Modified polyolefin resin and dispersion composition
By grafting and modifying polyolefin resin with α,β-unsaturated carboxylic acid, a modified polyolefin resin with excellent water-resistant adhesion and high-temperature stability is prepared, which solves the problem of high-temperature adhesion of coating films in the existing technology. Solving the problem of deficiencies, the coating film strength and adhesion under high temperature conditions are improved.
Patent Information
- Application Number
- CN202080060844.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-08-24
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-08-24
AI Technical Summary
Existing modified polyolefin resins have insufficient water-resistant adhesion when used for vehicle body coatings under high temperature conditions, especially in window frameless installation methods. This results in the coating film being prone to cohesion failure at high temperatures, making it unsatisfactory for automobile manufacturing. Requirements for bonding strength and durability.
By graft-modifying polyolefin resin with α,β-unsaturated carboxylic acid or its derivatives, the graft-modified product and its composition obtained have a modified polyolefin with a melting point between 85°C and above and below 110°C. The resin has a tensile elastic modulus of 250 MPa or more and a weight average molecular weight of 70,000 or more and less than 200,000. It is used to prepare coating films with excellent water-resistant adhesion under high temperature conditions.
It achieves an improvement in the adhesion and strength of the coating film under high temperature conditions, ensures the stable adhesion of the coating film to the substrate at high temperatures, and meets the requirements for coating film performance in automobile manufacturing.
Smart Images

Figure DEST_PATH_IMAGE002 
Figure DEST_PATH_IMAGE004
Abstract
Description
Technical Field
[0001] The present invention relates to a modified polyolefin resin and a dispersion composition, and more particularly to a modified polyolefin resin and a dispersion composition having excellent water-resistant adhesion under high temperature conditions. Background Art
[0002] Polyolefins such as polypropylene and polyethylene are generally inexpensive and have excellent properties such as moldability, chemical resistance, water resistance, and electrical properties. Therefore, polyolefins have been widely used as materials for sheets, films, and molded products in recent years. However, polyolefin substrates are non-polar and crystalline substrates, unlike polar substrates such as polyurethane resins, polyamide resins, acrylic resins, and polyester resins. Therefore, it is difficult to coat or bond polyolefin substrates.
[0003] As a method for improving the above-mentioned problem regarding adhesion, a method has been proposed in which a primer capable of bonding to a polyolefin resin is applied to the surface of a substrate, and a urethane resin coating or the like is applied on the primer. As such a primer, a modified polyolefin resin to which a polar group (carboxyl group, acid anhydride group, etc.) is added is used, and by adding the polar group, not only the affinity with the polyolefin resin substrate but also the affinity with the urethane resin coating or the like is improved, thereby improving adhesion (Patent Document 1).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2015-105294. Summary of the invention
[0007] Problems to be solved by the invention
[0008] Modified polyolefin resins are widely used as primers for resin substrates for automobile bumpers and the like. However, in recent years, automobile manufacturers have adopted a policy of replacing the steel plate substrate of the vehicle body with a resin substrate in order to reduce the weight of the vehicle body. As a result, there is a need for a primer for the resin substrate of the vehicle body that has a coating film performance equivalent to that of steel plate coating.
[0009] In the coating film of the vehicle body, especially in the adhesive for direct glazing that directly bonds the window glass and the vehicle body, or the adhesive for the side window glass and the window frame in the vehicle, it is required to have long-term bonding strength and to have little degradation even when exposed to high temperatures. Therefore, compared with the water-resistant adhesion of the primer for the bumper, it is a test under high temperature conditions.
[0010] More specifically, regarding the water-resistant adhesion of adhesives used for window frameless installation methods under high temperature conditions, first, a urethane adhesive is applied to a coating film applied to a resin substrate to prepare a test plate. Next, the prepared test plate is immersed in a constant temperature water bath set at 60°C for 10 days, and then a peeling test of the adhesive layer is performed for evaluation. On the other hand, regarding the hot water resistance test of the bumper coating film, a test piece obtained by coating a resin substrate is immersed in a constant temperature water bath at 40°C for 10 days, and then a peeling test of the coating film is performed for evaluation.
[0011] Therefore, the modified polyolefin resin used in conventional primers for bumpers cannot impart sufficient strength or adhesion to the coating film in adhesives used in window frameless installation methods with high test temperatures, and the coating film may suffer cohesive failure.
[0012] Therefore, it is difficult for a primer using a conventional polyolefin-based resin to exhibit sufficient coating film properties from the viewpoint of water-resistant adhesion.
[0013] An object of the present invention is to provide a modified polyolefin resin capable of producing a coating film having excellent water-resistant adhesion under high temperature conditions.
[0014] Means of solving problems
[0015] The present inventors have conducted intensive studies on the above-mentioned problems and have found that a graft-modified product obtained by graft-modifying a polyolefin resin with an α,β-unsaturated carboxylic acid or its derivatives so as to achieve a tensile elastic modulus and a weight-average molecular weight within a prescribed range and a dispersion composition containing the graft-modified product can solve the above-mentioned problems, thereby completing the present invention.
[0016] That is, the present inventors provide the following [1] to
[10] .
[0017] [1] A modified polyolefin resin comprising a graft-modified product obtained by graft-modifying a component (A): a polyolefin resin with a component (B): an α,β-unsaturated carboxylic acid or a derivative thereof, wherein the modified polyolefin resin has a melting point of 85°C or higher and lower than 110°C as measured by a differential scanning calorimeter, a tensile elastic modulus of 250 MPa or higher, and a weight average molecular weight of 70,000 or higher and lower than 200,000.
[0018] [2] The modified polyolefin resin according to [1] above, which has a melting point of 85° C. or higher and lower than 110° C. as measured by a differential scanning calorimeter.
[0019] [3] The modified polyolefin resin according to [1] or [2] above, wherein the component (A) contains at least one selected from the group consisting of ethylene-propylene copolymers, propylene-1-butene copolymers and ethylene-propylene-1-butene copolymers.
[0020] [4] The modified polyolefin resin according to any one of [1] to [3] above, wherein the graft weight of the component (B) in the graft modified product is 0.1 to 10% by weight.
[0021] [5] A dispersion composition comprising the modified polyolefin resin according to any one of [1] to [4] above.
[0022] [6] The dispersion composition according to [5] above, wherein the melting point measured by a differential scanning calorimeter is 90° C. or higher and lower than 110° C.
[0023] [7] The dispersion composition according to [5] or [6] above, which is a primer.
[0024] [8] The dispersion composition according to [5] or [6] above, which is a coating material.
[0025] [9] The dispersion composition according to [5] or [6] above, which is an ink.
[0026]
[10] The dispersion composition according to [5] or [6] above, which is an adhesive.
[0027] Effects of the Invention
[0028] According to the modified polyolefin resin of the present invention, a coating film having excellent water-resistant adhesion under high temperature conditions can be produced. DETAILED DESCRIPTION
[0029] Hereinafter, the present invention will be described in detail with reference to preferred embodiments thereof.
[0030] In this specification, the expression "AA to BB" means greater than AA and less than BB.
[0031] [1. Modified polyolefin resin]
[0032] The modified polyolefin resin of the present invention contains a graft-modified product obtained by graft-modifying component (A): polyolefin resin (hereinafter also referred to as "component (A)") with component (B): α,β-unsaturated carboxylic acid or its derivative (hereinafter also referred to as "component (B)"). The tensile elastic modulus of the modified polyolefin resin is 250 MPa or more, and the weight average molecular weight (hereinafter also referred to as "Mw") is 70,000 or more and less than 200,000. In addition, the melting point (hereinafter also referred to as "Tm") of the modified polyolefin resin measured by a differential scanning calorimeter (hereinafter also referred to as "DSC") is preferably 85°C or more and less than 110°C.
[0033] The reason why the modified polyolefin resin of the present invention can produce a coating film having excellent water-resistant adhesion under high temperature conditions is presumed to be as follows.
[0034] The Mw of the modified polyolefin resin of the present invention is within the specified range, and the tensile modulus is more than the specified value. If the Mw is within the specified range, while the film is given cohesion and adhesion, solvent solubility can be ensured. Therefore, adhesion with the substrate can be ensured. If the tensile modulus is more than the specified value, sufficient strength can be given to the film. Therefore, even under high temperature conditions, film strength can be maintained, adhesion with the substrate can be ensured. Therefore, it is inferred that the excellent effect of being able to make a film with excellent water-resistant adhesion under high temperature conditions can be shown.
[0035] In addition, when Tm is within the prescribed range, water resistance under high temperature conditions can be further improved, and good film forming properties can be ensured during coating film baking.
[0036] The Mw of the modified polyolefin resin of the present invention is 70,000 or more and less than 200,000, preferably 80,000 or more and less than 150,000. If the Mw is 70,000 or more, the coating film after drying exerts cohesive force, which can give the coating film strength and adhesion. On the other hand, if it is less than 200,000, sufficient solvent solubility can be ensured. In addition, when preparing an aqueous dispersion, good stability can be ensured.
[0037] In this specification, Mw is a value measured and calculated by gel permeation chromatography (standard substance: polystyrene).
[0038] The Tm of the modified polyolefin resin of the present invention is preferably 85° C. or higher and lower than 110° C., and more preferably 90° C. or higher and lower than 105° C. If the Tm is 85° C. or higher, sufficient water resistance under high temperature conditions can be further improved. On the other hand, if the melting point is lower than 110° C., good film forming properties can be ensured during coating film baking.
[0039] In this specification, Tm measured by DSC is a value measured under the following conditions. According to JIS K7121-1987, using a DSC measuring device (manufactured by TA Instruments), about 5 mg of a sample is heated at 150°C for 10 minutes to maintain a molten state. Then, the temperature is lowered at a rate of 10°C / min and kept stable at -50°C. Then, the temperature is raised to 150°C at 10°C / min, and the melting peak temperature during melting is evaluated as Tm.
[0040] The tensile modulus of the modified polyolefin resin of the present invention is more than 250MPa, preferably more than 300MPa. If the tensile modulus is more than 250MPa, sufficient strength can be given to the coating film. In addition, its upper limit is not particularly limited, usually below 8000MPa, preferably below 5000MPa, below 3000MPa, below 1000MPa, more preferably below 800MPa, further preferably below 600MPa, and more preferably below 500MPa.
[0041] In this specification, the tensile modulus of the modified polyolefin resin is a value measured under the following conditions. First, the aqueous dispersion composition of the modified polyolefin resin is dried to obtain a dried product. The obtained dried product is heated and dissolved in an organic solvent, and the obtained solution is coated on a release paper so that the film thickness is about 20 μm. Dry it for 5 minutes in an air-supplied dryer set at 100°C, and store it at a constant temperature and humidity of 23°C and a relative humidity of 50% for 24 hours. Then, cut it into a width of 15 mm and a length of 150 mm, peel off the release paper, and obtain a test film. For the obtained test film, the tensile modulus of elasticity is measured using a tensile testing machine under the conditions of a tensile speed of 10 mm / min and a distance between chucks of 100 mm.
[0042] As can be seen from the above measurement conditions, the tensile modulus of the modified polyolefin resin is a value measured using a 15 mm wide and 150 mm long test film made of the modified polyolefin resin at a tensile speed of 10 mm / min and a chuck distance of 100 mm.
[0043] [1-1. Component (A): polyolefin resin]
[0044] Component (A) is not particularly limited and may be a homopolymer of one olefin or a copolymer of two or more olefins. In the case of a copolymer, it may be a random copolymer or a block copolymer. As the olefin, α-olefins are preferably used. As the α-olefins, ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, and 1-octene may be cited.
[0045] As component (A), polypropylene (propylene homopolymer), ethylene-propylene copolymer, propylene-1-butene copolymer, and ethylene-propylene-1-butene copolymer are more preferably used from the viewpoint of exhibiting sufficient adhesion to non-polar resin substrates such as polypropylene substrates.
[0046] In this specification, polypropylene means a polymer whose basic unit is a structural unit derived from propylene. Ethylene-propylene copolymer means a copolymer whose basic unit is a structural unit derived from ethylene and a structural unit derived from propylene. Propylene-1-butene copolymer means a copolymer whose basic unit is a structural unit derived from propylene and a structural unit derived from 1-butene. These polymers may contain structural units derived from other olefins in addition to the above-mentioned basic units in small amounts. The content thereof is sufficient as long as the amount does not significantly damage the original performance of the resin. Such structural units derived from other olefins may be mixed in, for example, in the process before the preparation of the modified polyolefin resin.
[0047] Component (A) preferably contains 60 mol% or more of propylene-derived structural units in 100 mol% of the structural units. If the propylene-derived structural units are contained within the above range, adhesion to substrates such as non-polar resins (such as propylene resins) or molded products can be ensured.
[0048] Among the components (A), polyolefin resins obtained by using a metallocene catalyst as a polymerization catalyst are preferred because they have the following characteristics. The molecular weight distribution of the component (A) obtained by using a metallocene catalyst is narrow. In addition, when the component (A) is a copolymer, it has excellent random copolymerizability, a narrow composition distribution, and a wide range of copolymerizable comonomers.
[0049] As the metallocene catalyst, a known one can be used. The metallocene catalyst is preferably obtained by combining the following components (1) and (2) and, if necessary, (3).
[0050] Component (1): a metallocene complex, which is a transition metal compound of Groups 4 to 6 of the Periodic Table of Elements having at least one conjugated five-membered ring ligand;
[0051] Component (2): ion-exchange layered silicate;
[0052] · Component (3): an organoaluminum compound.
[0053] When the ethylene-propylene copolymer and the propylene-butene copolymer are random copolymers, they preferably contain 5 to 50 mol % of structural units derived from ethylene or structural units derived from butene, and contain 50 to 95 mol % of structural units derived from propylene, based on 100 mol % of the structural units.
[0054] From the viewpoint of giving sufficient strength to the coating film, the tensile modulus of component (A) is preferably more than 150MPa, more preferably more than 250MPa. Its upper limit is usually below 8000MPa, preferably below 5000MPa, below 3000MPa, below 1000MPa, more preferably below 800MPa, further preferably below 600MPa.
[0055] The tensile modulus of the component (A) can be measured in the same manner as the tensile modulus of the modified polyolefin resin.
[0056] The melting point of component (A) is preferably 80° C. or higher and lower than 110° C., more preferably 85° C. or higher and 105° C. This makes it easy to obtain a modified polyolefin resin having a melting point in the above range. The weight average molecular weight of component (A) is 70,000 or higher and lower than 500,000, preferably 80,000 or higher and lower than 400,000.
[0057] The component (A) may be used alone or in combination of two or more. When two or more are used in combination, the ratio thereof is not particularly limited.
[0058] [1-2. Component (B): α,β-unsaturated carboxylic acid or its derivative]
[0059] Component (B) is an α,β-unsaturated carboxylic acid or a derivative thereof. Examples of α,β-unsaturated carboxylic acids and derivatives thereof include maleic acid, maleic anhydride, fumaric acid, citraconic acid, citraconic anhydride, mesaconic acid, itaconic acid, itaconic anhydride, aconitic acid, aconitic anhydride, nadic anhydride, (meth)acrylic acid, and (meth)acrylate. Among them, maleic anhydride is preferred.
[0060] Component (B) may be at least one compound selected from α,β-unsaturated carboxylic acids and derivatives thereof, and may be a combination of one or more α,β-unsaturated carboxylic acids and one or more derivatives of α,β-unsaturated carboxylic acids, a combination of two or more α,β-unsaturated carboxylic acids, or a combination of two or more derivatives of α,β-unsaturated carboxylic acids.
[0061] When the grafted modified product is 100% by weight, the graft weight of component (B) in the grafted modified product is preferably 0.1 to 10% by weight, and more preferably 0.5 to 5% by weight. If the graft weight is 0.1% by weight or more, the adhesion of the obtained modified polyolefin resin to the topcoat coating can be ensured. In addition, good stability can be ensured when the aqueous dispersion is modulated. If the graft weight is 10% by weight or less, the generation of grafted unreacted products can be prevented, and sufficient adhesion to the resin substrate can be ensured.
[0062] The graft weight of the component (B) is a value determined by an alkali titration method.
[0063] [1-3. Graft-modified products]
[0064] The graft modified product can be prepared by graft-modifying (graft polymerizing) component (B) to component (A). The graft modification can be carried out by a known method, and component (C): a free radical generator (hereinafter, also referred to as "component (C)") can be used. Examples of the graft modification include: a solution method in which a mixture of components (A) and (B) is dissolved by heating in an organic solvent such as toluene, and component (C) is added; or a method in which components (A), (B) and (C) are added using a mixer such as a Banbury mixer, a kneader, or an extruder, and a melt-kneading reaction is performed under heating to obtain a graft modified product. Components (A), (B) and (C) may be added all at once or gradually.
[0065] Component (C) can be appropriately selected from known free radical generators, preferably organic peroxide compounds. As organic peroxide compounds, for example, di-tert-butyl peroxide, dicumyl peroxide, tert-butyl cumyl peroxide, benzoyl peroxide, dilauroyl peroxide, cumene hydroperoxide, tert-butyl hydroperoxide, 1,4-bis[(tert-butyl peroxy)isopropyl]benzene, 1,1-bis(tert-butyl peroxy)-3,5,5-trimethylcyclohexane, 1,1-bis(tert-butyl peroxy)-cyclohexane, cyclohexanone peroxide, tert-butyl peroxybenzoate, tert-butyl peroxyisobutyrate, tert-butyl peroxy 3,5,5-trimethylhexanoate, tert-butyl peroxy 2-ethylhexanoate, tert-butyl peroxyisopropyl carbonate, cumyl peroxyoctanoate. Among them, di-tert-butyl peroxide, dicumyl peroxide and dilauroyl peroxide are preferred.
[0066] Component (C) may be a single free radical generator or a combination of a plurality of free radical generators.
[0067] The amount of component (C) added in the graft polymerization reaction is preferably 1 to 100% by weight, more preferably 10 to 50% by weight, relative to the amount (weight) of component (B). If it is 1% by weight or more, sufficient grafting efficiency can be ensured. If it is 100% by weight or less, the reduction of the weight average molecular weight of the grafted modified product can be prevented.
[0068] The modified polyolefin resin only needs to contain at least one grafted modified product, and may contain a combination of two or more grafted modified products (e.g., two or more grafted modified products of different types and compositions of components (A) and / or (B)). The grafted modified product may also contain components other than the grafted modified product, such as components other than the grafted modified product generated during the graft modification (e.g., unreacted components (A) and (B), a polymer of component (B) itself).
[0069] The modified polyolefin resin of the present invention may be used directly (for example, in a solid state such as pellets), but is preferably added to a dispersion medium (solvent) to be used as a dispersion.
[0070] [2. Dispersion composition]
[0071] The dispersion composition of the present invention contains a modified polyolefin resin. The dispersion composition of the present invention may contain other components as required. The dispersion composition is preferably used as a film-forming composition such as a primer, a coating, an ink, an adhesive, etc.
[0072] The dispersion composition usually contains a modified polyolefin resin and a dispersion medium, and may also contain other resin components. As other resin components, for example, resins such as urethane resins, epoxy resins, acrylic resins, phenolic resins, alkyd resins, polyamide resins, polyimide resins, silicone resins, nitrocellulose, and combinations of two or more thereof can be cited. These resins can be mixed in modified polyolefins or their dispersions as water-based compounds (such as water-based acrylic resins and water-based polyurethane resins). According to the solid conversion, the ratio of the blending amount of modified polyolefin resins and other resins (when the other resins are two or more, the total amount of other resins) is usually modified polyolefin resin: other resins = 1~99:99~1, preferably 10~90:90~10, more preferably 20~80:80~20, and further preferably 30~70:70~30.
[0073] In addition, the dispersion composition may contain additive components such as aqueous acrylic resins, aqueous urethane resins, lower alcohols, lower ketones, lower esters, preservatives, leveling agents, antioxidants, light stabilizers, ultraviolet absorbers, dyes, pigments, metal salts, acids, etc. for the purpose of stabilizing quality.
[0074] The dispersion medium may be non-aqueous or aqueous (hereinafter, the dispersion composition containing an aqueous dispersion medium is also referred to as an "aqueous dispersion composition"). Examples of non-aqueous dispersion mediums include organic solvents such as xylene, toluene, and benzene. Aqueous dispersion mediums are usually water, and alcoholic solvents, glycol solvents, ketone solvents, and ester solvents may also be used in combination.
[0075] In the case where the dispersion composition is an aqueous dispersion composition, a crosslinking agent may be contained as another component. "Crosslinking agent" refers to a compound that reacts with hydroxyl, carboxyl, amino and other groups present in components such as modified polyolefin resins, surfactants, neutralizers, etc. to form a crosslinked structure. Examples of crosslinking agents include blocked isocyanate compounds, aliphatic or aromatic epoxy compounds, amine compounds, and amino resins. There is no particular limitation on the method for adding the crosslinking agent. For example, it can be added in the middle of the water-based process or after the water-based process.
[0076] As the surfactant, any of a nonionic surfactant and anionic surfactant can be used. A nonionic surfactant is preferably used because the resulting aqueous dispersion composition has better water resistance.
[0077] Examples of the nonionic surfactant include polyoxyethylene alkyl ethers, polyoxyethylene alkylene alkyl ethers, polyoxyethylene derivatives, polyoxyethylene fatty acid esters, polyoxyethylene polyol fatty acid esters, polyoxyethylene propylene polyols, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene hydrogenated castor oils, polyoxyalkylene polycyclic phenyl ethers, polyoxyethylene alkylamines, alkyl alkanolamides, and polyalkylene glycol (meth)acrylates. Among these, polyoxyethylene alkyl ethers, polyoxyethylene fatty acid esters, polyoxyethylene sorbitan fatty acid esters, and polyoxyethylene alkylamines are preferred.
[0078] Examples of the anionic surfactant include alkyl sulfate ester salts, polyoxyethylene alkyl ether sulfates, alkylbenzene sulfonates, α-olefin sulfonates, methyl taurates, sulfosuccinates, ether sulfonates, ether carboxylates, fatty acid salts, naphthalenesulfonic acid formaldehyde condensates, alkylamine salts, quaternary ammonium salts, alkyl betaines, and alkylamine oxides. Among them, polyoxyethylene alkyl ether sulfates and sulfosuccinates are preferred.
[0079] When a surfactant is used in preparing the aqueous dispersion composition, it is preferred that the surfactant be added in the smallest possible amount or not added at all. The reason for this is that the addition of a surfactant may reduce the coating performance when the coating is made, or may cause a plasticizing effect, bleeding, and blocking when the coating is dried.
[0080] The water dispersion composition may further contain a neutralizer, thereby further improving the dispersibility of the resin in the aqueous dispersion medium. Examples of the neutralizing agent include ammonia, methylamine, ethylamine, dimethylamine, diethylamine, triethylamine, propylamine, isopropylamine, dipropylamine, isobutylamine, hexylamine, octylamine, ethanolamine, propanolamine, diethanolamine, N-methyldiethanolamine, N,N-dimethylethanolamine, N,N-diethylethanolamine, N,N-dibutylethanolamine, 2-dimethylamino-2-methyl-1-propanol, 2-amino-2-methyl-1-propanol, 2-aminoethanol, 2-dimethylaminoethanol, 2-diethylaminoethanol, 3-ethoxypropylamine, 3-diethylaminopropylamine, sec-butylamine, n-butylamine, 2-methoxyethylamine, 3-methoxypropylamine, 2,2-dimethoxyethylamine, morpholine, N-methylmorpholine, N-ethylmorpholine, piperazines, pyrrole, pyridine, and metal hydroxides such as sodium hydroxide, potassium hydroxide, and magnesium hydroxide.
[0081] Among them, morpholine, N,N-dimethylethanolamine, N,N-diethylethanolamine, and 2-amino-2-methyl-1-propanol are preferred from the viewpoint of ease of emulsification and dispersion.
[0082] The boiling point of the neutralizing agent at normal pressure is preferably 200° C. or less. If the boiling point exceeds 200° C., for example, when the aqueous dispersion composition is formed into a coating film, it may be difficult to remove the neutralizing agent by drying treatment in the water removal step. Therefore, the water resistance and moisture resistance of the coating film may deteriorate, especially when dried at low temperature, or the adhesion to a substrate such as a non-polar resin molded article may deteriorate.
[0083] The neutralizing agent may be used alone or in combination of two or more. In the case of a combination of two or more, the blending ratio of each compound is not particularly limited.
[0084] In the water dispersion composition, the content of the neutralizing agent is not particularly specified, but is preferably 3.0 times or less equivalent relative to the carboxyl group in the grafted modified product. Thus, excessive increase in pH of the water dispersion composition can be suppressed. The lower limit is preferably 0.5 times or more equivalent. Thus, excessive decrease in pH of the water dispersion composition can be suppressed.
[0085] When the dispersion composition is an aqueous dispersion composition, the pH of the aqueous dispersion composition is preferably 5 or more, more preferably pH 6 to 11. If the pH is lower than 5, the neutralization is insufficient, and there is a situation where the modified polyolefin resin is not dispersed in water. In addition, even in the case of dispersion, there is a situation where precipitation and separation are easily generated over time, and the storage stability is poor. On the other hand, if the pH exceeds 11, there is a situation where problems arise in terms of compatibility with other components or operational safety. The pH can be adjusted by the amount of the neutralizer added when the aqueous dispersion composition is modulated.
[0086] In the case where the dispersion composition is an aqueous dispersion composition, the average particle size of the resin emulsified and dispersed in water is preferably 300 nm or less, more preferably 200 nm or less. If it exceeds 300 nm, the storage stability of the aqueous dispersion composition or the compatibility with other resins may deteriorate. In addition, when forming a film, the adhesion to the substrate, solvent resistance, water resistance, adhesion resistance and other film properties may be reduced. The average particle size can be adjusted by the composition of the modified polyolefin resin, the amount of the dispersion medium, the amount and type of the emulsifier added, the stirring force during dispersion and other conditions.
[0087] In this specification, the average particle size is a value obtained by particle size distribution measurement using a light diffusion method.
[0088] If the amount of emulsifier added is increased, the particle size can be infinitely reduced. However, increasing the amount of emulsifier added tends to reduce the coating properties such as adhesion to the substrate, water resistance, and anti-pore properties.
[0089] The Tm of the dispersion composition is preferably 85°C or higher and lower than 110°C or 90°C or higher and lower than 110°C, and more preferably 90°C or higher and lower than 105°C. If the Tm is 85°C or higher, sufficient water resistance under high temperature conditions can be further improved. On the other hand, if the melting point is lower than 110°C, good film forming properties can be ensured during coating film baking.
[0090] In the present specification, the Tm of the dispersion composition is obtained by measuring a dried product obtained by drying the dispersion composition at 40° C. for 24 hours using DSC (manufactured by TA Instruments) in the same manner as the Tm of the modified polyolefin resin.
[0091] The dispersion composition of the present invention can function as an intermediate medium for substrates with low adhesiveness and difficult coating of coatings, such as non-polar resin molded products. For example, it can also be used as an adhesive for polyolefin-based substrates such as polypropylene and polyethylene that lack adhesiveness, and can be used regardless of whether the surface of the substrate such as the non-polar resin molded product has been treated with plasma treatment, corona treatment, or the like.
[0092] Furthermore, by laminating the dispersion composition of the present invention on the surface of a non-polar resin molded product such as a polyolefin-based substrate by hot melt method and then applying a coating material thereon, the adhesion stability of the coating material can be improved.
[0093] Furthermore, it is also suitable for polar substrates such as polyester such as polyethylene terephthalate, polyurethane, and polyamide.
[0094] That is, the dispersion composition of the present invention can be suitably used as a primer, a coating material, an ink, an adhesive, and the like.
[0095] The preparation method of the dispersion composition is not particularly limited. For example, a method of a dispersion process including at least adding a modified polyolefin resin to a dispersion medium and dispersing it can be cited. In the case where the dispersion composition is an aqueous dispersion composition, a pre-process of adding a modified polyolefin resin to an organic solvent and dissolving (preferably under heating conditions) and then distilling off the organic solvent can be performed before the dispersion process. In the case of using a neutralizing agent, the neutralizing agent is preferably added at the stage of being dissolved in the organic solvent. In the case where the dispersion composition contains other resin components, the resin components are preferably blended after the above-mentioned dispersion process. For example, a resin component blending process of blending the resin components and adjusting the solid content (for example, adding a dispersion medium for dilution) as needed can be performed after the dispersion process. Example
[0096] Hereinafter, the present invention will be described in more detail by way of examples. The following examples are examples for appropriately describing the present invention and do not limit the present invention. The measuring methods of the physical property values, etc., are the measuring methods described above unless otherwise stated. In addition, "parts" refer to parts by weight unless otherwise stated.
[0097] [Methods for measuring physical properties]:
[0098] Mw and the graft weight of maleic anhydride were measured using a modified polyolefin resin. Tm, tensile modulus, and average particle size were measured using a water dispersion composition. Details of the measurement method are as follows.
[0099] [Mw (weight average molecular weight)]:
[0100] The resins prepared in the preparation examples were measured by GPC under the following conditions.
[0101] Device: HLC-8320GPC (Tosoh Company)
[0102] Column: TSK-gel G-6000 H×L, G-5000 H×L, G-4000 H×L, G-3000 H×L, G-2000 H×L (manufactured by Tosoh Company)
[0103] Eluent: THF
[0104] Flow rate: 1mL / min
[0105] Temperature: Pump thermostat, column thermostat 40°C
[0106] Injection volume: 100 μL
[0107] Standard substance: polystyrene EasiCal PS-1 (manufactured by Agilent Technology).
[0108] [Graft weight (wt%)]:
[0109] Determined by alkaline titration.
[0110] [Tm (melting point, °C)]:
[0111] According to JIS K7121-1987, using a DSC measuring apparatus (manufactured by TA Instruments), about 5 mg of a sample was heated at 150°C for 10 minutes and kept in a molten state. Then, the temperature was lowered at a rate of 10°C / min and kept stable at -50°C. Then, the temperature was raised to 150°C at a rate of 10°C / min, and the melting peak temperature during melting was taken as Tm.
[0112] The Tm of the water dispersion composition was measured using DSC (manufactured by TA Instruments) under the same conditions as above by drying the water dispersion composition at 40° C. for 24 hours.
[0113] [Tensile elastic modulus]:
[0114] The aqueous dispersion composition was dried at 40°C for 24 hours, and the obtained dried product was dissolved in an organic solvent to obtain a solution. The obtained solution was applied to a release paper in such a manner that the film thickness was about 20 μm, and dried for 5 minutes using an air supply dryer set at 100°C, and stored for 24 hours under constant temperature and humidity conditions of 23°C and 50% relative humidity to prepare a coating film. The coating film was cut into 15 mm wide and 150 mm long, and the release paper was peeled off to obtain a test film. For the obtained test film, the tensile modulus was measured using a tensile tester (Tensilon universal material testing machine: manufactured by A & D Company, Limited) at a tensile speed of 10 mm / min and a distance between chucks of 100 mm.
[0115] [Average particle size (nm)]:
[0116] The measurement was performed using a particle size distribution measuring apparatus (manufactured by Malvern Instruments).
[0117] [Example 1]
[0118] In a four-necked flask equipped with a stirrer, a cooling tube and a dropping funnel, a propylene-1-butene copolymer (I) (propylene component: 80 mol%, 1-butene component: 20 mol%, Mw: 100,000, Tm: 85°C, tensile elastic modulus: 160 MPa) and a propylene-1-butene copolymer (II) (propylene component: 90 mol%, 1-butene component: 10 mol%, Mw: 100,000, Tm: 100°C, tensile elastic modulus: 360 MPa) were heated and dissolved in 400 g of toluene at a weight ratio of 50:50. While the temperature in the system was maintained at 110°C and stirred, 4.5 parts of maleic anhydride and 3.0 parts of di-tert-butyl peroxide were added dropwise over 3 hours. After the reaction was allowed to proceed for another hour after the addition was completed, the mixture was cooled to room temperature. The reaction product was added to a large excess of acetone for purification, thereby obtaining a modified polyolefin resin (1) having a Mw of 100,000, a Tm of 90° C., and a graft weight of maleic anhydride of 3.0% by weight.
[0119] Next, 100 g of the obtained modified polyolefin resin (1), 20 g of toluene, and 60 g of ethylene glycol monobutyl ether (molecular weight = 118.2) were added to a four-necked flask equipped with a stirrer, a cooling tube, a thermometer, and a funnel, and stirred for 30 minutes at an internal temperature of 95°C. Next, 10 g of N,N-dimethylethanolamine [DMEA] was added, and stirred for 60 minutes at an internal temperature of 95°C. Then, 400 g of 90°C deionized water was added over 120 minutes, and the mixture was cooled while stirring until the internal temperature of the flask reached 30°C. The mixture was heated again while stirring until the internal temperature of the flask reached 95°C, and a portion of toluene and ethylene glycol monobutyl ether were distilled off under reduced pressure. Then, the mixture was cooled to room temperature while stirring, and the solid content was adjusted to 30 wt% with deionized water. Thus, an aqueous dispersion composition (1) containing a modified polyolefin resin (1) was obtained. The Tm of the dried product of the aqueous dispersion composition (1) was 91°C.
[0120] [Example 2]
[0121] 100 parts of propylene-1-butene copolymer (III) (propylene component: 90 mol%, 1-butene component: 10 mol%, Mw: 400,000, Tm: 100°C, tensile elastic modulus: 360 MPa), 3.0 parts of maleic anhydride, and 2.0 parts of dilauroyl peroxide were kneaded and reacted using a twin-screw extruder set at 200°C. Degassing was performed under reduced pressure in the extruder to remove the remaining unreacted products, thereby obtaining a modified polyolefin resin (2) having a Mw of 80,000, a Tm of 100°C, and a graft weight of maleic anhydride of 3.0 wt%.
[0122] Using the obtained modified polyolefin resin (2), a water dispersion composition (2) was prepared in the same manner as in Example 1 except that the amount of DMEA added was changed to 7 g. The Tm of the dried product of the water dispersion composition (2) was 94°C.
[0123] [Example 3]
[0124] Modified polyolefin resin (3) was obtained by the same method as in Example 2 except that the reaction temperature by the twin-screw extruder was 180° C. The obtained modified polyolefin resin (3) had an Mw of 100,000, a Tm of 100° C., and a graft weight of maleic anhydride of 3.0 wt %.
[0125] The water dispersion composition was also prepared in the same manner as in Example 2. The Tm of the dried product of the water dispersion composition (3) was 95°C.
[0126] [Comparative Example 1]
[0127] The modification was carried out in the same manner as in Example 1 except that 100 parts of the propylene-1-butene copolymer (I) was used instead of the propylene-1-butene copolymers (I) and (II) of Example 1, the amount of maleic anhydride added was 3.0 parts, and the amount of di-tert-butyl peroxide added was 2.0 parts. The obtained modified polyolefin resin (4) had an Mw of 100,000, a Tm of 85°C, and a graft weight of maleic anhydride of 3.0% by weight.
[0128] The water dispersion composition was prepared in the same manner as in Example 1 except that the amount of DMEA added was 7 g. The Tm of the dried product of the water dispersion composition (4) was 82°C.
[0129] [Comparative Example 2]
[0130] Propylene-1-butene copolymer (IV) (propylene component: 80 mol%, 1-butene component: 20 mol%, Mw: 60,000, Tm: 85°C) and propylene-1-butene copolymer (V) (propylene component: 90 mol%, 1-butene component: 10 mol%, Mw: 60,000, Tm: 100°C) were used instead of propylene-1-butene copolymer (I) and (II) of Example 1, and modification was performed in the same manner as in Example 1 except that the amount of maleic anhydride added was 3.0 parts and the amount of di-tert-butyl peroxide added was 2.0 parts. The obtained modified polyolefin resin (5) had Mw: 60,000, Tm: 90°C, and the graft weight of maleic anhydride was 3.0 wt%.
[0131] The water dispersion composition was prepared in the same manner as in Example 1 except that the amount of DMEA added was changed to 7 g. The Tm of the dried product of the water dispersion composition (5) was 89°C.
[0132] [Table 1]
[0133] Table 1
[0134]
[0135] The following tests were performed using the water dispersion compositions obtained in Examples 1 to 3 and Comparative Examples 1 to 2. Table 2 shows a summary of the test results.
[0136] [Water resistance peeling (water resistance adhesion) test under high temperature conditions]:
[0137] (Preparation of coating)
[0138] 40 parts of the aqueous dispersion composition obtained in the examples and comparative examples, calculated on a solid content basis, 40 parts of an aqueous acrylic resin (Bayhydrol XP2427, manufactured by Sumika Bayer Urethane Co., Ltd.), calculated on a solid content basis, 20 parts of an aqueous polyurethane resin (UCOAT UWS-145, manufactured by Sanyo Chemical Industries, Ltd.), 20 parts of conductive carbon Carbon ECP600JD (manufactured by Lion), and 80 parts of titanium dioxide Titan R-960 (manufactured by DuPont) were mixed according to a conventional method and diluted with ion-exchanged water to a solid content of 40%, thereby preparing an aqueous primer coating.
[0139] (Preparation of test panels)
[0140] For the resin substrate for the vehicle body, a water-based primer paint adjusted to a dry film thickness of about 25 μm was applied by an air spray gun, and after standing for 5 minutes, it was preheated at 60°C for 3 minutes. Next, a water-based metallic basecoat paint was applied to a dry film thickness of about 20 μm, and after standing for 5 minutes, it was preheated at 80°C for 3 minutes. Then, an acrylic urethane solvent-based clearcoat paint was applied to a dry film thickness of about 35 μm, and after standing for 7 minutes, it was baked at 120°C for 20 minutes to prepare a coated object.
[0141] Next, a urethane adhesive (trade name "3740", manufactured by Sunstar Co., Ltd., automotive windshield agent) was applied to the prepared object to a coating shape of 20 mm wide, 3 mm thick, and 100 mm long or more, and then covered with release paper and pressed evenly with a flat plate. After removing the flat plate, the object was left to cure under constant temperature and humidity conditions of 23°C and 50% relative humidity for 72 hours. Then, the release paper was peeled off to prepare a test plate.
[0142] (Test Procedure)
[0143] The prepared test plate was immersed in a constant temperature water bath set at 60° C. for 10 days, then immersed in water at 23° C. for 1 hour to cool, and then the following peel test was performed.
[0144] The cured adhesive layer was stretched by hand in a direction of 90 degrees or more relative to the coating film, and cut with a cutter at an angle of about 60 degrees relative to the coating film at intervals of 2 to 3 mm until it reached the coating film surface. The peeling state after peeling the adhesive layer was evaluated according to the following standards of "A", "B", "C", and "D".
[0145] A: No peeling of the adhesive layer was observed, and no exposure of the coating film was observed.
[0146] B: The coating film was not destroyed, and only the adhesive layer was peeled off due to cohesive failure, but the adhesion between the coating film and the adhesive layer was basically maintained.
[0147] C: The coating film undergoes cohesive failure and peels off.
[0148] D: Peeling was observed at the interface between the coating film and the adhesive layer.
[0149] [Checkerboard Adhesion Test]:
[0150] (Preparation of test pieces)
[0151] The surface of the ultra-high rigidity polypropylene plate was degreased with isopropyl alcohol, and the aqueous dispersion composition was spray-coated so as to have a dry film thickness of about 15 μm, and preheated at 80° C. for 5 minutes. Next, the base coating was spray-coated, and after standing for 10 minutes, the clear coating was applied and stood for 10 minutes. Then, a baking treatment was performed at 120° C. for 20 minutes, and the plate was left standing at room temperature for 72 hours to prepare a test piece.
[0152] (Test Procedure)
[0153] For the prepared test piece, 100 grid-like cuts were made on the coating film at 2 mm intervals with a cutter knife, reaching the substrate, a cellophane tape was adhered thereto, and the film was peeled off 10 times at an angle of 180° to determine the remaining coating film. Specifically, the number of remaining pieces was counted.
[0154] [Water resistance adhesion test]:
[0155] Prepare the test piece in the same way as in the checkerboard adhesion test. After immersing the test piece in warm water at 60°C for 10 days, visually observe the swelling state (bubbling) on the coating surface. Use a cutting knife to cut 100 checkerboard-shaped cuts reaching the substrate at 2 mm intervals on the coating, stick a cellophane tape on it, peel it off at an angle of 180°, and judge it according to the degree of residual coating. In addition, for samples that were not completely peeled off in this test, the same test was carried out 10 times in a row to determine the residue of the coating after peeling off 10 times. Specifically, count the number of remaining blocks.
[0156] Foaming was evaluated according to the following criteria.
[0157] Diameter: (large) 1~10 (small)
[0158] Frequency: None, (less) F, M, MD, D (more)
[0159] The diameter is the size of the bubbles, and the visually confirmed value is within 8. The frequency is the number of bubbles, and is an abbreviation of F (few), M (medium), MD (medium dense), and D (dense).
[0160] [Table 2]
[0161] Table 2
[0162]
[0163] (Footnote to Table 2)
[0164] (2M: means the bubble diameter is 2 and the bubble frequency is M).
[0165] The following contents can be known from Table 2. As can be seen from the result of the checkerboard adhesion test, the adhesion of the water dispersion composition of the embodiment and the comparative example is not problematic. In addition, according to the result of the water-resistant peeling test, the number of remaining pieces of the water dispersion composition of embodiment 1 to 3 is 100, and there is no bubbling, so the water-resistant adhesion under high temperature conditions is excellent. On the other hand, although the water dispersion composition of comparative example 1 does not have bubbling, the number of remaining pieces is 69, which is compared with the water dispersion composition of embodiment 1 to 3, and the water-resistant adhesion under high temperature conditions is poor. The bubbling of the water dispersion composition of comparative example 2 is 2M (the evaluation of diameter is 2, and the evaluation of frequency is M), and the number of remaining pieces is 0, so it is known that there is no water-resistant adhesion under high temperature conditions. In addition, according to the result of the water-resistant adhesion test under high temperature conditions, the evaluation of the water dispersion composition of embodiment 1 to 3 is "A" or "B", which can be used for purposes without window frame installation method, etc.
Claims
1. A modified polyolefin resin comprising a graft modified product obtained by grafting component (A): a polyolefin resin with component (B): an α,β-unsaturated carboxylic acid or a derivative thereof, wherein the graft weight of component (B) in the graft modified product is 0.1 to 10% by weight. The tensile elastic modulus of the modified polyolefin resin is greater than 250 MPa, The weight average molecular weight is 70,000 or more and less than 200,000, The tensile modulus is a tensile modulus measured as follows: a water dispersion composition of a modified polyolefin resin is dried, the obtained dried product is heated and dissolved in an organic solvent, the obtained solution is applied on a release paper so that the film thickness is 20 μm, and then dried for 5 minutes in a blower dryer set at 100° C., and then stored for 24 hours under constant temperature and humidity conditions of 23° C. and a relative humidity of 50%, and then cut into a width of 15 mm and a length of 150 mm, and the release paper is peeled off to obtain a test film. The tensile modulus of the obtained test film is measured using a tensile tester under the conditions of a tensile speed of 10 mm / min and a distance between chucks of 100 mm. The α,β-unsaturated carboxylic acid or its derivative is at least one selected from maleic acid, maleic anhydride, fumaric acid, citraconic acid, citraconic anhydride, mesaconic acid, itaconic acid, itaconic anhydride, aconitic acid, aconitic anhydride, nadic anhydride, (meth)acrylic acid, (meth)acrylate, The melting point measured by differential scanning calorimetry is 85°C or higher and lower than 110°C.
2. The modified polyolefin resin according to claim 1, wherein The melting point measured by differential scanning calorimetry is 85°C or higher and lower than 105°C.
3. The modified polyolefin resin according to claim 1 or 2, wherein The component (A) contains at least one selected from the group consisting of an ethylene-propylene copolymer, a propylene-1-butene copolymer and an ethylene-propylene-1-butene copolymer.
4. A dispersion composition comprising the modified polyolefin resin according to claim 1 or 2.
5. The dispersion composition according to claim 4, wherein The melting point measured by differential scanning calorimetry is 90°C or higher and lower than 110°C.
6. The dispersion composition according to claim 4 or 5, which is a primer.
7. The dispersion composition according to claim 4 or 5, which is a coating material.
8. The dispersion composition according to claim 4 or 5, which is an ink.
9. The dispersion composition according to claim 4 or 5, which is an adhesive.
Citation Information
Patent Citations
Modified poly olefine based resin
JP2015105294A
Resin dispersion, coating materials, laminates, and processes for production of the same