transformer
By setting a specific array of point-shaped laser irradiation marks on the Fe-based amorphous alloy thin strip, the problem of high no-load loss in the transformer in the prior art is solved, and low iron loss and High-efficiency transformer design.
Patent Information
- Application Number
- CN202010959323.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-09-14
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2040-09-14
AI Technical Summary
The prior art is difficult to effectively reduce the no-load loss of the transformer, especially when using a thin strip of Fe-based amorphous alloy, the laser scribe method fails to reach the minimum iron loss value, and deformation in the surface form leads to a lower duty factor. Influences the characteristics of the iron core.
A plurality of point-shaped laser irradiation marks orthogonal along the casting direction are arranged on at least one side of the Fe-based amorphous alloy thin strip, and the row intervals and hole intervals of the point-shaped laser irradiation marks are adjusted to ensure the number density of the laser irradiation marks. Between 0.05/mm2 and 0.50/mm2, a low iron loss core and winding are formed.
Low iron loss at 50Hz and 60Hz frequencies is achieved, reducing no-load loss, and improving the energy consumption efficiency and CO2 emission efficiency of the transformer.
Smart Images

Figure CN112582148B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a transformer including an iron core formed of a Fe-based amorphous alloy thin strip and a winding wound around the iron core. Background Art
[0002] Transformers have various structures from small to large, and are used in all scenes of the living environment. In addition, due to the large amount of use, it also becomes a factor of large power loss, and there is a demand to always suppress the loss in the transformer. Therefore, in various countries around the world, standards for suppressing this loss are formulated. As representative standards, there are: Japan's high-level standards JIS C 4304: 2013 and JIS C 4306: 2013, the US DOE standard US Department of Energy 10CFR Part 431.196, EU standard Commotions Regulation (EU) No. 548 / 2014, China's national standard GB 20052-2013, Indian standard IS 1180 (Part 1): 2018, etc., and the allowable loss or energy efficiency is tightened every time the regular revision work is carried out. Therefore, high-efficiency transformers with forms corresponding to these standards and less loss are gradually becoming popular.
[0003] The transformer is mainly composed of an iron core and a winding. Generally, the iron core is mostly made of a grain-oriented electromagnetic steel sheet. However, as a material with lower loss than the grain-oriented electromagnetic steel sheet, there is also an Fe-based amorphous alloy strip, and an iron core using this Fe-based amorphous alloy strip is also used.
[0004] The losses of transformers can be roughly divided into: no-load loss (iron loss) generated in the core and always generating a certain amount regardless of the load current; and load loss (copper loss) generated in the winding and generated in proportion to the square of the load current. Research on reducing each loss is repeatedly carried out, and the loss is improved, but further reduction of loss is required.
[0005] In order to reduce the no-load loss of the transformer, some methods have been proposed.
[0006] In the patent publication No. 2017-54896, in order to obtain an efficient iron core with reduced no-load loss, a wound iron core is adopted. The wound iron core uses an amorphous material in which the joint structure on the inner circumference is set to an overlapping joint, the joint structure on the outer circumference is set to a step joint, and the proportion of the iron core in the overlapping structure arranged on the inner circumference is set to 32 to 62%.
[0007] Japanese Patent Gazette No. 2008-71982 provides a transformer comprising an iron core formed into a ring shape by forming a plurality of layers of amorphous alloy strips and a winding for excitation, wherein an insulating film is formed on the surface of the amorphous alloy strips forming the iron core, and an insulating film is formed on the surface of the amorphous alloy strips, thereby suppressing the increase of eddy current loss and reducing the no-load loss of the transformer.
[0008] Japanese Patent Publication No. 2005-72160 provides a three-phase five-column wound core transformer, wherein a structure is set to use both amorphous alloy thin strips and electromagnetic steel plates for the magnetic material of the wound core. Specifically, the three-phase five-column wound core transformer has the following structure, the wound core that is linked to only one outer winding is set to the electromagnetic steel plate, and the central wound core that is linked to two windings is set to the amorphous alloy thin strip. As a result, it is not necessary to press the reinforcing material of the winding, and the structure is made compact, thereby providing an amorphous alloy thin strip wound core and a three-phase five-column wound core transformer that reduce the workload and material costs of the assembly work, and reduce the no-load loss compared to the case where the magnetic material is only the electromagnetic steel plate.
[0009] In addition, efforts are being made to reduce the loss in Fe-based amorphous alloy thin strips used as the material of the iron core.
[0010] For example, as a method for reducing the abnormal eddy current loss of Fe-based amorphous alloy thin strips, there are known methods: a method of mechanically scraping the surface of the Fe-based amorphous alloy thin strips; a laser scribing method in which the surface of the Fe-based amorphous alloy thin strips is irradiated with laser to cause local melting and rapid solidification to subdivide the magnetic domains, etc.
[0011] As a laser scribing method, for example, the following method is disclosed in the Special Publication No. 3-32886, which irradiates a pulsed laser along the width direction of an amorphous alloy strip to locally and instantly melt the surface of the amorphous alloy strip, and then forms the rapidly solidified and amorphized holes into a point array, thereby subdividing the magnetic domains.
[0012] Japanese Patent Application Laid-Open No. 61-258404 discloses irradiating a thin ribbon with laser light while scanning the thin ribbon in its width direction while the surface temperature of the thin ribbon is 300° C. or higher.
[0013] It is disclosed in the Gazette of Special Fair No. 2-53935 that, by locally heating a thin strip, strip-shaped crystallized regions are formed which are arranged in rows at intervals of 2 to 100 mm along the long side direction of the thin strip and at an angle θ of less than 30° with the width direction of the thin strip, and at the same time, the ratio d / D of the average depth d of the above-mentioned regions in the thickness direction of the plate to the thickness D of the thin strip is greater than 0.1, and the proportion of these regions in the thin strip is less than 8 volume %.
[0014] Japanese Patent Application No. 61-29103 discloses that in order to fully utilize the performance of amorphous alloys with a plate thickness (40 to 80 μm) greater than that of conventional materials (20 to 30 μm), the irradiation beam diameter is reduced to The following pulsed laser. Specifically, the frequency is 400 Hz and the beam diameter is An amorphous thin ribbon having a width of 50 mm and a thickness of 65 μm was irradiated with YAG laser under the conditions of an output of 5 W, a beam scanning speed of 10 cm / seg, and a spot array interval of 5 mm.
[0015] Prior art literature
[0016] Patent Literature
[0017] Patent Document 1: Japanese Patent Application Publication No. 2017-54896
[0018] Patent Document 2: Japanese Patent Application Publication No. 2008-71982
[0019] Patent Document 3: Japanese Patent Application Publication No. 2005-72160
[0020] Patent Document 4: Japanese Patent Publication No. 3-32886
[0021] Patent Document 5: Japanese Patent Application Laid-Open No. 61-258404
[0022] Patent Document 6: Japanese Patent Publication No. 2-53935
[0023] Patent Document 7: Japanese Patent Application Laid-Open No. 61-29103 Summary of the invention
[0024] Problems to be solved by the invention
[0025] As mentioned above, in terms of transformer losses, no-load losses generated in the core and load losses generated in the windings constitute the main losses. In order to reduce the no-load loss of the transformer, it is considered to use Fe-based amorphous alloy thin strips with smaller iron losses. In particular, in the case of distribution transformers, as described in Takagi, Yamamoto, and Yamaji: "Evaluation of amorphous transformers using a pole-mounted transformer load pattern model", P885-892, Electronic Theory B, Vol. 128, No. 6, 2008, or Final Report, LOT2: Distribution and power transformers Tasks 1-72010 / ETE / R / 106, January 2011, it is known that the average equivalent load factor equivalent to the effective value of the load factor throughout the year is as low as 15%, and transformers using Fe-based amorphous alloy thin strips with smaller no-load losses are extremely effective from the perspective of energy saving and CO2 emission reduction.
[0026] As described in Table 1 and Table 2 of JIS C 2534:2017 (corresponding to IEC standard IEC60404-8-11), Fe-based amorphous alloy strips used as transformer cores are roughly divided into two types: ordinary materials and high magnetic flux density materials. There are 16 types based on the maximum value of iron loss and the minimum value of duty cycle. Among the materials with the smallest iron loss, the maximum value of iron loss at a frequency of 50 Hz and a magnetic flux density of 1.3 T is 0.08 W / kg, and the maximum value of iron loss at a frequency of 60 Hz and a magnetic flux density of 1.3 T is 0.11 W / kg. However, in order to obtain a more efficient transformer, Fe-based amorphous alloy strips with a smaller iron loss than this need to be used for the core.
[0027] In order to reduce the iron loss of amorphous alloy thin strips, the above-mentioned laser scribing method was attempted, but its iron loss did not reach the minimum iron loss values recorded in Tables 1 and 2 of the above-mentioned JIS C 2534:2017 (for example, refer to the respective embodiments of Special Publication No. 3-32886, Special Publication No. 61-258404, Special Publication No. 2-53935, and Special Publication No. 61-29103).
[0028] In addition, sometimes the surface form of the amorphous alloy strip is greatly deformed due to laser irradiation. In the case of large deformation, the space factor of the amorphous alloy strip in the case of winding or stacking the amorphous alloy strip to form the iron core becomes low. Such large deformation of the surface form of the amorphous alloy strip is not a preferred form in the iron core characteristics. In addition, when the crystallized region is formed by locally heating the strip, the desired characteristics cannot be obtained due to crystallization.
[0029] The present disclosure aims to provide a transformer having an iron core formed of an Fe-based amorphous alloy thin strip having an iron loss value smaller than the minimum iron loss value described in Table 1 and Table 2 of JIS C2534:2017, wherein the no-load loss thereof is reduced.
[0030] Solutions to Solve Problems
[0031] Specific means for solving the above-mentioned problems include the following aspects.
[0032] <1> A transformer, wherein:
[0033] A plurality of point-array laser irradiation marks are provided on at least one surface of the Fe-based amorphous alloy thin strip along a direction perpendicular to the casting direction of the Fe-based amorphous alloy thin strip.
[0034] When the center line spacing of the central parts of the width direction orthogonal to the casting direction between the adjacent point-array laser irradiation marks among the plurality of point-array laser irradiation marks is set as the row spacing, and the center point spacing of each laser irradiation mark constituting the point-array laser irradiation marks is set as the hole spacing, the hole spacing is 0.10 mm to 0.50 mm, the row spacing is set as d1 (mm), and the hole spacing is set as d2 (mm), and the number density D of the laser irradiation marks is set as D = (1 / d1) × (1 / d2), the number density D of the laser irradiation marks is 0.05 pieces / mm 2 ~0.50pcs / mm 2 , comprising an iron core composed of an Fe-based amorphous alloy thin strip having an iron loss of less than 0.150 W / kg at a frequency of 60 Hz and a magnetic flux density of 1.45 T in a single plate using the Fe-based amorphous alloy thin strip, and a winding wound on the iron core.
[0035] <2> The transformer according to <1>, wherein the transformer is a single-phase transformer, and the no-load loss per unit weight of the core is less than 0.15 W / kg at 50 Hz, or less than 0.19 W / kg at 60 Hz.
[0036] <3> The transformer according to <1>, wherein the transformer is a three-phase transformer, and the no-load loss per unit weight of the core is less than 0.19 W / kg at 50 Hz, or less than 0.24 W / kg at 60 Hz.
[0037] <4> The transformer according to any one of <1> to <3>, wherein a rated capacity of the transformer is 10 kVA or more.
[0038] <5> The transformer according to any one of <1> to <4>, wherein the row interval d1 is 10 mm to 60 mm.
[0039] <6> A transformer according to any one of <1> to <5>, wherein the ratio of the length of the point-array laser irradiation marks in the width direction to the overall length of the Fe-based amorphous alloy strip in the width direction is in the range of 10% to 50% in the direction from the center in the width direction to both ends in the width direction.
[0040] <7> The transformer according to any one of <1> to <6>, wherein the Fe-based amorphous alloy thin strip has a thickness of 18 μm to 35 μm.
[0041] <8> A transformer according to any one of <1> to <7>, wherein the Fe-based amorphous thin strip is composed of Fe, Si, B, and impurities, and when the total content of Fe, Si, and B is set to 100 atomic %, the content of Fe is greater than 78 atomic %, the content of B is greater than 10 atomic %, and the total content of B and Si is 17 atomic % to 22 atomic %.
[0042] <9> A transformer according to any one of <1> to <8>, wherein the Fe-based amorphous alloy thin strip has a free solidification surface and a roll surface, and the maximum cross-sectional height Rt of the free solidification surface excluding the point-array laser irradiation mark portion is less than 3.0 μm.
[0043] <10> A transformer according to any one of <1> to <9>, wherein the point-array laser irradiation marks are formed in at least six regions in the center of the width direction, excluding two regions at both ends of eight regions obtained by dividing the width direction of the Fe-based amorphous alloy thin strip into eight equal parts.
[0044] Effects of the Invention
[0045] According to one embodiment of the present disclosure, a transformer having reduced no-load loss is provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 This is a schematic diagram showing an example of a transformer according to the present embodiment.
[0047] Figure 2 This is a schematic diagram showing another example of the transformer according to the present embodiment.
[0048] Figure 3 This is a schematic diagram showing still another example of the transformer according to the present embodiment.
[0049] Figure 4 It is a schematic diagram showing an example of the Fe-based amorphous alloy thin strip according to the present embodiment.
[0050] Figure 5 This is a graph showing the relationship between the magnetic flux density and the iron loss when the hole interval is changed.
[0051] Figure 6 This is a graph showing the relationship between the magnetic flux density and the exciting power when the hole interval is changed. DETAILED DESCRIPTION
[0052] In this specification, the numerical range represented by "to" refers to a range that includes the numerical values recorded before and after "to" as the lower limit and upper limit. In this specification, in the numerical range recorded step by step, the upper limit or lower limit recorded in one numerical range can also be replaced by the upper limit or lower limit of other numerical ranges recorded step by step. In addition, in the numerical range recorded in this specification, the upper limit or lower limit of the numerical range can also be replaced by the value shown in the embodiment.
[0053] In this specification, the expression "process" refers not only to independent processes, but also to processes that cannot be clearly distinguished from other processes, provided that the intended purpose of the process is achieved. In this specification, the Fe-based amorphous alloy ribbon refers to a ribbon composed of an Fe-based amorphous alloy.
[0054] In this specification, Fe-based amorphous alloy refers to an amorphous alloy with Fe (iron) as the main component. Here, the main component refers to the component with the highest content ratio (mass %). The following describes the embodiments related to the present disclosure. In addition, the present disclosure is not limited to the embodiments described below, and can be appropriately changed within the scope of the technical concept.
[0055] The embodiment of the present disclosure provides a transformer, wherein:
[0056] At least one side of the Fe-based amorphous alloy thin strip has a plurality of point-array laser irradiation marks arranged in a direction perpendicular to the casting direction of the above-mentioned Fe-based amorphous alloy thin strip, when the center line spacing of the central parts of the width direction perpendicular to the above-mentioned casting direction between the point-array laser irradiation marks adjacent to each other in the plurality of the above-mentioned point-array laser irradiation marks is set as the row spacing, and the center point spacing of each laser irradiation mark constituting the above-mentioned point-array laser irradiation marks is set as the hole spacing, the above-mentioned hole spacing is 0.10mm~0.50mm, the above-mentioned row spacing is set as d1 (mm), and the above-mentioned hole spacing is set as d2 (mm), and when the number density D of the above-mentioned laser irradiation marks is set as D=(1 / d1)×(1 / d2), the number density D of the above-mentioned laser irradiation marks is 0.05 pieces / mm 2 ~0.50pcs / mm 2 ,
[0057] The invention comprises an iron core made of an Fe-based amorphous alloy thin strip having an iron loss of 0.150 W / kg or less at a frequency of 60 Hz and a magnetic flux density of 1.45 T in a single plate using the Fe-based amorphous alloy thin strip, and a winding wound around the iron core.
[0058] In addition, the Fe-based amorphous alloy thin strip also reduces the iron loss in a single plate at a frequency of 50 Hz and a magnetic flux density of 1.45 T. The Fe-based amorphous alloy thin strip preferably has an iron loss of 0.120 W / kg or less in a single plate at a frequency of 50 Hz and a magnetic flux density of 1.45 T.
[0059] The Fe-based amorphous alloy thin strip preferably has an iron loss of 0.08 W / kg or less at a frequency of 50 Hz and a magnetic flux density of 1.3 T, or an iron loss of 0.11 W / kg or less at a frequency of 60 Hz and a magnetic flux density of 1.3 T.
[0060] In addition, the iron core of the present embodiment preferably uses a circumferential iron core in which multiple Fe-based amorphous alloy thin strips are bent and overlapped and wound. In addition, it is necessary to use a plurality of such circumferential iron cores in combination. In addition, as the iron core, a stacked iron core formed by stacking multiple Fe-based amorphous alloy thin strips may be used, or a rolled iron core formed by winding Fe-based amorphous alloy thin strips may be used.
[0061] In addition, the transformer of the present embodiment is preferably a single-phase transformer or a three-phase transformer, and the rated capacity of the transformer is preferably 10 kVA or more.
[0062] In the case of a single-phase transformer, the no-load loss per unit weight of the core is preferably 0.15 W / kg or less at 50 Hz, or 0.19 W / kg or less at 60 Hz.
[0063] In the case of a three-phase transformer, the no-load loss per unit weight of the core is preferably 0.19 W / kg or less at 50 Hz, or 0.24 W / kg or less at 60 Hz.
[0064] Example 1
[0065] Figure 1 An example of the structure of the core and winding of the transformer according to this embodiment is shown in FIG. Figure 1The transformer shown includes a circumferential core 1 in which a plurality of Fe-based amorphous alloy ribbons are bent and stacked and wound, and a winding 2 wound on the core. The winding 2 is installed in the core in an open state before the cores are stacked. The core 1 of the first embodiment is composed of a single circumferential core (single-phase two-leg wound core). The main characteristics and weight of a single-phase 50 Hz, 10 kVA rated capacity oil-filled transformer (hereinafter, Example 1) according to JIS C 4304: 2013 of the present invention using the core 1 of this embodiment are shown in Table 1 by comparison with the prior art example 1. Here, the Fe-based amorphous alloy ribbon used in Example 1 has the above-mentioned characteristics, and therefore, according to the definition of "Five types of amorphous ribbons" in JIS C 2534: 2017, the core material is described as 25AMP06-88. The Fe-based amorphous alloy ribbon used in the prior art example 1 is 25AMP08-88. In addition, the characteristics of the following Examples 1 to 8 are numerical values obtained through simulation analysis.
[0066] The Fe-based amorphous alloy ribbon used in Example 1 has a thickness of 25 μm and a width of 142.2 mm. A dot-shaped laser irradiation mark is formed on the free solidification surface. The row spacing of the dot-shaped laser irradiation mark is 20 mm, the hole spacing is 0.20 mm, and the number density D of the laser irradiation mark is 0.25 / mm 2 The iron loss at a frequency of 50Hz and a magnetic flux density of 1.45T is 0.083W / kg, and the iron loss at a frequency of 60Hz and a magnetic flux density of 1.45T is 0.105W / kg.
[0067] In addition, the Fe-based amorphous alloy thin strip used in the existing example 1 has a thickness of 25 μm and a width of 142.2 mm, and no laser irradiation marks are formed. The iron loss at a frequency of 50 Hz and a magnetic flux density of 1.45 T is 0.130 W / kg, and the iron loss at a frequency of 60 Hz and a magnetic flux density of 1.45 T is 0.167 W / kg.
[0068] In Example 1 and Conventional Example 1, the number of stacked layers of the annular iron core 1 is 1875, and the weights thereof are shown in Table 1.
[0069] The primary winding of the transformer uses a copper wire with a diameter of 0.9 mm and is wound with 3143 turns. The secondary winding uses an aluminum 3.2 mm × 6.0 mm rectangular wire and is connected in parallel with a 100-turn winding.
[0070]
Table 1
[0071]
[0072]
[0073] As can be seen from Table 1, in Example 1, the no-load loss per unit weight of the core is 0.149 W / kg, which is about 25% lower than the no-load loss per unit weight of the core of Conventional Example 1 of 0.197 W / kg.
[0074] It can also be seen that, in accordance with this, the ratio of the conventional example 1 to the energy efficiency standard value defined in JIS C 4304:2013 is 0.73 (described in the "Energy Efficiency Ratio" of Table 1. The same applies hereinafter.), while in Example 1, it can be improved to 0.70, and the annual CO2 emission when the average equivalent load rate of the distribution transformer is set to 15% is also improved by about 15%. This is known from the fact that the "Annual CO2 Emission Ratio when the Load Rate is 15%" described in Table 1 is 0.85 (the same applies hereinafter).
[0075] Example 2
[0076] As Figure 1 The second embodiment of the transformer having the structure of the core and winding of the present embodiment shown, the main characteristics and weight of the single-phase 60 Hz, rated capacity 10 kVA oil-filled transformer (hereinafter, embodiment 2) of the present invention according to JIS C 4304:2013 are shown in Table 2 by comparison with conventional example 2.
[0077] The Fe-based amorphous alloy thin strip used in Example 2 is the same as that in Example 1, and the Fe-based amorphous alloy thin strip used in Conventional Example 2 is the same as that in Conventional Example 1.
[0078] In Example 2 and Conventional Example 2, the number of stacked layers of the annular iron core 1 is 1785, and the weights thereof are shown in Table 2.
[0079] The primary winding of the transformer uses a copper wire with a diameter of 0.9 mm and is wound with 2776 turns. The secondary winding uses an aluminum 2.6 mm × 6.0 mm rectangular wire and is connected in parallel with an 88-turn winding.
[0080]
Table 2
[0081]
[0082]
[0083] As can be seen from Table 2, in Example 2, the no-load loss per unit weight of the core is 0.189 W / kg, which is about 27% lower than the no-load loss per unit weight of the core of Conventional Example 2, which is 0.259 W / kg.
[0084] It can also be seen that, correspondingly, the ratio of the existing example 2 to the energy efficiency standard value defined in JIS C 4304:2013 is 0.72, while in Example 2 it can be improved to 0.68, and the annual CO2 emission of the distribution transformer when the average equivalent load factor is set to 15% is also improved by about 18%.
[0085] Example 3
[0086] As Figure 1 The third embodiment of the transformer having the structure of the core and winding of the present embodiment shown, the main characteristics and weight of the single-phase 50 Hz, rated capacity 30 kVA oil-filled transformer (hereinafter, Example 3) of the present invention according to JIS C 4304:2013 are shown in Table 3 by comparison with the conventional example 3.
[0087] The Fe-based amorphous alloy ribbon used in Example 3 has a thickness of 25 μm and a width of 213.4 mm. A dot-shaped laser irradiation mark is formed on the free solidification surface. The row spacing of the dot-shaped laser irradiation mark is 20 mm, the hole spacing is 0.20 mm, and the number density D of the laser irradiation mark is 0.25 / mm 2 The iron loss at a frequency of 50Hz and a magnetic flux density of 1.45T is 0.085W / kg, and the iron loss at a frequency of 60Hz and a magnetic flux density of 1.45T is 0.108W / kg.
[0088] In addition, the Fe-based amorphous alloy thin strip used in the existing example 3 has a thickness of 25 μm and a width of 213.4 mm, and no laser irradiation marks are formed. The iron loss at a frequency of 50 Hz and a magnetic flux density of 1.45 T is 0.132 W / kg, and the iron loss at a frequency of 60 Hz and a magnetic flux density of 1.45 T is 0.168 W / kg.
[0089] In Example 3 and Conventional Example 3, the number of stacked layers of the annular iron core 1 is 3015, and the weights thereof are shown in Table 3.
[0090] The primary winding of the transformer uses a copper wire with a diameter of 1.4 mm and is wound with 1509 turns. The secondary winding uses an aluminum 3.2 mm × 15 mm rectangular wire and is connected in parallel with a 44-turn winding.
[0091]
Table 3
[0092]
[0093]
[0094] According to Table 3, in Example 3, the no-load loss per unit weight of the core is 0.138 W / kg, which is about 30% lower than the no-load loss per unit weight of the core of Conventional Example 3, which is 0.197 W / kg.
[0095] It can also be seen that, with respect to the energy efficiency standard value defined in JIS C 4304:2013, the ratio of the existing example 3 is 0.72, while in contrast, it can be improved to 0.68 in the embodiment 3, and the annual CO2 emission of the distribution transformer when the average equivalent load rate is set to 15% is also improved by about 18%. In addition, the no-load loss per unit weight of the core of the above-mentioned embodiment 1 is 0.149W / kg, while in contrast, in the embodiment 3, it is improved by 0.138W / kg and 0.011W / kg. The reason is that due to the enlargement of the core, the ratio of the length of the curved portion to the magnetic path length of the core becomes smaller, and the no-load loss caused by the residual stress of the curved portion of the core is suppressed.
[0096] Example 4
[0097] As Figure 1 The fourth embodiment of the transformer having the structure of the core and winding of the present embodiment shown, the main characteristics and weight of the single-phase 60 Hz, rated capacity 30 kVA oil-filled transformer (hereinafter, embodiment 4) of the present invention according to JIS C 4304:2013 are shown in Table 4 by comparison with the conventional example 4.
[0098] The Fe-based amorphous alloy thin strip used in Example 4 is the same as that in Example 3, and the Fe-based amorphous alloy thin strip used in Conventional Example 4 is the same as that in Conventional Example 3.
[0099] In Example 4 and Conventional Example 4, the number of stacked layers of the annular iron core 1 is 2715, and the weights thereof are shown in Table 4.
[0100] The primary winding of the transformer uses a copper wire with a diameter of 1.3 mm and is wound with 1509 turns. The secondary winding uses an aluminum 4.0 mm × 13 mm rectangular wire and is connected in parallel with a 44-turn winding.
[0101]
Table 4
[0102]
[0103]
[0104] According to Table 4, in Example 4, the no-load loss per unit weight of the core is 0.180 W / kg, which is about 30% lower than the no-load loss per unit weight of the core of Conventional Example 4, which is 0.256 W / kg.
[0105] It can also be seen that, in accordance with the energy efficiency standard value defined in JIS C 4304:2013, the ratio of the conventional example 4 is 0.72, while in contrast, it can be improved to 0.67 in the embodiment 4, and the annual CO2 emission of the distribution transformer when the average equivalent load rate is set to 15% is also improved by about 19%. In addition, the no-load loss per unit weight of the core of the above-mentioned embodiment 2 is 0.189W / kg, while in contrast, it is improved by 0.180W / kg and 0.009W / kg in the embodiment 4. This is reduced due to the reasons explained in the above-mentioned embodiment 3.
[0106] Example 5
[0107] Figure 2 2 shows another example of the structure of the core and winding of the transformer according to the present embodiment. Figure 2 The transformer shown in the figure comprises: a three-phase three-leg wound core (a combination of three circumferential cores) in which a circumferential core 1 is formed by bending and overlapping a plurality of Fe-based amorphous alloy thin strips stacked, and three sets of windings 2 are wound around the core. The main characteristics and weight of a three-phase 50 Hz, 100 kVA rated capacity oil-filled transformer (hereinafter, Example 5) according to the present invention in accordance with JIS C 4304:2013 using the core of this embodiment are shown in Table 5 by comparison with the prior art example 5.
[0108] The Fe-based amorphous alloy thin strip used in Example 5 is the same as that in Example 3, and the Fe-based amorphous alloy thin strip used in Conventional Example 5 is the same as that in Conventional Example 3.
[0109] In Example 5 and Conventional Example 5, the number of stacked layers of the circumferential iron cores 1 is 3480, respectively. The weights thereof (the total weight of three circumferential iron cores) are shown in Table 5.
[0110] The primary winding of the transformer uses a copper wire with a diameter of 2.2 mm and is wound 653 turns in a star connection. The secondary winding uses an aluminum sheet of 0.4 mm × 247 mm and is set to a 36-turn winding in a delta connection.
[0111]
Table 5
[0112]
[0113]
[0114] According to Table 5, in Example 5, the no-load loss per unit weight of the core is 0.188 W / kg, which is about 30% lower than the no-load loss per unit weight of the core of Conventional Example 5, which is 0.269 W / kg.
[0115] It can also be seen that, corresponding to the energy efficiency standard value defined in JIS C 4304:2013, the existing example 5 is 0.78, while in Example 5 it can be improved to 0.73, and the annual CO2 emission of the distribution transformer when the average equivalent load factor is set to 15% is also improved by about 20%.
[0116] Example 6
[0117] As Figure 2 Another embodiment of the transformer having the structure of the core and winding of the present embodiment shown, the main characteristics and weight of the three-phase 60 Hz, rated capacity 100 kVA oil-filled transformer (hereinafter, Example 6) of the present invention according to JIS C 4304:2013 are shown in Table 6 by comparison with the existing Example 6.
[0118] The Fe-based amorphous alloy thin strip used in Example 6 is the same as that in Example 3, and the Fe-based amorphous alloy thin strip used in Conventional Example 6 is the same as that in Conventional Example 3. In Example 6 and Conventional Example 6, the number of stacked layers of the annular iron core 1 is 2895, and the weight thereof is shown in Table 6.
[0119] The primary winding and secondary winding of the transformer are the same as those of Example 5 and Existing Example 5.
[0120]
Table 6
[0121]
[0122]
[0123] According to Table 6, in Example 6, the no-load loss per unit weight of the core is 0.238 W / kg, which is about 30% lower than the no-load loss per unit weight of the core of Conventional Example 6 of 0.339 W / kg.
[0124] It can also be seen that, correspondingly, the existing example 6 has a ratio of 0.81 to the energy efficiency standard value defined in JIS C 4304:2013, while the example 6 can be improved to 0.77, and the annual CO2 emission of the distribution transformer when the average equivalent load factor is set to 15% is also improved by about 19%.
[0125] Example 7
[0126] As Figure 2 Another embodiment of the transformer having the structure of the core and winding of the present embodiment shown, the main characteristics and weight of the three-phase 50 Hz, rated capacity 500 kVA oil-filled transformer (hereinafter, Example 7 of the present invention) of the present invention according to JIS C 4304:2013 are shown in Table 7 by comparison with the existing Example 7.
[0127] The Fe-based amorphous alloy thin strip used in Example 7 is the same as that in Example 3, and the Fe-based amorphous alloy thin strip used in Conventional Example 7 is the same as that in Conventional Example 3.
[0128] In Example 7 and Conventional Example 7, the number of stacked layers of the annular iron core 1 is 5685 in Example 7 and 5955 in Conventional Example 7. The weights thereof (total of three annular iron cores) are shown in Table 7.
[0129] The primary winding of the embodiment 7 uses a 3.5 mm × 4.5 mm square copper wire, which is wound 399 turns in a star connection, and the secondary winding uses a 1.3 mm × 438 mm aluminum sheet, which is connected in a delta connection to form a winding with 22 turns. In addition, the primary winding of the conventional example 7 uses a 3.2 mm × 5.0 mm square copper wire, which is wound 381 turns in a star connection, and the secondary winding uses a 1.4 mm × 383 mm aluminum sheet, which is connected in a delta connection to form a winding with 21 turns.
[0130]
Table 7
[0131]
[0132]
[0133] According to Table 7, in Example 7, the no-load loss per unit weight of the core is 0.172 W / kg, which is about 30% lower than the no-load loss per unit weight of the core of Conventional Example 7, which is 0.246 W / kg.
[0134] It can also be seen that, in accordance with the energy efficiency standard value defined in JIS C 4304:2013, the ratio of the existing example 7 is 0.93, while in contrast, it can be improved to 0.90 in the embodiment 7, and the annual CO2 emission of the distribution transformer when the average equivalent load rate is set to 15% is also improved by about 16%. In addition, the no-load loss per unit weight of the core of the above-mentioned embodiment 5 is 0.188W / kg, while in contrast, it is improved by 0.172W / kg and 0.016W / kg in the embodiment 7. The reason for this is that due to the enlargement of the core, the ratio of the length of the curved portion to the magnetic path length of the core becomes smaller, which suppresses the increase in no-load loss caused by the residual stress of the curved portion of the core.
[0135] Example 8
[0136] Figure 3Another example of the structure of the iron core and winding of the transformer of this embodiment is shown in FIG. The transformer comprises: a three-phase five-leg wound iron core which is a combination of a circumferential iron core 1 in which a plurality of Fe-based amorphous alloy thin strips are bent and overlapped and wound, and three sets of windings 2 wound on the iron core. The main characteristics and weight of a three-phase 50 Hz oil-filled transformer (hereinafter, Example 8) of the present invention according to JIS C 4304:2013 using the iron core of this embodiment are shown in Table 8 by comparison with the conventional example 8.
[0137] The Fe-based amorphous alloy thin strip used in Example 8 is the same as that in Example 3, and the Fe-based amorphous alloy thin strip used in Conventional Example 8 is the same as that in Conventional Example 3.
[0138] In the embodiment 8 and the prior art example 8, the annular iron core 1 is formed by laminating 2610 iron cores. Figure 3 The weight of two iron cores overlapped in the vertical direction (total of 8 annular iron cores) is shown in Table 8.
[0139] The primary winding of the embodiment 8 uses a 2.8 mm × 7.0 mm square copper wire, which is wound 377 turns by delta connection, and the secondary winding uses a 3.0 mm × 305 mm aluminum sheet, which is wound 12 turns by delta connection. In addition, the primary winding of the conventional example 8 uses a 2.8 mm × 7.0 mm square copper wire, which is wound 377 turns by delta connection, and the secondary winding uses a 3.2 mm × 306 mm aluminum sheet, which is wound 12 turns by delta connection.
[0140]
Table 8
[0141]
[0142]
[0143] According to Table 8, in Example 8, the no-load loss per unit weight of the core is 0.188 W / kg, which is about 30% lower than the no-load loss per unit weight of the core of Conventional Example 8, which is 0.269 W / kg.
[0144] It can also be seen that, correspondingly, the existing example 8 has a ratio of 0.999 to the energy efficiency standard value defined in JIS C 4304:2013, while the example 8 can be improved to 0.996, and the annual CO2 emission of the distribution transformer when the average equivalent load factor is set to 15% is also improved by about 15%.
[0145] As described above, the transformer disclosed in the present invention can reduce no-load loss, and is therefore particularly effective in reducing loss and CO2 emissions in distribution transformers with a low average equivalent load ratio. In addition, in this embodiment, the application of the wound core transformer is described in detail, but in the case of a stacked core transformer, the effect of reducing no-load loss can of course also be obtained.
[0146] 〔Fe-based amorphous alloy ribbon〕
[0147] The Fe-based amorphous alloy thin strip used in the present embodiment will be described in detail below.
[0148] The Fe-based amorphous alloy strip used in the present embodiment is as described above, and has a plurality of point-array laser irradiation marks arranged along a direction orthogonal to the casting direction of the Fe-based amorphous alloy strip on at least one side of the Fe-based amorphous alloy strip. Among the plurality of point-array laser irradiation marks, the center line spacing of the central parts in the width direction orthogonal to the casting direction between mutually adjacent point-array laser irradiation marks is set as the row spacing, and the center point spacing of each laser irradiation mark constituting the point-array laser irradiation marks is set as the hole spacing. When the hole spacing is 0.10 mm to 0.50 mm, the row spacing is set to d1 (mm), the hole spacing is set to d2 (mm), and when the number density D of the laser irradiation marks is set to D = (1 / d1) × (1 / d2), the number density D of the laser irradiation marks is 0.05 pieces / mm 2 ~0.50pcs / mm 2 The iron loss in a single plate of the Fe-based amorphous alloy thin strip at a frequency of 60 Hz and a magnetic flux density of 1.45 T is less than 0.150 W / kg.
[0149] In addition, the Fe-based amorphous alloy thin strip also reduces the iron loss at a frequency of 50 Hz and a magnetic flux density of 1.45 T in a single plate.
[0150] In addition, the Fe-based amorphous alloy thin strip reduces the iron loss at a frequency of 50 Hz and a magnetic flux density of 1.3 T, or the iron loss at a frequency of 60 Hz and a magnetic flux density of 1.3 T.
[0151] The Fe-based amorphous alloy ribbon (hereinafter referred to as “ribbon”) disclosed in the present invention has the above-mentioned structure, thereby reducing the iron loss under the condition of magnetic flux density of 1.45T and suppressing the increase of excitation power under the condition of magnetic flux density of 1.45T.
[0152] First, the effect of reducing the iron loss under the condition of a magnetic flux density of 1.45 T is described. As described above, the Fe-based amorphous alloy thin strip disclosed in the present invention has a point-array laser irradiation mark composed of a plurality of laser irradiation marks on at least one side. In the Fe-based amorphous alloy thin strip disclosed in the present invention, the magnetic domain is subdivided by having the point-array laser irradiation marks, and as a result, the iron loss under the condition of a magnetic flux density of 1.45 T is reduced.
[0153] Thus, the formation of point-array laser irradiation marks on the Fe-based amorphous alloy ribbon itself contributes to the reduction of iron loss under the condition of a magnetic flux density of 1.45T.
[0154] Next, the effect of suppressing the increase of the excitation power under the condition of a magnetic flux density of 1.45 T is described. The details will be described later, but the present inventors have found that the formation of laser irradiation marks on the Fe-based amorphous alloy thin strip sometimes causes the increase of the excitation power under the condition of a magnetic flux density of 1.45 T. The increase of the excitation power under the condition of a magnetic flux density of 1.45 T leads to a decrease in the magnetic flux density B0.08, so it is not preferred.
[0155] Regarding this point, in the Fe-based amorphous alloy thin strip disclosed in the present invention, the center line spacing, i.e., the row spacing, of the central part of the direction orthogonal to the casting direction (hereinafter referred to as the width direction) between mutually adjacent point-array laser irradiation marks among the multiple point-array laser irradiation marks arranged along the casting direction of the thin strip is set to d1 (mm), and the center point spacing, i.e., the hole spacing, of each laser irradiation mark constituting the point-array laser irradiation marks is set to d2 (mm). Moreover, when the hole spacing is 0.10 mm to 0.50 mm, and the number density D of the laser irradiation marks is set to D = (1 / d1) × (1 / d2), the number density D of the laser irradiation marks becomes 0.05 / mm 2 ~0.50pcs / mm 2 In summary, in the Fe-based amorphous alloy ribbon disclosed in the present invention, the hole spacing and line spacing of the laser irradiation marks are expanded to a certain extent, and the number of laser irradiation marks is reduced to a certain extent (that is, the number density of laser irradiation marks is reduced to a certain extent).
[0156] In the Fe-based amorphous alloy ribbon disclosed herein, the hole spacing and line spacing of laser irradiation marks are expanded to a certain extent and the number density of laser irradiation marks is reduced to a certain extent, thereby suppressing the increase in excitation power under the condition of a magnetic flux density of 1.45 T.
[0157] Furthermore, when the point array laser irradiation marks do not reach the center portion in the width direction of the ribbon, the line interval can be measured by extending the point array laser irradiation marks in the width direction of the ribbon to a position where the point array laser irradiation marks reach the center portion.
[0158] In addition, a decrease in the magnetic flux density B0.08 that accompanies an increase in the exciting power is also suppressed.
[0159] As described above, in the Fe-based amorphous alloy ribbon of the present disclosure, the iron loss under the condition of the magnetic flux density of 1.45 T is reduced, and the increase in the exciting power under the condition of the magnetic flux density of 1.45 T is suppressed.
[0160] Hereinafter, the above-mentioned effects of the Fe-based amorphous alloy thin strip disclosed in the present invention will be described in more detail by comparison with the prior art.
[0161] At present, iron loss and excitation power are usually measured under the condition of magnetic flux density of 1.3 T. For example, the embodiment of the above-mentioned Japanese Patent Publication No. 61-29103 discloses that the free solidification surface of the Fe-based amorphous alloy thin strip is irradiated with YAG laser (the number density D at this time is 0.8 / mm) with the interval of the point array set to 5 mm. 2 ), thereby reducing the iron loss under the condition of magnetic flux density 1.3T.
[0162] In addition, in Example 4 of the above-mentioned International Publication No. 2011 / 030907, it is disclosed that when a laser is irradiated on the free solidification surface of an Fe-based amorphous alloy thin strip to form a row of recesses at intervals of 5 mm in the long side direction (the number density D at this time is 0.8 pieces / mm 2 ), under the condition that the ratio t1 / T of the depth t1 of the concave portion and the thickness T of the thin strip is 0.025 to 0.18, the iron loss and the apparent power under the condition of the magnetic flux density of 1.3 T are reduced. The apparent power in International Publication No. 2011 / 030907 corresponds to the excitation power mentioned in this specification.
[0163] In addition, Example 1 of the above-mentioned International Publication No. 2012 / 102379 discloses that wavy projections and depressions are formed on the free solidification surface of the Fe-based amorphous alloy thin strip, and the wavy projections and depressions have width-direction valleys arranged at approximately regular intervals in the long side direction. When the average amplitude of the valleys becomes less than 20 mm, the iron loss and excitation power under the condition of a magnetic flux density of 1.3 T are reduced.
[0164] However, in recent years, from the perspective of miniaturization of transformers made of Fe-based amorphous alloy thin strips, it is sometimes required to reduce the iron loss and excitation power under the condition of magnetic flux density of 1.45T without reducing the iron loss and excitation power under the condition of magnetic flux density of 1.3T.
[0165] Regarding this point, the research conducted by the present inventors has revealed that in a certain Fe-based amorphous alloy strip (specifically, an Fe-based amorphous alloy strip with a high number density of laser irradiation marks), when measured under the condition of a magnetic flux density of 1.3 T, even if the excitation power is reduced to a certain extent, when measured under the condition of a magnetic flux density of 1.45 T, the excitation power increases significantly.
[0166] Below, refer to Figure 5 and Figure 6 Describe this point in detail.
[0167] Figure 5 This is a graph showing the relationship between magnetic flux density and iron loss for four types of Fe-based amorphous alloy strips: an Fe-based amorphous alloy strip that has not been laser processed, an Fe-based amorphous alloy strip that has been laser processed with a hole spacing of 0.05 mm, an Fe-based amorphous alloy strip that has been laser processed with a hole spacing of 0.10 mm, and an Fe-based amorphous alloy strip that has been laser processed with a hole spacing of 0.20 mm.
[0168] Figure 6 This is also a graph showing the relationship between magnetic flux density and excitation power.
[0169] Figure 5 and Figure 6 In the example, a Fe-based amorphous alloy thin strip laser processed with a hole spacing of 0.05 mm was produced under the same conditions as in Comparative Example 102 described below, except that the row spacing was set to 60 mm. The number density D at this time was 0.33 pieces / mm 2 .
[0170] Figure 5 and Figure 6 In the example 101, a Fe-based amorphous alloy thin strip laser processed with a hole spacing of 0.10 mm was produced under the same conditions as in Example 101 described later, except that the row spacing was set to 60 mm. The number density D at this time was 0.167 pieces / mm 2 .
[0171] Figure 5 and Figure 6 In the example 103, the Fe-based amorphous alloy thin strip processed by laser with a hole spacing of 0.20 mm was produced under the same conditions as those of Example 103 described later (row spacing of 20 mm). The number density D at this time was 0.25 pieces / mm 2 .
[0172] Figure 5 and Figure 6 In the example, a Fe-based amorphous alloy thin strip that is not laser processed is produced under the same conditions as in Comparative Example 101 described later.
[0173] like Figure 5 As shown in the figure, it can be seen that, even in the Fe-based amorphous alloy thin strip under any conditions, the iron loss gradually increases as the magnetic flux density increases.
[0174] In addition, it can be seen that the iron loss is reduced by laser processing the Fe-based amorphous alloy thin strip under the conditions of hole spacing of 0.05 mm, hole spacing of 0.10 mm, and hole spacing of 0.20 mm. The effect of reducing iron loss by laser processing itself is described in the known documents such as Japanese Patent Publication No. 61-29103 and International Publication No. 2011 / 030907.
[0175] like Figure 6 As shown in the figure, under the condition of magnetic flux density of 1.3T, there is almost no difference in excitation power among the four Fe-based amorphous alloy ribbons. That is, under the condition of magnetic flux density of 1.3T, the presence or absence of laser processing has almost no effect on the excitation power. Therefore, under the premise of measuring iron loss and excitation power at a magnetic flux density of 1.3T, laser processing is performed on Fe-based amorphous alloy ribbons, thereby almost no increase in excitation power, and the effect of reducing iron loss can be obtained.
[0176] but, Figure 6 In the results, it is found that when the magnetic flux density exceeds 1.3 T, the excitation power rises sharply when focusing on the Fe-based amorphous alloy ribbon with a hole spacing of 0.05 mm. As a result, it is found that under the condition of a magnetic flux density of 1.45 T, the excitation power of the Fe-based amorphous alloy ribbon with a hole spacing of 0.05 mm is significantly higher than that of the other three Fe-based amorphous alloy ribbons.
[0177] As described above, the inventors of the present invention have found that when the hole spacing of the laser irradiation mark is too narrow, such as when the hole spacing is 0.05 mm, there is a tendency for the excitation power under the condition of a magnetic flux density of 1.45 T to become significantly higher (see Figure 6 ). In addition, the inventors of the present invention have also found that by increasing the hole spacing to 0.20 mm (i.e., by reducing the number density of laser irradiation marks), the increase in excitation power under the condition of a magnetic flux density of 1.45 T can be suppressed (see Figure 6 ).
[0178] The inventors of the present invention have also found that even if the hole interval is increased to 0.10 mm or 0.20 mm, the effect of reducing the iron loss caused by laser processing can be obtained (see Figure 5 ).
[0179] These findings are also shown in Table 9 of Examples described later.
[0180] Based on this insight, it is found that by increasing the hole spacing and reducing the number density D, the increase in excitation power can be suppressed under the condition of a magnetic flux density of 1.45 T, thereby obtaining a low-loss Fe-based amorphous alloy thin strip.
[0181] In addition, the inventors found that by expanding the row spacing of the plurality of point-line laser irradiation marks (for example, by setting the row spacing to 10 mm or more), the increase in excitation power under the condition of a magnetic flux density of 1.45 T can be suppressed, and the effect of reducing the iron loss caused by laser processing can be obtained, as in the case of expanding the hole spacing. This finding is shown in Table 10 of the Examples described later.
[0182] However, for example, as described in the International Publication No. 2012 / 102379 mentioned above, it is currently being conducted to reduce iron loss by forming wavy concavities and convexities on the free solidification surface of the Fe-based amorphous alloy thin strip. Wavy concavities and convexities are also called chatter marks, etc., and are generated due to the vibration of the paddle when manufacturing (casting) the Fe-based amorphous alloy thin strip (for example, refer to paragraph 0008 of the International Publication No. 2012 / 102379). In the technology of forming wavy concavities and convexities to reduce iron loss, the wavy concavities and convexities are intentionally formed on the free solidification surface by adjusting the manufacturing conditions of the Fe-based amorphous alloy thin strip.
[0183] With respect to the technology of reducing iron loss by forming wavy concave-convex, the existing laser processing technology described in, for example, Japanese Patent Publication No. 61-29103 and International Publication No. 2011 / 030907 is a technology that, instead of forming wavy concave-convex on the free solidification surface, performs laser processing on the free solidification surface to obtain the same effect as the wavy concave-convex (the effect of reducing iron loss, etc.). Therefore, in the existing laser processing technology, in order to form a shape similar to the wavy concave-convex, the line spacing is reduced (for example, as described in the embodiments of Japanese Patent Publication No. 61-29103 and International Publication No. 2011 / 030907, the line spacing is set to 5 mm), that is, the number density of laser irradiation marks is made relatively high, and laser irradiation marks are formed.
[0184] At present, the excitation power is measured under the condition of magnetic flux density of 1.3 T, and therefore, the disadvantage of increasing the number density of laser irradiation marks (i.e., the increase in excitation power) has not been recognized. However, as described above, the present inventors have found that when the number density of laser irradiation marks is increased, the excitation power measured under the condition of magnetic flux density of 1.45 T increases, and by reducing the number density of laser irradiation marks, the increase in excitation power measured under the condition of magnetic flux density of 1.45 T can be suppressed.
[0185] The Fe-based amorphous alloy thin strip disclosed in the present invention is a thin strip developed based on this finding.
[0186] Therefore, the Fe-based amorphous alloy thin strip disclosed in the present invention is the same as the technology described in Japanese Patent Publication No. 61-29103 and International Publication No. 2011 / 030907 in terms of forming laser irradiation marks on the surface of the thin strip, but the Fe-based amorphous alloy thin strip disclosed in the present invention is completely different from the technology described in Japanese Patent Publication No. 61-29103 and International Publication No. 2011 / 030907 in terms of suppressing the increase in excitation power measured under the condition of a magnetic flux density of 1.45 T by reducing the number density of laser irradiation marks.
[0187] Hereinafter, the Fe-based amorphous alloy ribbon disclosed in the present invention and its preferred embodiments will be described in more detail.
[0188] The Fe-based amorphous alloy thin strip disclosed in the present invention is a Fe-based amorphous alloy thin strip having a free solidification surface and a roll surface.
[0189] The Fe-based amorphous alloy thin strip having a free solidification surface and a roll surface is a thin strip manufactured (cast) by a single roll method. During casting, the surface that contacts the cooling roll and is rapidly solidified is the roll surface, and the surface on the opposite side of the roll surface (i.e., the surface exposed to the atmosphere during casting) is the free solidification surface. For the single roll method, reference can be made to known documents such as International Publication No. 2012 / 102379.
[0190] The Fe-based amorphous alloy ribbon of the present disclosure may be a ribbon in an uncut state after casting (for example, a roll body wound up into a roll after casting), or may be cut into ribbon pieces of a desired size after casting.
[0191] <Laser irradiation marks, spot-shaped laser irradiation marks>
[0192] The Fe-based amorphous alloy thin strip disclosed in the present invention has a plurality of laser irradiation marks in a point array shape consisting of a plurality of laser irradiation marks on at least one surface.
[0193] Each of the plurality of laser irradiation marks constituting the point-array laser irradiation marks may be a mark to which energy is imparted by laser processing (ie, laser irradiation), and the shape (shape in plan view and cross-sectional shape) of the laser irradiation marks is not particularly limited.
[0194] If each of the plurality of laser irradiation marks is a mark to which energy is imparted by laser irradiation, the effect of reducing the iron loss due to laser irradiation can be obtained.
[0195] The shape of the laser irradiation mark in plan view may be a crown shape, a ring shape, a flat shape, or the like.
[0196] From the viewpoint of weather resistance (rust prevention) of the laser irradiation marks of the Fe-based amorphous alloy thin strip and improvement of the space factor of the Fe-based amorphous alloy thin strip, the shape of the laser irradiation marks when viewed from above is preferably annular or planar, and more preferably planar. When it is planar, when the thin strips are stacked to form an iron core, the space between the thin strips can be suppressed, and the thin strip density of the iron core can be increased.
[0197] In the Fe-based amorphous alloy strip disclosed in the present invention, when the center line spacing in the central part of the width direction orthogonal to the casting direction of the Fe-based amorphous alloy strip between adjacent point-array laser irradiation marks among a plurality of point-array laser irradiation marks arranged along the casting direction of the Fe-based amorphous alloy strip is set as the row spacing, the row spacing is preferably 10 mm to 60 mm.
[0198] In addition, the width direction is a direction orthogonal to the casting direction of the Fe-based amorphous alloy thin strip. In addition, when the point-array laser irradiation marks are formed on both sides of the free solidification surface and the roller surface of the thin strip, the line interval is measured with the point-array laser irradiation marks on both sides when the thin strip is observed in a transmission manner as the object. For example, when the point-array laser irradiation marks are alternately formed on both sides in the casting direction of the thin strip, among the "adjacent point-array laser irradiation marks", the point-array laser irradiation marks formed on one side and the point-array laser irradiation marks formed on the other side and adjacent in the casting direction become the object.
[0199] When the row interval is 10 mm or more, the increase in the exciting power measured under the condition of the magnetic flux density of 1.45 T can be suppressed compared with the case where the row interval is less than 10 mm.
[0200] When the row spacing is 60 mm or less, the effect of reducing the iron loss measured under the condition of a magnetic flux density of 1.45 T is superior to the case where the row spacing exceeds 60 mm.
[0201] The row interval is more preferably 10 mm to 50 mm, more preferably 10 mm to 40 mm, and even more preferably 10 mm to 30 mm.
[0202] The directions of the multiple point-array laser irradiation marks are preferably approximately parallel, but are not limited to approximately parallel. Preferably, the row spacing is 10 mm to 60 mm in the center of the width direction of the thin strip. The directions of the multiple point-array laser irradiation marks may be parallel or non-parallel.
[0203] The "central portion in the width direction" of the Fe-based amorphous alloy thin strip can be set as a portion that maintains a certain degree of width from the center in the width direction to both ends in the width direction. For example, from the center in the width direction to both ends in the width direction, the range of the region where the "certain degree of width" becomes 1 / 4 of the entire width can be set as the central portion. Among them, it is more preferable to set the range of the region where the "certain degree of width" becomes 1 / 2 of the entire width as the central portion.
[0204] As one embodiment of the present disclosure, the Fe-based amorphous alloy ribbon may have a plurality of point-array laser irradiation marks arranged in non-parallel directions relative to a width direction orthogonal to the casting direction of the Fe-based amorphous alloy ribbon.
[0205] That is, the angle formed by the direction of each of the plurality of point-array laser irradiation marks and the width direction of the Fe-based amorphous alloy ribbon may be set to be 10° or more and may intersect while maintaining an acute or obtuse inclination angle with respect to the casting direction.
[0206] As another embodiment of the present disclosure, the Fe-based amorphous alloy ribbon preferably has a plurality of point-array laser irradiation marks each oriented in a direction substantially parallel to a direction orthogonal to the casting direction and thickness direction of the Fe-based amorphous alloy ribbon.
[0207] The direction of each of the plurality of point-array laser irradiation marks is approximately parallel to the direction orthogonal to the casting direction and the thickness direction of the Fe-based amorphous alloy thin strip, which means that the angle formed by the direction of each of the plurality of point-array laser irradiation marks and the direction orthogonal to the casting direction and the thickness direction of the Fe-based amorphous alloy thin strip is less than 10°. However, it is not limited to that the plurality of point-array laser irradiation marks are approximately parallel.
[0208] In the Fe-based amorphous alloy ribbon of the present disclosure, as one embodiment, it is preferred that the directions of the plurality of point-array laser irradiation marks are substantially parallel to the width direction of the Fe-based amorphous alloy ribbon.
[0209] The direction of each of the plurality of point-array laser irradiation marks being substantially parallel to the width direction of the Fe-based amorphous alloy ribbon means that the angle formed by the direction of each of the plurality of point-array laser irradiation marks and the width direction of the Fe-based amorphous alloy ribbon is 10° or less.
[0210] However, the plurality of spot-array laser irradiation marks are not limited to being substantially parallel.
[0211] As mentioned above, the direction of the point-line laser irradiation marks may not be parallel to the direction orthogonal to the casting direction of the Fe-based amorphous alloy thin strip, and the angle formed by the direction of the point-line laser irradiation marks and the casting direction of the Fe-based amorphous alloy thin strip may also maintain an inclination angle of 10° or more. In this way, it is interpreted that even if the inclination angle of 10° is maintained, the point-line laser irradiation marks are arranged along the direction orthogonal to the casting direction of the Fe-based amorphous alloy thin strip. The inclination angle is preferably less than 45°, more preferably less than 40°, more preferably less than 30°, and more preferably less than 20°. It is most preferably less than 10°.
[0212] The Fe-based amorphous alloy ribbon disclosed herein may have one laser irradiation mark array arranged at regular intervals along the casting direction of the ribbon in the width direction of the ribbon, or may have two or more laser irradiation marks in the width direction of the ribbon.
[0213] Specifically, the Fe-based amorphous alloy strip disclosed in the present invention may also be a strip having multiple point-array laser irradiation marks arranged along the casting direction of the Fe-based amorphous alloy strip in the width direction orthogonal to the casting direction, (1) having one row in the above-mentioned "central part in the width direction" (hereinafter referred to as a single row group), (2) having multiple rows in the above-mentioned "central part in the width direction" (hereinafter referred to as multiple row groups).
[0214] Hereinafter, a plurality of point-array laser irradiation marks provided along the casting direction of the Fe-based amorphous alloy thin strip are collectively referred to as a “group of irradiation mark arrays”.
[0215] In the latter multiple column groups, there are multiple groups of irradiation mark columns in the width direction of the thin strip, and between the multiple groups, the positions of the respective point-column-shaped laser irradiation marks do not need to be on the same line in the width direction, and the point-column-shaped laser irradiation marks can also be in a positional relationship that is deviated in the casting direction. For example, in the case where there are two groups of irradiation mark columns in the width direction of the thin strip, the two groups are separated by the irradiation mark column non-forming area in the central part of the width direction of the thin strip, and the multiple point-column-shaped laser irradiation marks arranged in one group and the multiple point-column-shaped laser irradiation marks arranged in the other group can also be in a positional relationship that is deviated by a certain distance in the casting direction and exists alternately.
[0216] The line interval in the present disclosure is a value obtained as follows.
[0217] As in (1) above, when the "central portion in the width direction" is a single column group having a plurality of point-column laser irradiation marks arranged along the casting direction, as for the row spacing, the spacing between two point-column laser irradiation marks adjacent to each other in the casting direction in the single column group can be measured at 5 locations selected arbitrarily, and the average value of the measured values can be set. In this case, the plurality of point-column laser irradiation marks constituting the single column group are preferably present at a certain interval, but may be present at any interval.
[0218] In addition, as in (2) above, when the “central portion in the width direction” has a plurality of point-column laser irradiation marks arranged along the casting direction as a plurality of column groups consisting of a plurality of columns, the row spacing can be made a further average value by using the value (average value) obtained in the same manner as the above method for each “group of irradiation mark columns” in the plurality of column groups. In this case, the plurality of point-column laser irradiation marks constituting each “group of irradiation mark columns” are preferably present at a certain interval, but may be present at any interval.
[0219] In the Fe-based amorphous alloy ribbon disclosed herein, when the center point interval of each laser irradiation mark constituting a plurality of point-line laser irradiation marks is defined as the hole interval, the hole interval is 0.10 mm to 0.50 mm. Therefore, a structure in which the hole interval is less than 0.10 mm and is continuously formed is not included.
[0220] By setting the hole spacing to 0.10 mm or more, the increase in excitation power measured under the condition of a magnetic flux density of 1.45 T can be suppressed compared to the case where the hole spacing is less than 0.10 mm (see the above). Figure 6 ).
[0221] When the hole interval is 0.50 mm or less, the effect of reducing the iron loss measured under the condition of the magnetic flux density of 1.45 T is superior to the case where the hole interval exceeds 0.50 mm.
[0222] The hole interval is preferably 0.15 mm to 0.40 mm, more preferably 0.20 mm to 0.40 mm.
[0223] As described above, the Fe-based amorphous alloy ribbon of the present disclosure suppresses the increase in the excitation power measured under the condition of a magnetic flux density of 1.45 T by reducing the number density of laser irradiation marks constituting point-array laser irradiation marks compared with conventional methods.
[0224] In the Fe-based amorphous alloy ribbon of the present disclosure, when the line interval is d1 (mm) and the hole interval is d2 (mm), the number density D of the laser irradiation marks is set to a value calculated by the following formula.
[0225] D=(1 / d1)×(1 / d2)
[0226] The number density D is a value calculated from the line spacing and hole spacing, and represents the density of the laser irradiation marks formed. That is, the unit area (mm2) with a certain line spacing and hole spacing is 2 ), the number density (D) satisfying d1×d2×D=1 is 0.05 pieces / mm 2 ~0.50pcs / mm 2 .
[0227] By setting the number density D of laser irradiation marks to an appropriate value (a smaller value than conventional values), it is possible to suppress an increase in the excitation power measured under the condition of a magnetic flux density of 1.45 T.
[0228] The number density D of the laser irradiation marks constituting the point array laser irradiation marks was set to 0.05 pieces / mm 2 ~0.50pcs / mm 2 .
[0229] The number density D of the laser irradiation marks constituting the point array laser irradiation marks is more preferably 0.10 / mm 2 ~0.50pcs / mm 2 .
[0230] When there are a plurality of point array-shaped laser irradiation marks of the present disclosure, the number density D can be obtained as follows depending on the situation.
[0231] As described in (1), when the "central portion in the width direction" has a plurality of point-column laser irradiation marks arranged along the casting direction as a single column group having one column, as for the number density D, 5 positions of "adjacent point-column laser irradiation marks" are randomly selected from the plurality of point-column laser irradiation marks constituting the single column group, and the row spacing and hole spacing of each are measured and the average of the measured values is obtained respectively. The number density D is obtained by the above formula based on the average of the row spacing and the average of the hole spacing. The obtained number density D is within 0.05 pieces / mm 2 ~0.50pcs / mm 2 range to achieve the effect of the present invention.
[0232] In addition, as in (2) above, when the “central portion in the width direction” has a plurality of point-column-shaped laser irradiation marks arranged along the casting direction as a plurality of column groups consisting of a plurality of columns, the number density D is obtained by the same method for each “group of irradiation mark columns” in the plurality of column groups. Then, the obtained number density D and the number density D of at least one “group of irradiation mark columns” in the plurality of column groups are within 0.05 pieces / mm 2 ~0.50pcs / mm 2 In order to further achieve the effect of the present invention, the average value of the number density D is preferably 0.05 pieces / mm 2~0.50pcs / mm 2 The number density D of all "groups of irradiation marks" in the plurality of column groups is more preferably 0.05 pieces / mm 2 ~0.50pcs / mm 2 range.
[0233] Here, the “casting direction” is a direction corresponding to the circumferential direction of the cooling roll when casting the Fe-based amorphous alloy strip, in other words, a direction corresponding to the long side direction of the Fe-based amorphous alloy strip after casting and before cutting.
[0234] In addition, in the cut thin strip, by observing the free solidification surface and / or roller surface of the thin strip, it is also possible to confirm which direction the "casting direction" is. For example, thinner stripes along the casting direction are observed on the free solidification surface and / or roller surface of the thin strip. In addition, the direction orthogonal to the casting direction is the width direction.
[0235] In addition, the ratio of the length of the point-line laser irradiation marks in the width direction to the overall length of the Fe-based amorphous alloy ribbon in the width direction is preferably 10% to 50% in the direction from the center in the width direction to both ends in the width direction. In addition, the "%" here is set to 100% for the overall length of the Fe-based amorphous alloy ribbon in the width direction.
[0236] In addition, when the direction of the point-array laser irradiation mark remains inclined relative to the width direction, the length of the inclined point-array laser irradiation mark itself is not maintained, but the value of the length in the width direction of the thin strip converted in the portion where the point-array laser irradiation mark is formed is set as the length of the point-array laser irradiation mark.
[0237] The above-mentioned length ratio of 50% means that the point-line laser irradiation marks start from the center of the width direction of the Fe-based amorphous alloy thin strip and reach one end and the other end in the width direction. The "starting from the center and reaching one end and the other end in the width direction" means that at each of the one end and the other end, the interval between the laser irradiation marks at the end of the point-line laser irradiation marks and the end of the Fe-based amorphous alloy thin strip is less than the hole interval of the laser irradiation marks.
[0238] For example, when the direction of the point-array laser irradiation marks is parallel to the width direction of the Fe-based amorphous alloy ribbon, the length of the point-array laser irradiation marks in the direction of the Fe-based amorphous alloy ribbon corresponds to the full width of the Fe-based amorphous alloy ribbon.
[0239] In addition, the above-mentioned length ratio of 10% means that the length of the point-line laser irradiation marks is 10% from the center in the width direction to the two ends in the width direction, that is, the center area in the entire width has a length of 20% of the width length. In other words, the point-line laser irradiation marks are formed at the two ends in the width direction of the Fe-based amorphous alloy thin strip with a blank space of 40% relative to the entire length in the width direction.
[0240] More preferably, the ratio of the length of the point-array laser irradiation marks in the width direction of the Fe-based amorphous alloy ribbon to the total length in the width direction is 25% or more in the direction from the center in the width direction to both ends in the width direction.
[0241] Furthermore, it is preferred that the point-array laser irradiation marks are formed in at least six regions in the center in the width direction, excluding two regions at both ends from eight regions obtained by dividing the Fe-based amorphous alloy ribbon into eight equal regions in the width direction.
[0242] <Roughness of free solidification surface (maximum cross-sectional height Rt)>
[0243] However, as described in, for example, International Publication No. 2012 / 102379 mentioned above, currently, the iron loss is reduced by providing corrugated irregularities on the free solidification surface.
[0244] However, according to the study by the present inventors, it was found that the wave-like irregularities may cause an increase in the excitation power measured under the condition of a magnetic flux density of 1.45 T.
[0245] Therefore, from the viewpoint of suppressing the increase in the exciting power measured under the condition of the magnetic flux density of 1.45 T, it is preferable to reduce the wave-like irregularities as much as possible.
[0246] Specifically, the maximum cross-sectional height Rt of the free solidification surface other than the plurality of point array laser irradiation marks is preferably 3.0 μm or less. The maximum cross-sectional height Rt being 3.0 μm or less means that there is no wavy irregularities on the free solidification surface or the wavy irregularities are reduced.
[0247] In this specification, with respect to the maximum cross-sectional height Rt of the portion other than the multiple point-array laser irradiation marks of the free solidification surface, for the portion other than the multiple point-array laser irradiation marks of the free solidification surface, according to JIS B 0601:2001, the evaluation length is set to 4.0 mm, the critical value is set to 0.8 mm, and the critical type is set to 2RC (phase compensation) for measurement (evaluation). Here, the direction of the evaluation length is set to the casting direction of the Fe-based amorphous alloy thin strip. In addition, in detail, the above measurement with the evaluation length set to 4.0 mm is performed by continuously measuring 5 times with a critical value of 0.8 mm.
[0248] The maximum cross-sectional height Rt of the portion other than the plurality of point array laser irradiation marks of the free solidification surface is more preferably 2.5 μm or less.
[0249] In addition, the lower limit of the maximum cross-sectional height Rt is not particularly limited, but from the viewpoint of the production applicability of the Fe-based amorphous alloy ribbon, the lower limit of the maximum cross-sectional height Rt is preferably 0.8 μm, and more preferably 1.0 μm.
[0250] <Chemical composition>
[0251] The chemical composition of the Fe-based amorphous alloy ribbon disclosed in the present invention is not particularly limited, as long as it is the chemical composition of the Fe-based amorphous alloy (i.e., the chemical composition with Fe (iron) as the main component). However, from the perspective of more effectively obtaining the effect of the Fe-based amorphous alloy ribbon disclosed in the present invention, the chemical composition of the Fe-based amorphous alloy ribbon disclosed in the present invention is preferably the following chemical composition A.
[0252] Chemical composition A, which is a preferred chemical composition, is composed of Fe, Si, B, and impurities. When the total content of Fe, Si, and B is set to 100 atomic %, the Fe content is more than 78 atomic %, the B content is more than 10 atomic %, and the total content of B and Si is 17 atomic % to 22 atomic %.
[0253] Hereinafter, the chemical composition A will be described in more detail.
[0254] In the chemical composition A, the Fe content is 78 atomic % or more.
[0255] Fe (iron) is one of the transition metals with the largest magnetic moment even in an amorphous structure, and serves as a magnetic carrier in Fe-Si-B-based amorphous alloys.
[0256] When the Fe content is 78 atomic % or more, the saturation magnetic flux density (Bs) of the Fe-based amorphous alloy ribbon can be increased (for example, a Bs of about 1.6 T can be achieved). In addition, the preferred magnetic flux density B0.08 (1.52 T or more) described later can be easily achieved.
[0257] The Fe content is preferably 80 atomic % or more, more preferably 80.5 atomic % or more, and even more preferably 81.0 atomic % or more, and is preferably 82.5 atomic % or less, and even more preferably 82.0 atomic % or less.
[0258] In the chemical composition A, the content of B is 10 atomic % or more.
[0259] B (boron) is an element that contributes to amorphous formation. When the content of B is 10 atomic % or more, the amorphous formation ability is further improved.
[0260] In addition, when the B content is 10 atomic % or more, the magnetic domains are easily oriented in the casting direction, and the magnetic flux density (B0.08) is easily increased by widening the magnetic domain width.
[0261] The B content is preferably 11 atomic % or more, more preferably 12 atomic % or more, and further preferably 13 atomic % or more.
[0262] The upper limit of the B content also varies depending on the total content of B and Si described later, but is preferably 16 atomic %.
[0263] In the chemical composition A, the total content of B and Si is 17 atomic % to 22 atomic %.
[0264] Si (silicon) is an element that segregates on the surface in a molten metal state and has the effect of preventing oxidation of the molten metal. In addition, Si also acts as an auxiliary agent for amorphous formation, has the effect of increasing the glass transition temperature, and forms a more thermally stable amorphous phase.
[0265] When the total content of B and Si is 17 atomic % or more, the above-mentioned effect of Si is effectively exhibited.
[0266] In addition, when the total content of B and Si is 22 atomic % or less, a large amount of Fe as a magnetic carrier can be ensured, which is advantageous in terms of improving the saturation magnetic flux density Bs and the magnetic flux density B0.08.
[0267] The Si content is preferably 2.0 atomic % or more, more preferably 2.4 atomic % or more, and further preferably 3.5 atomic % or more.
[0268] The upper limit of the Si content also varies depending on the total content of B and Si, but is preferably 6.0 atomic %.
[0269] In the above-mentioned chemical composition A, from the viewpoint of further improving the iron loss and excitation power described later, the more preferred chemical composition of the Fe-based amorphous alloy strip is composed of Fe, Si, B, and impurities. When the total content of Fe, Si, and B is set to 100 atomic %, the content of Fe is more than 80 atomic %, the content of B is more than 12 atomic %, and the total content of B and Si is 17 atomic % to 20 atomic %.
[0270] Chemical composition A contains impurities.
[0271] In this case, the impurities contained in the chemical composition A may be only one kind or two or more kinds.
[0272] Impurities include all elements other than Fe, Si, and B. Specifically, for example, C, Ni, Co, Mn, O, S, P, Al, Ge, Ga, Be, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, rare earth elements, etc.
[0273] These elements can be contained in a range of 1.5 mass % or less in total relative to the total mass of Fe, Si, and B. The total content of these elements is preferably 1.0 mass % or less, more preferably 0.8 mass % or less, and further preferably 0.75 mass % or less. In addition, these elements may be added within this range.
[0274] <Thickness>
[0275] The thickness of the Fe-based amorphous alloy ribbon disclosed in the present invention is not particularly limited, but the thickness is preferably 18 μm to 35 μm.
[0276] A thickness of 18 μm or more is advantageous in that the undulation of the Fe-based amorphous alloy ribbon can be suppressed and the space factor can be improved.
[0277] A thickness of 35 μm or less is advantageous in terms of suppressing embrittlement of the Fe-based amorphous alloy ribbon and improving magnetic saturation.
[0278] The thickness of the Fe-based amorphous alloy ribbon is more preferably 20 μm to 30 μm.
[0279] <Iron loss>
[0280] As described above, in the Fe-based amorphous alloy ribbon of the present disclosure, the magnetic domains are subdivided by laser processing (formation of laser irradiation marks), thereby reducing the iron loss under the conditions of a frequency of 60 Hz and a magnetic flux density of 1.45 T.
[0281] The iron loss under the conditions of a frequency of 60 Hz and a magnetic flux density of 1.45 T is 0.150 W / kg or less, preferably 0.140 W / kg or less, and more preferably 0.130 W / kg or less.
[0282] The lower limit of the iron loss under the conditions of a frequency of 60 Hz and a magnetic flux density of 1.45 T is not particularly limited, but from the viewpoint of the production suitability of the Fe-based amorphous alloy ribbon, the lower limit of the iron loss is preferably 0.050 W / kg.
[0283] In the Fe-based amorphous alloy strip disclosed herein, the iron loss CL at a frequency of 50 Hz and a magnetic flux density of 1.45 T is also reduced. In the Fe-based amorphous alloy strip disclosed herein, the iron loss CL at a frequency of 50 Hz and a magnetic flux density of 1.45 T is preferably 0.120 W / kg or less.
[0284] In addition, in the Fe-based amorphous alloy thin strip disclosed in the present invention, the iron loss at a frequency of 50 Hz and a magnetic flux density of 1.3 T, or the iron loss at a frequency of 60 Hz and a magnetic flux density of 1.3 T is also reduced. Preferably, the iron loss at a frequency of 50 Hz and a magnetic flux density of 1.3 T is 0.08 W / kg or less, or the iron loss at a frequency of 60 Hz and a magnetic flux density of 1.3 T is 0.11 W / kg or less.
[0285] The iron loss of the Fe-based amorphous alloy strip is measured in accordance with JIS C 2535:2017 or JIS H7152:1996.
[0286] <Excitation power>
[0287] As described above, in the Fe-based amorphous alloy ribbon of the present disclosure, the increase in excitation power under the condition of a magnetic flux density of 1.45 T is suppressed.
[0288] The exciting power under the conditions of a frequency of 60 Hz and a magnetic flux density of 1.45 T is preferably 0.200 VA / kg or less, more preferably 0.170 VA / kg or less, and further preferably 0.165 VA / kg or less.
[0289] The lower limit of the excitation power under the conditions of a frequency of 60 Hz and a magnetic flux density of 1.45 T is not particularly limited, but from the viewpoint of the production applicability of the Fe-based amorphous alloy ribbon, the lower limit of the excitation power is preferably 0.100 VA / kg.
[0290] <Magnetic flux density B0.08>
[0291] As described above, in the Fe-based amorphous alloy thin strip of the present disclosure, the increase in excitation power under the condition of a magnetic flux density of 1.45 T is suppressed, thereby suppressing the decrease in magnetic flux density B0.08 accompanying the increase in excitation power, and as a result, the magnetic flux density B0.08 can be maintained at a high level.
[0292] In the Fe-based amorphous alloy ribbon disclosed herein, the magnetic flux density B0.08 under the conditions of a frequency of 60 Hz and a magnetic field of 8 A / m is preferably 1.52 T or more.
[0293] The upper limit of the magnetic flux density B0.08 under the conditions of a frequency of 60 Hz and a magnetic field of 8 A / m is not particularly limited, but the upper limit is preferably 1.62 T.
[0294] <Ratio〔Operating magnetic flux density Bm / Saturation magnetic flux density Bs〕>
[0295] As described above, in the Fe-based amorphous alloy ribbon of the present disclosure, the iron loss and the excitation power under the condition of the magnetic flux density of 1.45 T which is higher than the conventional condition of 1.3 T can be suppressed to be low.
[0296] Therefore, even when using an operating magnetic flux density Bm under a ratio [operating magnetic flux density Bm / saturation magnetic flux density Bs] (hereinafter referred to as “Bm / Bs ratio”) higher than conventional conditions, iron loss and excitation power can be suppressed.
[0297] In this regard, as an existing example, an Fe-based amorphous alloy thin strip is used under conditions where the saturation magnetic flux density Bs is 1.56 T and the operating magnetic flux density Bm is 1.35 T (i.e., Bm / Bs ratio = 0.87) (for example, refer to IEEE TRANSACTIONSON MAGNETICS Vol: 44, Issue: 11, Nov. 2008, pp. 4104-4106 (especially, p. 4106)).
[0298] In contrast, the Fe-based amorphous alloy ribbon of the present disclosure, for example, has the chemical composition (Fe 82 4B 14 ) has a Bs of 1.63T. Bs is roughly determined by the chemical composition. In this case, the Fe-based amorphous alloy thin strip of the present disclosure can be used with a Bm of 1.43T or more (preferably 1.45T to 1.50T). The Bm / Bs ratio is 0.88 when Bm is 1.43T, and the Bm / Bs ratio is 0.92 when Bm is 1.50T.
[0299] For the reasons described above, the Fe-based amorphous alloy thin strip disclosed in the present invention is particularly suitable for use in applications where the operating magnetic flux density Bm satisfies the Bm / Bs ratio of 0.88 to 0.94 (preferably 0.89 to 0.92).
[0300] The Fe-based amorphous alloy ribbon disclosed herein can suppress increases in iron loss and excitation power even when used at an operating magnetic flux density Bm satisfying a Bm / Bs ratio of 0.88 to 0.94 (preferably 0.89 to 0.92).
[0301] -Method for producing Fe-based amorphous alloy ribbon (production method X) -
[0302] The Fe-based amorphous alloy thin strip of the present disclosure can be produced by the following production method X, which is preferably the following.
[0303] Process X has:
[0304] A step of preparing a raw material strip composed of an Fe-based amorphous alloy and having a free solidification surface and a roll surface (hereinafter referred to as a "raw material preparation step");
[0305] A process for forming a plurality of point-array laser irradiation marks composed of a plurality of laser irradiation marks on at least one of the free solidification surface and the roller surface of the raw material thin strip by laser processing, thereby obtaining an Fe-based amorphous alloy thin strip having a plurality of point-array laser irradiation marks (hereinafter referred to as "laser processing process");
[0306] When the center line spacing of the central parts of the width direction orthogonal to the casting direction between the adjacent point-array laser irradiation marks in the plurality of point-array laser irradiation marks arranged along the casting direction of the above-mentioned Fe-based amorphous alloy thin strip is set as the row spacing, and the center point spacing of the plurality of point-array laser irradiation marks of each of the plurality of point-array laser irradiation marks is set as the hole spacing, the hole spacing is 0.10 mm to 0.50 mm, the row spacing is set as d1 (mm), the hole spacing is set as d2 (mm), and the number density D of the laser irradiation marks is set as D = (1 / d1) × (1 / d2), the number density D of the laser irradiation marks is 0.05 pieces / mm 2 ~0.50pcs / mm 2 .
[0307] The manufacturing method X may include other steps besides the raw material preparation step and the laser processing step as necessary.
[0308] -Raw material preparation process-
[0309] The raw material preparation step in the manufacturing method X is a step of preparing a raw material thin strip having a free solidification surface and a roll surface.
[0310] The raw material strip mentioned here may be a strip in an uncut state after casting (for example, a roll body wound into a roll after casting), or a strip piece cut into a desired size after casting. It can be said that the raw material strip is the Fe-based amorphous alloy strip of the present disclosure at a stage before the laser irradiation mark is formed.
[0311] The free solidification surface and the roll surface of the raw material thin strip are synonymous with the free solidification surface and the roll surface of the Fe-based amorphous alloy thin strip of the present disclosure, respectively.
[0312] Preferred aspects of the raw material ribbon (eg, preferred chemical composition, preferred Rt) are the same as those of the Fe-based amorphous alloy ribbon disclosed herein, except for the presence or absence of laser irradiation marks.
[0313] The raw material preparation step may be a step of merely preparing a previously cast (ie, already completed) raw material strip for supplying to the laser processing step, or may be a step of recasting the raw material strip.
[0314] Furthermore, the raw material preparation step may be a step of performing at least one of casting of the raw material strip and cutting out strip pieces from the raw material strip.
[0315] -Laser processing steps-
[0316] In the laser processing step in the manufacturing method X, a plurality of laser irradiation marks (specifically, point-array laser irradiation marks composed of a plurality of laser irradiation marks) are formed by laser processing (i.e., by irradiating laser) on at least one of the free solidification surface and the roller surface of the raw material thin strip. The preferred forms of the laser irradiation marks and point-array laser irradiation marks formed by the laser irradiation step (preferred row spacing, hole spacing, number density of laser irradiation marks, etc.) are the same as the preferred forms of the laser irradiation marks and point-array laser irradiation marks of the Fe-based amorphous alloy thin strip disclosed above.
[0317] As described above, if each of the plurality of laser irradiation marks is a mark to which energy is imparted by laser irradiation, the effect of reducing the iron loss due to laser irradiation can be obtained.
[0318] Therefore, the conditions of the laser in the laser processing step are not particularly limited, but the preferred conditions are as follows.
[0319] By controlling the irradiation energy of the laser with respect to the thickness of the Fe-based amorphous alloy ribbon, the diameter of the recess and the depth of the recess can be controlled.
[0320] In the laser processing step, the output of the laser used to form each laser irradiation mark (hereinafter referred to as "laser output") is preferably 0.4mJ to 2.5mJ, more preferably 0.6mJ to 2.5mJ, further preferably 0.8mJ to 2.5mJ, further preferably 1.0mJ to 2.0mJ, and further preferably 1.3mJ to 1.8mJ.
[0321] The diameter of the laser beam (hereinafter referred to as "spot diameter") is preferably 50 μm to 200 μm.
[0322] When the value obtained by dividing the laser output by the hole area is defined as the energy density of the laser, the energy density is preferably 0.01 J / mm 2 ~1.50J / mm 2 , more preferably 0.02 J / mm 2 ~1.30J / mm 2 , more preferably 0.03 J / mm 2 ~1.02J / mm 2 .
[0323] The pulse width of the laser is preferably 50 nsec or more, and more preferably 100 nsec or more. By setting the pulse width in the above range, magnetic properties such as iron loss of the ribbon piece having the laser irradiation mark formed thereon can be effectively improved.
[0324] The pulse width refers to the time of laser irradiation, and a smaller pulse width means a shorter irradiation time. That is, the total energy of the irradiated laser is the product of the energy per unit time and the pulse width.
[0325] In the laser processing, when forming the recessed portion, the pulsed laser is irradiated while scanning in the width direction of the ribbon.
[0326] As a laser source, YAG laser, CO2 gas laser, fiber laser, etc. can be used. Among them, fiber laser is preferred in that it is possible to irradiate high-frequency pulsed laser with high output for a long time and stably. In the fiber laser, the laser introduced into the optical fiber oscillates according to the principle of FBG (Fiber Bragg grating) through the diffraction gratings at both ends of the optical fiber. The laser is excited in a slender optical fiber, so there is no problem of thermal lens effect that reduces the quality of the beam due to the temperature gradient generated inside the crystal. In addition, the optical fiber core is as thin as a few microns, so not only does the laser propagate in a single mode even at high output, but also reduces the beam diameter to obtain a laser with high energy density. On this basis, the focal depth is long, so it is also possible to form a column of recesses with high precision in a thin strip with a width of more than 200 mm. The pulse width of a fiber laser is usually in the range of microseconds to picoseconds.
[0327] The wavelength of the laser light is about 250 nm to 1100 nm, depending on the laser source, but a wavelength of 900 nm to 1100 nm is preferably used because it is sufficiently absorbed in the alloy ribbon.
[0328] The beam diameter of the laser is preferably 10 μm or more, more preferably 30 μm or more, and more preferably 50 μm or more. The beam diameter is preferably 500 μm or less, more preferably 400 μm or less, and more preferably 300 μm or less.
[0329] In addition, the laser processing step can also be a process of performing laser processing on the raw material strip after casting and before winding in the single-roll method, or a process of performing laser processing on the raw material strip wound from the raw material strip (roll body) after winding, or a process of performing laser processing on the strip sheet cut from the raw material strip wound from the raw material strip (roll body) after winding.
[0330] When the laser processing step is a step of laser processing a raw material strip after casting and before winding in a single roll method, the manufacturing method X is implemented using a system in which a laser processing device is arranged between a cooling roll and a winding roll, for example.
[0331] Examples of Fe-based amorphous alloy thin strips suitable for the transformer of the present disclosure are shown below.
[0332] [Example 101]
[0333] <Manufacturing of raw material ribbon (Fe-based amorphous alloy ribbon before laser processing)>
[0334] The single roll method was used to produce Fe 82 4B 14 A raw material strip (i.e., a Fe-based amorphous alloy strip before laser processing) having a chemical composition of , a thickness of 25 μm, and a width of 210 mm. 82 4B 14 The “chemical composition” refers to a chemical composition consisting of Fe, Si, B, and impurities, wherein, when the total content of Fe, Si, and B is set to 100 atomic %, the content of Fe is 82 atomic %, the content of B is 14 atomic %, and the content of Si is 4 atomic %.
[0335] The following describes in detail the production of the raw material strip.
[0336] In the production of raw material strips, Fe 82 4B 14 The molten metal of the chemical composition is maintained at a temperature of 1300°C, and then the molten metal is ejected from the slit nozzle onto the surface of the axially rotating cooling roller. The ejected molten metal is quenched and solidified on the surface of the cooling roller to obtain a raw material strip. At this time, the atmosphere around the slit nozzle of the paddle forming the molten metal on the surface of the cooling roller is set to a non-oxidizing gas atmosphere. The slit length of the slit nozzle is set to 210mm, and the slit width is set to 0.6mm. The material of the cooling roller is set to a Cu-based alloy, and the circumferential speed of the cooling roller is set to 27m / s. The pressure of the ejected molten metal and the nozzle gap (i.e., the gap between the front end of the slit nozzle and the surface of the cooling roller) are adjusted so that the maximum cross-sectional height Rt of the free solidification surface of the manufactured raw material strip (in detail, the maximum cross-sectional height Rt of the raw material strip measured along the casting direction) becomes less than 3.0μm.
[0337] <Laser processing>
[0338] A sample piece is cut out from the raw material ribbon, and the cut sample piece is subjected to laser processing, thereby obtaining a laser processed Fe-based amorphous alloy ribbon piece.
[0339] The following describes the details.
[0340] Figure 4 1 is a schematic plan view schematically showing a free solidification surface of a Fe-based amorphous alloy thin ribbon piece (the thin ribbon 10 ) subjected to laser processing.
[0341] Figure 4The length L1 of the thin strip 10 shown (i.e., the length of the sample piece cut from the raw material thin strip) is set to 120 mm, and the width W1 of the thin strip 10 (i.e., the width of the sample piece cut from the raw material thin strip) is set to 25 mm. The sample piece is cut in a direction in which the length direction of the sample piece coincides with the length direction of the raw material thin strip, and the width direction of the sample piece coincides with the width direction of the raw material thin strip.
[0342] The free solidification surface of the cut sample piece is irradiated with pulsed laser light to form a plurality of laser irradiation marks 12 in a point array consisting of a plurality of laser irradiation marks 14 , thereby obtaining a thin ribbon 10 .
[0343] Specifically, on the free solidification surface of the sample piece (the strip 10 before laser processing. The same applies hereinafter.), a plurality of laser irradiation marks 14 are formed in a row in a direction parallel to the width direction of the sample piece, thereby forming a point-line laser irradiation mark 12. The point-line laser irradiation mark 12 is formed to the entire area in the width direction of the sample piece. That is, the length of the sample piece with the point-line laser irradiation mark in the width direction is 100% relative to the full width of the sample piece. This is equivalent to the ratio of the length of the linear laser irradiation mark in the width direction to the total length of the Fe-based amorphous alloy strip in the width direction being 50% in the direction from the center in the width direction to the two ends in the width direction.
[0344] A plurality of point-array laser irradiation marks 12 are formed. The directions of the plurality of point-array laser irradiation marks 12 are parallel.
[0345] Table 9 shows the hole spacing SP1 (i.e., the center point spacing of the laser irradiation marks 14 ) and the line spacing LP1 (i.e., the center line spacing of the laser irradiation marks 12 ) in the point array shape laser irradiation marks 12 .
[0346] In addition, the number density (number / mm) of laser irradiation marks on the ribbon 10 2 ) are shown in Table 9. The number density D of laser irradiation marks (pieces / mm 2 ) is calculated according to the following formula.
[0347] D=(1 / d1)×(1 / d2)
[0348] Wherein, d1 represents the row spacing (unit: mm), and d2 represents the hole spacing (unit: mm).
[0349] The pulse laser irradiation conditions are as follows.
[0350] - Pulse laser irradiation conditions -
[0351] As a laser oscillator, a pulse fiber laser (YLP-HP-2-A30-50-100) from IPG Photonics was used. The laser medium of the laser oscillator was Yb-doped glass fiber, and the oscillation wavelength was 1064 nm. The diameter of the emitted beam from the collimator at the fiber end of the above laser oscillator was set to 6.2 mm.
[0352] On the other hand, the spot diameter of the laser light on the free solidification surface of the sample piece was adjusted to 60.8 μm. The beam diameter was adjusted using a beam expander (BE) as an optical component and a condenser lens with fθ:f254 mm (focal length 254 mm).
[0353] The beam mode M2 is set to 3.3 (multi-mode).
[0354] The output of the laser was set to 2.0 mJ, and the pulse width of the laser was set to 250 nsec.
[0355] The magnification of the beam by BE was set to 3 times, and the Focus was set to 0 mm. Here, Focus refers to the difference (absolute value) between the focal length of the condenser (254 mm) and the actual distance from the condenser to the free solidification surface of the ribbon.
[0356] In addition, between the incident diameter D and the spot diameter D0, the relationship D0=4λf / πD (here, λ represents the wavelength of the laser and f represents the focal distance) holds. Therefore, as the beam expansion factor BE increases (that is, as the incident diameter D increases), the spot diameter D0 tends to decrease.
[0357] In the above irradiation conditions, when the energy density is defined as the value of the laser output (2.0 mJ) divided by the beam diameter (60.8 μm) of the laser on the free solidification surface of the sample, the energy density is expressed in J / mm. 2 When the unit indicates energy density, it becomes 0.689J / mm 2 .
[0358] <Measurement and evaluation>
[0359] Fe-based amorphous alloy ribbon ( Figure 4 The following measurements and evaluations were performed on the thin strip 10). The results are shown in Table 9.
[0360] (Maximum cross-sectional height Rt of non-laser processing area)
[0361] In the free solidification surface of the Fe-based amorphous alloy thin strip that has been laser processed, for the portion other than the point-array laser irradiation marks 12 (i.e., the non-laser processed area), the maximum cross-sectional height Rt is measured according to JIS B 0601:2001, with the evaluation length set to 4.0 mm, the critical value set to 0.8 mm, and the critical type set to 2RC (phase compensation). Here, the direction of the evaluation length is set in a manner that becomes the casting direction of the raw material thin strip. In detail, the above measurement with the evaluation length set to 4.0 mm is performed by continuously measuring 5 times with the critical value of 0.8 mm. The above measurement with the evaluation length set to 4.0 mm is performed on 3 locations in the non-laser processed area, and the average value of the three measured values obtained is set as the maximum cross-sectional height Rt (μm) of this embodiment.
[0362] (Determination of Iron Loss CL)
[0363] The iron loss CL of the laser processed Fe-based amorphous alloy strip was measured using an AC magnetometer with sinusoidal excitation under two conditions: a frequency of 60 Hz and a magnetic flux density of 1.45 T and a frequency of 60 Hz and a magnetic flux density of 1.50 T.
[0364] (Determination of excitation power VA)
[0365] The excitation power VA of the laser processed Fe-based amorphous alloy strip was measured by using an AC magnetic measuring device with sinusoidal excitation under the conditions of a frequency of 60 Hz and a magnetic flux density of 1.45 T and a frequency of 60 Hz and a magnetic flux density of 1.50 T.
[0366] (Measurement of magnetic flux density B0.08)
[0367] The magnetic flux density B0.08 of the laser-processed Fe-based amorphous alloy ribbon was measured under the conditions of a frequency of 60 Hz and a magnetic field of 8 A / m.
[0368] [Comparative Example 101]
[0369] The same operation as in Example 101 was performed except that the laser processing was not performed. The results are shown in Tables 9 and 10.
[0370] [Examples 102 to 114, Comparative Examples 102 to 104]
[0371] The same operation as in Example 101 was performed except that the combination of the hole spacing and the row spacing was changed as shown in Tables 9 and 10.
[0372] In addition, in these examples, the maximum cross-sectional height Rt has different values, but the maximum cross-sectional height Rt is not intentionally controlled. In the range of the maximum cross-sectional height Rt being 3.0 μm or less, it is technically difficult to intentionally control the maximum cross-sectional height Rt. The results are shown in Tables 9 and 10.
[0373] [Comparative Example 105]
[0374] The same evaluation as in Comparative Example 101 was performed except that the pressure and the nozzle gap for ejecting the molten metal were adjusted so that the maximum cross-sectional height Rt exceeded 3.0 μm. The results are shown in Table 10. In the Fe-based amorphous alloy ribbon of Comparative Example 105, wavy irregularities were formed on the free solidification surface.
[0375]
[0376]
[0377] As shown in Tables 9 and 10, the hole spacing (i.e., the center point spacing of the plurality of laser irradiation marks) is 0.10 mm to 0.50 mm, and the number density D of the laser irradiation marks is 0.05 / mm 2 ~0.50pcs / mm 2 The Fe-based amorphous alloy ribbons of Examples 101 to 114 reduce the iron loss CL and the excitation power VA under the condition of a magnetic flux density of 1.45 T. In addition, the row interval (i.e., the center line interval of a plurality of point-line laser irradiation marks) of Examples 101 to 114 is 10 mm to 60 mm.
[0378] On the other hand, in the Fe-based amorphous alloy ribbon of Comparative Example 101 in which no laser irradiation mark is formed, the iron loss CL is high.
[0379] In addition, in the Fe-based amorphous alloy ribbon of Comparative Example 102 in which the hole interval is less than 0.10 mm, although the iron loss CL is reduced, the excitation power VA is high.
[0380] In addition, in the Fe-based amorphous alloy ribbons of Comparative Examples 103 and 104 in which the line interval is less than 10 mm, although the iron loss CL is reduced, the excitation power VA is high.
[0381] In addition, in the Fe-based amorphous alloy ribbon of Comparative Example 105 which has no laser irradiation marks and in which the maximum cross-sectional height Rt in the non-laser processed region of the free solidification surface exceeds 3.0 μm, although the iron loss CL is reduced, the excitation power VA is high.
[0382] <Shape of laser irradiation marks>
[0383] The shapes of the laser irradiation marks of the Fe-based amorphous alloy ribbons of Examples 101 to 114 when viewed from above were observed using an optical microscope. As a result, in any of the Examples, the shapes of the laser irradiation marks when viewed from above were all crown-shaped. Here, the crown-shaped means a shape in which traces of molten alloy scattering remain at the edge of the laser irradiation mark.
[0384] However, Fe 82 4B 14 The saturation magnetic flux density Bs of the Fe-based amorphous alloy ribbons of Examples 101 to 114 with the chemical composition is 1.63T.
[0385] In Examples 101 to 114, the iron loss CL and excitation power VA under the condition of a magnetic flux density of 1.45 T are examples in which it is assumed that an Fe-based amorphous alloy thin strip is used to satisfy the ratio [operating magnetic flux density Bm / saturation magnetic flux density Bs] of 0.89 (=1.45 / 1.63), and the iron loss CL and excitation power VA under the condition of a magnetic flux density of 1.50 T are examples in which it is assumed that an Fe-based amorphous alloy thin strip is used to satisfy the ratio [operating magnetic flux density Bm / saturation magnetic flux density Bs] of 0.92 (=1.50 / 1.63).
[0386] Based on the results of Tables 9 and 10, it can be expected that the Fe-based amorphous alloy thin strips of Examples 101 to 114 can suppress iron loss and excitation power even when used with an operating magnetic flux density Bm that satisfies the ratio [operating magnetic flux density Bm / saturation magnetic flux density Bs] of 0.88 to 0.94.
Claims
1. A transformer, characterized in that: A plurality of point-array laser irradiation marks are provided on at least one surface of the Fe-based amorphous alloy thin strip along a direction perpendicular to the casting direction of the Fe-based amorphous alloy thin strip. When the center line spacing of the central parts of the width direction orthogonal to the casting direction between the adjacent point-array laser irradiation marks among the plurality of point-array laser irradiation marks is set as the row spacing, and the center point spacing of each laser irradiation mark constituting the point-array laser irradiation marks is set as the hole spacing, the hole spacing is 0.10 mm to 0.50 mm, the row spacing is set as d1 (mm), and the hole spacing is set as d2 (mm), and the number density D of the laser irradiation marks is set as D = (1 / d1) × (1 / d2), the number density D of the laser irradiation marks is 0.05 pieces / mm 2 ~0.50pcs / mm 2 , The invention comprises an iron core composed of an Fe-based amorphous alloy thin strip having an iron loss of 0.150 W / kg or less at a frequency of 60 Hz and a magnetic flux density of 1.45 T in a single plate using the Fe-based amorphous alloy thin strip, and a winding wound on the iron core.
2. The transformer according to claim 1, characterized in that: The transformer is a single-phase transformer, and the no-load loss per unit weight of the iron core is less than 0.15 W / kg at 50 Hz, or less than 0.19 W / kg at 60 Hz.
3. The transformer according to claim 1, characterized in that: The transformer is a three-phase transformer, and the no-load loss per unit weight of the iron core is less than 0.19 W / kg at 50 Hz, or less than 0.24 W / kg at 60 Hz.
4. The transformer according to any one of claims 1 to 3, characterized in that: The rated capacity of the transformer is above 10 kVA.
5. The transformer according to any one of claims 1 to 3, characterized in that: The row interval d1 is 10 mm to 60 mm.
6. The transformer according to any one of claims 1 to 3, characterized in that: The ratio of the length of the point array laser irradiation marks in the width direction to the entire length of the Fe-based amorphous alloy ribbon in the width direction is in the range of 10% to 50% in the direction from the center in the width direction to both ends in the width direction.
7. The transformer according to any one of claims 1 to 3, characterized in that: The Fe-based amorphous alloy thin strip has a thickness of 18 μm to 35 μm.
8. The transformer according to any one of claims 1 to 3, characterized in that: The Fe-based amorphous alloy strip is composed of Fe, Si, B, and impurities. When the total content of Fe, Si, and B is set to 100 atomic %, the content of Fe is more than 78 atomic %, the content of B is more than 10 atomic %, and the total content of B and Si is 17 atomic % to 22 atomic %.
9. The transformer according to any one of claims 1 to 3, characterized in that: The Fe-based amorphous alloy thin strip has a free solidification surface and a roll surface, and the maximum cross-sectional height Rt of the free solidification surface excluding the point array laser irradiation mark portion is 3.0 μm or less.
10. The transformer according to any one of claims 1 to 3, characterized in that: The point array laser irradiation marks are formed in at least six regions in the center in the width direction, excluding two regions at both ends, from eight regions obtained by dividing the Fe-based amorphous alloy thin strip into eight equal regions in the width direction.
Citation Information
Patent Citations
Magnetic improving method of amorphous alloy thin strip
JP1986029103A
Thermal battery
JP1986029103B2
Manufacture of amorphous alloy thin strip of excellent magnetic properties and device thereof
JP1986258404A
Manufacture of amorphous alloy thin belt having extremely low iron loss
JP1990053935B2
JP1991032886B2