A method for preparing polyimide and polytetrafluoroethylene insulation composite film for electric wire

By applying lubricating oil on the surface of polyimide and polytetrafluoroethylene composite film and soaking in curing agent and ink connecting material, combined with plasma treatment, the problem of poor anti-adhesion of composite film is solved, and the use of wires and cables is significantly improved Lifespan and safety.

CN114121341BActive Publication Date: 2024-11-05JIANGSU BAITONG CABLE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111324134.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-10
Publication Date
2024-11-05
Estimated Expiration
2041-11-10

AI Technical Summary

Technical Problem

The existing polyimide and polytetrafluoroethylene insulating composite films for wires have poor anti-adhesion properties, which leads to easy bonding of wires and cables after long-term use, which affects use and may cause short circuits.

Method used

By applying lubricating oil on the surface of the polyimide and polytetrafluoroethylene composite film and soaking in a processing tank where curing agent and ink connecting material are added, combined with plasma treatment, the anti-adhesion performance of the composite film is enhanced.

Benefits of technology

It effectively improves the anti-adhesion performance of polyimide and polytetrafluoroethylene composite films, prevents wires and cables from being bonded in later use, and avoids line damage and short circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114121341B_ABST
    Figure CN114121341B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a polyimide / polytetrafluoroethylene insulation composite film for electric wires, and the specific steps of the method for preparing the polyimide / polytetrafluoroethylene insulation composite film for electric wires are as follows: step 1: placing a polyimide / polytetrafluoroethylene composite film in a production pool, adding an excessive amount of anhydrous ethanol to the interior of the production pool, and completely immersing the polyimide / polytetrafluoroethylene composite film in the anhydrous ethanol for 20-30 minutes, applying lubricating oil on the surface of the composite film, and immersing the composite film in a processing pool with a curing agent and an ink connecting material for a long time, thereby increasing the anti-adhesion performance of the polyimide / polytetrafluoroethylene composite film, and effectively preventing the bonding between the wires and cables in the later use, thereby causing line damage and line short circuit.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite films, in particular to a method for preparing a polyimide and polytetrafluoroethylene insulating composite film for electric wires. Background Art

[0002] As a special engineering material, polyimide has been widely used in aviation, aerospace, microelectronics, nanotechnology, liquid crystal, separation membrane, laser and other fields. In the 1960s, all countries listed the research, development and utilization of polyimide as one of the most promising engineering plastics in the 21st century. Due to its outstanding characteristics in performance and synthesis, the huge application prospects of polyimide, whether as a structural material or as a functional material, have been fully recognized;

[0003] Polytetrafluoroethylene, commonly known as the "king of plastics", is a high molecular polymer made by polymerizing tetrafluoroethylene as a monomer. It is white waxy, translucent, heat-resistant and cold-resistant, and can be used for a long time at -180 to 260°C. This material is resistant to acids, alkalis, and various organic solvents, and is almost insoluble in all solvents. At the same time, polytetrafluoroethylene is resistant to high temperatures and has an extremely low friction coefficient, so it can be used as a lubricant and has also become an ideal coating for the inner layer of easy-to-clean water pipes.

[0004] However, the existing polyimide and polytetrafluoroethylene insulation composite films for wires have relatively poor anti-adhesion properties. After long-term use of wires and cables, adhesion will occur between the wires and cables, thus affecting their use and easily causing short circuits between the wires and cables. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing a polyimide and polytetrafluoroethylene insulating composite film for electric wires, so as to solve the problem that the existing polyimide and polytetrafluoroethylene insulating composite films for electric wires proposed in the above-mentioned background technology have poor anti-adhesion properties, and after the electric wires and cables are used for a long time, adhesion will occur between the electric wires and cables, thereby affecting the use and easily causing a short circuit between the electric wires and cables.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A method for preparing a polyimide and polytetrafluoroethylene insulation composite film for electric wires, the specific steps of the method for preparing a polyimide and polytetrafluoroethylene insulation composite film for electric wires are as follows:

[0008] Step 1: Place the polyimide / polytetrafluoroethylene composite membrane into the production pool, add an excess of anhydrous ethanol into the production pool, and completely immerse the polyimide / polytetrafluoroethylene composite membrane in the anhydrous ethanol for 20-30 minutes;

[0009] Step 2: Take out the polyimide / polytetrafluoroethylene composite membrane, use filter paper to absorb excess anhydrous ethanol on the surface of the polyimide / polytetrafluoroethylene composite membrane, leave it for 10-20 minutes after complete treatment, and then apply a layer of adhesive glue on the surface of the polyimide / polytetrafluoroethylene composite membrane;

[0010] Step 3: Apply a layer of curing agent on the outer surface of the polyimide / polytetrafluoroethylene composite film, dry it for 30-40 minutes, and then apply another layer of curing agent. Repeat the operation three times;

[0011] Step 4: Place the polyimide / polytetrafluoroethylene composite membrane in step 3 inside a treatment tank, add excess lubricating oil and ink vehicle into the tank, mix the lubricating oil and ink vehicle completely, and soak the polyimide / polytetrafluoroethylene composite membrane in the tank for 30-40 minutes;

[0012] Step 5: Place the soaked polyimide / polytetrafluoroethylene composite film into the interior of the plasma multifunctional experimental table reaction chamber, adjust the voltage to 400-500V, and perform plasma treatment for 2-3 hours under inert gas and a certain working pressure.

[0013] Preferably, the inert gas includes nitrogen, argon and helium, and the working pressure needs to be set to 500-1000Pa.

[0014] Preferably, the curing agent includes vinyltriamine, aminoethylpiperazine, and aromatic amines; and the lubricating oil includes perfluoropolyether, perfluorotripentylamine, and perfluorotributylamine.

[0015] Preferably, the polyimide / polytetrafluoroethylene composite membrane is prepared by a tape casting method, and the polyimide / polytetrafluoroethylene composite membrane is 200-300 um.

[0016] Preferably, the bonding glue and curing agent need to be evenly applied by machine.

[0017] Preferably, the temperature of the polyimide / polytetrafluoroethylene composite membrane needs to be controlled at 20-30 degrees Celsius during the entire processing process.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] During the processing of the polyimide / polytetrafluoroethylene composite film, lubricating oil is applied to the surface of the polyimide / polytetrafluoroethylene composite film, and the film is immersed in a processing pool to which a curing agent and an ink connecting material are added for a long time, thereby increasing the anti-adhesion performance of the polyimide / polytetrafluoroethylene composite film, and effectively preventing the wires and cables from adhering to each other during their later use, thereby causing line damage and line short circuit. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The figure is a flow chart of the steps of the method for preparing the insulating composite film. DETAILED DESCRIPTION

[0021] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] In the description of the present invention, it is necessary to understand that the terms "upper", "lower", "front", "back", "left", "right", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0023] See also Figure 1 , the present invention provides a technical solution:

[0024] A method for preparing a polyimide and polytetrafluoroethylene insulation composite film for electric wires, the specific steps of the method for preparing a polyimide and polytetrafluoroethylene insulation composite film for electric wires are as follows:

[0025] Step 1: Place the polyimide / polytetrafluoroethylene composite membrane into the production pool, add an excess of anhydrous ethanol into the production pool, and completely immerse the polyimide / polytetrafluoroethylene composite membrane in the anhydrous ethanol for 20-30 minutes;

[0026] Step 2: Take out the polyimide / polytetrafluoroethylene composite membrane, use filter paper to absorb excess anhydrous ethanol on the surface of the polyimide / polytetrafluoroethylene composite membrane, leave it for 10-20 minutes after complete treatment, and then apply a layer of adhesive glue on the surface of the polyimide / polytetrafluoroethylene composite membrane;

[0027] Step 3: Apply a layer of curing agent on the outer surface of the polyimide / polytetrafluoroethylene composite film, dry it for 30-40 minutes, and then apply another layer of curing agent. Repeat the operation three times;

[0028] Step 4: Place the polyimide / polytetrafluoroethylene composite membrane in step 3 inside a treatment tank, add excess lubricating oil and ink vehicle into the tank, mix the lubricating oil and ink vehicle completely, and soak the polyimide / polytetrafluoroethylene composite membrane in the tank for 30-40 minutes;

[0029] Step 5: Place the soaked polyimide / polytetrafluoroethylene composite film into the interior of the plasma multifunctional experimental table reaction chamber, adjust the voltage to 400-500V, and perform plasma treatment for 2-3 hours under inert gas and a certain working pressure.

[0030] The inert gas includes nitrogen, argon and helium, and the working pressure needs to be set to 500-1000Pa.

[0031] The curing agent includes vinyl triamine, aminoethyl piperazine, and aromatic amines; the lubricating oil includes perfluoropolyether, perfluorotripentylamine, and perfluorotributylamine.

[0032] The polyimide / polytetrafluoroethylene composite membrane is prepared by a tape casting method, and the polyimide / polytetrafluoroethylene composite membrane is 200-300 um.

[0033] The bonding glue and curing agent need to be evenly applied by machine.

[0034] The temperature of the polyimide / polytetrafluoroethylene composite film needs to be controlled at 20-30 degrees Celsius during the entire processing process.

[0035] Embodiment 1:

[0036] The specific steps of the preparation method of the polyimide and polytetrafluoroethylene insulation composite film for electric wire are as follows:

[0037] Step 1: Place the polyimide / polytetrafluoroethylene composite membrane into the production pool, add an excess of anhydrous ethanol into the production pool, and completely immerse the polyimide / polytetrafluoroethylene composite membrane in the anhydrous ethanol for 20 minutes;

[0038] Step 2: Take out the polyimide / polytetrafluoroethylene composite membrane, use filter paper to absorb excess anhydrous ethanol on the surface of the polyimide / polytetrafluoroethylene composite membrane, leave it for 10 minutes after complete treatment, and then apply a layer of adhesive glue on the surface of the polyimide / polytetrafluoroethylene composite membrane;

[0039] Step 3: Apply a layer of curing agent on the outer surface of the polyimide / polytetrafluoroethylene composite film, dry it for 30 minutes, and then apply another layer of curing agent. Repeat the operation three times;

[0040] Step 4: placing the polyimide / polytetrafluoroethylene composite membrane in step 3 inside a treatment tank, adding excess lubricating oil and ink vehicle into the tank, mixing the lubricating oil and ink vehicle completely, and soaking the polyimide / polytetrafluoroethylene composite membrane therein for 30 minutes;

[0041] Step 5: Place the soaked polyimide / polytetrafluoroethylene composite film into the interior of the plasma multifunctional experimental table reaction chamber, adjust the voltage to 400V, and perform plasma treatment for 2 hours under inert gas and a certain working pressure;

[0042] Embodiment 2:

[0043] The specific steps of the preparation method of the polyimide and polytetrafluoroethylene insulation composite film for electric wire are as follows:

[0044] Step 1: Place the polyimide / polytetrafluoroethylene composite membrane into the production pool, add an excess of anhydrous ethanol into the production pool, and completely immerse the polyimide / polytetrafluoroethylene composite membrane in the anhydrous ethanol for 25 minutes;

[0045] Step 2: Take out the polyimide / polytetrafluoroethylene composite membrane, use filter paper to absorb excess anhydrous ethanol on the surface of the polyimide / polytetrafluoroethylene composite membrane, leave it for 15 minutes after complete treatment, and then apply a layer of adhesive glue on the surface of the polyimide / polytetrafluoroethylene composite membrane;

[0046] Step 3: Apply a layer of curing agent on the outer surface of the polyimide / polytetrafluoroethylene composite film, dry it for 35 minutes, and then apply another layer of curing agent. Repeat the operation three times;

[0047] Step 4: placing the polyimide / polytetrafluoroethylene composite membrane in step 3 inside a treatment tank, adding excess lubricating oil and ink vehicle into the tank, mixing the lubricating oil and ink vehicle completely, and soaking the polyimide / polytetrafluoroethylene composite membrane therein for 35 minutes;

[0048] Step 5: Place the soaked polyimide / polytetrafluoroethylene composite film into the interior of the plasma multifunctional experimental table reaction chamber, adjust the voltage to 450V, and perform plasma treatment for 2.5 hours under inert gas and a certain working pressure;

[0049] Embodiment 3:

[0050] The specific steps of the preparation method of the polyimide and polytetrafluoroethylene insulation composite film for electric wire are as follows:

[0051] Step 1: Place the polyimide / polytetrafluoroethylene composite membrane into the production pool, add an excess of anhydrous ethanol into the production pool, and completely immerse the polyimide / polytetrafluoroethylene composite membrane in the anhydrous ethanol for 30 minutes;

[0052] Step 2: Take out the polyimide / polytetrafluoroethylene composite membrane, use filter paper to absorb excess anhydrous ethanol on the surface of the polyimide / polytetrafluoroethylene composite membrane, leave it for 20 minutes after complete treatment, and then apply a layer of adhesive glue on the surface of the polyimide / polytetrafluoroethylene composite membrane;

[0053] Step 3: Apply a layer of curing agent on the outer surface of the polyimide / polytetrafluoroethylene composite film, dry it for 40 minutes, and then apply another layer of curing agent. Repeat the operation three times;

[0054] Step 4: placing the polyimide / polytetrafluoroethylene composite membrane in step 3 inside a treatment tank, adding excess lubricating oil and ink vehicle into the tank, mixing the lubricating oil and ink vehicle completely, and soaking the polyimide / polytetrafluoroethylene composite membrane therein for 40 minutes;

[0055] Step 5: Place the soaked polyimide / polytetrafluoroethylene composite film into the interior of the plasma multifunctional experimental table reaction chamber, adjust the voltage to 500 V, and perform plasma treatment for 3 hours under inert gas and a certain working pressure.

[0056] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. For those skilled in the art, it is obvious that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention; therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the attached claims rather than the above description, so it is intended to include all changes within the meaning and scope of the equivalent elements of the claims, and any figure mark in the claims should not be regarded as limiting the claims involved. Although the embodiments of the present invention have been shown and described, it is understood by those of ordinary skill in the art that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of the present invention, and the scope of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing a polyimide and polytetrafluoroethylene insulation composite film for electric wires, characterized in that: The specific steps of the preparation method of the polyimide and polytetrafluoroethylene insulation composite film for electric wire are as follows: Step 1: Place the polyimide / polytetrafluoroethylene composite membrane into the production pool, add an excess of anhydrous ethanol into the production pool, and completely immerse the polyimide / polytetrafluoroethylene composite membrane in the anhydrous ethanol for 20-30 minutes; Step 2: Take out the polyimide / polytetrafluoroethylene composite membrane, use filter paper to absorb excess anhydrous ethanol on the surface of the polyimide / polytetrafluoroethylene composite membrane, leave it for 10-20 minutes after complete treatment, and then apply a layer of adhesive glue on the surface of the polyimide / polytetrafluoroethylene composite membrane; Step 3: Apply a layer of curing agent on the outer surface of the polyimide / polytetrafluoroethylene composite film, dry it for 30-40 minutes, and then apply another layer of curing agent. Repeat the operation three times; Step 4: Place the polyimide / polytetrafluoroethylene composite membrane in step 3 inside a treatment tank, add excess lubricating oil and ink vehicle into the tank, mix the lubricating oil and ink vehicle completely, and soak the polyimide / polytetrafluoroethylene composite membrane in the tank for 30-40 minutes; Step 5: Place the soaked polyimide / polytetrafluoroethylene composite film into the interior of the plasma multifunctional experimental table reaction chamber, adjust the voltage to 400-500V, and perform plasma treatment for 2-3 hours under inert gas and a certain working pressure.

2. The method for preparing a polyimide and polytetrafluoroethylene insulation composite film for electric wire according to claim 1, characterized in that: The inert gas includes nitrogen, argon and helium, and the working pressure needs to be set to 500-1000Pa.

3. The method for preparing a polyimide and polytetrafluoroethylene insulation composite film for electric wire according to claim 1, characterized in that: The curing agent includes vinyl triamine, aminoethyl piperazine, and aromatic amines; the lubricating oil includes perfluoropolyether, perfluorotripentylamine, and perfluorotributylamine.

4. The method for preparing a polyimide and polytetrafluoroethylene insulation composite film for electric wire according to claim 1, characterized in that: The polyimide / polytetrafluoroethylene composite membrane is prepared by a tape casting method, and the thickness of the polyimide / polytetrafluoroethylene composite membrane is 200-300 um.

5. The method for preparing a polyimide and polytetrafluoroethylene insulation composite film for electric wire according to claim 1, characterized in that: The bonding glue and curing agent need to be evenly applied by machine.

6. The method for preparing a polyimide and polytetrafluoroethylene insulation composite film for electric wire according to claim 1, characterized in that: The temperature of the polyimide / polytetrafluoroethylene composite film needs to be controlled at 20-30 degrees Celsius during the entire processing process.