A method for regenerating waste lithium-ion battery positive electrode material
By soaking and roasting the waste positive electrode material in the alkali liquid in the recycling of lithium-ion batteries, combining boron source and F elements, the problems of high energy consumption and complex operation of the lithium-ion battery recycling process in the prior art are solved, and high efficiency is achieved. Recycled positive electrode material with excellent performance.
Patent Information
- Application Number
- CN202210391522.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-14
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-04-14
AI Technical Summary
In the existing lithium-ion battery recycling technology, the energy consumption of the pyrometallurgy process is high and harmful gas emissions are high, while the hydrometallurgy process is long and difficult to operate, and there is a lack of a short process and efficient regeneration method.
The used lithium-ion battery positive electrode sheet is soaked, filtered and dried in alkali liquid and added to a boron source for grinding and calcining. It is resintered through two calcining processes, and the residual lithium and introduced F element are used to combine with B element to form a stable Recycled materials.
The regeneration process without lithium supplementation is achieved, and quasi-single crystal particles with smooth surface and uniform size are obtained, which improves the assembly performance of the regenerated positive electrode material, simplifies the process and reduces energy consumption.
Smart Images

Figure CN114927786B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of processing of waste lithium-ion batteries, and in particular relates to a method for regenerating positive electrode materials of waste lithium-ion batteries. Background Art
[0002] Lithium-ion batteries are widely used due to their excellent performance, such as high operating voltage, high energy density, no memory effect, light weight, small size, low self-discharge rate, long cycle life, and wide operating temperature range. Due to the comprehensive advantages of lithium-ion batteries in performance and price, they have become a kind of energy storage device widely used in consumer electronics and electric vehicles. The world's LIB production reached 2.05 billion in 2005 and 5.86 billion in 2012. China's lithium-ion battery production was 4.18 billion in 2012 and increased to 7.84 billion in 2016. With the sharp increase in the demand for lithium-ion batteries, it is of great significance to recycle and reuse waste lithium-ion batteries.
[0003] So far, many recycling technologies based on pyrometallurgical or hydrometallurgical processes have been developed. SONY, OnTo, Accurec and other companies have commercialized and developed pyrometallurgical processes. Pyrometallurgical processes are often combined with hydrometallurgical processes to recover valuable metals. For example, the Val Eas process adopted by Umicore first smelts waste lithium in a furnace to obtain Co Ni Cu Fe alloy, and then uses hydrometallurgical processes to recover Co, Ni and Cu from the alloy. In the pyrometallurgical process, acetylene black, organic electrolyte and binder contained in the waste liquid are often burned, which consumes high energy and emits harmful gases. In addition, lithium and aluminum are active metals with strong reducing properties. During the smelting process, lithium and aluminum are easily oxidized and enter the smelting slag in the form of oxides. In contrast, the hydrometallurgical process has the advantages of high metal recovery rate, high product purity, low energy consumption and low gas emissions, but it also has disadvantages such as long process and difficult operation.
[0004] Therefore, in view of the recycling technology problems of the above-mentioned pyrometallurgical or hydrometallurgical processes, it is particularly important to develop a short-process and efficient regeneration method for waste lithium-ion battery positive electrode materials. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the deficiencies and defects mentioned in the above background technology and provide a method for regenerating waste lithium-ion batteries.
[0006] In order to solve the above technical problems, the technical solution proposed by the present invention is:
[0007] A method for regenerating anode materials of waste lithium-ion batteries comprises the following steps:
[0008] (1)Discharge, disassemble the waste lithium-ion battery, and then soak the disassembled positive electrode sheet in an alkaline solution, filter to obtain black powder;
[0009] (2)Wash and dry the black powder obtained in step (1), then add a boron source to the dried black powder, grind, and calcine to complete the regeneration of the waste lithium-ion battery positive electrode material.
[0010] In the above method for regenerating the positive electrode material of a waste lithium-ion battery, preferably, the waste lithium-ion battery has the chemical formula LiNi x Co y Mn z O2, 0.3 ≤ x < 1, 0 < y ≤ 0.3, 0 < z ≤ 0.3, and the electrolyte of the waste lithium-ion battery contains HF. During the long cycle of the lithium-ion battery, HF in the electrolyte infiltrates into the ternary material, and during the recycling of waste lithium batteries, the F element enters the material as a doping element.
[0011] In the above method for regenerating the positive electrode material of a waste lithium-ion battery, preferably, in step (2), the boron source is any one of boron oxide, boron trichloride, and boric hydroxide, and the addition amount of the boron source accounts for 0.1% - 3% of the molar amount of the lithium-ion battery positive electrode material body in terms of molar percentage.
[0012] In the above method for regenerating the positive electrode material of a waste lithium-ion battery, preferably, in step (2), the rotation speed of grinding is 200 - 500 rpm, and the grinding time is 10 - 30 min.
[0013] In the above method for regenerating the positive electrode material of a waste lithium-ion battery, preferably, in step (2), the calcination is carried out in an oxygen-rich atmosphere.
[0014] In the above method for regenerating the positive electrode material of a waste lithium-ion battery, preferably, in step (2), the calcination is carried out in two stages. The temperature of the first-stage calcination is 500 - 550 °C, and the calcination time is 5 - 15 h. The temperature of the second-stage calcination is 600 - 850 °C, and the calcination time is 5 - 50 h.
[0015] In the above method for regenerating the positive electrode material of a waste lithium-ion battery, preferably, in step (1), the discharge means soaking the waste lithium-ion battery in a sodium chloride solution with a mass concentration of 0.2 - 15% for 10 - 72 h.
[0016] In the above method for regenerating the positive electrode material of a waste lithium-ion battery, preferably, in step (1), the alkaline solution is one or more of sodium hydroxide solution, ammonia water, and potassium hydroxide solution, or a mixed solution composed of calcium hydroxide solution and sodium hydroxide solution, ammonia water, or potassium hydroxide solution; the concentration of the alkaline solution is 1 - 3 mol / L, and the pH is 12 - 14.
[0017] In the above-mentioned method for regenerating positive electrode materials of waste lithium-ion batteries, preferably, in step (1), the positive electrode sheet is immersed in the alkaline solution for 1 to 24 hours.
[0018] In the above-mentioned method for regenerating the positive electrode material of waste lithium-ion batteries, preferably, in step (2), the chemical formula of the regenerated waste lithium-ion battery is LiNi x Co y Mn z B a F b O2, where x, y, z, a, b, c are mole numbers, 0.3≤x<1, 0 <y≤0.3,0<z≤0.3,x+y+z=1,0.001≤a≤0.03,0<b≤0.1。
[0019] Compared with the prior art, the advantages of the present invention are:
[0020] (1) The method for regenerating waste lithium-ion battery positive electrode materials of the present invention is simple, and there is no need to recover the metal elements in the ternary positive electrode materials or to perform lithium replenishment operations. Boron sources can be directly added to the waste lithium-ion positive electrode materials and re-sintered.
[0021] (2) The present invention makes full use of the residual lithium on the surface of the positive electrode material during the regeneration and sintering process of the waste lithium-ion battery positive electrode material, so that it does not need to be replenished with lithium, and utilizes the F element introduced during the battery cycle, combined with the added B element, to ensure that B and F are doped in the lattice of the material. The B element heals the cracks in the waste ternary material, and the F element doping stabilizes the skeleton of the material and accelerates the transmission of lithium ions, so that the obtained regenerated particles are typical quasi-single crystal particles with a smooth surface without cracks, uniform size, and a particle size of 3 to 5 μm. The full battery assembled with the regenerated positive electrode material has excellent performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 is a SEM image of the regenerated positive electrode material in Example 1 of the present invention;
[0023] Figure 2 is a SEM image of the positive electrode material of the waste lithium-ion battery in Example 1 of the present invention;
[0024] Figure 3 1 is an electrochemical diagram of a full battery prepared by regenerating positive electrode materials of Example 1 of the present invention and Comparative Example 1;
[0025] Figure 4 is a SEM image of the regenerated positive electrode material in Example 2 of the present invention;
[0026] Figure 5 is a SEM image of the regenerated positive electrode material in Example 3 of the present invention;
[0027] Figure 6 It is a SEM picture of the regenerated positive electrode material in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0028] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the specification, but the protection scope of the present invention is not limited to the following specific embodiments.
[0029] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0030] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0031] Embodiment 1:
[0032] A method for regenerating anode materials of waste lithium-ion batteries comprises the following steps:
[0033] (1) The positive electrode material is LiNi 0.83 Co 0.11 Mn 0.06 The waste ternary lithium-ion battery of O2 (the electrolyte of the battery contains HF) was immersed in a sodium chloride solution with a concentration of 0.5% for 36 hours for discharge, and then disassembled to obtain the positive electrode sheet;
[0034] (2) The positive electrode sheet obtained by disassembling step (1) was immersed in a mixed solution of NaOH and NH3·H2O with a total molar amount of 3 mol / L for 12 h to completely dissolve the aluminum foil, and the pH of the system was controlled to 12.5 with liquid alkali. The powder was filtered to obtain a black powder (electron microscopy image as shown in FIG. Figure 2 As shown, the particles are broken single crystal particles with a rough surface and cracks, and the particle size is 3 to 5 μm);
[0035] (3) Weigh 10 g (about 0.1 mol) of black powder, then add 0.007 g (0000.1 mol) of B2O3 to the black powder and grind at 400 rpm for 30 min;
[0036] (4) The ground black powder was calcined in two stages in an oxygen-rich atmosphere: first, the temperature was raised to 500°C for 10 h, and then the temperature was raised to 820°C for 16 h to obtain the regenerated positive electrode material LiNi 0.83 Co 0.11 Mn 0.06 B 0.002 F 0.001O2.
[0037] The SEM image of the regenerated positive electrode material in this embodiment is as follows Figure 1 As shown by Figure 1 It can be seen that the regenerated ternary positive electrode material particles are typical quasi-single crystal particles with a smooth surface without cracks, uniform size, and a particle size of 3 to 5 μm.
[0038] The regenerated positive electrode material LiNi 0.83 Co 0.11 Mn 0.06 B 0.002 F 0.001 O2 was assembled into a full battery and tested at 25°C in the voltage range of 2.75 to 4.6 V. The results are shown in Figure 3 As shown, at a rate of 0.1C, the first discharge capacity is 212.3 mAh / g, at a rate of 1C, the first discharge capacity is 200.6 mAh / g, after 200 cycles at 1C, the capacity is 178.35 mAh / g, and the capacity retention rate is 88.9%.
[0039] Embodiment 2:
[0040] A method for regenerating anode materials of waste lithium-ion batteries comprises the following steps:
[0041] (1) The positive electrode material is LiNi 0.88 Co 0.06 Mn 0.06 The waste ternary lithium-ion battery of O2 (the electrolyte of the battery contains HF) is placed in a sodium chloride solution with a mass concentration of 0.8% and is immersed and discharged for 35 hours, and then disassembled to obtain the positive electrode sheet;
[0042] (2) Soak the positive electrode sheet in a mixed solution of NaOH and NH3·H2O with a total molar amount of 3 mol / L for 11 hours, control the pH of the system to 12.8 with liquid alkali, and filter after the aluminum foil is completely dissolved to obtain a black powder;
[0043] (3) Weigh 10 g (about 0.1 mol) of black powder, add 0.014 g (0000.2 mol) of B2O3 to the black powder, and grind at 400 rpm for 30 min;
[0044] (4) The ground black powder was calcined in two stages under an oxygen-rich atmosphere: first, the temperature was raised to 520°C and calcined at this temperature for 11 h, and then the temperature was raised to 830°C and calcined for 17 h to obtain the regenerated positive electrode material LiNi 0.88 Co 0.06 Mn 0.06 B 0.004 F 0.002 O2.
[0045] The SEM image of the regenerated positive electrode material obtained in this example is as follows Figure 4 As shown, the particles of the positive electrode material are typical quasi-single crystal particles with a smooth surface without cracks, uniform size, and a particle size of 3 to 5 μm.
[0046] The regenerated positive electrode material obtained in this embodiment was assembled into a full battery and tested at 25°C in the voltage range of 2.75 to 4.6 V. At a rate of 0.1C, the first discharge capacity reached 216.3 mAh / g, and at a rate of 1C, the first discharge capacity reached 205.6 mAh / g. After 200 cycles at 1C, the capacity was 178 mAh / g, and the capacity retention rate reached 86.58%.
[0047] Embodiment 3:
[0048] A method for regenerating anode materials of waste lithium-ion batteries comprises the following steps:
[0049] (1) The positive electrode material is LiNi 0.8 Co 0.1 Mn 0.1 The waste ternary lithium-ion battery of O2 (the electrolyte of the battery contains HF) was placed in a sodium chloride solution with a mass concentration of 0.9% and discharged for 34 hours, and the positive electrode sheet was disassembled;
[0050] (2) Soak the positive electrode sheet in a mixed solution of NaOH and NH3·H2O with a total molar amount of 3 mol / L for 10 h, control the pH of the system to 12.7, and filter after the aluminum foil is completely dissolved to obtain a black powder;
[0051] (3) Weigh 10 g (about 0.1 mol) of black powder, add 0.007 g (0000.1 mol) of B2O3 to the black powder, and grind at 400 rpm for 30 min;
[0052] (4) The ground black powder was calcined in two stages in an oxygen-rich atmosphere: first, the temperature was raised to 550°C and calcined for 10 h, and then the temperature was raised to 840°C and calcined at this temperature for 16 h to obtain the regenerated positive electrode material LiNi 0.8 Co 0.1 Mn 0.1 B 0.002 F 0.003 O2.
[0053] The SEM image of the regenerated ternary cathode material obtained in this example is as follows Figure 5 As shown, the particles are typical quasi-single crystal particles with a smooth surface without cracks, uniform size, and a particle size of 3 to 5 μm.
[0054] The regenerated ternary positive electrode material obtained in this embodiment was assembled into a full battery and tested at 25°C in the voltage range of 2.75 to 4.6 V. At a rate of 0.1C, the first discharge capacity reached 208.4.3 mAh / g, and at a rate of 1C, the first discharge capacity reached 198.3 mAh / g. After 200 cycles at 1C, the capacity was 169.09 mAh / g, and the capacity retention rate reached 85.1%.
[0055] Comparative Example 1
[0056] The method for regenerating the positive electrode material of waste lithium-ion batteries in this comparative example comprises the following steps:
[0057] (1) The positive electrode material is LiNi 0.83 Co 0.11 Mn 0.06 The waste ternary lithium-ion battery of O2 (the electrolyte of the battery contains HF) was placed in a sodium chloride solution with a concentration of 0.5% and discharged for 36 hours, and the positive electrode sheet was disassembled;
[0058] (2) Soak the positive electrode sheet in a mixed solution of NaOH and NH3·H2O with a total molar weight of 3 mol / L for 12 h, and use liquid alkali to control the pH of the system to 12.5. After the aluminum foil is completely dissolved, filter to obtain a black powder;
[0059] (3) Weigh 10 g (about 0.1 mol) of black powder and grind it at a speed of 400 rpm for 30 min. The ground black powder is calcined in two stages in an oxygen-rich atmosphere: first, the temperature is raised to 500 ° C and calcined for 10 h, and then the temperature is raised to 820 ° C and calcined for 16 h to obtain the regenerated positive electrode material LiNi 0.83 Co 0.11 Mn 0.06 F 0.001 O2.
[0060] The SEM image of the regenerated positive electrode material obtained in this comparative example is as follows Figure 6 As shown, the particles are broken single crystal particles with a rough surface and cracks, and the particle size is 3 to 5 μm.
[0061] The regenerated positive electrode material of this comparative example was assembled into a full battery and tested at 25°C in the voltage range of 2.75 to 4.6 V. Figure 3 It shows that at a rate of 0.1C, the first discharge capacity is 130.4 mAh / g, at a rate of 1C, the first discharge capacity is 115.3 mAh / g, after 200 cycles at 1C, the capacity is 48.43 mAh / g, and the capacity retention rate is only 42%.
Claims
1. A method for regenerating anode materials of waste lithium-ion batteries, characterized in that: The following steps are involved: (1) Discharge and disassemble the waste lithium-ion battery, and then soak the disassembled positive electrode sheet in an alkaline solution, filter to obtain a black powder; the chemical formula of the waste lithium-ion battery positive electrode material is LiNi x Co y Mn z O2, 0.3 ≤ x < 1, 0 < y ≤ 0.3, 0 < z ≤ 0.3, and the electrolyte of the waste lithium-ion battery contains HF; (2) Washing and drying the black powder obtained in step (1), then adding a boron source to the dried black powder, grinding it, and roasting it to complete the regeneration of the waste lithium-ion battery positive electrode material. The chemical formula of the regenerated lithium-ion battery positive electrode material is LiNi x Co y Mn z B a F b O2, where x, y, z, a, b, c are mole numbers, 0.3≤x<1, 0 <y≤0.3,0<z≤0.3,x+y+z=1,0.001≤a≤0.03,0<b≤0.1。 2. The method for regenerating the positive electrode material of waste lithium-ion batteries according to claim 1, characterized in that: In step (2), the boron source is any one of boron oxide, boron trichloride and boron hydroxide.
3. The method for regenerating the positive electrode material of waste lithium-ion batteries according to claim 1, characterized in that: In step (2), the grinding speed is 200-500 rpm and the grinding time is 10-30 min.
4. The method for regenerating the positive electrode material of waste lithium-ion batteries according to claim 1, characterized in that: In step (2), the calcination is carried out in an oxygen-rich atmosphere.
5. The method for regenerating the positive electrode material of waste lithium-ion batteries according to claim 1, characterized in that: In step (2), the calcination is carried out in two stages. The temperature of the first stage is 500-550°C and the calcination time is 5-15 hours. The temperature of the second stage is 600-850°C and the calcination time is 5-50 hours.
6. The method for regenerating the positive electrode material of waste lithium-ion batteries according to claim 1, characterized in that: In step (1), the discharge refers to soaking the waste lithium-ion battery in a sodium chloride solution with a mass concentration of 0.2-15% for 10-72 hours.
7. The method for regenerating the positive electrode material of waste lithium-ion batteries according to claim 1, characterized in that: In step (1), the alkali solution is one or more of sodium hydroxide solution, ammonia water, and potassium hydroxide solution, or a mixed solution of calcium hydroxide solution and sodium hydroxide solution, ammonia water or potassium hydroxide solution; the concentration of the alkali solution is 1-3 mol / L, and the pH is 12-14.
8. The method for regenerating the positive electrode material of waste lithium-ion batteries according to claim 1, characterized in that: In step (1), the positive electrode sheet is immersed in the alkaline solution for 1 to 24 hours.