Slow tensile and creep test device in high temperature liquid lead-bismuth environment and use method

By designing a slow tensile and creep test device in a high-temperature liquid lead-bismuth environment, the problem of insufficient corrosion performance data of domestic materials in a high-temperature liquid lead-bismuth environment is solved, and the slow tensile and creep of metal materials in this environment is achieved. Reliable tests of variable behavior provide an assessment of material mechanical behavior and embrittlement damage.

CN113203633BActive Publication Date: 2024-11-22INST OF METAL RESEARCH - CHINESE ACAD OF SCI +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110408489.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-04-16
Publication Date
2024-11-22
Estimated Expiration
2041-04-16

AI Technical Summary

Technical Problem

In high-temperature liquid lead-bismuth environments, the corrosion performance data of domestic materials accumulates less, and the lack of suitable testing devices limits the development of lead-cooled fast reactors.

Method used

A slow tensile and creep test device in a high-temperature liquid lead-bismuth environment is designed, including a slow tensile test machine, a tensile kettle body, a storage kettle, a heater, a hydraulic lifting cylinder, a pallet, a conduction pipe, etc., through The control cabinet realizes precise control of test parameters, including real-time recording of temperature, dissolved oxygen concentration, displacement and load.

Benefits of technology

This device can conduct slow tensile and creep behavior research on metal materials in high-temperature liquid lead-bismuth environment, realizing stable tensile and creep tests of the sample in liquid lead-bismuth, providing simple operation and no contact with lead-bismuth steam test conditions to help evaluate the mechanical behavior of materials and brittle damage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003023232060000011
    Figure HDA0003023232060000011
  • Figure HDA0003023232060000021
    Figure HDA0003023232060000021
  • Figure HDA0003023232060000022
    Figure HDA0003023232060000022
Patent Text Reader

Abstract

The present invention relates to the field of slow tensile testing, and specifically to a slow tensile and creep testing device in a high-temperature liquid lead-bismuth environment and a method of use. The device comprises: a slow tensile testing machine, a tensile kettle body, a storage kettle, a heater, a column, a hydraulic lifting cylinder, a tray, a conducting pipe, a tensile shaft, a first support plate, a second support plate, a bottom steel plate, a clamping block, a tensile kettle cover, and a hydraulic pump. When the temperature of the tensile kettle, the storage kettle, and the conducting pipe is greater than 250°C, high-purity argon or high-purity nitrogen is passed through the air inlet of the storage kettle to make the liquid lead-bismuth alloy in the storage kettle flow into the tensile kettle, and high-purity argon or high-purity nitrogen is passed through the air inlet of the tensile kettle to make the liquid lead-bismuth alloy in the tensile kettle flow into the storage kettle. The present invention can accurately control the test parameters such as the temperature, tensile rate (displacement control or load control), constant load, and constant strain of the liquid lead-bismuth alloy, and evaluate the slow tensile and creep behavior of metal materials in a high-temperature liquid lead-bismuth environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of tensile and creep testing, and in particular to a slow tensile and creep testing device in a high-temperature liquid lead-bismuth environment and a use method thereof, which are used for testing the tensile and creep properties of a tensile specimen in a liquid lead-bismuth environment, and for evaluating the mechanical behavior and embrittlement damage behavior of a metal material in the liquid lead-bismuth environment. Background Art

[0002] Due to its high boiling point, no heat release from reaction with water or air, strong transmutation ability and excellent neutron economy, lead or lead-bismuth eutectic is the preferred coolant for special reactor types such as the fourth-generation commercial lead-cooled fast reactor and accelerator-driven advanced nuclear energy system, as well as future space reactors and small reactors. It has broad application prospects and is currently a hot topic in international research. The operating temperature of the lead-bismuth reactor is as high as 450-550°C, and the service performance and safety of its equipment materials are key. The corrosion performance of metal materials in a high-temperature liquid lead-bismuth environment is one of the key issues restricting the development of lead-cooled fast reactors. my country is working hard to tackle the fourth-generation lead-cooled fast reactor. However, there is little accumulation of basic data on the corrosion of domestic candidate materials in a liquid lead-bismuth environment. To carry out research on the environmental compatibility of materials in liquid lead-bismuth, it is first necessary to independently develop relevant testing devices. Based on this, the present invention develops a slow tensile and creep test device and a method of use in a high-temperature liquid lead-bismuth environment, which can be used to carry out research on the slow tensile and creep behavior of metal materials in a liquid lead-bismuth environment. Summary of the invention

[0003] The purpose of the present invention is to provide a slow tensile and creep test device and a use method in a high-temperature liquid lead-bismuth environment, so as to realize the study of the slow tensile and creep behavior of metal materials in a high-temperature liquid lead-bismuth environment.

[0004] The technical solution of the present invention is:

[0005] A slow tensile and creep test device in a high-temperature liquid lead-bismuth environment, characterized in that the device comprises: a slow tensile testing machine, a tensile kettle body, a storage kettle, a heater, a column, a hydraulic lifting cylinder, a tray, a conducting pipe, a tensile shaft, a first support plate, a second support plate, a bottom steel plate, a clamping block, a tensile kettle cover, and a hydraulic pump. The specific structure is as follows:

[0006] The fuselage fixing frame is composed of a bottom steel plate, two columns, a first support plate, and a second support plate. The bottom steel plate is fixed to the ground by anchor bolts. Two vertical columns are relatively parallel and respectively connected to the bottom steel plate by threads. The horizontal first support plate and the second support plate are relatively parallel and arranged on the two columns. The first support plate is fixed to the upper part of the two columns by a clamping block, and the second support plate is in sliding cooperation with the two columns.

[0007] The stretching kettle body is buckled with a stretching kettle cover, and the outer side of the stretching kettle body is wrapped with a heater to form a stretching kettle; the first support plate is fixedly mounted on the two columns of the fuselage fixing frame by threaded tightening and clamping, the slow stretching tester is connected to the first support plate by bolts, and the output end of the slow stretching tester is connected to the stretching sample in the stretching kettle body through the first support plate and the stretching kettle cover through the stretching shaft, and the stretching sample is mounted on the sample rack;

[0008] The outer side of the stretching kettle cover is connected to the tray by threads, and the horizontal tray is fixed on the two columns of the fuselage fixing frame by tightening and clamping the threads; the stretching kettle body is arranged on the second support plate, the bottom of the second support plate is connected to the hydraulic lifting cylinder, and the output end of the hydraulic pump is connected to the hydraulic lifting cylinder to realize the lifting and lowering of the stretching kettle body on the two columns, as well as the opening and closing of the stretching kettle cover; the inner cavity of the stretching kettle body is connected to the inner cavity of the storage kettle by a conducting pipe, the outer side of the storage kettle and the conducting pipe is wrapped with a heater, and the lead-bismuth alloy is placed in the stretching kettle body or the storage kettle.

[0009] The control cabinet of the slow tensile testing machine and the creep testing device in the high-temperature liquid lead-bismuth environment is connected with the slow tensile testing machine, the tensile kettle heater and its thermocouple, the storage kettle heater and its thermocouple, the conduction tube heater and its thermocouple, and the hydraulic lifting cylinder to realize the control of the slow tensile testing machine and the hydraulic lifting cylinder, as well as the temperature control of the tensile kettle, the storage kettle, and the conduction tube heaters, and collect test data.

[0010] The slow stretching and creep test device in a high-temperature liquid lead-bismuth environment has a copper gasket placed between the stretching kettle body and the stretching kettle cover, and sealing is achieved by tightening the bolts. The stretching kettle cover is provided with an air inlet, an air outlet, a conducting pipe mounting port, an electrode mounting port, a displacement sensor mounting port, a thermocouple mounting port and a stretching shaft through hole, and the stretching shaft and the stretching kettle cover are dynamically sealed by an O-ring and a water cooling jacket.

[0011] The slow tensile and creep test device in a high-temperature liquid lead-bismuth environment uses a linear slider to clamp two columns, and uses bolts to connect the linear slider to the bottom steel plate, so that the two columns are fixed on the bottom steel plate without gap.

[0012] The method for using the slow tensile and creep test device in a high-temperature liquid lead-bismuth environment comprises the following specific steps:

[0013] (1) placing the lead-bismuth alloy into a storage kettle;

[0014] (2) Use a wiping paper to clean the storage kettle body and the sealing surface of the storage kettle cover, wipe the copper gasket clean and put it into the sealing groove on the top of the storage kettle body, and place the kettle cover on the kettle body;

[0015] (3) Install the tensile test specimen in the tensile kettle body, wipe the tensile kettle body and the sealing surface of the tensile kettle cover with wiping paper, wipe the copper gasket clean and put it into the sealing groove on the top of the tensile kettle body, and place the tensile kettle cover on the tensile kettle body;

[0016] (4) Inert gas is filled into the kettle body from the air inlet of the storage kettle and the stretching kettle respectively, and the air in the kettle body is removed, so that the inside of the kettle body is in an inert gas protection state;

[0017] (5) Setting the target temperature on the control cabinet, the initial target temperature of the storage kettle and the conducting tube is 250°C ± 10°C, and the target temperature of the stretching kettle body is 200°C. The temperature is then raised and maintained for 20 to 40 minutes after reaching the target temperature value, so that the lead-bismuth alloy in the storage kettle is completely melted;

[0018] (6) Connect high-purity argon gas to the air inlet of the storage kettle, open the air inlet valve of the storage kettle, close the air outlet valve of the storage kettle, close the air inlet valve of the stretching kettle, and open the air outlet valve of the stretching kettle;

[0019] (7) starting to blow high-purity argon gas into the storage kettle at a rate of 0.1 to 1 L / min, and using gas pressure to push the liquid lead-bismuth alloy into the stretching kettle through the conducting pipe;

[0020] (8) After the liquid lead-bismuth alloy in the stretching kettle body completely immerses the stretching specimen, close the air inlet valve of the storage kettle and keep the air outlet valve closed, and close the air outlet valve of the stretching kettle body and keep the air inlet valve closed;

[0021] (9) Lower the temperature of the stretching kettle to 180°C ± 10°C;

[0022] (10) After preheating the dissolved oxygen electrode at a temperature of 150 to 200° C. for 20 to 40 minutes, the dissolved oxygen electrode is completely inserted into the liquid lead-bismuth alloy and sealed; the dissolved oxygen electrode is connected to a high-precision voltmeter to measure and collect the dissolved oxygen value in the liquid lead-bismuth alloy in real time;

[0023] (11) Starting to heat the stretching kettle body to the target value;

[0024] (12) Turn on the slow tensile testing machine and enter the test parameters;

[0025] (13) Start the experiment;

[0026] (14) The specimen is pulled apart or the test is continued until the target time. After the test is completed, the experimental data is saved;

[0027] (15) Start cooling down. When the temperature drops to 250°C ± 10°C, take out the dissolved oxygen electrode and keep the kettle sealed;

[0028] (16) Connect high-purity argon gas to the air inlet of the stretching kettle, open the air outlet valve of the storage kettle, keep the air inlet valve closed, open the air inlet valve of the stretching kettle, and keep the air outlet valve closed;

[0029] (17) starting to blow high-purity argon gas into the stretching kettle body at a rate controlled at 0.1 to 1 L / min, and using gas pressure to push the liquid lead-bismuth alloy into the storage kettle through the conducting pipe;

[0030] (18) Cool the storage kettle, the stretching kettle body and the conducting tube to room temperature, open the stretching kettle body, remove the sample and store it properly;

[0031] (19) Close the tensile test chamber lid and the test is complete.

[0032] The method for using the slow stretching and creep testing device in a high-temperature liquid lead-bismuth environment is as follows: when the temperature of the stretching kettle, the storage kettle, and the conducting tube is greater than 250°C, high-purity argon or high-purity nitrogen is passed through the air inlet of the storage kettle to allow the liquid lead-bismuth alloy in the storage kettle to flow into the stretching kettle; and high-purity argon or high-purity nitrogen is passed through the air inlet of the stretching kettle to allow the liquid lead-bismuth alloy in the stretching kettle to flow into the storage kettle.

[0033] The advantages and beneficial effects of the present invention are:

[0034] 1. The present invention provides a slow tensile and creep test device in a high-temperature liquid lead-bismuth environment and a method for using the same. The test device includes a slow tensile test machine, a fuselage fixing frame, a tensile kettle, a sample rack, a tray, a storage kettle, a conducting pipe, a hydraulic lifting cylinder, a control cabinet, a heater, a lead-bismuth alloy, etc., and can carry out slow tensile and creep tests of tensile specimens in a high-temperature liquid lead-bismuth environment, and record and collect test parameters such as temperature, dissolved oxygen concentration, displacement, load, and strain in real time. The tensile specimen is mounted on the sample rack, the lead-bismuth alloy is placed in the tensile kettle body, and the temperature is raised to the target value using the control cabinet and the heater, so that the slow tensile and creep behavior of metal materials in a high-temperature liquid lead-bismuth environment can be studied.

[0035] 2. The device of the present invention connects the stretching kettle and the storage kettle through a conducting pipe to realize the transfer of high-temperature liquid lead and bismuth between the stretching kettle and the storage kettle, which is convenient for loading and unloading the stretching specimen in normal temperature air. The operation is simple and convenient and does not contact the lead and bismuth vapor.

[0036] 3. The present invention can accurately control the temperature, stretching rate (displacement control or load control), constant load, constant strain and other test parameters of the liquid lead-bismuth alloy, and evaluate the slow stretching and creep behavior of metal materials in a high-temperature liquid lead-bismuth environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1The structure diagram of the device of the present invention is shown in the figure: 1 slow tensile testing machine; 2 tensile kettle body; 3 storage kettle; 4 heater; 5 column; 6 hydraulic lifting cylinder; 7 tray; 8 conducting pipe; 9 tensile shaft; 10 first support plate; 11 second support plate; 12 bottom steel plate; 13 control cabinet; 14 sample rack; 15 clamp block; 16 tensile kettle cover; 17 hydraulic pump.

[0038] Figure 2 This is the tensile curve in liquid lead-bismuth environment. In the figure, the horizontal axis Stroke represents displacement (mm), and the vertical axis Stress represents stress (MPa).

[0039] Figure 3 This is the morphology of the tensile specimen after the liquid lead-bismuth slow tensile test in the example. DETAILED DESCRIPTION

[0040] like Figure 1 As shown, the slow tensile and creep test device in a high-temperature liquid lead-bismuth environment of the present invention comprises: a slow tensile testing machine 1, a tensile kettle body 2, a storage kettle 3, a heater 4, a column 5, a hydraulic lifting cylinder 6, a tray 7, a conducting pipe 8, a tensile shaft 9, a first support plate 10, a second support plate 11, a bottom steel plate 12, a control cabinet 13, a sample rack 14, a clamping block 15, a tensile kettle cover 16, a hydraulic pump 17, etc. The specific structure is as follows:

[0041] The fuselage fixing frame is composed of a bottom steel plate 12, two columns 5, a first support plate 10, and a second support plate 11. The bottom steel plate 12 is fixed to the ground by anchor bolts. The two vertical columns 5 are arranged relatively parallel and connected to the bottom steel plate 12 by threads respectively, and the two columns 5 can be clamped by a linear slider. The linear slider is connected to the bottom steel plate 12 by bolts, and the two columns 5 are tightly fixed to the bottom steel plate 12 without gaps. The horizontal first support plate 10 and the second support plate 11 are arranged relatively parallel to the two columns 5 up and down. The first support plate 10 is tightly fixed to the upper part of the two columns 5 by a clamping block 15, and the second support plate 11 is in sliding cooperation with the two columns 5.

[0042] The stretching kettle body 2 is buckled with a stretching kettle cover 16, a copper gasket is placed between the stretching kettle body 2 and the stretching kettle cover 16, and the seal is achieved by tightening the bolts. The outer side of the stretching kettle body 2 is wrapped with a heater 4, and the stretching kettle cover 16 is provided with an air inlet, an air outlet, a conducting pipe mounting port, an electrode mounting port, a displacement sensor mounting port, a thermocouple mounting port and a stretching shaft through hole to form a stretching kettle; the control cabinet 13 is connected to the heater 4 (matching the thermocouple) through a line, and the control cabinet 13 is used for power supply and temperature control to achieve temperature control of the lead-bismuth alloy in the stretching kettle body 2; the first support plate 10 is fixedly mounted on the two ends of the fuselage fixing frame by threaded tightening and clamping. On the root column 5, the slow tensile testing machine 1 is connected to the first support plate 10 by bolts, the control cabinet 13 is connected to the slow tensile testing machine 1 through the line, the output end of the slow tensile testing machine 1 passes through the first support plate 10 and the tensile kettle cover 16 through the tensile shaft 9 and is connected to the tensile specimen in the tensile kettle body 2, the tensile shaft 9 is used to connect the tensile specimen (standard rod-shaped and sheet-shaped tensile specimen) and the slow tensile testing machine 1, the tensile shaft 9 and the tensile kettle cover 16 are dynamically sealed by the O-ring and the water cooling jacket, the slow tensile testing machine 1 has load control and displacement control modes, and can realize slow strain rate stretching, constant load, constant strain, strain measurement and other functions.

[0043] The outer side of the stretching kettle cover 16 is connected to the tray 7 by threads, and the horizontal tray 7 is fixedly installed on the two columns 5 of the fuselage fixing frame by tightening and clamping the threads; the stretching kettle body 2 is arranged on the second support plate 11, and the bottom of the second support plate 11 is connected to the hydraulic lifting cylinder 6, and the control cabinet 13 is connected to the hydraulic pump 17 through the line, and the output end of the hydraulic pump 17 is connected to the hydraulic lifting cylinder 6, so as to realize the lifting and lowering of the stretching kettle body 2 on the two columns 5, and the opening and closing of the stretching kettle cover 16; the inner cavity of the stretching kettle body 2 is connected to the inner cavity of the storage kettle 3 through the conducting pipe 8, and the outer side of the storage kettle 3 is wrapped with a heater 4 (matching thermocouple), and the control cabinet 13 is connected to the heater 4 through the line, and the control cabinet 13 is powered and temperature controlled, and the lead-bismuth alloy is placed in the stretching kettle body 2 or the storage kettle 3. In addition, the outer side of the conducting pipe 8 can also be wrapped with a heater (matching thermocouple), and the control cabinet 13 is connected to the heater through the line, and the control cabinet 13 is powered and temperature controlled.

[0044] The tensile specimen is mounted on the specimen rack 14, the lead-bismuth alloy is placed in the tensile kettle body 2 or the storage kettle 3, and the temperature is raised to the target value by the control cabinet 13 and the heater 4, so that the slow tensile and creep behavior of the metal material in the high-temperature liquid lead-bismuth environment can be studied. When the temperature of the tensile kettle, the storage kettle 3, and the conducting pipe 8 is greater than 250°C, the liquid lead-bismuth alloy in the storage kettle 3 can flow into the tensile kettle by passing high-purity argon or high-purity nitrogen (99.999% by volume) into the air inlet of the storage kettle 3, and the liquid lead-bismuth alloy in the tensile kettle can flow into the storage kettle by passing high-purity argon or high-purity nitrogen (99.999% by volume) into the air inlet of the tensile kettle. The control cabinet 13 is connected to the slow tensile testing machine 1, the stretching kettle heater and thermocouple, the storage kettle heater and thermocouple, the conduction tube heater and thermocouple, and the hydraulic lifting cylinder to realize the control of the slow tensile testing machine and the hydraulic lifting cylinder, as well as the temperature control of the stretching kettle, storage kettle, and the conduction tube heater, and collect test data.

[0045] Example

[0046] In this embodiment, the tensile test specimen is P92 ferrite / martensitic steel, and the slow tensile test is carried out in a 350°C liquid lead-bismuth environment under saturated dissolved oxygen concentration conditions, with a tensile rate of 4×10 -6 s -1 , rod-shaped tensile specimen, gauge section diameter is 5mm and length is 30mm.

[0047] like Figure 1 As shown, the device of the present invention can carry out slow tensile and creep test research of metal materials in a liquid lead-bismuth environment, and can control / collect test temperature, dissolved oxygen concentration in liquid lead-bismuth alloy, displacement, load, strain and other parameters in real time. The use steps are as follows:

[0048] (1) Place an appropriate amount of lead-bismuth alloy into a storage kettle.

[0049] (2) Use a cleaning paper to clean the storage kettle body and the sealing surface of the storage kettle cover. After cleaning, put the copper gasket into the sealing groove on the top of the storage kettle body. Place the storage kettle cover on the kettle body and tighten the bolts with a torque wrench. The recommended maximum torque is 100-150N·m.

[0050] (3) Install the tensile specimen in the tensile kettle body, wipe the tensile kettle body and the sealing surface of the tensile kettle cover with a wipe paper, wipe the copper gasket clean and put it into the sealing groove on the top of the tensile kettle body, place the tensile kettle cover on the tensile kettle body, and tighten the bolts with a torque wrench. The recommended maximum torque is 100-150N·m.

[0051] (4) Inert gas (high-purity argon or high-purity nitrogen) is filled into the kettle body from the air inlet of the storage kettle and the stretching kettle respectively, and the air in the kettle body is removed, so that the inside of the kettle body is in an inert gas protection state.

[0052] (5) Set the target temperature on the control cabinet. The recommended initial target temperature of the storage kettle and the conducting tube is about 250°C (higher than the melting point of the lead-bismuth eutectic, so that the lead-bismuth alloy is converted from solid to liquid). The target temperature of the stretching kettle is 200°C. Start heating and maintain the target temperature for about 30 minutes after reaching the target temperature value to completely melt the lead-bismuth alloy in the storage kettle.

[0053] (6) Connect high-purity argon gas to the air inlet of the storage kettle, open the air inlet valve of the storage kettle, close the air outlet valve of the storage kettle, close the air inlet valve of the stretching kettle, and open the air outlet valve of the stretching kettle.

[0054] (7) High-purity argon gas is blown into the storage kettle at a rate of 0.1 to 1 L / min. The liquid lead-bismuth alloy is forced into the stretching kettle through the conducting tube by gas pressure. At the same time, the thermocouple in the stretching kettle is observed. When the temperature suddenly changes, it indicates that the liquid level of the liquid lead-bismuth alloy has reached the position where the thermocouple is installed.

[0055] (8) After the liquid lead-bismuth alloy in the stretching kettle body completely immerses the stretching specimen, close the air inlet valve of the storage kettle (while keeping the air outlet valve closed), and close the air outlet valve of the stretching kettle body (while keeping the air inlet valve closed).

[0056] (9) Reduce the temperature of the stretching kettle to about 180°C.

[0057] (10) After preheating the dissolved oxygen electrode at 180° C. for 30 minutes, the dissolved oxygen electrode is completely inserted into the liquid lead-bismuth alloy and sealed. The dissolved oxygen electrode is connected to a high-precision voltmeter (with an accuracy of 0.01 mV) to measure and collect the dissolved oxygen value in the liquid lead-bismuth alloy in real time.

[0058] (11) Start heating the stretching kettle to the target temperature.

[0059] (12) Turn on the slow tensile testing machine and enter the test parameters (tensile rate or constant load value).

[0060] (13) Start the experiment.

[0061] (14) After the specimen breaks or the test is carried out to the target time, save the experimental data (displacement, load, time, strain, etc.).

[0062] (15) Start cooling down. When the temperature drops to about 250°C (it is forbidden to cool down to the solidification point of lead-bismuth eutectic to avoid damaging the dissolved oxygen electrode), take out the dissolved oxygen electrode and keep the kettle sealed.

[0063] (16) Connect high-purity argon gas to the air inlet of the stretching kettle body, open the air outlet valve of the storage kettle (keep the air inlet valve closed), and open the air inlet valve of the stretching kettle body (keep the air outlet valve closed).

[0064] (17) High-purity argon gas is blown into the stretching kettle body at a rate of 0.1 to 1 L / min. The liquid lead-bismuth alloy is forced into the storage kettle through the conducting tube by gas pressure. At the same time, the thermocouple in the storage kettle is observed. When the temperature suddenly changes, it indicates that the liquid level of the liquid lead-bismuth alloy has reached the position where the thermocouple is installed, and the liquid lead-bismuth alloy in the storage kettle is completely discharged.

[0065] (18) Cool the storage kettle, stretching kettle body and conducting tube to room temperature, open the stretching kettle body, remove the specimen and store it properly.

[0066] (19) Close the tensile test chamber lid and the test is complete.

[0067] Figure 2 is the tensile curve in liquid lead-bismuth environment, Figure 3 is the macroscopic morphology of the sample after the test. Figure 2 and Figure 3 It can be seen that during the stretching process, the displacement and load are controlled stably, the tensile specimen breaks in the gauge section, and the test is effective.

[0068] The results of the embodiments show that the slow tensile and creep test device in a high-temperature liquid lead-bismuth environment of the present invention has reliable performance, can realize the mutual transfer of high-temperature liquid lead-bismuth alloy between the stretching kettle and the storage kettle, and is convenient for loading and unloading samples under normal temperature and air conditions; can accurately control the test temperature in the liquid lead-bismuth environment; the test device remains sealed to prevent leakage of lead-bismuth vapor during the test, and can carry out slow strain rate stretching and constant load (creep) tests on tensile specimens in a liquid lead-bismuth environment.

Claims

1. A method for using a slow tensile and creep test device in a high-temperature liquid lead-bismuth environment, characterized in that: The device includes: a slow tensile testing machine, a tensile kettle body, a storage kettle, a heater, a column, a hydraulic lifting cylinder, a tray, a guide pipe, a tensile shaft, a first support plate, a second support plate, a bottom steel plate, a clamping block, a tensile kettle cover, and a hydraulic pump. The specific structure is as follows: The fuselage fixing frame is composed of a bottom steel plate, two columns, a first support plate, and a second support plate. The bottom steel plate is fixed to the ground by anchor bolts. Two vertical columns are relatively parallel and respectively connected to the bottom steel plate by threads. The horizontal first support plate and the second support plate are relatively parallel and arranged on the two columns. The first support plate is fixed to the upper part of the two columns by a clamping block, and the second support plate is in sliding cooperation with the two columns. The stretching kettle body is buckled with a stretching kettle cover, and the outer side of the stretching kettle body is wrapped with a heater to form a stretching kettle; the first support plate is fixedly mounted on the two columns of the fuselage fixing frame by threaded tightening and clamping, the slow stretching tester is connected to the first support plate by bolts, and the output end of the slow stretching tester is connected to the stretching sample in the stretching kettle body through the first support plate and the stretching kettle cover through the stretching shaft, and the stretching sample is mounted on the sample rack; The outer side of the stretching kettle cover is connected to the tray through threads, and the horizontal tray is fixedly installed on the two columns of the fuselage fixing frame by tightening and clamping the threads; the stretching kettle body is arranged on the second support plate, the bottom of the second support plate is connected to the hydraulic lifting cylinder, and the output end of the hydraulic pump is connected to the hydraulic lifting cylinder to realize the lifting and lowering of the stretching kettle body on the two columns, and the opening and closing of the stretching kettle cover; the inner cavity of the stretching kettle body is connected to the inner cavity of the storage kettle through a conducting pipe, the outer sides of the storage kettle and the conducting pipe are wrapped with a heater, and the lead-bismuth alloy is placed in the stretching kettle body or the storage kettle; The method for using the slow tensile and creep test device in a high-temperature liquid lead-bismuth environment comprises the following specific steps: (1) placing the lead-bismuth alloy into a storage kettle; (2) Use a wiping paper to clean the storage kettle body and the sealing surface of the storage kettle cover, wipe the copper gasket clean and put it into the sealing groove on the top of the storage kettle body, and place the kettle cover on the kettle body; (3) Install the tensile specimen in the tensile kettle body, wipe the tensile kettle body and the sealing surface of the tensile kettle cover with wiping paper, wipe the copper gasket clean and put it into the sealing groove on the top of the tensile kettle body, and place the tensile kettle cover on the tensile kettle body; (4) Inert gas is filled into the kettle body from the air inlet of the storage kettle and the stretching kettle respectively, and the air in the kettle body is removed, so that the inside of the kettle body is in an inert gas protection state; (5) Set the target temperature on the control cabinet. The initial target temperature of the storage kettle and the conducting tube is 250°C ± 10°C, and the target temperature of the stretching kettle is 200°C. Start heating. After reaching the target temperature, maintain it for 20 to 40 minutes to completely melt the lead-bismuth alloy in the storage kettle. (6) Connect high-purity argon gas to the air inlet of the storage kettle, open the air inlet valve of the storage kettle, close the air outlet valve of the storage kettle, close the air inlet valve of the stretching kettle, and open the air outlet valve of the stretching kettle; (7) High-purity argon gas is blown into the storage kettle at a rate of 0.1-1 L / min, and the liquid lead-bismuth alloy is forced into the stretching kettle through the conducting pipe by gas pressure; (8) After the liquid lead-bismuth alloy in the stretching kettle body completely immerses the stretching specimen, close the air inlet valve of the storage kettle and keep the air outlet valve closed, and close the air outlet valve of the stretching kettle body and keep the air inlet valve closed; (9) Reduce the temperature of the stretching kettle to 180℃±10℃; (10) After preheating the dissolved oxygen electrode at a temperature of 150 to 200° C. for 20 to 40 minutes, the dissolved oxygen electrode is completely inserted into the liquid lead-bismuth alloy and sealed; the dissolved oxygen electrode is connected to a high-precision voltmeter to measure and collect the dissolved oxygen value in the liquid lead-bismuth alloy in real time; (11) Start heating the stretching kettle to the target value; (12) Turn on the slow tensile testing machine and enter the test parameters; (13) Start the experiment; (14) After the specimen is broken or the test is carried out to the target time, save the experimental data; (15) Start cooling down. When the temperature drops to 250℃±10℃, take out the dissolved oxygen electrode and keep the kettle sealed; (16) Connect high-purity argon gas to the air inlet of the stretching kettle, open the air outlet valve of the storage kettle, keep the air inlet valve closed, open the air inlet valve of the stretching kettle, and keep the air outlet valve closed; (17) High-purity argon gas is blown into the stretching kettle at a rate of 0.1-1 L / min, and the liquid lead-bismuth alloy is forced into the storage kettle through the conducting pipe by gas pressure; (18) Cool the storage kettle, stretching kettle body and conducting tube to room temperature, open the stretching kettle body, remove the specimen and store it properly; (19) Close the tensile test chamber cover and the test is complete.

2. The method for using the slow tensile and creep test device in a high temperature liquid lead-bismuth environment according to claim 1, characterized in that: When the temperature of the stretching kettle, storage kettle and conducting pipe is greater than 250°C, high-purity argon or high-purity nitrogen is passed through the air inlet of the storage kettle to make the liquid lead-bismuth alloy in the storage kettle flow into the stretching kettle. High-purity argon or high-purity nitrogen is passed through the air inlet of the stretching kettle to make the liquid lead-bismuth alloy in the stretching kettle flow into the storage kettle.

3. The method for using the slow tensile and creep test device in a high temperature liquid lead-bismuth environment according to claim 1, characterized in that: The control cabinet is connected to the slow tensile testing machine, the stretching kettle heater and its thermocouple, the storage kettle heater and its thermocouple, the conduction tube heater and its thermocouple, and the hydraulic lifting cylinder to realize the control of the slow tensile testing machine and the hydraulic lifting cylinder, as well as the temperature control of the stretching kettle, storage kettle, and the conduction tube heaters, and collect test data.

4. The method for using the slow tensile and creep test device in a high temperature liquid lead-bismuth environment according to claim 1, characterized in that: A copper gasket is placed between the stretching kettle body and the stretching kettle cover, and sealing is achieved by tightening the bolts. The stretching kettle cover is provided with an air inlet, an air outlet, a guide tube mounting port, an electrode mounting port, a displacement sensor mounting port, a thermocouple mounting port and a stretching shaft through hole. The stretching shaft and the stretching kettle cover are dynamically sealed by an O-ring and a water cooling jacket.

5. The method for using the slow tensile and creep test device in a high temperature liquid lead-bismuth environment according to claim 1, characterized in that: A linear slider is used to clamp the two columns, and the linear slider is connected to the bottom steel plate by bolts, so that the two columns are fixed on the bottom steel plate without any gap.