Three-dimensional ordered cobalt-nitrogen microporous carbon material with strong catalytic effect and preparation method and application thereof

The preparation of three-dimensional ordered cobalt-nitrogen microporous carbon materials through the complexation reaction and co-precipitation steps of soluble zinc salt and citric acid, solving the problem of insufficient pore structure and morphology in the energy field of metal organic frame carbon materials in the prior art. , achieving the improvement of high specific surface area and catalytic performance, and is suitable for sodium-sulfur battery positive electrode materials.

CN114220971BActive Publication Date: 2024-11-29SOUTHWEST UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202111545529.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-16
Publication Date
2024-11-29
Estimated Expiration
2041-12-16

Smart Images

  • Figure CN114220971B_ABST
    Figure CN114220971B_ABST
Patent Text Reader

Abstract

The invention discloses a three-dimensional ordered cobalt-nitrogen microporous carbon material with strong catalytic effect, a preparation method and application thereof, and belongs to the technical field of materials. The preparation method comprises the following steps: first, a soluble zinc salt and citric acid are added to an organic solvent to generate a complex, then a high molecular weight polymer is added and continuously stirred, and then a zinc oxide-containing precursor is obtained through calcination; the obtained precursor, a soluble cobalt salt and an organic ligand are added to an organic solvent for coprecipitation, and centrifugal washing is performed; and the obtained metal organic framework material is carbonized under an inert atmosphere to obtain a three-dimensional ordered cobalt-nitrogen microporous carbon material, wherein the carbon material has a uniform regular polyhedral morphology, has a large specific surface area and porosity, has a large number of micropores and has catalytic performance, and can be used as a positive electrode material for a sodium-sulfur battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of material technology, and in particular to a three-dimensional ordered cobalt-nitrogen microporous carbon material with strong catalytic effect, and a preparation method and application thereof. Background Art

[0002] The depletion of fossil resources and the intensification of the greenhouse effect have forced humans to turn their attention to renewable and cleaner energy. The integration of renewable energy sources such as wind and solar energy into the power grid requires energy storage systems to have higher safety, high energy, low cost and long cycle life. In addition, the use of rechargeable battery systems as energy storage units can minimize the loss of transportation energy, so the research on electrode materials has received widespread attention. In recent years, materials such as metal organic frameworks, carbon materials with different nanostructures and MXene have been widely used in many fields, especially in the fields of energy conversion and energy storage. Among them, carbon materials derived from metal organic frameworks (MOFs) are a new type of porous material in recent years. MOFs refer to crystalline materials with periodic one-dimensional, two-dimensional or three-dimensional network structures constructed in the form of self-assembly through metal centers or metal clusters and multi-dentate organic ligands. After nearly two decades of research and development, metal organic framework-derived carbon materials have made a series of major progress in theoretical research and corresponding practical applications. The rich pore structure and low cost have been widely used in many fields.

[0003] However, when existing metal-organic framework-derived carbon materials are applied in the fields of energy conversion and energy storage, the pore structure and morphology still need to be improved, and an ultra-high specific surface area is required. Summary of the invention

[0004] In view of this, one of the objects of the present invention is to provide a method for preparing a three-dimensional ordered cobalt-nitrogen microporous carbon material with strong catalytic effect; a second object of the present invention is to provide a three-dimensional ordered cobalt-nitrogen microporous carbon material with strong catalytic effect prepared by the method, the prepared carbon material is a three-dimensional ordered cobalt-nitrogen microporous structure, has a high specific surface area, abundant micropores and catalytic performance; a third object of the present invention is to provide the application of the three-dimensional ordered cobalt-nitrogen microporous carbon material with strong catalytic effect in the positive electrode material of sodium-sulfur battery.

[0005] In order to achieve the above purpose, the present invention adopts the following technical solution:

[0006] 1. A method for preparing a three-dimensional ordered cobalt-nitrogen microporous carbon material with strong catalytic effect, comprising the following steps:

[0007] (1) Soluble zinc salt and citric acid are added to an organic solvent to undergo a complex reaction to obtain a suspension;

[0008] (2) adding polymethyl methacrylate to the suspension obtained in step (1), mixing and reacting, filtering, drying, first calcining in an inert atmosphere, and then calcining in air to obtain a precursor containing zinc oxide;

[0009] (3) adding the zinc oxide-containing precursor obtained in step (2), a soluble cobalt salt, and dimethylimidazole to an organic solvent, mixing and stirring, centrifuging after a coprecipitation reaction, washing, and drying to obtain a metal cobalt organic framework material;

[0010] (4) Carbonizing the metal cobalt organic framework material obtained in step (3) under an inert atmosphere to obtain a cobalt-nitrogen microporous carbon material.

[0011] Preferably, in step (1), the soluble zinc salt is selected from but not limited to zinc nitrate, zinc chloride, zinc sulfate, and zinc acetate; the organic acid is selected from but not limited to anhydrous citric acid, formic acid, sulfonic acid, and acetic acid; the molar ratio of the soluble zinc salt to the organic acid is 1:3; and the reaction conditions are a temperature of 70-140° C. and a reaction time of 8 to 28 hours.

[0012] Preferably, in step (2), the amount of polymethyl methacrylate added is equivalent to twice the molar number of zinc salt, and the reaction conditions are a reaction temperature of 50-100°C for 20 to 48 hours; the calcination conditions in an inert atmosphere are a temperature of 300°C for 3 hours; the calcination conditions in air are two-step calcination, with the first stage being heated at 300°C for 1-2 hours and the second stage being heated at 600°C for 2-3 hours.

[0013] Preferably, in step (3), the soluble cobalt salt is selected from but not limited to cobalt chloride hexahydrate, cobalt nitrate hexahydrate, and cobalt acetate hexahydrate; and the molar ratio of the zinc oxide-containing precursor, the soluble cobalt salt, and dimethylimidazole is 1:4:2.

[0014] Preferably, in step (3), the coprecipitation reaction is carried out at a temperature of 30-60° C. for 20 to 48 hours.

[0015] Preferably, in step (4) of the present invention, the carbonization is carried out at 800° C. for 2 hours.

[0016] Preferably, in steps (1) and (3), the organic solvent is selected from but not limited to methanol, ethanol, isopropanol, and ethylene glycol.

[0017] Preferably, the present invention further comprises the following steps: oxidizing the cobalt-nitrogen microporous carbon material obtained in step (4) in a strong acid to wash away the metal ions in the material.

[0018] 2. The three-dimensional ordered cobalt-nitrogen microporous carbon material with strong catalytic effect prepared by the preparation method.

[0019] 3. Application of the three-dimensional ordered cobalt-nitrogen microporous carbon material with strong catalytic effect in positive electrode materials of sodium-sulfur batteries.

[0020] Beneficial effects of the present invention:

[0021] The present invention first reacts citric acid with zinc ions to generate a metal complex, and then carbonizes the complex with high molecular weight polymer polymethyl methacrylate to generate a zinc oxide-containing precursor, and then composites the zinc oxide-containing precursor with a metal cobalt organic framework material to obtain a three-dimensional ordered cobalt-nitrogen microporous carbon material with a strong catalytic effect. The carbon material has a specific regular polyhedral structure, a unique pore structure, an ultra-high specific surface area, abundant micropores and metal catalytic performance. Compared with 2D materials, this structural microporous material will greatly increase the specific surface area and facilitate the penetration of electrolytes and the electron transmission rate, thereby improving its energy storage performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is the FESEM image of the three-dimensional ordered cobalt-nitrogen microporous carbon material M4 with strong catalytic effect;

[0023] Figure 2 M4Mapping diagram of the three-dimensional ordered cobalt-nitrogen microporous carbon material M4 with strong catalytic effect;

[0024] Figure 3 The XRD pattern of M4 is a three-dimensional ordered cobalt-nitrogen microporous carbon material M4 with strong catalytic effect;

[0025] Figure 4 The BET diagram and pore size distribution diagram of the three-dimensional ordered cobalt-nitrogen microporous carbon material M4 with strong catalytic effect;

[0026] Figure 5 CV curves of the positive electrodes of sodium-sulfur batteries prepared by M4 and M0;

[0027] Figure 6 This is the TGA diagram of the melted sulfur of the sodium-sulfur battery cathode material made from M4;

[0028] Figure 7 The positive electrode impedance curves of sodium-sulfur batteries made from M4 and M0;

[0029] Figure 8 The charge and discharge curves of the sodium-sulfur battery cathode material made from M4 at different current densities;

[0030] Fig. 9 The rate performance diagram of the sodium-sulfur battery positive electrode made of M4 and M0;

[0031] Fig.10 Long cycle performance curve of the positive electrode of the sodium-sulfur battery prepared by M4 and M0;

[0032] Fig.11 The voltage capacity diagram of the sodium-sulfur battery positive electrode made of M4 and M0;

[0033] Fig.12 The voltage-capacity diagram of the positive electrode of the sodium-sulfur battery made from M4, M9, and M2. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is further described below with reference to the accompanying drawings.

[0035] Example 1

[0036] The method of preparing a three-dimensional ordered cobalt-nitrogen microporous carbon material with strong catalytic effect is as follows:

[0037] (1) firstly, zinc nitrate and anhydrous citric acid are measured in a molar ratio of 1:3, and the zinc nitrate and anhydrous citric acid are added to a methanol solution, mixed evenly, and stirred overnight. The stirring reaction temperature is 70° C. and the reaction time is 28 hours to prepare a solution A;

[0038] (2) Add polymethyl methacrylate equivalent to twice the molar number of zinc salt to solution A to prepare solution B, mix and stir solution B for 12 hours, the mixing and stirring reaction temperature is 50°C, the reaction time is 48 hours, then filter and dry it and transfer it to a porcelain boat, under an inert atmosphere, heat it to 300°C at a rate of 1°C / min and keep it for 3 hours, then put it into a muffle furnace and calcine it in stages under air atmosphere, first heat it to 300°C at a rate of 1°C / min and keep it for 1 hour, then heat it to 600°C at 1°C / min and keep it for 3 hours, to obtain a ZnO-containing precursor.

[0039] (3) A ZnO-containing precursor, cobalt nitrate hexahydrate and dimethylimidazole were measured in a molar ratio of 1:4:2, added to methanol, and stirred evenly to obtain a solution C. The reaction temperature was 30° C. and the reaction time was 48 hours. After coprecipitation for 24 hours, the solution was centrifuged and washed with methanol and dried in an oven at 60° C. for 12 hours.

[0040] (4) The dried product is carbonized at 800° C. for 2 hours under an inert atmosphere to obtain a metal cobalt-containing organic framework carbon material.

[0041] (5) The three-dimensional ordered cobalt-nitrogen microporous carbon material with strong catalytic activity obtained in step (4) is placed in concentrated hydrochloric acid, stirred for 24 hours, the metal ions in the material are washed away, and then placed in a drying oven at 80° C. for 24 hours.

[0042] Example 2

[0043] The method of preparing a three-dimensional ordered cobalt-nitrogen microporous carbon material with strong catalytic effect is as follows:

[0044] (1) firstly, zinc nitrate and anhydrous citric acid are measured in a molar ratio of 1:3, and the zinc nitrate and anhydrous citric acid are added to a methanol solution, mixed evenly, and stirred overnight. The stirring reaction temperature is 140° C. and the reaction time is 8 hours to prepare a solution A;

[0045] (2) Add polymethyl methacrylate equivalent to twice the molar number of zinc salt to solution A to prepare solution B, mix and stir solution B for 12 hours, the temperature of the mixing and stirring reaction is 100°C, the reaction time is 20 hours, then filter and dry it and transfer it to a porcelain boat, under an inert atmosphere, heat it to 300°C at a rate of 5°C / min and keep it for 3 hours, then put it into a muffle furnace and calcine it in stages under air atmosphere, first heat it to 300°C at a rate of 5°C / min and keep it for 2 hours, then heat it to 600°C at 5°C / min and keep it for 3 hours, to obtain a ZnO-containing precursor.

[0046] (3) A ZnO-containing precursor, cobalt nitrate hexahydrate and dimethylimidazole were measured in a molar ratio of 1:4:2, added to methanol, and stirred evenly to obtain a solution C. The reaction temperature was 60° C. and the reaction time was 20 hours. After coprecipitation for 24 hours, the solution was centrifuged and washed with methanol and dried in an oven at 60° C. for 12 hours.

[0047] (4) The dried product is carbonized at 800° C. for 2 hours under an inert atmosphere to obtain a metal cobalt-containing organic framework carbon material.

[0048] (5) The three-dimensional ordered cobalt-nitrogen microporous carbon material with strong catalytic activity obtained in step (4) is placed in concentrated hydrochloric acid, stirred for 24 hours, the metal ions in the material are washed away, and then placed in a drying oven at 80° C. for 24 hours.

[0049] Comparative Example 1

[0050] Prepare as follows:

[0051] (1) Cobalt nitrate hexahydrate and dimethylimidazole were weighed in a molar ratio of 2:1, added to methanol, and stirred to obtain solution C. The reaction temperature was 30° C. and the reaction time was 20 hours. After coprecipitation for 48 hours, the solution was centrifuged and washed with methanol and dried in an oven at 60° C. for 12 hours.

[0052] (4) The dried product was carbonized at 800° C. for 2 hours under an inert atmosphere to obtain a metal organic framework carbon material with cobalt.

[0053] (5) The three-dimensional ordered cobalt-nitrogen microporous carbon material with strong catalytic activity obtained in step (4) is placed in concentrated hydrochloric acid, stirred for 24 hours, the metal ions in the material are washed away, and then placed in a drying oven at 80° C. for 24 hours.

[0054] Comparative Example 2

[0055] The method of preparing a three-dimensional ordered cobalt-nitrogen microporous carbon material with strong catalytic effect is as follows:

[0056] (1) firstly, zinc nitrate and anhydrous citric acid are measured in a molar ratio of 1:3, and the zinc nitrate and anhydrous citric acid are added to a methanol solution, mixed evenly, and stirred overnight. The stirring reaction temperature is 70° C. and the reaction time is 28 hours to prepare a solution A;

[0057] (2) Add polymethyl methacrylate equivalent to twice the molar number of zinc salt to solution A to prepare solution B, mix and stir solution B for 12 hours, the mixing and stirring reaction temperature is 50°C, the reaction time is 48 hours, then filter and dry it and transfer it to a porcelain boat, under an inert atmosphere, heat it to 300°C at a rate of 3°C / min and keep it for 3 hours, then put it into a muffle furnace and calcine it in stages under air atmosphere, first heat it to 300°C at a rate of 3°C / min and keep it for 2 hours, then heat it to 600°C at 3°C / min and keep it for 3 hours, to obtain a ZnO-containing precursor.

[0058] (3) A ZnO-containing precursor, cobalt nitrate hexahydrate and dimethylimidazole were measured in a molar ratio of 1:9:2, added to methanol, and stirred evenly to obtain a solution C. The reaction temperature was 30° C. and the reaction time was 48 hours. After coprecipitation for 24 hours, the solution was centrifuged and washed with methanol and dried in an oven at 60° C. for 12 hours.

[0059] (4) The dried product is carbonized at 800° C. for 2 hours under an inert atmosphere to obtain a metal cobalt-containing organic framework carbon material.

[0060] (5) The three-dimensional ordered cobalt-nitrogen microporous carbon material with strong catalytic activity obtained in step (4) is placed in concentrated hydrochloric acid, stirred for 24 hours, the metal ions in the material are washed away, and then placed in a drying oven at 80° C. for 24 hours.

[0061] Comparative Example 3

[0062] The method of preparing a three-dimensional ordered cobalt-nitrogen microporous carbon material with strong catalytic effect is as follows:

[0063] (1) firstly, zinc nitrate and anhydrous citric acid are measured in a molar ratio of 1:3, and the zinc nitrate and anhydrous citric acid are added to a methanol solution, mixed evenly, and stirred overnight. The stirring reaction temperature is 70° C. and the reaction time is 28 hours to prepare a solution A;

[0064] (2) Add polymethyl methacrylate equivalent to twice the molar number of zinc salt to solution A to prepare solution B, mix and stir solution B for 12 hours, the mixing and stirring reaction temperature is 50°C, the reaction time is 48 hours, then filter and dry it and transfer it to a porcelain boat, under an inert atmosphere, heat it to 300°C at a rate of 3°C / min and keep it for 3 hours, then put it into a muffle furnace and calcine it in stages under air atmosphere, first heat it to 300°C at a rate of 3°C / min and keep it for 2 hours, then heat it to 600°C at 3°C / min and keep it for 3 hours, to obtain a ZnO-containing precursor.

[0065] (3) A ZnO-containing precursor, cobalt nitrate hexahydrate and dimethylimidazole were measured in a molar ratio of 1:2:3, added to methanol, and stirred evenly to obtain a solution C. The reaction temperature was 30° C. and the reaction time was 48 hours. After coprecipitation for 24 hours, the solution was centrifuged and washed with methanol and dried in an oven at 60° C. for 12 hours.

[0066] (4) The dried product is carbonized at 800° C. for 2 hours under an inert atmosphere to obtain a metal cobalt-containing organic framework carbon material.

[0067] (5) The three-dimensional ordered cobalt-nitrogen microporous carbon material with strong catalytic activity obtained in step (4) is placed in concentrated hydrochloric acid, stirred for 24 hours, the metal ions in the material are washed away, and then placed in a drying oven at 80° C. for 24 hours.

[0068] The carbon materials prepared in Examples 1 and 2 were named M4, the carbon material prepared in Comparative Example 1 was named M0, the carbon material prepared in Comparative Example 2 was named M9, and the carbon material prepared in Comparative Example 3 was named M2.

[0069] Figure 1 This is a FESEM image of the three-dimensional ordered cobalt-nitrogen microporous carbon material M4 with strong catalytic activity. From the field emission scanning electron microscope image, it can be seen that the material has a regular polyhedron structure.

[0070] Figure 2 This is the mapping diagram of the three-dimensional ordered cobalt-nitrogen microporous carbon material M4 with strong catalytic effect. It can be seen from the figure that the material contains cobalt and nitrogen elements, and they are evenly distributed.

[0071] Figure 3The XRD pattern of the three-dimensional ordered cobalt-nitrogen microporous carbon material M4 with strong catalytic effect is shown in Figure 1. The broad diffraction peaks at about 23 degrees and 42 degrees indicate that the obtained material is an amorphous carbon material, and no other impurity peaks are detected.

[0072] Figure 4 The BET and pore size distribution diagram of the three-dimensional ordered cobalt-nitrogen microporous carbon material M4 with strong catalytic activity. The specific surface area of ​​M4 is 791.05 m 2 ·g -1 The specific surface area of ​​M0 is only 203.71m 2 ·g -1 ; As can be seen from the figure, M4 has a much larger number of micropores than M0.

[0073] Example 3

[0074] Take M4, M0, M9, M2 and sulfur powder in a mass ratio of 1:1, grind them evenly in an agate mortar, put them into a reactor, and heat them in an oven at 155°C for 12 hours to melt the sulfur in the materials.

[0075] The molten sulfur material was mixed with Ketjen black and PVDF binder in a mass ratio of 80:10:10, and then an appropriate amount of N-methylpyrrolidone was added. The mixture was ground into a paste in an agate mortar and applied on a carbon-coated aluminum foil with a coating area of ​​1.0×1.0cm 2 , coating an electrode active material with a mass of about 1 mg. The electrode was then dried at 60°C for 24 hours to obtain a sodium-sulfur battery positive electrode. The voltage range was 0.5-2.7V. The test platform was an electrochemical workstation CHI760E.

[0076] Figure 5 The CV curves of the positive electrodes of sodium-sulfur batteries prepared by M4 and M0 are shown in Figure 1. As can be seen from the figure, compared with M0, not only the position of the reduction peak of M4 has changed, but also the position of the oxidation peak has changed significantly, indicating that the reaction process of the main body of the reaction has changed after the addition of the precursor metal oxide.

[0077] Figure 6 The sulfur content of the positive electrode material of the sodium-sulfur battery made by M4. As can be seen from the figure, the positive electrode material contains 50% sulfur.

[0078] Figure 7 The impedance spectra of the positive electrode of sodium-sulfur batteries made of M4 and M0. It can be seen from the figure that compared with M0, M4 has a smaller impedance value.

[0079] Figure 8 The charge and discharge curves of the sodium-sulfur battery cathode material made of M4 at different current densities. As can be seen from the figure, the specific capacity gradually decreases with the increase of current density.

[0080] Fig. 9The rate curves of the sodium-sulfur battery positive electrode made of M4 and M0. M4 at 0.1A·g -1 , 0.2A·g -1 , 0.5A·g -1 , 1A·g -1 , 2A·g -1 , 5A g -1 At current densities of , the capacities can reach 710mAh / g, 630mAh / g, 562mAh / g, 491mAh / g, 415mAh / g and 310mAh / g respectively. It can be seen from the figure that compared with M0, its rate performance has been greatly improved.

[0081] Fig.10 The long cycle performance diagram of the positive electrode of the sodium-sulfur battery made of M4 and M0. M4 at 1A·g -1 After 850 cycles at a current density of , the capacity is 310 mAh g -1 ,Compared with M0, M4 not only has a higher initial capacity, but also its cycle stability is better than M0.

[0082] Fig.11 The voltage capacity diagram of the sodium-sulfur battery positive electrode made of M4 and M0. M0 and M4 at 0.5A·g -1 The voltage-capacity diagram under current density of . It can be seen from the figure that compared with M0, M4 has smaller polarization.

[0083] Fig.12 The voltage capacity diagram of the sodium-sulfur battery positive electrode made of M4, M9, and M2. -1 At a current density of , when the ZnO precursor, cobalt nitrate hexahydrate and dimethylimidazole are in a molar ratio of 1:4:2 (M4), it has a higher capacity than 1:9:2 (M9) in Comparative Experimental Example 2 and 1:2:3 (M2) in Comparative Example 3.

[0084] It should be understood by those skilled in the art that the key to the present invention is to first generate a metal compound, then generate a metal oxide, and then compound the metal oxide and the metal salt to obtain a metal organic framework, and then carbonize to obtain a microporous carbon material. The specific type and amount of the organic solvent, the reaction temperature, the reaction time and other parameters can be adjusted accordingly according to common knowledge, and the purpose of the present invention can be achieved.

[0085] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. Application of three-dimensional ordered cobalt-nitrogen microporous carbon material with strong catalytic effect in positive electrode material of sodium-sulfur battery, characterized in that: The method for preparing the three-dimensional ordered cobalt-nitrogen microporous carbon material with strong catalytic effect comprises the following steps: (1) Soluble zinc salt and organic acid are added to an organic solvent to undergo a complex reaction to obtain a suspension; (2) adding polymethyl methacrylate to the suspension obtained in step (1), mixing and reacting, filtering, drying, first calcining in an inert atmosphere, and then calcining in air to obtain a precursor containing zinc oxide; (3) adding the zinc oxide-containing precursor obtained in step (2), soluble cobalt salt, and dimethylimidazole into an organic solvent, mixing and stirring, centrifuging after coprecipitation reaction, washing, and drying to obtain a metal cobalt organic framework material; (4) carbonizing the metal cobalt organic framework material obtained in step (3) under an inert atmosphere to obtain a cobalt-nitrogen microporous carbon material; In step (1), the soluble zinc salt is selected from at least one of zinc nitrate, zinc chloride, zinc sulfate, and zinc acetate; the organic acid is selected from at least one of anhydrous citric acid, formic acid, sulfonic acid, and acetic acid; the molar ratio of the soluble zinc salt to the organic acid is 1:3; the reaction conditions are a temperature of 70-140° C. and a reaction time of 8-28 hours; In step (2), the amount of polymethyl methacrylate added is equivalent to twice the molar number of zinc salt, and the reaction conditions are 50-100°C for 20-48 hours; the calcination conditions in an inert atmosphere are 300°C for 3 hours; the calcination conditions in air are two-step calcination, with the first stage being 300°C for 1-2 hours and the second stage being 600°C for 2-3 hours; In step (3), the soluble cobalt salt is selected from cobalt chloride hexahydrate, cobalt nitrate hexahydrate, and cobalt acetate hexahydrate; the molar ratio of the zinc oxide-containing precursor, the soluble cobalt salt, and dimethylimidazole is 1:4:2; and the coprecipitation reaction is carried out at a temperature of 30-60° C. for 20-48 hours; In steps (1) and (3), the organic solvent is selected from at least one of methanol, ethanol, isopropanol, and ethylene glycol; In step (4), the carbonization is carried out at 800° C. for 2 hours. The method further comprises the following steps: oxidizing the cobalt-nitrogen microporous carbon material obtained in step (4) in a strong acid to wash away the metal ions in the material.

Citation Information

Patent Citations

  • Preparation method of nitrogen-doped three-dimensional porous carbon loaded with nano cobalt and application thereof in lithium sulfur batteries