 14 nm or more, the toner does not show a red hue, and black is desirable for forming a full-color image. If the average particle size of carbon black is 80 nm or less, it is easy to disperse, and since the tinting strength is not too low, suitable tinting strength can be easily imparted.

[0144] The enlarged photograph taken with a scanning electron microscope is used to measure the average particle size of carbon black. The longest axis (major axis) and the shortest axis (minor axis) of the black particles observed as primary particles in the enlarged photograph are measured, and the average value of the major axis and the minor axis is calculated and used as the particle size of each measured particle. The diameter of 100 carbon black particles is measured, and the average value is used as the average particle size. The magnification of the scanning electron microscope can be any magnification that can distinguish the primary particles of carbon black.

[0145] Yellow colorant

[0146] A yellow colorant known in the toner field can be used as the yellow colorant.

[0147] Typical examples of pigment yellow colorants include condensed polycyclic pigments, isoindolinone compounds, anthraquinone compounds, azo metal complexes, methine compounds, and allylamide compounds. Specific examples include CI Pigment Yellow 3, 7, 10, 12, 13, 14, 15, 17, 23, 24, 60, 62, 74, 75, 83, 93, 94, 95, 99, 100, 101, 104, 108, 109, 110, 111, 117, 123, 128, 129, 138, 139, 147, 148, 150, 155, 166, 168, 169, 177, 179, 180, 181, 183, 185, 191:1, 191, 192, 193, and 199.

[0148] Examples of the dye-based yellow colorant include CI Solvent Yellow 33, 56, 79, 82, 93, 112, 162, and 163 and CI Disperse Yellow 42, 64, 201, and 211.

[0149] Magenta colorant

[0150] A magenta colorant known in the toner field can be used as the magenta colorant.

[0151] For example, condensed polycyclic pigments, diketopyrrolopyrrole compounds, anthraquinone compounds, quinacridone compounds, basic dye lake compounds, naphthol compounds, benzimidazolone compounds, thioindigo compounds or perylene compounds can be used as magenta colorants. Specific examples include CI Pigment Red 2, 3, 5, 6, 7, 23, 48:2, 48:3, 48:4, 57:1, 81:1, 122, 146, 150, 166, 169, 177, 184, 185, 202, 206, 220, 221, 238, 254 and 269 and CI Pigment Violet 19.

[0152] Cyan colorant

[0153] Cyan colorants known in the toner field can be used as cyan colorants. Phthalocyanine compounds or derivatives, anthraquinone compounds or basic dye lake compounds can be used as cyan colorants. Specific examples include CI Pigment Blue 1, 7, 15, 15:1, 15:2, 15:3, 15:4, 60, 62 and 66.

[0154] Release agent

[0155] The toner particles may also contain a release agent. Examples of release agents include the following: aliphatic hydrocarbon waxes, such as low molecular weight polyethylene, low molecular weight polypropylene, microcrystalline wax, Fischer-Tropsch wax, and paraffin wax; oxides of aliphatic hydrocarbon waxes, such as polyethylene oxide wax, and block copolymers thereof; waxes composed mainly of fatty acid esters, such as carnauba wax and montanate wax, and those such as deoxygenated carnauba wax in which the fatty acid ester has been partially or completely deoxygenated; saturated straight-chain fatty acids, such as palmitic acid, stearic acid, and montanic acid; unsaturated fatty acids, such as brassene acid, eleostearic acid, and octadecatetraenoic acid; saturated alcohols, such as stearyl alcohol, aralkyl alcohol, behenyl alcohol, carnauba alcohol, wax alcohol, and myristyl alcohol; polyols, such as sorbitol; fatty acid amides, such as linoleamide, oleamide, and lauramide; saturated fatty acid bisamides, such as methylenebisstearamide, ethylenebishexylene glycol, and octadecatetraenoic acid; unsaturated fatty acid amides, such as ethylenebisoleamide, hexamethylenebisoleamide, N,N'-dioleyladipamide and N,N'-dioleylsebacamide; aromatic bisamides, such as meta-xylylbisstearamide and N,N'-distearylisophthalamide; fatty acid metal salts (commonly known as metal soaps), such as calcium stearate, calcium laurate, zinc stearate and magnesium stearate; waxes obtained by grafting aliphatic hydrocarbon waxes with vinyl monomers such as styrene and acrylic acid; partial ester compounds of fatty acids and polyols, such as monoglyceride of behenic acid; and hydroxyl-containing methyl ester compounds obtained by hydrogenation of vegetable oils and fats.

[0156] From the viewpoint of demolding performance and granulation stability, the total content (addition amount) of the releasing agent is preferably in the range of 2.5 to 25.0 parts by mass relative to 100 parts by mass of the binder resin or the polymerizable monomer used to produce the binder resin. If the amount of the releasing agent is 2.5 parts by mass or more, demolding is easier during fixing, while if it is 25.0 parts by mass or less, a uniform surface layer can be easily formed without disturbing the particle size distribution.

[0157] Charge control agent

[0158] The charge control agent can also be used to stably maintain the charging performance of the toner particles regardless of the environment.

[0159] Known charge control agents can be used, and those that can provide a fast charging speed and stably maintain a constant charge amount are preferred. When toner particles are produced by a direct polymerization method, charge control agents that have low polymerization inhibition and are substantially insoluble in water in an aqueous dispersion medium are preferred.

[0160] Specific examples of the negative charge control agent include metal compounds of aromatic carboxylic acids such as salicylic acid, alkyl salicylic acid, dialkyl salicylic acid, naphthoic acid and dicarboxylic acids, metal salts or metal complexes of azo dyes or azo pigments, and boron compounds, silicon compounds and calixarene.

[0161] Examples of the positive charge control agent include quaternary ammonium salts, polymer-type compounds having such quaternary ammonium salts on side chains, as well as guanidine compounds, nigrosine-based compounds, and imidazole compounds.

[0162] One charge control agent or a combination of two or more may be used.

[0163] In addition to the resin-based charge control agent, a metal-containing salicylic acid-based compound is preferred as the charge control agent, and a metal-containing salicylic acid-based compound in which the metal is aluminum or zirconium is particularly desirable. Aluminum salicylate compounds are particularly desirable as the charge control agent.

[0164] Examples of the resin-based charge control agent include polymers or copolymers having a sulfonic acid group, a sulfonate group, a sulfonate ester group, a salicylic acid moiety, or a benzoic acid moiety.

[0165] The content (compounding amount) of the charge control agent is preferably in the range of 0.01 to 20.00 parts by mass, or more preferably in the range of 0.05 to 10.00 parts by mass relative to 100.00 parts by mass of the binder resin or the polymerizable monomer for producing the binder resin.

[0166] Chain transfer agent, polymerization inhibitor

[0167] Chain transfer agents and polymerization inhibitors may also be added to control the degree of polymerization of the polymerizable monomers.

[0168] For example, α-methylstyrene dimer, tert-dodecyl mercaptan, n-dodecyl mercaptan, n-octyl mercaptan, carbon tetrachloride or carbon tetrabromide can be used as the chain transfer agent.

[0169] For example, quinone compounds such as p-benzoquinone, chloroaniline, anthraquinone, phenanthrenequinone or dichlorobenzoquinone, organic hydroxy compounds such as phenol, tert-butylcatechol, hydroquinone, catechol or hydroxy monomethyl ether, nitro compounds such as dinitrobenzene, dinitrotoluene or dinitrophenol, nitroso compounds such as nitrosobenzene or nitrosonaphthol, amino compounds such as methylaniline, p-phenylenediamine, N,N′-tetraethyl-p-phenylenediamine or diphenylamine, or organic sulfur compounds such as tetraalkyluranium disulfide or dithiobenzoyl disulfide, etc. can be used as inhibitors.

[0170] [Polymerization Step]

[0171] In a dispersion containing poorly water-soluble inorganic particles and polymerizable monomer composition particles, the polymerizable monomer in the polymerizable monomer composition particles is polymerized (suspension polymerization) to produce toner particles. It is preferred to add a water-soluble metal salt in the second half of the polymerization step to suppress cracking. This can be added during the distillation step or after the distillation step is completed.

[0172] [Distillation Steps]

[0173] In order to remove volatile impurities such as unreacted polymerizable monomers and by-products, the polymerization reaction solution containing the particles obtained by the polymerization step can be distilled after the polymerization is completed to distill off a portion of the dispersion. The distillation step can be carried out under normal pressure (101325Pa) or reduced pressure (in the range of 0.5kPa to 0.95MPa).

[0174] [Maintaining step (alkali treatment step)]

[0175] In order to crosslink the toner particle surface after adding the water-soluble metal salt, it is preferred to carry out a maintenance step of maintaining the pH in the range of 7.5 to 10.0. This alkali treatment step may be carried out in the latter half of the polymerization or during or after the distillation.

[0176] [Washing, Filtration and Drying Steps]

[0177] In order to remove the dispersion stabilizer attached to the surface of the polymer particles, the dispersion liquid containing the toner particles obtained from the distillation step or the like may also be treated with an acid or an alkali. In this case, the polymer particles such as the toner particles are separated from the liquid phase by a conventional solid-liquid separation method, but in order to completely remove the acid or alkali and the dispersion stabilizer component dissolved therein, water is added again to wash the polymer particles. After this washing step is repeated several times to perform thorough washing, toner particles are obtained by further solid-liquid separation. The obtained toner particles may then be dried by a known drying method as required.

[0178] [External addition steps]

[0179] The toner particles can be used as a toner as they are. Preferably, an external additive is attached to the surface of the toner particles to impart various properties to the toner. The toner preferably contains the toner particles and the external additive.

[0180] In consideration of durability when the external additive is added to toner particles, the particle diameter of the external additive is preferably 1 / 10 or less of the average particle diameter of toner particles before the external additive is added.

[0181] Examples of external additives include metal oxides such as aluminum oxide, titanium oxide, strontium titanate, cerium oxide, magnesium oxide, chromium oxide, tin oxide, and zinc oxide; nitrides such as silicon nitride; carbides such as silicon carbide; inorganic metal salts such as calcium sulfate, barium sulfate, and calcium carbonate; fatty acid metal salts such as zinc stearate and calcium stearate; and carbon black and silicon dioxide. Among them, silicon dioxide is preferred.

[0182] The content of the external additive is preferably in the range of 0.01 to 10 parts by mass, or more preferably in the range of 0.05 to 5 parts by mass, relative to 100 parts by mass of the toner particles. A single external additive or a combination of multiple external additives may be used. From the viewpoint of charge stability, the surface of these external additives is preferably subjected to a hydrophobic treatment.

[0183] Examples of the hydrophobic treatment agent include silane coupling agents such as methyltrimethoxysilane, methyltriethoxysilane, isobutyltrimethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, trimethylmethoxysilane, hexamethylenedisilazane, and the like.

[0184] Toner particles

[0185] The toner particles (toner) can be applied to an image forming method using a known one-component developing system and a two-component developing system.

[0186] The toner particles (toner) can be used in any system. For example, it can be applied to an image forming method using a known one-component developing system and a two-component developing system, such as a toner for a high-speed system, a toner for an oil-free fixing system, a toner for a detergent-free system, and a toner for a developing system in which a carrier deteriorated for a long time in a developing device is successively recovered and a fresh carrier is supplied.

[0187] Next, the measuring method used in the present invention will be described.

[0188] <Measurement of Dynamic Viscoelasticity of Toner>

[0189] Ares rotating plate rheometer (manufactured by TA Instruments) was used as a measuring apparatus.

[0190] For the measurement sample, 0.1 g of the toner was press-molded into a disk having a diameter of 7.9 mm and a thickness of 2.0±0.3 mm using a tablet press machine at 25° C. The press molding was performed under the conditions of 15 MPa and 60 seconds.

[0191] The sample was mounted on parallel plates, the temperature was raised from room temperature (25°C) to 120°C within 15 minutes to adjust the shape of the sample, and then cooled to the measurement start temperature for measuring viscoelasticity, and the measurement was started. The sample was set so that the initial normal force was 0. In addition, as described below, in subsequent measurements, the influence of the normal force can be offset by setting "Automatic Tensile Adjustment" to "On".

[0192] The measurement was performed under the following conditions.

[0193] (1) Use a parallel plate with a diameter of 7.9 mm.

[0194] (2) The frequency is set to 1.0 Hz.

[0195] (3) The initial value of applied strain (Strain) was set to 0.1%.

[0196] (4) The temperature was increased at a rate of 2.0°C / min between 30°C and 200°C. The measurement was performed under the following automatic adjustment mode settings: The measurement was performed in the automatic strain adjustment mode (Auto Strain).

[0197] (5) The maximum applied strain is set to 20.0%

[0198] (6) The maximum allowable torque is set to 200.0 g·cm, and the minimum allowable torque is set to 0.2 g·cm.

[0199] (7) The strain adjustment is set to 20.0% of the current strain and the measurement is performed in the automatic tension adjustment mode (Auto Tension).

[0200] (8) Automatic stretching direction is set to compression

[0201] (9) The initial static force was set to 10.0 g and the automatic stretch sensitivity was set to 40.0 g.

[0202] (10) The automatic stretching operation condition is that the sample modulus is 1.0×10 3 (Pa) or above.

[0203] The storage elastic modulus at 70° C. is determined by the above measurement.

[0204] <Measurement of Surface Viscoelasticity of Toner (Toner Particles)>

[0205] The measurement of the surface storage elastic modulus of the toner or toner particles by the nanoindentation method is performed using TI-950 System Triboindenter (manufactured by Hysitron).

[0206] For the measurement sample, toner or toner particles (hereinafter referred to as toner) were attached to the tip of a Johnson cotton swab under an environment of 25° C., and 0.1 mg of the toner was spread on a 1 cm×1 cm silicon wafer.

[0207] The sample was mounted on a sample stage, and measurement was started under nanoindentation conditions at room temperature (25° C.) using a Bosch diamond indenter (TI-0039, angle 142.3°, manufactured by Hysitron).

[0208] It is important to set the focus of the measurement sample before starting the measurement so that the measurement can be performed under uniform focusing conditions.

[0209] Use the microscope to focus the measurement sample on the software. At this time, focus the objective lens at 5x, 20x, and 50x magnifications in sequence. Then, adjust the objective lens to 50x.

[0210] Next, the measurement space and load force are calibrated using a dedicated Al plate. The position of the indenter tip and the focus position of the microscope camera are also configured, and the Z axis of the indenter is aligned.

[0211] The indenter tip with attached toner is then moved over the silicon wafer and the microscope is focused on the toner to be measured.

[0212] After these calibrations, measurements were performed under the following conditions.

[0213] Under the condition of 30μN indenter load, load was applied between 0μN and 30μN at a rate of 0.5μN / s. Then vibration was applied in sequence with frequency and time of 3.0Hz and 3 seconds, 30Hz and 5 seconds, 150Hz and 15 seconds, 301.5Hz and 40 seconds, and nano viscoelasticity was measured. With the change of frequency, 1 second of stabilization time was provided between each frequency. The number of data graphs was set to 200 points at 100pts / sec, and the average value was calculated.

[0214] The measurement was started, and the horizontal axis was calculated as the frequency (Hz), and the vertical axis was calculated as the storage elastic modulus (GPa) and the loss modulus (GPa).

[0215] Thirty toner particles are measured in this manner, and the average value is used.

[0216] Always clean the indenter (X and Y axis rods) every time you measure 1 particle.

[0217] When the load condition is 150 μN, the measurement is performed in the same manner as when the load condition is 30 μN, except that the load is applied between 0 μN and 150 μN at a rate of 0.5 μN / s.

[0218] (Separation of toner particles from toner)

[0219] When toner particles are used as a sample, toner particles obtained by removing an external additive from a toner by the following method are used.

[0220] Specific methods of removing the external additive from the toner include, for example, the following methods.

[0221] (1) 5 g of the toner to which the external additive is added is placed in a sample bottle, and 200 ml of methanol is added. A few drops of a surfactant are added as needed. "Contaminon N" (a 10 mass % aqueous solution of a neutral detergent for cleaning precision measuring instruments at pH 7, comprising a nonionic surfactant, an anionic surfactant and an organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) can be used as a surfactant.

[0222] (2) The sample was dispersed for 5 minutes using an ultrasonic cleaner to separate the external additives.

[0223] (3) The external additives are separated from the toner particles by suction filtration using a 10 μm membrane filter.

[0224] (4) The above steps (2) and (3) are repeated three times.

[0225] Through these operations, toner particles from which external additives have been removed can be obtained.

[0226] <Measurement of Surface Metal Content of Toner Particles>

[0227] The metal elements on the toner particle surfaces are measured using TOF-SIMS (TRIVAC-IV, manufactured by ULVAC-PHI, Inc.) The analysis conditions are as follows.

[0228]

[0229]

[0230] Total P(M) of the peak intensities of Mg, Al, Ca and Fe:

[0231] P(M)=P(Mg)+P(Al)+P(Ca)+P(Fe)

[0232] Calculation of the peak intensity P(C) of C (carbon): The total peak counts of mass numbers 11.75 to 12.25 were taken as the peak intensity P(C) according to ULVAC-PHI, Inc. standard software (Win Cadense).

[0233] Calculate P(M) / P(C): Calculate P(M) / P(C) using P(M) and P(C) calculated as shown above.

[0234] <Determination of Acid Value and pKa of Polar Resins>

[0235] The acid value of the polar resin is the number of mg of potassium hydroxide required to neutralize the acid contained in 1 g of the sample. The acid value of the polar resin is measured in accordance with JIS K 0070-1992, specifically, according to the following procedure.

[0236] First, titration is performed using a 0.1 mol / L potassium hydroxide ethanol solution (manufactured by Kishida Chemical Co., Ltd.) The coefficient of the potassium hydroxide ethanol solution can be determined using a potentiometric titrator (AT-510 (trade name) potentiometric titrator, manufactured by Kyoto Electronics Manufacturing Co., Ltd.).

[0237] Specifically, 100 ml of 0.100 mol / l hydrochloric acid was placed in a 250 ml high beaker and titrated with the previous potassium hydroxide ethanol solution to determine the amount of potassium hydroxide ethanol solution required for neutralization. 0.100 mol / l hydrochloric acid was prepared according to JIS K8001-1998.

[0238] The measurement conditions for the acid value measurement are as follows.

[0239]

[0240] Titration parameters

[0241]

[0242] Main test

[0243] 0.100 g of the sample (polar resin) was accurately weighed into a 250 ml high beaker, 150 ml of a toluene / ethanol (3:1) mixed solution was added, and the sample was dissolved within 1 hour. The sample was titrated with a potassium hydroxide ethanol solution using the above-mentioned potentiometric titrator.

[0244] Blank test

[0245] Titration was performed by the same operation, but without using a sample (ie, using only a toluene / ethanol (3:1) mixed solution).

[0246] Enter the results into the formula to calculate the acid value (Av) of the polar resin:

[0247] Av=[(CB)×f×5.61] / S

[0248] (In the formula, Av is the acid value (mg KOH / g), B is the amount of potassium hydroxide ethanol solution added in the blank test (ml), C is the amount of potassium hydroxide ethanol solution added in the main test (ml), f is the coefficient of potassium hydroxide ethanol solution, and S is the mass of the sample (polar resin) (g).

[0249] Since the pKa is the same value as the pH of half volume of a 0.1 mol / l potassium hydroxide ethanol solution required to reach the neutralization point, the pH value at half volume is read from the titration curve.

[0250] <Measurement of Glass Transition Temperature (Tg) of Polar Resin>

[0251] The Tg of the polar resin is measured using a differential scanning calorimeter (DSC measurement unit).

[0252] Using a Q1000 differential scanning calorimeter (manufactured by TA Instruments), the measurement was performed as follows according to ASTM D3418-82. 3 mg of the measurement sample (polar resin) was accurately weighed and placed in an aluminum pan, and an empty aluminum pan was used as a reference. The equilibrium was maintained at 20° C. for 5 minutes, and then the measurement was performed at a heating rate of 10° C. / min in the measurement range of 20° C. to 180° C. The glass transition temperature was determined by the midpoint method.

[0253] <Determination of polymer conversion rate of polymerizable monomer>

[0254] The polymer conversion rate of the polymerizable monomer in the toner is determined by gas chromatography (GC) as follows.

[0255] 2.55 mg of DMF (dimethylformamide) was added to 100 ml of acetone to prepare a solvent containing an internal standard. 0.2 g of the polymer slurry was then accurately weighed and made into a solution with 10 ml of the above solvent. It was treated in an ultrasonic oscillator for 30 minutes and then left to stand for 1 hour. It was then filtered with a 0.5 μm membrane filter and 4 μl of the filtrate was analyzed by gas chromatography.

[0256] A calibration curve was prepared in advance, and the mass ratio / area ratio of the polymerizable vinyl monomer to the internal standard DMF was determined. The amount of unreacted polymerizable monomer was calculated from the obtained chromatogram and used to determine the polymer conversion rate.

[0257] The measurement unit and measurement conditions are as follows.

[0258] GC: Shimadzu Corporation GC-14A

[0259] Column: J&W Scientific DB-WAX (249μm×0.25μm×30m)

[0260] Carrier gas: N2 Furnace: (1) maintain at 70°C for 2 minutes, (2) increase the temperature to 220°C at a rate of 5°C / min

[0261] Inlet: 200℃

[0262] Split ratio: 1:20

[0263] Detector: 200℃(FID)

[0264] Example

[0265] The following is a detailed description of the embodiments of the present invention. The present invention is not limited to these embodiments. Unless otherwise specified, the parts in the embodiments and comparative examples are parts by mass.

[0266] <Manufacturing of Polar Resins>

[0267] (Production Example of Polyester Resin 1)

[0268] The monomers in the amounts shown in Table 1 were placed in a reaction tank equipped with a nitrogen introduction tube, a dehydration tube, a stirrer and a thermocouple, and 1.5 parts of dibutyltin oxide as a catalyst was added relative to 100 parts of the total monomers. Then, in a nitrogen atmosphere, the temperature was rapidly raised to 180° C. under normal pressure, and then raised at a rate of 10° C. / hour between 180° C. and 210° C. to distill off water and perform polycondensation.

[0269] Once the temperature reached 210°C, the reaction tank was depressurized to 5 kPa or less, and polycondensation was performed under the conditions of 210°C and 5 kPa to obtain polyester resin 1. In this process, the polymerization time was adjusted so that the conversion rate of the obtained polyester resin A1 was the value (126°C) shown in Table 2. The physical properties of polyester resin 1 are shown in Table 2.

[0270] The composition of polyester resin 1 was analyzed by 1 The specific measurement method is as follows.

[0271]

[0272] 50 mg of a sample was placed in a sample tube having an inner diameter of 5 mm, deuterated chloroform (CDCl3) was added as a solvent, and the mixture was dissolved in a thermostatic bath at 40° C. to prepare a measurement sample. The measurement was performed under the above-mentioned conditions using the measurement sample.

[0273] <Production of Polyester Resins 2 to 4>

[0274] Polyester resins 2 to 4 were produced by the same operation as that of polyester resin 1, except that the input amounts of the acid component and the alcohol component were changed as shown in Table 1. The reaction time was also appropriately adjusted to adjust physical properties such as the acid value of each polyester resin.

[0275] [Table 1]

[0276]

[0277] Tg is in ° C. The abbreviations in the table are as follows.

[0278] TPA: Terephthalic acid

[0279] IPA: Isophthalic acid

[0280] TMA: trimellitic acid

[0281] BPA-PO: Bisphenol A propylene oxide 2 molar adduct

[0282] BPA-EO: Bisphenol A ethylene oxide 2 molar adduct

[0283] (Production Example of Polar Group-Containing Styrene Resin 1)

[0284] 300 parts of xylene (boiling point: 144° C.) were added to a pressurizable and depressurizable flask and stirred, and the system was thoroughly purged with nitrogen and heated to reflux.

[0285] A mixture of the following components was added under reflux, and polymerized at a polymerization temperature of 175° C. and a pressure of 0.100 MPa during the reaction for 5 minutes.

[0286]

[0287] Then, a solvent removal step was performed under reduced pressure for 3 hours to remove xylene, and the product was pulverized to obtain a polar group-containing styrene resin 1.

[0288] (Production Example of Polar Group-Containing Styrene Resin 2)

[0289] The polar group-containing styrene resin 2 was obtained by changing the monomer composition ratio in the production example of the polar group-containing styrene resin 1 shown in Table 2.

[0290] [Table 2]

[0291]

[0292] Tg is in ° C. The abbreviations in the table are as follows.

[0293] St:Styrene

[0294] MMA: Methyl Methacrylate

[0295] 2HEMA: 2-Hydroxyethyl Methacrylate

[0296] MAA: Methacrylic acid

[0297] (Production Example of Polar Group-Containing Styrene Resin 3)

[0298] 200 parts of xylene were placed in a reactor equipped with a stirrer, a condenser, a thermometer and a nitrogen inlet tube, and refluxed in a nitrogen stream. The following monomers were mixed, dripped into the reactor under stirring, and maintained for 10 hours.

[0299] · 6.0 parts of 2-acrylamido-2-methylpropanesulfonic acid

[0300] ·Styrene 72.0 parts

[0301] · 2-Ethylhexyl acrylate 18.0 parts

[0302] Then, the solvent was distilled off, and the product was dried under reduced pressure at 40° C. to obtain a polar group-containing styrene resin 3.

[0303] (Production Example of Polar Group-Containing Styrene Resin 4)

[0304] Step 1 Intermediate synthesis of polymerizable monomer M

[0305] 100 g of 2,5-dihydroxybenzoic acid and 1441 g of 80% sulfuric acid were heated and mixed at 50° C. 144 g of tert-butyl alcohol was added to the dispersion, followed by stirring at 50° C. for 30 minutes. Thereafter, an operation of adding 144 g of tert-butyl alcohol and stirring for 30 minutes was performed three times.

[0306] The reaction solution was cooled to room temperature and slowly injected into 1 kg of ice water. The precipitate was filtered out, washed with water, and then washed with hexane. The precipitate was dissolved in 200 mL of methanol and reprecipitated with 3.6 L of water. After filtration, it was dried at 80° C. to obtain 74.9 g of a salicylic acid intermediate represented by the following structural formula (2).

[0307]

[0308] Step 2 Synthesis of polymerizable monomer M

[0309] 25.0 g of the obtained salicylic acid intermediate was dissolved in 150 ml of methanol, 36.9 g of potassium carbonate was added, and the mixture was heated to 65° C. A mixture of 18.7 g of 4-(chloromethyl)styrene and 100 ml of methanol was added dropwise to the reaction solution, which was then reacted at 65° C. for 3 hours. The reaction solution was cooled and filtered, and the filtrate was concentrated to obtain a crude product. The crude product was dispersed in 1.5 L of pH 2 water and extracted by adding ethyl acetate.

[0310] This was then washed with water and dried with magnesium sulfate, and ethyl acetate was distilled off under reduced pressure to obtain a precipitate. The precipitate was washed with hexane and purified by recrystallization with toluene and ethyl acetate to obtain 20.1 g of a polymerizable monomer M represented by the following structural formula (3).

[0311]

[0312] Step 3 Synthesis of styrene resin 4 containing polar groups

[0313] 9.2 g of polymerizable monomer M represented by structural formula (3) and 60.8 g of styrene were dissolved in 42.0 ml of DMF, stirred for 1 hour under nitrogen bubbling, and then heated to 110° C. A mixture of 45 ml of toluene and 1.8 g of tert-butyl peroxyisopropyl monocarbonate (NOF Corp., product name Perbutyl I) as an initiator was added dropwise to the reaction solution. The mixture was then allowed to react further at 100° C. for 5 hours. The mixture was then cooled and dropped into 1 L of methanol to obtain a precipitate.

[0314] The obtained precipitate was dissolved in 120 ml of THF and added dropwise to 1.80 L of methanol to precipitate a white precipitate, which was then filtered and dried under reduced pressure at 100° C. to obtain a polar group-containing styrene resin 4.

[0315] <Manufacturing of Toner 1>

[0316] (Preparation of dispersion liquid)

[0317] 100.0 parts of ion exchange water, 2.0 parts of sodium phosphate and 0.9 parts of 10% by mass hydrochloric acid were added to a granulation tank to prepare an aqueous sodium phosphate solution, which was then heated to 50° C. An aqueous calcium chloride solution in which 1.2 parts of calcium chloride hexahydrate were dissolved in 8.2 parts of ion exchange water was then added to the granulation tank, and the mixture was then stirred at 25 m / s for 30 minutes using a TK homomixer (product name, TokushuKika Kogyo Co., Ltd.). In this way, a dispersion (aqueous dispersion) containing (fine particles of) calcium phosphate as poorly water-soluble inorganic fine particles was obtained (dispersion preparation step).

[0318] (Preparation of Pigment Dispersion Composition)

[0319] ·Polymerizable monomer (styrene) 39.0 parts

[0320] Colorant (CI Pigment Blue 15:3) 7.0 parts

[0321] These materials were introduced into an attritor (Nippon Coke & Engineering Co., Ltd.) and stirred at 25° C. and 200 rpm for 180 minutes with zirconia beads having a diameter of 1.25 mm to prepare a pigment dispersion composition.

[0322] (Preparation of Colorant-Containing Composition)

[0323] The following materials were introduced into the same container, and mixed and dispersed with a TK homomixer (product name, Tokushu Kika Kogyo Co., Ltd.) at a peripheral speed of 20 m / s.

[0324]

[0325] This was further heated to 60°C, 10.0 parts of behenyl behenate was added as a releasing agent, and the mixture was dispersed and mixed for 30 minutes to prepare a colorant-containing composition.

[0326] (Preparation of polymerizable monomer composition particles)

[0327] The above-mentioned colorant-containing composition is added to the dispersion containing calcium phosphate fine particles, and stirred with a TK homomixer (product name, Tokushu Kika Kogyo Co., Ltd.) at a peripheral speed of 30 m / s in a nitrogen atmosphere at a temperature of 60° C. 9.0 parts of a polymerization initiator tert-butyl peroxypivalate (NOF Corp., product name “Perbutyl PV”, molecular weight 174.2, 10-hour half-life temperature 58° C.) is added thereto to prepare a dispersion containing particles of a polymerizable monomer composition (granulation step).

[0328] (Preparation of Toner Particles 1)

[0329] The dispersion of the above-mentioned polymerizable monomer composition particles is transferred to another tank, stirred with a paddle stirring blade as the temperature rises to 70°C, and reacted for 1 hour. Here, the conversion rate of the polymerizable monomer is 45.0%. It is further reacted for 4 hours, and then reacted for 4 hours after the temperature rises to 80°C (heating step). The pH of the polymer slurry at this time is 5.0. Aluminum chloride is then added to a concentration of 2.0mmol / L at 80°C (addition step). The conversion rate of the polymerizable monomer at this time is 100.0%. It is then further reacted for 2 hours under the same conditions. In this way, a polymer reaction solution (polymer slurry) containing toner particles 1 is obtained (polymerization step).

[0330] After the polymerization step was completed, water vapor (steam) at 120° C. was supplied to the polymer slurry at a flow rate of 5 kg / hr. After the water vapor supply started, distillation was started once the temperature reached 98° C., and distillation was performed for 8 hours (distillation step).

[0331] After the distillation step, a 7.0 mass % sodium carbonate aqueous solution was added to adjust the pH of the polymer slurry to 8.5, and the slurry was maintained at 80° C. for 30 minutes (maintaining step (alkali treatment step)).

[0332] It was cooled, hydrochloric acid was added to pH 1.4, and the slurry was stirred for 2 hours to dissolve the sparingly water-soluble inorganic fine particles on the toner particle surfaces. The toner particle dispersion was filtered out, washed with water, and dried at 40° C. for 48 hours to obtain toner particles 1 (washing / filtering / drying step).

[0333] Toner 1 having inorganic fine powder on the surface is prepared as follows (external addition step).

[0334] 1.5 parts of the inorganic fine powder and 100.0 parts of the toner particles 1 were mixed with a Henschel mixer (Mitsui Miike Chemical Engineering Machinery Co., Ltd.) at 3,000 rpm (min -1 ) for 15 minutes, thereby obtaining Toner 1 having inorganic fine powder on the surface.

[0335] The inorganic fine powder is hydrophobic silica fine particles (the average particle size of the primary particles is 10 nm, the BET specific surface area is 170 m 2 / g) which had been treated with dimethyl silicone oil (20% by mass) to improve fluidity and triboelectrically charged to the same polarity (negative polarity) as Toner Particles 1 before addition of the inorganic fine particles.

[0336] Table 3 shows various conditions for the polar resin and the addition of the water-soluble metal salt used for producing the toner particles 1.

[0337] <Manufacturing of Toner 2>

[0338] Toner Particles 2 were obtained by the same manufacturing method as for Toner 1 except for the changes shown in Table 3.

[0339] Furthermore, in addition to 1.5 parts of hydrophobic silica fine particles (primary particle number average particle size: 10 nm, BET specific surface area: 170 m 2 / g) was replaced with 1.0 part of hydrophobic silica fine particles and 0.5 part of strontium titanate fine particles (strontium titanate fine particles hydrophobized with 4.5 mass % isobutyltrimethoxysilane and 4.5 mass % trifluoropropyltrimethoxysilane, with a primary particle number average particle size of 35 nm and a BET specific surface area of ​​60 m 2 Toner 2 was obtained by the same external addition procedure as that of Toner 1, except for the combination of 1:1 and 2:1.

[0340] <Manufacturing of Toners 3 to 21>

[0341] Toner particles 3 to 21 were obtained by the same production method as for Toner 1 except for having the changes shown in Table 3. Toner particles 3 to 21 were also obtained by the same external addition procedure as for Toner 1.

[0342] The pH of the slurry before the water-soluble metal salt adding step was controlled by adding a 10 mass % sodium carbonate aqueous solution.

[0343] [Table 3]

[0344]

[0345] <Manufacturing of Toner 22>

[0346] (Manufacture of polyester resin 5)

[0347] 20 parts of propylene oxide-modified bisphenol A (2 mol adduct), 80 parts of propylene oxide-modified bisphenol A (3 mol adduct), 80 parts of terephthalic acid, 20 parts of isophthalic acid and 0.50 parts of tetrabutoxytitanium were placed in a reaction apparatus equipped with a stirrer, a thermometer and an outflow cooler, and an esterification reaction was carried out at 190° C. Then 1 part of trimellitic anhydride (TMA) was added, and as the pressure in the system gradually decreased, the temperature was raised to 220° C., and a polycondensation reaction was carried out at 150 Pa, thereby obtaining polyester resin 5. The acid value of polyester resin 5 was 12 mg KOH / g, and Tg was 57° C.

[0348] (Preparation of Binder Resin Particle Dispersion Liquid 1)

[0349] ·Polyester resin 5 200.0 parts

[0350] 500.0 parts of ion exchange water

[0351] These materials were placed in a stainless steel container, heated to melt at 95° C. in a warm bath, and thoroughly stirred at 7800 rpm with a homogenizer (IKA Ultra-Turrax T50), while adding 0.1 mol / L sodium bicarbonate thereto to increase the pH to more than 7.0. Then, a mixed solution of 3 parts of sodium dodecylbenzenesulfonate and 297 parts of ion-exchanged water was slowly dropped to emulsify and disperse the mixture and obtain a binder resin particle dispersion 1.

[0352] When the particle size distribution of the binder resin particle dispersion 1 was measured using a particle size measuring device (Horiba LA-920), the number average particle size of the binder resin particles contained therein was 0.25 μm, and no coarse particles larger than 1 μm were observed.

[0353] (Preparation of Wax Particle Dispersion)

[0354] 500.0 parts of ion exchange water

[0355] Wax (behenyl behenate, melting point 72.1°C) 250.0 parts

[0356] These materials were placed in a stainless steel container, heated to melt at 95°C in a warm bath, and thoroughly stirred at 7800 rpm with a homogenizer (IKA Ultra-Turrax T50), while adding 0.1 mol / L sodium bicarbonate to increase the pH to greater than 7.0. Then, a mixed solution of 5 parts of sodium dodecylbenzene sulfonate and 245 parts of ion-exchanged water was slowly dripped in to emulsify and disperse the mixture.

[0357] When the particle size distribution of the wax particles contained in the wax particle dispersion was measured using a particle size measuring device (Horiba LA-920), the number average particle size of the wax particles contained was 0.35 μm, and no coarse particles larger than 1 μm were observed.

[0358] (Preparation of Colorant Particle Dispersion Liquid)

[0359] ·CI Pigment Blue 15:3 100.0 parts

[0360] 5.0 parts of sodium dodecylbenzene sulfonate

[0361] ·400.0 parts of ion exchange water

[0362] These materials were mixed and then dispersed with a hand grinder. When the particle size distribution of the colorant particles contained in the colorant particle dispersion was measured using a particle size measuring device (Horiba LA-920), the number average particle size of the colorant particles contained was 0.2 μm, and no coarse particles larger than 1 μm were observed.

[0363] Preparation of Toner Particles 22

[0364]

[0365] Binder resin particle dispersion 1, wax particle dispersion and sodium dodecylbenzene sulfonate were loaded into a reactor (1-L flask, fixed wing with baffles) and uniformly mixed. At the same time, the colorant particle dispersion was uniformly mixed and stirred in a 500 ml beaker, and was gradually added to the reactor to obtain a mixed dispersion. The resulting mixed dispersion was stirred, and an aqueous solution of magnesium sulfate in an amount of 1.0 part of solid content was added dropwise to form aggregated particles.

[0366] After the dropwise addition was completed, the system was purged with nitrogen and maintained at 50° C. for 1 hour and at 55° C. for 1 hour. Aluminum chloride was added at 55° C. to a concentration of 2.0 mmol / L.

[0367] The temperature was then raised, a 7.0 mass % sodium carbonate aqueous solution was added at 80°C to a pH of 8.5, and the system was maintained at 80°C for 30 minutes. The temperature was then lowered to 63°C and maintained for 3 hours to form molten particles. The reaction was carried out under a nitrogen atmosphere. After a predetermined time, the temperature was lowered to room temperature at a cooling rate of 0.5°C / min.

[0368] After cooling, the reaction product was subjected to solid-liquid separation in a 10L pressure filter at a pressure of 0.4MPa to obtain a toner filter cake. Ion exchange water was then added until the pressure filter was full, and the filter cake was washed at a pressure of 0.4MPa. The same washing was then repeated for a total of 3 times. The toner filter cake was dispersed in 1000 parts of a 50:50 mixed solvent of methanol / water containing 0.15 parts of a dissolved nonionic surfactant to obtain a surface-treated toner particle dispersion.

[0369] The toner particle dispersion was injected into a pressure filter, and 5 L of ion exchange water was added, followed by solid-liquid separation at a pressure of 0.4 MPa and fluidized bed drying at 45° C., thereby obtaining Toner Particles 1.

[0370] (External addition steps)

[0371] Toner particles 22 are obtained in the same manner as the external addition step of toner particles 1 except that toner particles 22 are used.

[0372] <Manufacturing of Toner 23>

[0373] (Preparation of Binder Resin Particle Dispersion Liquid 2)

[0374] 78.0 parts of styrene, 20.7 parts of butyl acrylate, 1.3 parts of acrylic acid as a carboxyl group-donating monomer, and 3.2 parts of n-lauryl mercaptan were mixed and dissolved. An aqueous solution of 1.5 parts of Neogen RK (DKS Co., Ltd.) dissolved in 150 parts of ion-exchanged water was added to the solution and dispersed.

[0375] Then, the mixture was slowly stirred for 10 minutes, and an aqueous solution of 0.3 parts of potassium persulfate in 10 parts of ion exchange water was added. After nitrogen purging, emulsion polymerization was carried out at 70° C. for 6 hours. After the polymerization, the reaction solution was cooled to room temperature, and ion exchange water was added to obtain a binder resin particle dispersion 2 having a solid concentration of 12.5% ​​by mass and a volume-based median particle size of 0.2 μm.

[0376] (Preparation of Toner Particles 23)

[0377]

[0378] The binder resin particle dispersion 2, the wax particle dispersion and sodium dodecylbenzene sulfonate were loaded into a reactor (1-L flask, fixed wing with baffles) and uniformly mixed. At the same time, the colorant particle dispersion was uniformly mixed and stirred in a 500 ml beaker, and was gradually added to the reactor to obtain a mixed dispersion. The resulting mixed dispersion was stirred, and an aqueous solution of magnesium sulfate in an amount of 1.0 part of solid components was added dropwise to form aggregated particles.

[0379] After the dropwise addition was completed, the system was purged with nitrogen and maintained at 50° C. for 1 hour and at 55° C. for 1 hour. Aluminum chloride was added at 55° C. to a concentration of 2.0 mmol / L.

[0380] The temperature was then raised, a 7.0 mass % sodium carbonate aqueous solution was added at 80°C to a pH of 8.5, and the system was maintained at 80°C for 30 minutes. The temperature was then lowered to 63°C and maintained for 3 hours to form molten particles. The reaction was carried out under a nitrogen atmosphere. After a predetermined time, the temperature was lowered to room temperature at a cooling rate of 0.5°C / min.

[0381] After cooling, the reaction product was subjected to solid-liquid separation in a 10L pressure filter at a pressure of 0.4MPa to obtain a toner filter cake. Ion exchange water was then added until the pressure filter was full, and the filter cake was washed at a pressure of 0.4MPa. The same washing was then repeated for a total of 3 times. The toner filter cake was dispersed in 1000 parts of a 50:50 mixed solvent of methanol / water containing 0.15 parts of a dissolved nonionic surfactant to obtain a surface-treated toner particle dispersion.

[0382] The toner particle dispersion was injected into a pressure filter, and 5 L of ion exchange water was added. The dispersion was then subjected to solid-liquid separation at a pressure of 0.4 MPa, and then fluidized bed drying was performed at 45° C., thereby obtaining toner particles 23 .

[0383] (External addition steps)

[0384] Toner 23 is obtained by the same external addition procedure as that for Toner Particles 1 except that Toner Particles 23 are used.

[0385] <Manufacturing of Toner 24>

[0386] (Preparation of Toner Particles 24)

[0387]

[0388] These components were dispersed in a ball mill for 10 hours, and the resulting dispersion was added to 2000 parts of ion exchange water containing 3.5% by mass of tricalcium phosphate, and granulated at 15000 rpm for 10 minutes in a TK homomixer high-speed mixing device. It was then maintained at 75° C. in a water bath for 4 hours with a three-in-one motor under stirring at 150 rpm to remove the solvent.

[0389] Aluminum chloride was then added to a concentration of 2.0 mmol / L, and the temperature was raised to 80°C. A 7.0 mass % sodium carbonate aqueous solution was added at 80°C until the pH was 8.5, and the temperature was maintained at 80°C for 30 minutes. The slurry was cooled, hydrochloric acid was added to make the pH of the cooled slurry 1.4, and the slurry was stirred for 1 hour to dissolve the calcium phosphate salt. It was then washed with 10 times the volume of water of the slurry, filtered and dried, and then classified to adjust the particle size and obtain toner particles 24.

[0390] (External addition steps)

[0391] Toner 24 is obtained by the same external addition procedure as that for Toner Particles 1 except that Toner Particles 24 are used.

[0392] <Manufacturing of Toner 25>

[0393] When preparing a colorant-containing composition for producing Toner 1, the following materials were replaced, and aluminum chloride was not added in the polymerization step.

[0394]

[0395] Furthermore, after the distillation step was completed, cooling was performed without alkali treatment. Toner 25 was obtained in the same manner as Toner 1 except for these steps.

[0396] <Manufacturing of Toner 26>

[0397] Aluminum chloride was not added in the polymerization step of the production of Toner 1. In addition, after the distillation step was completed, cooling was performed without alkali treatment. Toner 26 was obtained in the same manner as Toner 1 except for these steps.

[0398] <Manufacturing of Toner 27>

[0399] When preparing a colorant-containing composition for producing Toner 1, the following materials were replaced, and aluminum chloride was not added in the polymerization step.

[0400]

[0401] Furthermore, after the distillation step was completed, cooling was performed without alkali treatment. Toner 27 was obtained in the same manner as Toner 1 except for these steps.

[0402] <Manufacturing of Toner 28>

[0403] When toner particles 22 were prepared in the manufacturing example of toner 22, the temperature was maintained at 50°C for 1 hour and at 55°C for 1 hour after aggregate particles were formed, and aluminum chloride was not added. Toner 28 was obtained in the same manner as toner 22 except for these steps.

[0404] <Manufacturing of Toner 29>

[0405] (Manufacture of polyester resin 6)

[0406] 20 parts of propylene oxide-modified bisphenol A (2 mol adduct), 80 parts of propylene oxide-modified bisphenol A (3 mol adduct), 20 parts of terephthalic acid, 80 parts of fumaric acid and 0.50 parts of tetrabutoxytitanium were placed in a reaction unit equipped with a stirrer, a thermometer and an outflow cooler, and an esterification reaction was carried out at 190°C.

[0407] Then, 1 part of trimellitic anhydride (TMA) was added, the temperature was raised to 220°C as the system was gradually depressurized, and polycondensation reaction was carried out at 150 Pa to obtain polyester resin 6. The acid value of polyester resin 6 was 11 mg KOH / g, and Tg was 62°C.

[0408] (Preparation of Binder Resin Particle Dispersion Liquid 3)

[0409] ·Polyester resin 6 200.0 parts

[0410] 500.0 parts of ion exchange water

[0411] These materials were placed in a stainless steel container, heated to melt at 95° C. in a warm bath, and thoroughly stirred at 7800 rpm with a homogenizer (IKA Ultra-Turrax T50), while adding 0.1 mol / L sodium bicarbonate to increase the pH to more than 7.0. Then, a mixed solution of 3.5 parts of sodium dodecylbenzenesulfonate and 297 parts of ion-exchanged water was slowly dropped to emulsify and disperse the mixture, thereby obtaining a binder resin particle dispersion 3.

[0412] When the particle size distribution of the binder resin particle dispersion 3 was measured using a particle size measuring device (Horiba LA-920), the number average particle size of the binder resin particles contained therein was 0.19 μm, and no coarse particles larger than 1 μm were observed.

[0413] (Preparation of Toner Particles 29)

[0414]

[0415]

[0416] Binder resin particle dispersion 1, binder resin particle dispersion 3, wax particle dispersion and sodium dodecylbenzene sulfonate are loaded into a reactor (1-L flask, fixed wing with baffles) and uniformly mixed. At the same time, the colorant particle dispersion is uniformly mixed and stirred in a 500ml beaker, and is gradually added to the reactor to obtain a mixed dispersion. The resulting mixed dispersion is stirred, and a magnesium sulfate aqueous solution having an amount of 1.0 part is added dropwise to form aggregated particles. Once the particle diameter reaches 5.0 μm, a mixture of 100 parts of binder resin particle dispersion 1 and 100 parts of binder resin particle dispersion 3 is added and maintained for 60 minutes.

[0417] The temperature was then raised to 85° C., 3 parts of sodium hydroxyiminodisuccinate were added, and an aqueous sodium hydroxide solution was added until the pH was 9.0. A solution of 15 parts of potassium persulfate (KPS) dissolved in 150 parts of ion exchange water was then added, and the mixture was maintained at 85° C. for 30 minutes. After a predetermined time, the mixture was cooled to room temperature at a rate of 0.5° C. per minute.

[0418] After cooling, the reaction product was subjected to solid-liquid separation in a 10L pressure filter at a pressure of 0.4MPa to obtain a toner filter cake. Ion exchange water was then added until the pressure filter was full, and the filter cake was washed at a pressure of 0.4MPa. The toner filter cake was then washed in the same manner for a total of 3 times. The toner filter cake was dispersed in 1000 parts of a 50:50 mixed solvent of methanol / water containing 0.15 parts of a dissolved nonionic surfactant to obtain a surface-treated toner particle dispersion.

[0419] The toner particle dispersion was injected into a pressure filter, and 5 L of ion exchange water was added, followed by solid-liquid separation at a pressure of 0.4 MPa, and then fluidized bed drying was performed at 45° C., thereby obtaining toner particles 29 .

[0420] (External addition steps)

[0421] Toner 29 is obtained by the same external addition procedure as that for Toner Particles 1 except that Toner Particles 29 is used.

[0422] <Manufacturing of Toner 30>

[0423] (Manufacture of polyester resin 7)

[0424] 20 parts of propylene oxide-modified bisphenol A (2 mol adduct), 70 parts of propylene oxide-modified bisphenol A (3 mol adduct), 20 parts of ethylene glycol, 80 parts of terephthalic acid, 20 parts of isophthalic acid and 0.50 parts of tetrabutoxytitanium were placed in a reaction unit equipped with a stirrer, a thermometer and an effluent cooler, and an esterification reaction was carried out at 190°C.

[0425] Then, 1 part of trimellitic anhydride (TMA) was added, and as the internal pressure of the system gradually decreased, the temperature was raised to 220°C, and polycondensation reaction was carried out at 150 Pa to obtain polyester resin 7. The acid value of polyester resin 7 was 11 mg KOH / g, and Tg was 39°C.

[0426] (Preparation of Binder Resin Particle Dispersion Liquid 4)

[0427] ·Polyester resin 7 200.0 parts

[0428] 500.0 parts of ion exchange water

[0429] These materials were placed in a stainless steel container, heated and melted at 95° C. in a warm bath, and thoroughly stirred at 7800 rpm with a homogenizer (IKA Ultra-Turrax T50), while adding 0.1 mol / L sodium bicarbonate to increase the pH to more than 7.0. Then, a mixed solution of 3.5 parts of sodium dodecylbenzene sulfonate and 297 parts of ion-exchanged water was slowly dropped to emulsify and disperse the mixture and obtain a binder resin particle dispersion 4.

[0430] When the particle size distribution of the binder resin particle dispersion 4 was measured using a particle size measuring device (LA-920, manufactured by Horiba, Ltd.), the number average particle size of the contained binder resin particles was 0.17 μm, and no coarse particles larger than 1 μm were observed.

[0431] (Preparation of Toner Particles 30)

[0432] Toner particles 30 are obtained in the same manner as the toner particles 29 except that the binder resin particle dispersion 4 is used instead of the binder resin particle dispersion 3 .

[0433] (External addition steps)

[0434] Toner 30 is obtained by the same external addition procedure as that for Toner Particles 1 except that Toner Particles 30 is used.

[0435] <Manufacturing of Toner 31>

[0436] (Preparation of Binder Resin Particle Dispersion Liquid 5)

[0437] Mix and dissolve 73.0 parts of styrene, 15.7 parts of methyl acrylate, 3.1 parts of methacrylic acid as a carboxyl group-supplying monomer, and 1.5 parts of n-lauryl mercaptan. Add an aqueous solution of 1.5 parts of Neogen RK (DKS Co., Ltd.) dissolved in 150 parts of ion exchange water to the solution and disperse it. Then stir it slowly for 10 minutes, while adding an aqueous solution of 0.15 parts of potassium persulfate in 10 parts of ion exchange water. After nitrogen purging, emulsion polymerization is carried out at 70°C for 6 hours. After the polymerization is completed, the reaction solution is cooled to room temperature and ion exchange water is added to obtain a binder resin particle dispersion 5 having a solid concentration of 12.5% ​​by mass and a volume-based median particle size of 0.15 μm.

[0438] (Preparation of Toner Particles 31)

[0439]

[0440] Binder resin particle dispersion 5, wax particle dispersion and sodium dodecylbenzene sulfonate were loaded into a reactor (1-L flask, fixed wing with baffles) and uniformly mixed. At the same time, the colorant particle dispersion was uniformly mixed and stirred in a 500ml beaker, and was gradually added to the reactor to obtain a mixed dispersion. The resulting mixed dispersion was stirred, and an aqueous solution of magnesium sulfate was added dropwise in an amount of 1.0 part of solid component to form aggregated particles. Once the particle size reached 5.0 μm, 25 parts of binder resin particle dispersion 5 were added and maintained for 60 minutes.

[0441] After the dropwise addition was completed, the system was purged with nitrogen and maintained at 50°C for 1 hour and at 55°C for 1 hour. The temperature was then lowered to 63°C and maintained for 3 hours to form molten particles. The reaction was carried out under a nitrogen atmosphere. After a predetermined time, the temperature was lowered to room temperature at a cooling rate of 0.5°C / min.

[0442] After cooling, the reaction product was subjected to solid-liquid separation in a 10L pressure filter at a pressure of 0.4MPa to obtain a toner filter cake. Ion exchange water was then added until the pressure filter was full, and the filter cake was washed at a pressure of 0.4MPa. The toner filter cake was washed again in the same manner for a total of 3 times. The toner filter cake was dispersed in 1000 parts of a 50:50 mixed solvent of methanol / water containing 0.15 parts of a dissolved nonionic surfactant to obtain a surface-treated toner particle dispersion.

[0443] The toner particle dispersion was injected into a pressure filter, and 5 L of ion exchange water was added, followed by solid-liquid separation at a pressure of 0.4 MPa and fluidized bed drying at 45° C., thereby obtaining toner particles 31 .

[0444] (External addition steps)

[0445] Toner 31 is obtained by the same external addition procedure as that for Toner Particles 1 except that Toner Particles 31 is used.

[0446] <Image Evaluation>

[0447] A modified LBP712Ci (Canon Inc.) was used as the evaluation apparatus. The process speed of the main unit was modified to 270 mm / sec. Necessary adjustments were then made to allow image formation under these conditions. The toner was taken out from the black box and then filled with 200 g of toner 1.

[0448] <Durable fogging evaluation in high temperature and high humidity environment>

[0449] The fogging was evaluated in a high temperature and high humidity environment (30°C, 80% RH). Xerox 4200 paper (Xerox Co., 75 g / m 2 ) as evaluation paper.

[0450] Intermittent endurance printing was performed by printing 20,000 sheets of a letter E image with a printing rate of 1% at an output rate of 2 sheets per 4 seconds under a high temperature and high humidity environment.

[0451] A solid white image is then output, and Ds is taken as the worst value of the reflection density of the white background, Dr is taken as the average reflection density of the transfer material before image formation, and Dr–Ds is taken as the fogging value.

[0452] The reflection density of the white background was measured using a reflection densitometer (Reflectometer Model TC-6DS, Tokyo Denshoku Co., Ltd.) using an amber filter.

[0453] A lower value indicates a better fogging level. The evaluation criteria are as follows.

[0454] (Evaluation Criteria)

[0455] A: less than 0.5%

[0456] B: 0.5% or more and less than 1.5%

[0457] C: 1.5% or more and less than 3.0%

[0458] D: 3.0% or more

[0459] <Evaluation of Development Streaks>

[0460] Development streaks are vertical streaks of about 0.5 mm caused by toner chipping or breaking, and this image defect is easily observed when a full-page halftone image is output.

[0461] The development streaks were evaluated in a low-temperature and low-humidity environment (15° C., 10% RH).

[0462] Use Xerox 4200 paper (Xerox Co., 75g / m 2 ) as evaluation paper.

[0463] Intermittent endurance printing was performed by printing 20,000 sheets of a letter E image with a printing rate of 1% at an output rate of 2 sheets per 4 seconds under a low temperature and low humidity environment. Then a full-page halftone image was output and the presence or absence of streaks was observed. The results are shown in Table 4.

[0464] (Evaluation Criteria)

[0465] A: No streaks

[0466] B: Development streaks occur at 1 to 3 locations

[0467] C: Development streaks occur at 4 to 6 locations

[0468] D: Development streaks occur at 7 or more locations, or development streaks with a width of 0.5 mm or more occur

[0469] <Low Temperature Fixability>

[0470] Using an LBP712Ci color laser printer (Canon Inc.) from which the fixing unit had been removed, the toner was removed from the black cartridge and then filled with the toner for evaluation. Color laser copy paper (Canon Inc., 80 g / m 2 ) was used as a recording medium. Next, a new toner was used and 0.20 mg / cm 2An unfixed image of 2.0 cm in length and 15.0 cm in width was formed with a toner loading of 1.5 %. Then, the removed fixing unit was remodeled so that the fixing temperature and the process speed could be adjusted, and used to perform a fixing test of the unfixed image.

[0471] Under normal temperature and humidity environment (23°C, 60% RH), the process speed was first set to 270 mm / s, the fixing line pressure was set to 27.4 kgf, and the set temperature was increased from an initial temperature of 110°C in increments of 5°C to fix the unfixed image at each temperature.

[0472] The evaluation criteria for low temperature fixability are as follows. The low temperature fixation starting point is when the temperature is 4.9 kPa (50 g / cm 2 The lowest temperature at which the image density after abrasion decreases to less than 10.0% when the image surface is rubbed 5 times with Silbon paper (Dusper K-3) at a speed of 0.2 m / sec under a load of 10.0%. When the image cannot be fixed correctly, the image density reduction rate tends to increase. The image density is measured using a 500 series spectrodensitometer (X-Rite Inc.).

[0473] (Evaluation Criteria)

[0474] A: Low temperature fixing starting point is below 120℃

[0475] B: Low temperature fixing starting point is 125℃ or 130℃

[0476] C: Low temperature fixing starting point is 135℃ or 140℃

[0477] D: Low temperature fixing starting point is above 145℃

[0478] [Examples 1 to 24]

[0479] In Examples 1 to 24, the above-mentioned image evaluation, toner storage elastic modulus measurement, surface viscoelasticity measurement, and surface metal content measurement were performed on Toners 1 to 24. The results are shown in Table 4.

[0480] [Comparative Examples 1 to 6]

[0481] In Comparative Examples 1 to 6, the above-mentioned image evaluation, toner storage elastic modulus measurement, surface viscoelasticity measurement, and surface metal content measurement were performed on Toners 25 to 30. The results are shown in Table 4.

[0482] [Table 4]

[0483]

[0484] In the table, “CE” means “Comparative Example”, and “Storage elastic modulus MPa” means the storage elastic modulus at 70° C. in the dynamic viscoelasticity measurement of the toner.

[0485] While the present disclosure has been described with reference to exemplary embodiments, it is to be understood that the present disclosure is not limited to the disclosed exemplary embodiments.The scope of the following claims is to be accorded the broadest interpretation so as to encompass all such modifications and equivalent structures and functions.

Claims

1. A method for producing a toner, It is characterized in that The toner includes toner particles including a binder resin, wherein in a dynamic viscoelasticity measurement of the toner, a storage elastic modulus of the toner at 70° C. is 0.10 MPa to 3.00 MPa, and In nanoindentation measurement of the toner, the surface storage elastic modulus of the toner at 25° C. and 150 μN load is 2.80 GPa to 4.50 GPa, and The manufacturing method includes a granulation step in which particles of a polymerizable monomer composition containing a polar resin A and a polymerizable monomer for producing a binder resin are formed in an aqueous medium, This is followed by a polymerization step in which the polymerizable monomer contained in the particles of the polymerizable monomer composition is polymerized to produce resin particles, wherein The polymerization step includes adding a water-soluble metal salt to an aqueous medium, and maintaining the aqueous medium containing the obtained resin particles at a pH of 7.5 to 10.

0. The polar resin A has an acid group, and the acid dissociation constant pKa of the polar resin A is 7.5 or less, and The water-soluble metal salt is a salt of a divalent or higher valent metal. 2 . The method for producing a toner according to claim 1 , wherein the adding step is performed at a polymer conversion rate of 50% to 100% of the polymerizable monomer. 3 . The method for producing a toner according to claim 1 , wherein the adding step is performed at a polymer conversion rate of 75% to 100% of the polymerizable monomer. 4 . The method for producing a toner according to claim 1 , wherein the water-soluble metal salt is a salt of at least one metal selected from the group consisting of Al, Ca, Mg, and Fe. 5 . The method for producing a toner according to claim 1 , wherein the polymerizable monomer is at least one selected from the group consisting of styrene-based monomers and (meth)acrylate monomers. 6 . The method for producing a toner according to claim 1 , wherein a concentration of the water-soluble metal salt in the aqueous medium in the adding step is 0.2 mmol / L to 40.0 mmol / L. 7 . The method for producing a toner according to claim 1 , wherein when the water-soluble metal salt is added to the aqueous medium, the pH of the aqueous medium is 4.0 to 9.

0. 8 . The method for producing a toner according to claim 1 , wherein in a nanoindentation measurement of the toner, a surface storage elastic modulus of the toner at 25° C. and a load of 30 μN is 3.50 GPa to 8.00 GPa. 9 . The method for producing a toner according to claim 1 , wherein in a nanoindentation measurement of the toner, a surface loss modulus of the toner at 25° C. and a load of 30 μN is 0.25 GPa to 1.20 GPa.

10. The method for producing a toner according to claim 1 or 2, wherein the sum of the peak intensities of Mg, Al, Ca and Fe of the toner particles obtained by time-of-flight secondary ion mass spectrometry (TOF-SIMS) is taken as P(M), and the peak intensity of C of the toner particles obtained by TOF-SIMS is taken as P(C), satisfying the following formula (1): 2.0≤P(M) / P(C)≤30.0 (1).

11. The method for producing a toner according to claim 1 or 2, wherein the toner particles include a polar resin A on the surface thereof, The polar resin A has an acid value, The acid value is 2 mg KOH / g to 30 mg KOH / g, and The polar resin A is cross-linked by a polyvalent metal. 12 . The method for producing a toner according to claim 11 , wherein the polyvalent metal is at least one selected from the group consisting of Al, Ca, Mg, and Fe. 13 . The method for producing a toner according to claim 11 , wherein the polar resin A contains a polyester resin. 14 . The method for producing a toner according to claim 1 , wherein the toner contains toner particles and an external additive.