A viscosity-reducing polycarboxylic acid water-reducing agent and a preparation method thereof
By optimizing the molecular structure of polycarboxylic acid water reducing agent, the problem of high viscosity of high strength concrete is solved, and the viscosity and fluidity of concrete are efficiently reduced, construction costs are reduced, and it is suitable for high-grade concrete.
Patent Information
- Application Number
- CN202110738955.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-06-30
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-06-30
AI Technical Summary
The method of reducing the viscosity of high-strength concrete in the prior art has limited effect, and increasing the amount of water reducing agent will lead to an increase in construction costs and cannot fully meet the needs of construction construction.
By designing and optimizing the molecular structure of polycarboxylic acid water reducer, allyl polyoxyethylene ether and methyl allyl polyoxyethylene ether with specific molecular weight and hydroxyl value are used as polyether monomers to combine unsaturated carboxylic acid and its The dehydration products and amide compounds form polycarboxylic acid water reducing agents with viscosity reduction functions, improving the flowability and dispersion effect of concrete.
It has achieved efficient reduction of concrete viscosity, increased flow rate, reduced construction difficulties and pumping problems, reduced water reducing agent usage, and is low in cost, suitable for high-grade concrete.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of CO4 B 24, and in particular to a viscosity-reducing polycarboxylic acid water-reducing agent and a preparation method thereof. Background Art
[0002] In recent years, with the continuous development of my country's construction industry and the growing strength of the high-speed rail industry, ordinary low-grade concrete can no longer meet the requirements of construction. New concrete with good durability and high strength is gaining more and more attention for its excellent characteristics. In order to make the concrete reach high-strength or ultra-high-strength grades and meet the strength requirements of construction, it is necessary to increase the amount of cementitious materials in the concrete mix or reduce the water-cement ratio of the concrete. However, while improving the strength of concrete, the viscosity and shrinkage of the concrete also increase greatly, the flow rate of the concrete slows down, making mixing and transportation difficult, the concrete pumping performance decreases, and the construction efficiency is seriously affected. In order to ensure the effective construction of high-strength concrete, it is particularly important to study methods that can reduce the viscosity of concrete.
[0003] The existing methods for reducing the viscosity of high-strength concrete mainly include (1) increasing the amount of water-reducing agent, (2) increasing the amount of external admixtures in cementitious materials, and (3) optimizing the particle size distribution of aggregates. Among them, the method of reducing the viscosity of concrete by increasing the amount of water-reducing agent can achieve the purpose of reducing viscosity to a certain extent, but the effect is not obvious when the amount of water-reducing agent reaches a certain value, and it may even cause serious bleeding of concrete and make it impossible to construct normally. On the other hand, increasing the amount of water-reducing agent will also greatly increase the cost of concrete construction. Researchers have recorded many methods of reducing the viscosity of concrete by increasing the amount of external admixtures in cementitious materials and optimizing the particle size distribution of aggregates. However, due to the large differences and various types of materials on the construction site, this method has great limitations and cannot completely achieve the purpose of reducing the viscosity of concrete.
[0004] In view of the strong designability of the molecular structure of polycarboxylic acid water-reducing agent, there are many records in the literature on the use of water-reducing agent to reduce the viscosity of concrete, but there is a lack of systematic and targeted research, and the product effect is not obvious. At present, there are no good viscosity-reducing water-reducing agent products in the domestic market. The products with more significant viscosity-reducing effects in the foreign market include the RHEOPLUS series products of BASF of Germany, but the product dosage is large and the price is expensive. The use of it will greatly increase the cost of concrete construction, limiting its application. Under such circumstances, the research and development of a viscosity-reducing polycarboxylic acid high-performance water-reducing agent with high water reduction rate, good viscosity-reducing effect, simple synthesis process, good working performance, environmental friendliness and low price is of great significance to the development of the construction industry. Summary of the invention
[0005] The present invention provides a viscosity-reducing polycarboxylic acid water-reducing agent, thereby solving the problems of limited water-reducing and plasticizing effects of water-reducing agents on concrete, large addition amount and high cost in the prior art, and realizing a viscosity-reducing polycarboxylic acid high-performance water-reducing agent with high water-reducing rate, good viscosity-reducing effect, simple synthesis process, good working performance, environmental friendliness and low price.
[0006] The first aspect of the present invention provides a viscosity reducing polycarboxylic acid water reducer, wherein the raw materials thereof include, by weight, 50-200 parts of a polyether monomer, 12-76 parts of an unsaturated carboxylic acid and its dehydration product, 0-28 parts of an amide compound, 0.1-6 parts of an initiator and 48-150 parts of a solvent.
[0007] In some preferred embodiments, the raw materials include, by weight, 75-156 parts of polyether monomers, 22-46 parts of unsaturated carboxylic acids and their dehydration products, 4-20 parts of amide compounds, 1-3 parts of initiators and 70-120 parts of solvents.
[0008] In some preferred embodiments, the polyether monomer includes one or more combinations of allyl polyoxyethylene ether, methyl allyl polyoxyethylene ether, polyethylene glycol monomethyl ether, and isopentanol polyoxyethylene ether.
[0009] Preferably, the polyether monomer comprises allyl polyoxyethylene ether and methyl allyl polyoxyethylene ether, and the weight ratio of allyl polyoxyethylene ether to methyl allyl polyoxyethylene ether is (1.5-4):1.
[0010] Preferably, the average molecular weight of the polyether monomer is 200-5000, and the hydroxyl value is 15-200 mg / g.
[0011] More preferably, the average molecular weight of the allyl polyoxyethylene ether is 400-3000, and the hydroxyl value is 25-150 mg / g.
[0012] More preferably, the allyl polyoxyethylene ether has a model of APEG 700 and a hydroxyl value of 80 mg / g; it is purchased from Hai'an Petrochemical Plant in Jiangsu Province.
[0013] More preferably, the average molecular weight of the methyl allyl polyoxyethylene ether is 600-2400, and the hydroxyl value is 22-72 mg / g.
[0014] More preferably, the model of the methyl allyl polyoxyethylene ether is TPEG-800B, and the hydroxyl value is 66 mg / g; it is purchased from Wuhan Xinxin Jiali Biotechnology Co., Ltd.
[0015] Compared with other types of water reducers, polycarboxylic acid water reducers have excellent characteristics such as high water reduction rate, strong anti-slump effect, and strong weather resistance. In current research, the practical value and theoretical significance of new polycarboxylic acid water reducers have been increasingly valued, but based on the complexity of the water reducer structure and the particularity of the application occasions, as well as the cost perspective and technical limitations, the existing domestically developed polycarboxylic acid water reducers are still far from practical application. The present invention realizes the high performance of polycarboxylic acid water reducers by controlling the main chain polymerization degree, side chain length and functional group type of the product through the optimized combination of different functional structural units, and prepares a polycarboxylic acid water reducer with viscosity reduction function, so as to achieve the purpose of reducing concrete viscosity and accelerating concrete flow rate. Through a large number of experimental studies, it was found that the use of allyl polyoxyethylene ether and methyl allyl polyoxyethylene ether with specific molecular weight and hydroxyl value as polyether monomers can enhance the dispersing effect of polycarboxylic acid water reducer on cement. The branched polyether macromolecules polymerize with small molecular unsaturated carboxylic acids to form unique carboxylic acid ether polymer macromolecules, which act on the surface of inorganic particles in concrete to form an adsorption protective layer, generate appropriate spatial repulsion, and prevent the condensation and agglomeration of tiny concrete particles. At the same time, the amphiphilic protective layer effectively isolates the penetration of water vapor into the concrete particles, inhibits the generation of bound water, reduces the flow resistance of cement paste, and achieves a viscosity reduction effect.
[0016] In some preferred embodiments, the unsaturated carboxylic acid and its dehydration product include a combination of one or more of acrylic acid, sodium allyl sulfonate, methyl acrylate, hydroxyethyl acrylate, and maleic anhydride.
[0017] More preferably, the unsaturated carboxylic acid and its dehydration product are acrylic acid, sodium allyl sulfonate and maleic anhydride; the weight ratio of acrylic acid, sodium allyl sulfonate and maleic anhydride is (1.6-3):1:(0.7-2).
[0018] The difference in the main chain and side chain structure in the water reducer has an important influence on the steric hindrance effect and electrostatic repulsion in the process of concrete and water combination. In some preferred embodiments, the unsaturated carboxylic acid and its dehydration product are acrylic acid, sodium allyl sulfonate and maleic anhydride, and the weight ratio of acrylic acid, sodium allyl sulfonate and maleic anhydride is (1.6-3): 1: (0.7-2). The present invention has found through experimental exploration that when the above-mentioned small molecule monomer is polymerized with a polyether of a specific molecular weight and hydroxyl value, the obtained polycarboxylic acid water reducer can maintain appropriate fluidity, exert a stable intrinsic dispersing force and retention effect in the dispersed molecules, and can maintain a small slump for a long time when acting on concrete, the three-dimensional dispersibility is enhanced, the collision and adsorption of solid particles in the liquid phase are weakened, the workability of concrete during mixing is enhanced, and a lasting and stable suspension state is formed under the action of the double-layer adsorption film, further improving the water reduction rate.
[0019] In some preferred embodiments, the amide compound is a combination of one or more of acrylamide, 2-acrylamido-2-methylpropanesulfonic acid, and N-isopropylacrylamide.
[0020] More preferably, the amide compound is acrylamide and N-isopropylacrylamide; the weight ratio of acrylamide to N-isopropylacrylamide is (2-3):1.
[0021] The polycarboxylic acid-based water reducer formed by the polymerization of polyether macromonomers and unsaturated carboxylic acid small monomers can significantly reduce the water reduction rate of premixed concrete while reducing the dosage. From the perspective of actual production application, in some preferred embodiments, amide compounds are added to the water reducer, especially acrylamide and N-isopropylacrylamide, and active groups such as carboxyl and amide groups form an amphiphilic structure, which not only improves the dispersion stability of the water reducer, but also further improves the binding and adsorption effect of inorganic particles and polycarboxylic acid molecules; at the same time, the water reducer with amide compounds can promote the precipitation of metal silicates and hydrated crystal products, improve the early strength and long-lasting shape retention ability of concrete, and improve the two-way adaptability of water reducers and concrete, so that water reducers are suitable for concrete of various specifications (especially high grades).
[0022] In some preferred embodiments, the initiator includes at least one of persulfate, benzoyl peroxide, and azobisisobutyronitrile.
[0023] Examples of persulfates include, but are not limited to, ammonium persulfate, potassium persulfate, and sodium persulfate.
[0024] In some preferred embodiments, the weight ratio of the polyether monomer, the unsaturated carboxylic acid and its dehydration product and the amide compound is (8-17): (2.5-5): (0.5-1).
[0025] In order to improve the lubricating and penetrating effect of the polycarboxylic acid water reducer, in some preferred embodiments, the weight ratio of the polyether monomer, the unsaturated carboxylic acid and its dehydration product and the amide compound is (8-17): (2.5-5): (0.5-1). Under this condition, the hydrophilic polar groups in the water reducer are directionally adsorbed on the surface of the inorganic particles, and form a large number of hydrogen bonds with water molecules, while entraining a proper amount of microbubbles to form a lubricating film between the concrete particles, thereby achieving excellent water reduction, plasticization and lubrication effects with a small amount of water reducer. The concrete processed by the water reducer of the present invention has a uniform and stable internal structure, reduced porosity, can maintain high strength and high durability, improved impermeability and freeze-thaw resistance, and significantly slowed carbonization rate.
[0026] The second aspect of the present invention provides a method for preparing a viscosity-reducing polycarboxylate water-reducing agent, and the specific preparation steps include:
[0027] S1. Add the polyether monomer and 2 / 3 of the solvent into the reactor, stir and heat to 70-86°C, add 1 / 2 of the initiator, and react for 1-4h to obtain product A;
[0028] S2. Cooling to 40-50°C, adding unsaturated carboxylic acid and its dehydration product, amide compound and remaining initiator to product A, reacting for 1-3h after addition to obtain product B;
[0029] S3. Cool down to 20-35°C, adjust the pH of product B to 5-7, add the remaining solvent, stir evenly, cool and discharge the material to obtain the finished product.
[0030] Beneficial effects:
[0031] The present invention polymerizes specific polyether and carboxylic acid compounds, and cooperates with amide compounds and other substances to design a polycarboxylic acid water reducer with unique functional structural units. The polycarboxylic acid water reducer has a significant viscosity reduction function and can achieve the polycarboxylic acid water reducer; at the same time, the present invention has the effects of high water reduction rate, small dosage, and lasting plasticity. When the viscosity-reducing water reducer of the present invention is added during concrete mixing, it can effectively solve the construction problems of high-strength concrete that is difficult to pump and easy to block pipes. The present invention is of great significance for promoting the development of building materials. At the same time, the present invention provides a test method for cement paste, which can accurately measure the viscosity of concrete, and has positive significance for the definition and unification of industry standards. DETAILED DESCRIPTION
[0032] Example 1.
[0033] The present embodiment provides a viscosity-reducing polycarboxylic acid water-reducing agent, and its raw materials include, by weight, 120 parts of polyether monomers, 30 parts of unsaturated carboxylic acids and dehydration products thereof, 8 parts of amide compounds, 1.6 parts of initiators and 90 parts of solvents.
[0034] The polyether monomers are allyl polyoxyethylene ether and methyl allyl polyoxyethylene ether, and the weight ratio of allyl polyoxyethylene ether to methyl allyl polyoxyethylene ether is 3:1.
[0035] The model of the allyl polyoxyethylene ether is APEG 700, and the hydroxyl value is 80 mg / g; it was purchased from Haian Petrochemical Plant in Jiangsu Province.
[0036] The model of the methyl allyl polyoxyethylene ether is TPEG-800B, and the hydroxyl value is 66 mg / g; it was purchased from Wuhan Xinxin Jiali Biotechnology Co., Ltd.
[0037] The unsaturated carboxylic acid and its dehydration product are acrylic acid (CAS No.: 79-10-7), sodium allyl sulfonate (CAS No.: 2495-39-8) and maleic anhydride (CAS No.: 108-31-6); the weight ratio of acrylic acid, sodium allyl sulfonate and maleic anhydride is 2.5:1:1.2; the maleic anhydride is prepared into a maleic anhydride aqueous solution with a mass fraction of 10% before use.
[0038] The amide compounds are acrylamide (CAS No.: 79-06-1) and N-isopropylacrylamide (CAS No.: 2210-25-5); the weight ratio of acrylamide to N-isopropylacrylamide is 2.4:1.
[0039] The initiator is ammonium persulfate and the solvent is water.
[0040] The specific preparation steps of the viscosity-reducing polycarboxylate water-reducing agent include:
[0041] S1. Add the polyether monomer and 2 / 3 of the solvent into the reactor, stir and heat to 84°C, add 1 / 2 of the initiator, and react for 2h to obtain product A;
[0042] S2. Cool down to 45°C, add unsaturated carboxylic acid and its dehydration product, amide compound and remaining initiator to product A, and react for 3h to obtain product B;
[0043] S3. Cool to 32°C, add 20 wt% sodium hydroxide aqueous solution to adjust the pH of product B to 6.5±0.5, add the remaining solvent, stir evenly, cool and discharge to obtain the finished product.
[0044] Example 2.
[0045] The present embodiment provides a viscosity-reducing polycarboxylic acid water-reducing agent, and its raw materials include, by weight, 96 parts of polyether monomers, 24 parts of unsaturated carboxylic acids and their dehydration products, 6 parts of amide compounds, 1 part of initiator and 72 parts of solvents.
[0046] The polyether monomers are allyl polyoxyethylene ether and methyl allyl polyoxyethylene ether, and the weight ratio of allyl polyoxyethylene ether to methyl allyl polyoxyethylene ether is 3:1.
[0047] The model of the allyl polyoxyethylene ether is APEG 700, and the hydroxyl value is 80 mg / g; it was purchased from Haian Petrochemical Plant in Jiangsu Province.
[0048] The model of the methyl allyl polyoxyethylene ether is TPEG-800B, and the hydroxyl value is 66 mg / g; it was purchased from Wuhan Xinxin Jiali Biotechnology Co., Ltd.
[0049] The unsaturated carboxylic acid and its dehydration product are acrylic acid (CAS No.: 79-10-7), sodium allyl sulfonate (CAS No.: 2495-39-8) and maleic anhydride (CAS No.: 108-31-6); the weight ratio of acrylic acid, sodium allyl sulfonate and maleic anhydride is 2.5:1:1.2; the maleic anhydride is prepared into a maleic anhydride aqueous solution with a mass fraction of 10% before use.
[0050] The amide compounds are acrylamide (CAS No.: 79-06-1) and N-isopropylacrylamide (CAS No.: 2210-25-5); the weight ratio of acrylamide to N-isopropylacrylamide is 2.4:1.
[0051] The initiator is ammonium persulfate and the solvent is water.
[0052] The specific preparation steps of the viscosity-reducing polycarboxylate water-reducing agent include:
[0053] S1. Add the polyether monomer and 2 / 3 of the solvent into the reactor, stir and heat to 84°C, add 1 / 2 of the initiator, and react for 2h to obtain product A;
[0054] S2. Cool down to 45°C, add unsaturated carboxylic acid and its dehydration product, amide compound and remaining initiator to product A, and react for 3h to obtain product B;
[0055] S3. Cool to 32°C, add 20 wt% sodium hydroxide aqueous solution to adjust the pH of product B to 6.5±0.5, add the remaining solvent, stir evenly, cool and discharge to obtain the finished product.
[0056] Example 3.
[0057] The present embodiment provides a viscosity-reducing polycarboxylic acid water-reducing agent, and its raw materials include, by weight, 96 parts of polyether monomers, 30 parts of unsaturated carboxylic acids and their dehydration products, 8 parts of amide compounds, 1.6 parts of initiators and 90 parts of solvents.
[0058] The polyether monomers are allyl polyoxyethylene ether and methyl allyl polyoxyethylene ether, and the weight ratio of allyl polyoxyethylene ether to methyl allyl polyoxyethylene ether is 3:1.
[0059] The model of the allyl polyoxyethylene ether is APEG 700, and the hydroxyl value is 80 mg / g; it was purchased from Haian Petrochemical Plant in Jiangsu Province.
[0060] The model of the methyl allyl polyoxyethylene ether is TPEG-800B, and the hydroxyl value is 66 mg / g; it was purchased from Wuhan Xinxin Jiali Biotechnology Co., Ltd.
[0061] The unsaturated carboxylic acid and its dehydration product are acrylic acid (CAS No.: 79-10-7), sodium allyl sulfonate (CAS No.: 2495-39-8) and maleic anhydride (CAS No.: 108-31-6); the weight ratio of acrylic acid, sodium allyl sulfonate and maleic anhydride is 2:1:1.5; the maleic anhydride is prepared into a maleic anhydride aqueous solution with a mass fraction of 10% before use.
[0062] The amide compounds are acrylamide (CAS No.: 79-06-1) and N-isopropylacrylamide (CAS No.: 2210-25-5); the weight ratio of acrylamide to N-isopropylacrylamide is 2.4:1.
[0063] The initiator is ammonium persulfate and the solvent is water.
[0064] The specific preparation steps of the viscosity-reducing polycarboxylate water-reducing agent include:
[0065] S1. Add the polyether monomer and 2 / 3 of the solvent into the reactor, stir and heat to 84°C, add 1 / 2 of the initiator, and react for 2h to obtain product A;
[0066] S2. Cool down to 45°C, add unsaturated carboxylic acid and its dehydration product, amide compound and remaining initiator to product A, and react for 3h to obtain product B;
[0067] S3. Cool to 32°C, add 20 wt% sodium hydroxide aqueous solution to adjust the pH of product B to 6.5±0.5, add the remaining solvent, stir evenly, cool and discharge to obtain the finished product.
[0068] Example 4.
[0069] The present embodiment provides a viscosity-reducing polycarboxylic acid water-reducing agent, and its raw materials include, by weight, 96 parts of polyether monomers, 30 parts of unsaturated carboxylic acids and their dehydration products, 8 parts of amide compounds, 1.6 parts of initiators and 90 parts of solvents.
[0070] The polyether monomers are allyl polyoxyethylene ether and methyl allyl polyoxyethylene ether, and the weight ratio of allyl polyoxyethylene ether to methyl allyl polyoxyethylene ether is 3:1.
[0071] The model of the allyl polyoxyethylene ether is APEG 700, and the hydroxyl value is 80 mg / g; it was purchased from Haian Petrochemical Plant in Jiangsu Province.
[0072] The model of the methyl allyl polyoxyethylene ether is TPEG-800B, and the hydroxyl value is 66 mg / g; it was purchased from Wuhan Xinxin Jiali Biotechnology Co., Ltd.
[0073] The unsaturated carboxylic acid and its dehydration product are acrylic acid (CAS No.: 79-10-7), sodium allyl sulfonate (CAS No.: 2495-39-8) and maleic anhydride (CAS No.: 108-31-6); the weight ratio of acrylic acid, sodium allyl sulfonate and maleic anhydride is 2.5:1:1.2; the maleic anhydride is prepared into a maleic anhydride aqueous solution with a mass fraction of 10% before use.
[0074] The amide compound is 2-acrylamide-2-methylpropanesulfonic acid (CAS No.: 15214-89-8) and N-isopropylacrylamide (CAS No.: 2210-25-5); the weight ratio of 2-acrylamide-2-methylpropanesulfonic acid to N-isopropylacrylamide is 2:1.
[0075] The initiator is ammonium persulfate and the solvent is water.
[0076] The specific preparation steps of the viscosity-reducing polycarboxylate water-reducing agent include:
[0077] S1. Add the polyether monomer and 2 / 3 of the solvent into the reactor, stir and heat to 84°C, add 1 / 2 of the initiator, and react for 2h to obtain product A;
[0078] S2. Cool down to 45°C, add unsaturated carboxylic acid and its dehydration product, amide compound and remaining initiator to product A, and react for 3h to obtain product B;
[0079] S3. Cool to 32°C, add 20 wt% sodium hydroxide aqueous solution to adjust the pH of product B to 6.5±0.5, add the remaining solvent, stir evenly, cool and discharge to obtain the finished product.
[0080] Comparative Example 1.
[0081] This embodiment provides a viscosity-reducing polycarboxylic acid water-reducing agent, and the specific implementation method is the same as that of Example 1; the difference is that, in parts by weight, its raw materials include 80 parts of polyether monomers, 60 parts of unsaturated carboxylic acids and their dehydration products, 5 parts of amide compounds, 1 part of initiator and 100 parts of solvent.
[0082] Comparative Example 2.
[0083] This embodiment provides a viscosity-reducing polycarboxylic acid water-reducing agent, and the specific implementation manner is the same as that of Embodiment 1; the difference is that the polyether monomer is allyl polyoxyethylene ether.
[0084] Comparative Example 3.
[0085] This embodiment provides a viscosity-reducing polycarboxylic acid water-reducing agent, and the specific implementation method is the same as that of Example 1; the difference is that the model of the methyl allyl polyoxyethylene ether is TPEG-2600B, the average molecular weight is 2600, and the hydroxyl value is 20 mg / g; it is purchased from Wuhan Xinxin Jiali Biotechnology Co., Ltd.
[0086] Comparative Example 4.
[0087] This embodiment provides a viscosity-reducing polycarboxylic acid water-reducing agent, and the specific implementation manner is the same as that of Embodiment 1; the difference is that the weight ratio of acrylic acid, sodium allyl sulfonate and maleic anhydride is 1:1:3.
[0088] Comparative Example 5.
[0089] This embodiment provides a viscosity-reducing polycarboxylic acid water-reducing agent, and the specific implementation method is the same as that of Embodiment 1; the difference is that no amide compound is added.
[0090] Performance Testing Methods
[0091] The viscosity-reducing polycarboxylic acid water-reducing agents prepared in Examples 1-4 and Comparative Examples 1-5 were mixed with C30 concrete to obtain a sample to be tested; the amount of the water-reducing agent was 0.4% of the mass of the C30 concrete.
[0092] Water reduction rate:
[0093] Refer to GB 8076 to test the water reduction rate of the sample to be tested.
[0094] Slump:
[0095] Refer to GB 8076 to test the initial slump T1 and the slump T2 after 2 hours of testing. Cement paste fluidity:
[0096] A mixture of cement and water (cement to water weight ratio of 3.5:1) and the viscosity reducing polycarboxylic acid water reducer prepared in Examples 1-4 and Comparative Examples 1-5 are mixed to obtain a mixture, and the water reducer dosage is 0.4%. The mixture is transferred to a mixer and stirred for 5 minutes. The stirred cement paste is quickly injected into a truncated cone mold, the cement paste on the upper surface of the truncated cone mold is flattened, and the truncated cone mold is lifted vertically. The maximum diameter of the flowing part of the cement paste is recorded to characterize the fluidity d of the cement paste. The test temperature is 22°C; the higher the fluidity of the cement paste, the better the viscosity reducing effect of the water reducer. After 60 minutes, the same steps are repeated to calculate the loss rate of fluidity. Each group of samples is measured 10 times in parallel, and the relative standard deviation RSD of the loss rate is calculated; the RSD results of Examples 1-4 are all less than 4%, and the above cement paste fluidity detection method is accurate and effective.
[0097] The cement is specifically Dalian Huari Xiaoyetian brand 42.5 cement.
[0098] The specifications of the truncated cone circular mold are: upper diameter 36mm, lower diameter 60mm, and height 60mm.
[0099] Performance test data
[0100] Table 1. Performance test results
[0101] Water reduction rate / % T1 / mm T2 / mm d / mm Example 1 37.6 234 216 283 Example 2 32.4 209 188 254 Example 3 34.1 218 200 266 Example 4 32.7 210 192 272 Comparative Example 1 26.8 184 162 236 Comparative Example 2 28.6 193 175 245 Comparative Example 3 27.5 188 160 241 Comparative Example 4 30.4 199 171 258 Comparative Example 5 27.1 195 168 253
Claims
1. A viscosity reducing polycarboxylate water reducer, characterized in that: The raw materials include, by weight, 75-156 parts of polyether monomer, 22-46 parts of unsaturated carboxylic acid and its dehydration product, 4-20 parts of amide compound, 1-3 parts of initiator and 70-120 parts of solvent; The polyether monomer comprises allyl polyoxyethylene ether and methyl allyl polyoxyethylene ether, and the weight ratio of allyl polyoxyethylene ether to methyl allyl polyoxyethylene ether is (1.5-4):1; The average molecular weight of the allyl polyoxyethylene ether is 400-3000, and the hydroxyl value is 25-150 mg / g; The average molecular weight of the methyl allyl polyoxyethylene ether is 600-2400, and the hydroxyl value is 22-72 mg / g; The unsaturated carboxylic acid and its dehydration product are acrylic acid, sodium allyl sulfonate and maleic anhydride, and the weight ratio of acrylic acid, sodium allyl sulfonate and maleic anhydride is (1.6-3):1:(0.7-2); The amide compound is acrylamide and N-isopropylacrylamide; the weight ratio of acrylamide to N-isopropylacrylamide is (2-3):1; The weight ratio of the polyether monomer, the unsaturated carboxylic acid and its dehydration product and the amide compound is (8-17): (2.5-5): (0.5-1).
2. A method for preparing the viscosity-reducing polycarboxylate water-reducing agent according to claim 1, characterized in that: The preparation method of the viscosity-reducing polycarboxylate water-reducing agent comprises: S1. Add the polyether monomer and 2 / 3 of the solvent to the reactor, stir and heat to 70-86°C, add 1 / 2 of the initiator, and react for 1-4h to obtain product A; S2. Cooling to 40-50°C, adding unsaturated carboxylic acid and its dehydration product, amide compound and remaining initiator to product A, reacting for 1-3h to obtain product B; S3. Cool down to 20-35°C, adjust the pH of product B to 5-7, add the remaining solvent, stir evenly, cool and discharge the material to obtain the finished product.