A correction lens and preparation method thereof
By coating the lens with a mixture layer of nickel, titanium and niobium oxide, combined with a multi-layer film structure, the "invisible" blocking and anti-reflection effect of light is achieved, solving the problems of occlusion and visual interference in existing lenses, and providing an effective Astigmatism correction and visual comfort.
Patent Information
- Application Number
- CN202210426211.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-22
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-04-22
AI Technical Summary
When existing lenses correct astigmatism, the rotation of the shielding piece will cause the wearer to feel an uncomfortable floating feeling, affecting the visual effect. Moreover, the blocking material interferes with vision greatly, making it difficult to achieve an "invisible" effect.
A mixture layer of nickel, titanium and niobium oxide is used as the light blocking layer. A ring-shaped light blocking layer is formed on the lens substrate through coating technology. Combined with the outer anti-reflection film layer and the inner anti-reflection film layer, it limits the entry of peripheral light and reduces the Strabismus, restore visual brightness perception, and achieve "invisible" correction.
It reduces the visual interference of the lens on the wearer. The wearer can focus on the central area of the lens to prevent astigmatism, and the visual experience is not affected. The market application prospect is broad.
Smart Images

Figure FDA0004986643390000022
Abstract
Description
Technical Field
[0001] The invention relates to the protection and adjustment functions of a lens, in particular to a correction lens and a preparation method thereof. Background Art
[0002] Astigmatism is a manifestation of abnormal refraction. Because the patient's eyes cannot focus normally, they cannot form a clear image. For regular astigmatism, lenses can be used for correction. Usually, a shielding piece is set on the outside of the lens. When correction is needed, the shielding piece is rotated to a preset position to adjust the external light entering the eyeball.
[0003] However, this type of lens will cause discomfort to the wearer, that is, the wearer will clearly feel that there is an obstruction in front of the eyes, which will cause a bad feeling psychologically. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of existing lenses and provide a corrective lens that can "invisibly" process light without interfering with the user's vision, including blocking the light from the edge of the lens from entering the human eye through incidence, reflection and scattering at different angles, so that the wearer's eyes can focus, concentrate and observe in the forward direction, and has the effect of preventing and improving problems such as astigmatism and strabismus of the eyes.
[0005] In the present invention, the corrective lens forms a functional film layer on the substrate by coating, including a light blocking layer and a permeability-enhancing film layer, wherein the light blocking layer has the function of limiting and blocking peripheral light, and the light blocking layer will cause a reduction in the light entering the eyeball, resulting in a darker visual experience. Conventional blocking materials are generally effective in blocking light, and are likely to interfere with the wearer's vision, that is, forming a dark-colored coating, so that the wearer can clearly feel the existence of the blocking layer. The present invention uses a mixture layer of nickel, titanium and niobium oxide, which can not only ensure the light blocking effect, but also not interfere with the wearer's observation window. The light blocking layer is arranged on the outer ring of the lens, and has a limited width, so that the user himself does not feel any obstruction, which is consistent with the visual experience of normal glasses. Therefore, the processing of light can be achieved "invisibly". On the other hand, the light blocking layer can also play a role in limiting scattered light, reducing the occurrence of strabismus, and allowing the eyes to have better light focusing, thereby achieving a correction effect.
[0006] Since the light blocking layer will reduce the light entering the eyeball, the present invention adjusts the light through the outer anti-reflection film layer and the inner anti-reflection film layer to restore the normal visual brightness of the eye. Preferably, the outer anti-reflection film layer and the inner anti-reflection film layer are alternately stacked high refractive index layers and low refractive index layers, with a thickness of 1500-4500 angstroms. The anti-reflection film layer and the light blocking layer have opposite effects on light, and the film layers on the surface of the lens form a whole, which will jointly form an anti-reflection and blocking effect on light. In order to prevent the transmittance-enhancing film layer from excessively interfering with the lens's blocking effect on the light at the edge of the lens, thereby causing an adverse effect on the overall correction effect, the transmittance-enhancing film layer in the present invention is preferably an 8-layer film, wherein the first, third, fifth and seventh layers are high refractive index layers with thicknesses of 50-150 angstroms, 150-350 angstroms, 500-800 angstroms and 150-350 angstroms, respectively, and the second, fourth, sixth and eighth layers are low refractive index layers with thicknesses of 200-600 angstroms, 50-250 angstroms, 50-250 angstroms and 600-1100 angstroms, respectively.
[0007] The specific plan is as follows:
[0008] A corrective lens, comprising a substrate, wherein the side of the corrective lens that is away from the user in the use state is defined as the outer side, and the outer surface of the substrate is provided with a light blocking layer and an outer transmittance increasing film layer that are connected to each other; the inner surface of the substrate is provided with an inner transmittance increasing film layer; the light blocking layer is a mixture layer of nickel, titanium and niobium oxide, and the light blocking layer is distributed in an annular shape on the outer edge of the substrate, thereby limiting the light around the substrate from entering the user's glasses.
[0009] Furthermore, the light blocking layer extends from the outer edge of the substrate to the central area by 4-8 mm, preferably 6-7 mm.
[0010] Furthermore, the content of nickel in the light blocking layer is 1-5wt%, the content of titanium is 5-10wt%, and the content of niobium oxide is 85-94wt%.
[0011] Furthermore, the light blocking layer includes a first light blocking layer and a second light blocking layer. Specifically, the first light blocking layer is located between the outer surface of the substrate and the first outer transmittance increasing film layer, the outer surface of the first outer transmittance increasing film layer is connected to the second light blocking layer, and the outer surface of the second light blocking layer is connected to the second outer transmittance increasing film layer and / or the protective layer.
[0012] Furthermore, the thickness of the first light blocking layer and the second light blocking layer are 2000-3000 angstroms and 3000-5000 angstroms respectively; the thickness of the protective layer is 300-500 angstroms.
[0013] Furthermore, the transmittance of the first light blocking layer and the second light blocking layer in the visible light spectrum region is less than 1%.
[0014] Furthermore, the outer transmittance-enhancing film layer and the inner transmittance-enhancing film layer are alternately stacked high refractive index layers and low refractive index layers, the refractive index of the high refractive index layer is 1.90-2.50, the refractive index of the low refractive index layer is 1.3-1.5, and the thickness of the outer transmittance-enhancing film layer and the inner transmittance-enhancing film layer is 1500-4500 angstroms.
[0015] Furthermore, the outer permeability-enhancing film layer and the inner permeability-enhancing film layer include 8 layers of films connected sequentially from the inside to the outside, the first layer, the third layer, the fifth layer and the seventh layer are high refractive index layers with thicknesses of 50-150 angstroms, 150-350 angstroms, 500-800 angstroms and 150-350 angstroms, respectively, the second layer, the fourth layer, the sixth layer and the eighth layer are low refractive index layers with thicknesses of 200-600 angstroms, 50-250 angstroms, 50-250 angstroms and 600-1100 angstroms, respectively; the outer permeability-enhancing film layer and the inner permeability-enhancing film layer have a transmittance greater than 99% in the visible light spectrum region with a wavelength range of 380-720nm.
[0016] The present invention also protects a method for preparing the corrective lens, comprising the following steps:
[0017] S1, cleaning the substrate and drying it to obtain a clean substrate;
[0018] S2. Place the clean substrate on the fixture, send it into the vacuum coating chamber and evacuate it. When the vacuum degree in the vacuum chamber reaches below 3*10-5Torr, turn on the ion source to clean the surface of the substrate. When the vacuum degree in the vacuum chamber reaches below 1.5*10-5Torr, control the temperature in the vacuum chamber at 50-70℃ and the evaporation rate at Using an electron gun to bombard the materials of the light blocking layer, the outer transmission film layer and the inner transmission film layer in sequence, so as to form the inner transmission film layer on the inner surface of the substrate and the light blocking layer and the outer transmission film layer on the outer surface;
[0019] Optionally, a protective layer may be deposited on the outermost side of the corrective lens. Specifically, the vacuum degree in the vacuum chamber is maintained below 1.5*10-5 Torr, the temperature in the vacuum chamber is controlled at 50-70° C., and the deposition rate is controlled at The waterproof material is heated by group evaporation, and after evaporation, the waterproof material is deposited on the outer surface of the light blocking layer in the form of molecular crystals to form a protective layer.
[0020] The present invention also protects a pair of spectacles comprising the corrective lenses.
[0021] Beneficial effects:
[0022] In the present invention, the corrective lens can reduce the interference of peripheral light of the lens on the user, so that the user can focus on the central area of the lens for observation, thereby adjusting the viewing angle and preventing astigmatism, and has a corrective effect for people with regular astigmatism.
[0023] Furthermore, the present invention arranges a light blocking layer, an outer transmittance increasing film layer, and an inner transmittance increasing film layer on the surface of the lens, so that the user's normal visual experience does not change, and a correction effect is achieved invisibly, which has a good market application prospect. DETAILED DESCRIPTION
[0024] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. In the examples, those without specifying specific techniques or conditions are carried out according to the techniques or conditions described in the literature in this area or according to the product specification. Those without specifying the manufacturer of reagents or instruments used are all conventional products that can be obtained commercially. In the following examples, if not clearly stated, "%" refers to weight percentage.
[0025] In the present invention, the corrective lens comprises a substrate, which can be selected from any one of an acrylic substrate, a polycarbonate substrate, a nylon substrate, a CR-39 substrate and a glass substrate. The side of the corrective lens that is away from the user in the use state is defined as the outer side, and the outer surface of the substrate is provided with a light blocking layer and an outer transmission film layer connected to each other; the inner surface of the substrate is provided with an inner transmission film layer.
[0026] Among them, the light blocking layer is a mixture layer of nickel, titanium and niobium oxide. In order to ensure the blocking effect, preferably, the nickel content in the light blocking layer is 1-5wt%, the titanium content is 5-10wt%, and the niobium oxide content is 85-94wt%. For example, the nickel content is 2-4wt%, the titanium content is 6-9wt%, and the niobium oxide content is 88-93wt%.
[0027] The light blocking layer is distributed in an annular shape on the outer edge of the substrate, thereby limiting the light around the substrate from entering the user's glasses. The outer edge of the light blocking layer coincides with the outer edge of the substrate, and the inner edge can be a regular shape, such as an elliptical ring, a circular ring, a flower shape, etc., or an irregular shape, such as a continuous wave with different arcs, etc.
[0028] In a specific embodiment, the light blocking layer extends 4-8 mm, preferably 6-7 mm, from the outer edge of the substrate to the central area to ensure a balance between the wearer's visual brightness and protecting the eyes from damage by oblique light and scattered light.
[0029] The light blocking layer can be one layer, or two layers or more layers, in which case an anti-reflection film layer is arranged between adjacent light blocking layers. Too many layers of light blocking layers will cause visual interference, that is, the wearer will feel a shadow in front of the eyes. Preferably, the light blocking layer includes a first light blocking layer and a second light blocking layer. Specifically, the first light blocking layer is located between the outer surface of the substrate and the first outer anti-reflection film layer, the outer surface of the first outer anti-reflection film layer is connected to the second light blocking layer, and the outer surface of the second light blocking layer is connected to the second outer anti-reflection film layer and / or the protective layer. In this case, the edge area of the lens can achieve a transmittance value of less than 1%. For example, the thickness of the first light blocking layer and the second light blocking layer are 2000-3000 angstroms and 3000-5000 angstroms respectively, and the wearer has a better visual experience.
[0030] The lens of the present invention contains an outer anti-reflection film layer and an inner anti-reflection film layer, which can adopt the existing anti-reflection technology. In a specific embodiment, it can be composed of a high refractive index layer and a low refractive index layer stacked in sequence. The refractive index of the high refractive index layer is 1.90-2.50, and Ti3O5, Ta2O5, ZrO2, etc. can be selected. The refractive index of the low refractive index layer is 1.3-1.5, and SiO2, MgF2, etc. can be selected. Preferably, the anti-reflection film layer includes 8 layers of thin films connected in sequence, the first layer, the third layer, the fifth layer and the seventh layer are high refractive index layers, and the thicknesses are 50-150 angstroms, 150-350 angstroms, 500-800 angstroms and 150-350 angstroms respectively, and the second layer, the fourth layer, the sixth layer and the eighth layer are low refractive index layers, and the thicknesses are 200-600 angstroms, 50-250 angstroms, 50-250 angstroms and 600-1100 angstroms respectively. The 8-layer structure achieves a transmittance of more than 99% in the visible light spectrum range of 380-720nm to compensate for the weakening of brightness by the light blocking layer, while not producing too much visual disparity and preventing the wearer from perceiving the limiting effect of the light blocking layer outside the lens.
[0031] Example 1
[0032] A corrective lens includes a substrate with a thickness of 2 mm and made of glass. In other embodiments, the substrate can also be selected from any one of an acrylic substrate, a polycarbonate substrate, a nylon substrate, and a CR-39 substrate, and a more suitable substrate has a thickness of 0.5-3.5 mm.
[0033] The side of the corrective lens that is away from the user in the use state is defined as the outer side, and the outer surface of the substrate is provided with a light blocking layer and an outer transmittance-enhancing film layer connected to each other; the inner surface of the substrate is provided with an inner transmittance-enhancing film layer.
[0034] The light blocking layer is distributed in a ring shape on the outer edge of the substrate, thereby limiting the light around the substrate from entering the user's glasses. For example, it can be an elliptical ring, or a wavy line on the inside, and overlap the outer edge of the substrate on the outside. In order to ensure the visual effect, the width of the light blocking layer should be limited, for example, it can extend 4mm from the outer edge of the substrate to the central area, so that enough space for light to pass through the central area of the lens is left.
[0035] Specifically, the outer surface of the substrate is sequentially laminated with a first light blocking layer, an outer transmittance increasing film layer, and a second light blocking layer. The first light blocking layer and the second light blocking layer are made of the same material, which is a mixture layer of nickel, titanium and niobium oxide, wherein the content of nickel is 5wt%, the content of titanium is 5wt%, and the content of niobium oxide is 90wt%. The thicknesses of the first light blocking layer and the second light blocking layer are 2000 angstroms and 4000 angstroms, respectively.
[0036] The outer anti-reflection film layer is an alternating stack of high refractive index layers and low refractive index layers, specifically an alternating stack of Ti3O5 and SiO2, including 8 layers, the first, third, fifth and seventh layers are Ti3O5 material layers, with thicknesses of 100 angstroms, 250 angstroms, 600 angstroms and 250 angstroms respectively, the second, fourth, sixth and eighth layers are SiO2 layers, with thicknesses of 400 angstroms, 150 angstroms, 150 angstroms and 1000 angstroms respectively. The structure of the inner anti-reflection film layer is the same as that of the outer anti-reflection film layer, that is, it includes 8 layers of high and low refractive index layers stacked alternately, of which the first layer is connected to the outer surface of the substrate.
[0037] The overall appearance of the corrective lens is colorless, and a dark band area can be seen at the edge of the lens. After wearing it, the user cannot feel the dark band area at the edge of the lens, but when observing, he will naturally observe through the center of the lens, because the visual observation area of the lens is smaller than the actual size of the lens. At the same time, the light near the periphery of the lens is blocked, reducing the overall width of vision. Through optical testing of the corrective lens, the transmittance of the center of the lens in the visible light wavelength range of 380-720nm is greater than 99%, while the transmittance of the outer edge (2-3mm wide from the outside of the substrate to the center area) in the visible light wavelength range of 380-720nm is less than 1%.
[0038] Example 2
[0039] A corrective lens comprises a nylon substrate, wherein the thickness of the substrate is 1.5 mm.
[0040] The side of the corrective lens that is away from the user in the use state is defined as the outer side, and the outer surface of the substrate is provided with a light blocking layer and an outer transmittance-enhancing film layer connected to each other; the inner surface of the substrate is provided with an inner transmittance-enhancing film layer.
[0041] The light blocking layer is distributed in a ring shape on the outer edge of the substrate, thereby limiting the light around the substrate from entering the user's glasses. For example, it can be an elliptical ring, or a wavy line on the inside, and overlap the outer edge of the substrate on the outside. In order to ensure the visual effect, the width of the light blocking layer should be limited to 8mm from the outer edge of the substrate to the central area, so that enough space for light to pass through the central area of the lens can be left.
[0042] Specifically, the outer surface of the substrate is sequentially laminated with a first light blocking layer, an outer transmittance increasing film layer, and a second light blocking layer. The first light blocking layer and the second light blocking layer are made of the same material, which is a mixture layer of nickel, titanium and niobium oxide, wherein the content of nickel is 3wt%, the content of titanium is 3wt%, and the content of niobium oxide is 94wt%. The thicknesses of the first light blocking layer and the second light blocking layer are 2300 angstroms and 4500 angstroms, respectively.
[0043] The outer transmittance-enhancing film layer is an alternating stack of high-refractive index layers and low-refractive index layers, specifically an alternating stack of Ta2O5 and SiO2, including 8 layers. The 1st, 3rd, 5th and 7th layers are Ta2O5 material layers with thicknesses of 50 angstroms, 150 angstroms, 800 angstroms and 150 angstroms respectively, and the 2nd, 4th, 6th and 8th layers are SiO2 layers with thicknesses of 300 angstroms, 100 angstroms, 250 angstroms and 600 angstroms respectively.
[0044] The preparation method comprises the following steps:
[0045] S1, cleaning the substrate and drying it to obtain a clean substrate;
[0046] S2. Place the clean substrate on the fixture, send it into the vacuum coating chamber and evacuate it. When the vacuum degree in the vacuum chamber reaches 3*10 -5 When the vacuum degree in the vacuum chamber reaches 1.5*10 -5 When the temperature in the vacuum chamber is below 50-70°C, the evaporation rate is controlled at An electron gun is used to bombard a plurality of film materials in sequence to form an inner transmittance-enhancing film layer on the inner surface of the substrate and a first light-blocking layer, an outer transmittance-enhancing film layer, and a second light-blocking layer on the outer surface.
[0047] The overall appearance of the corrective lens is colorless, and a dark band area can be seen at the edge of the lens. After wearing it, the user cannot feel the dark band area at the edge of the lens, but when observing, he will naturally observe through the center of the lens, because the visual observation area of the lens is smaller than the actual size of the lens. At the same time, the light near the periphery of the lens is blocked, reducing the overall width of vision. Through optical testing of the corrective lens, the transmittance of the center of the lens in the visible light wavelength range of 380-720nm is greater than 99%, while the transmittance of the outer edge (2-3mm wide from the outside of the substrate to the center area) in the visible light wavelength range of 380-720nm is less than 1%.
[0048] Example 3
[0049] A corrective lens comprises a polycarbonate substrate with a thickness of 1 mm. The side of the corrective lens that is away from the user in the use state is defined as the outer side, and the outer surface of the substrate is provided with a light blocking layer, an outer transmittance-enhancing film layer and a protective layer; the inner surface of the substrate is provided with an inner transmittance-enhancing film layer.
[0050] The light blocking layer is distributed in a ring shape on the outer edge of the substrate, thereby limiting the light around the substrate from entering the user's glasses. For example, it can be an elliptical ring, or a wavy line on the inside, and overlap the outer edge of the substrate on the outside. In order to ensure the visual effect, the width of the light blocking layer should be limited to 6mm from the outer edge of the substrate to the central area, so that enough space for light to pass through the central area of the lens can be left.
[0051] Specifically, the outer surface of the substrate is sequentially laminated with a first light blocking layer, an outer transmittance increasing film layer, a second light blocking layer and a protective layer. The first light blocking layer and the second light blocking layer are made of the same material, which is a mixture layer of nickel, titanium and niobium oxide, wherein the content of nickel is 4wt%, the content of titanium is 10wt%, and the content of niobium oxide is 86wt%. The thickness of the first light blocking layer and the second light blocking layer are 3000 angstroms and 5000 angstroms respectively.
[0052] The outer transmittance-enhancing film layer is an alternating stack of high-refractive index layers and low-refractive index layers, specifically an alternating stack of ZrO2 and MgF2, including 8 layers. The 1st, 3rd, 5th and 7th layers are ZrO2 material layers with thicknesses of 80 angstroms, 160 angstroms, 700 angstroms and 350 angstroms respectively, and the 2nd, 4th, 6th and 8th layers are MgF2 layers with thicknesses of 500 angstroms, 250 angstroms, 150 angstroms and 1100 angstroms respectively.
[0053] The preparation method comprises the following steps:
[0054] S1, cleaning the substrate and drying it to obtain a clean substrate;
[0055] S2. Place the clean substrate on the fixture, send it into the vacuum coating chamber and evacuate it. When the vacuum degree in the vacuum chamber reaches 3*10 -5 When the vacuum degree in the vacuum chamber reaches 1.5*10 -5 When the temperature in the vacuum chamber is below 50-70°C, the evaporation rate is controlled at An electron gun is used to bombard a plurality of film materials in sequence to form an inner transmittance-enhancing film layer on the inner surface of the substrate and a first light-blocking layer, an outer transmittance-enhancing film layer, and a second light-blocking layer on the outer surface.
[0056] S3, maintain the vacuum degree in the vacuum chamber at 1.5*10 -5 Torr, the temperature in the vacuum chamber is controlled at 50-70°C and the evaporation rate is controlled at The waterproof material is heated by group evaporation, and after evaporation, the waterproof material is deposited on the outer surface of the light blocking layer in the form of molecular crystals to form a protective layer, and the thickness of the protective layer is 300 angstroms. In other embodiments, the thickness of the protective layer can also be 400 angstroms or 500 angstroms.
[0057] The overall appearance of the corrective lens is colorless, and a dark band area can be seen at the edge of the lens. After wearing it, the user cannot feel the dark band area at the edge of the lens, but when observing, he will naturally observe through the center of the lens, because the visual observation area of the lens is smaller than the actual size of the lens. At the same time, the light near the periphery of the lens is blocked, reducing the overall width of vision. Through optical testing of the corrective lens, the transmittance of the center of the lens in the visible light wavelength range of 380-720nm is greater than 99%, while the transmittance of the outer edge (2-3mm wide from the outside of the substrate to the center area) in the visible light wavelength range of 380-720nm is less than 1%.
[0058] Example 4
[0059] A corrective lens includes a substrate with a thickness of 1.5 mm and made of glass. In other embodiments, the substrate can also be selected from any one of an acrylic substrate, a polycarbonate substrate, a nylon substrate, and a CR-39 substrate, and a more suitable substrate has a thickness of 0.5-3.5 mm.
[0060] The side of the corrective lens that is away from the user in the use state is defined as the outer side, and the outer surface of the substrate is provided with a light blocking layer and an outer transmittance-enhancing film layer connected to each other; the inner surface of the substrate is provided with an inner transmittance-enhancing film layer.
[0061] The light blocking layer is distributed in a ring shape on the outer edge of the substrate, thereby limiting the light around the substrate from entering the user's glasses. For example, it can be an elliptical ring, or a wavy line on the inside, and overlap the outer edge of the substrate on the outside. In order to ensure the visual effect, the width of the light blocking layer should be limited to 5mm from the outer edge of the substrate to the central area, so that enough space for light to pass through the central area of the lens can be left.
[0062] Specifically, the outer surface of the substrate is sequentially laminated with a first light blocking layer, an outer transmittance increasing film layer, and a second light blocking layer. The first light blocking layer and the second light blocking layer are made of the same material, which is a mixture layer of nickel, titanium and niobium oxide, wherein the content of nickel is 1wt%, the content of titanium is 10wt%, and the content of niobium oxide is 89wt%. The thicknesses of the first light blocking layer and the second light blocking layer are 2300 angstroms and 3800 angstroms, respectively.
[0063] The outer anti-reflection film layer is an alternating stack of high refractive index layers and low refractive index layers, specifically an alternating stack of Ti3O5 and SiO2, including 8 layers, the first, third, fifth and seventh layers are Ti3O5 material layers, with thicknesses of 100 angstroms, 150 angstroms, 5500 angstroms and 150 angstroms respectively, the second, fourth, sixth and eighth layers are SiO2 layers, with thicknesses of 600 angstroms, 150 angstroms, 100 angstroms and 900 angstroms respectively. The structure of the inner anti-reflection film layer is the same as that of the outer anti-reflection film layer, that is, it includes 8 layers of high and low refractive index layers stacked alternately, of which the first layer is connected to the outer surface of the substrate.
[0064] The overall appearance of the corrective lens is colorless, and a dark band area can be seen at the edge of the lens. After wearing it, the user cannot feel the dark band area at the edge of the lens, but when observing, he will naturally observe through the center of the lens, because the visual observation area of the lens is smaller than the actual size of the lens. At the same time, the light near the periphery of the lens is blocked, reducing the overall width of vision. Through optical testing of the corrective lens, the transmittance of the center of the lens in the visible light wavelength range of 380-720nm is greater than 99%, while the transmittance of the outer edge (2-3mm wide from the outside of the substrate to the center area) in the visible light wavelength range of 380-720nm is less than 1%.
[0065] Comparative Example 1
[0066] Referring to Example 1, the difference is that the materials of the first light blocking layer and the second light blocking layer are different from those of Example 1, and a mixture layer of nickel, titanium and niobium oxide is used, wherein the content of nickel is 10wt%, the content of titanium is 40wt%, and the content of niobium oxide is 50wt%. The rest is carried out according to the structure and preparation method of Example 1 to obtain a comparative lens.
[0067] The light test of the comparison lens shows that the transmittance of the center of the lens in the visible light wavelength range of 380-720nm is greater than 99%, while the transmittance of the outer edge (2-3mm from the outside of the substrate to the center area) in the visible light wavelength range of 380-720nm is less than 1%. However, after wearing the lens, the user can see the annular area on the outer edge of the lens, which has a different color perception from the central visual area, which brings a poor wearing experience.
[0068] Comparative Example 2
[0069] A contrast lens comprises a substrate, which is 2 mm thick and made of glass. The side of the correction lens away from the user in the use state is defined as the outer side, and the outer surface of the substrate is provided with a light blocking layer and an outer transmittance-enhancing film layer connected to each other.
[0070] The light blocking layer is distributed in a ring shape on the outer edge of the substrate, thereby limiting the light around the substrate from entering the user's glasses. For example, it can be an elliptical ring, or a wavy line on the inside, and overlap the outer edge of the substrate on the outside. In order to ensure the visual effect, the width of the light blocking layer should be limited, for example, it can extend 4mm from the outer edge of the substrate to the central area, so that enough space for light to pass through the central area of the lens is left.
[0071] Specifically, the outer surface of the substrate is sequentially laminated with a first light blocking layer, an outer transmittance increasing film layer, and a second light blocking layer. The first light blocking layer and the second light blocking layer are made of the same material, which is a mixture layer of nickel, titanium and niobium oxide, wherein the content of nickel is 5wt%, the content of titanium is 5wt%, and the content of niobium oxide is 90wt%. The thicknesses of the first light blocking layer and the second light blocking layer are 2000 angstroms and 4000 angstroms, respectively.
[0072] The outer transmittance-enhancing film layer is an alternating stack of high-refractive index layers and low-refractive index layers, specifically an alternating stack of Ti3O5 and SiO2, including 8 layers. The 1st, 3rd, 5th and 7th layers are Ti3O5 material layers with thicknesses of 100 angstroms, 250 angstroms, 600 angstroms and 250 angstroms respectively, and the 2nd, 4th, 6th and 8th layers are SiO2 layers with thicknesses of 400 angstroms, 150 angstroms, 150 angstroms and 1000 angstroms respectively.
[0073] After the comparison lens was tested under light, the transmittance of the center of the lens in the visible light wavelength range of 380-720nm was 95%, while the transmittance of the outer edge (2-3mm from the outside of the substrate to the center area) in the visible light wavelength range of 380-720nm was less than 1%. However, after wearing the lens, the user can partially see the annular area on the outer edge of the lens, which has a different color perception from the central visual area, bringing a poor wearing experience. At the same time, the brightness of the lens image is significantly different from the actual situation, the overall image is dark, there is discomfort, and it is not conducive to accurate observation.
[0074] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0075] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0076] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A corrective lens, characterized in that: The corrective lens comprises a substrate, and the side of the corrective lens away from the user in the use state is defined as the outer side, and the outer surface of the substrate is provided with a light blocking layer and an outer transmittance increasing film layer connected to each other; the inner surface of the substrate is provided with an inner transmittance increasing film layer; the light blocking layer is a mixture layer of nickel, titanium and niobium oxide, and the light blocking layer is distributed in an annular shape on the outer edge of the substrate, and the light blocking layer extends 4-8 mm from the outer edge of the substrate to the central area, thereby limiting the light around the substrate from entering the user's glasses; The outer permeability enhancing film layer and the inner permeability enhancing film layer are alternately stacked high refractive index layers and low refractive index layers, the refractive index of the high refractive index layer is 1.90-2.50, the refractive index of the low refractive index layer is 1.3-1.5, and the thickness of the outer permeability enhancing film layer and the inner permeability enhancing film layer is 1500-4500 angstroms; The outer permeability-enhancing film layer and the inner permeability-enhancing film layer include 8 layers of films connected sequentially from the inside to the outside, wherein the first layer, the third layer, the fifth layer and the seventh layer are high refractive index layers, with thicknesses of 50-150 angstroms, 150-350 angstroms, 500-800 angstroms and 150-350 angstroms respectively, and the second layer, the fourth layer, the sixth layer and the eighth layer are low refractive index layers, with thicknesses of 200-600 angstroms, 50-250 angstroms, 50-250 angstroms and 600-1100 angstroms respectively; the light transmittance of the outer permeability-enhancing film layer and the inner permeability-enhancing film layer in the visible light spectrum region wavelength range of 380-720nm is greater than 99%; The light blocking layer includes a first light blocking layer and a second light blocking layer. Specifically, the first light blocking layer is located between the outer surface of the substrate and the first outer transmittance increasing film layer, the outer surface of the first outer transmittance increasing film layer is connected to the second light blocking layer, and the outer surface of the second light blocking layer is connected to the second outer transmittance increasing film layer and / or the protective layer.
2. The corrective lens according to claim 1, characterized in that: The light blocking layer extends 6-7 mm from the outer edge of the substrate toward the central area.
3. The corrective lens according to claim 1, characterized in that: The content of nickel in the light blocking layer is 1-5wt%, the content of titanium is 5-10wt%, and the content of niobium oxide is 85-94wt%.
4. The corrective lens according to claim 1, characterized in that: The thickness of the first light blocking layer and the second light blocking layer are 2000-3000 angstroms and 3000-5000 angstroms respectively; the thickness of the protective layer is 300-500 angstroms.
5. The corrective lens according to claim 4, characterized in that: The transmittance of the first light blocking layer and the second light blocking layer in the visible light spectrum region is less than 1%.
6. The method for preparing the corrective lens according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1, cleaning the substrate and drying it to obtain a clean substrate; S2. Place the clean substrate on the fixture, send it into the vacuum coating chamber and evacuate it. When the vacuum degree in the vacuum chamber reaches 3*10 -5 When the vacuum degree in the vacuum chamber reaches 1.5*10 -5 When the temperature in the vacuum chamber is below 50-70°C, the evaporation rate is controlled at An electron gun is used to bombard the materials of the light blocking layer, the outer transmittance increasing film layer and the inner transmittance increasing film layer in sequence to form the inner transmittance increasing film layer on the inner surface of the substrate and the light blocking layer and the outer transmittance increasing film layer on the outer surface.
7. The preparation method according to claim 6, characterized in that: A protective layer may also be evaporated on the outermost side of the corrective lens.
8. The preparation method according to claim 7, characterized in that: Maintain the vacuum degree in the vacuum chamber at 1.5*10 -5 Torr, the temperature in the vacuum chamber is controlled at 50-70°C and the evaporation rate is controlled at The waterproof material is heated by group evaporation, and after evaporation, the waterproof material is deposited on the outer surface of the light blocking layer in the form of molecular crystals to form a protective layer.