Fibrillated regenerated cellulose fiber and fabric made of the same
By controlling the degree of polymerization of regenerated cellulose fibers and modifying them in an acid solution, combined with friction/rubbing treatment in a wet state, the problem of original fiber shedding during water washing of regenerated cellulose fibers was solved, thus maintaining the characteristic surface feel and hand feel of the fibers.
Patent Information
- Application Number
- CN202080091831.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-01-14
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-01-14
AI Technical Summary
In existing technologies, regenerated cellulose fibers lose their original fibers during water washing, resulting in damage to the surface and feel, and making it difficult to maintain the fibrillation effect.
By controlling the degree of polymerization of regenerated cellulose fibers to 100–250 and subjecting them to a modification treatment in an acid solution at 110–150°C for 10–30 minutes, combined with a rubbing/kneading treatment in a moist state, a fibril aggregate of cellulose microfibrils is formed.
It achieves the re-emergence of the original fibers during the water washing process, maintaining the characteristic surface texture, softness, and elasticity, and improving the wash resistance of cellulose fibers.
Smart Images

Figure CN114929962B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a high-quality fibrillated regenerated cellulose fiber having a characteristic surface feel, softness and a resilient feel, which is fibrillated by rubbing / kneading the cloth in a wet state and has excellent durability of the surface feel and feel after washing with water, and a fabric containing the fiber as a constituent thread. Background Art
[0002] Regenerated cellulose fibers include cuprammonium rayon, organic solvent-processed cellulose fibers, etc. All cellulose fibers have the following characteristics: they are formed of a fibril aggregate mainly composed of cellulose microfibrils, and when rubbed / kneaded in a wet state, the fibers are split in the fiber axis direction and fibrillated.
[0003] Clothing products made of regenerated cellulose fibers have characteristic surface feel, softness, and a resilient feel, so there are many products that utilize these characteristics to fibrillate the regenerated cellulose fibers constituting the clothing products. However, when the fibrillated clothing products are repeatedly washed with water, the fibers fall off, which impairs the surface feel and the feel. In addition, although there are prior art documents on fibrillation of regenerated cellulose fibers, there are no prior art documents that provide a specific solution to this problem.
[0004] For example, as a fibrillation processing method, the following patent document 1 discloses a method using a fluffing treatment and an impact during dyeing with a liquid jet dyeing machine. However, the amount of fibrils produced cannot be constant depending on dyeing conditions such as dyeing time, bath ratio, cloth speed, and the concentration of the alkali used, so there is a disadvantage that the same quality of products cannot be repeatedly provided. In addition, the polymerization degree of regenerated cellulose fibers is specified to be 400 or more, and there is no discussion on the shedding of fibrils due to water washing.
[0005] The following Patent Document 2 discloses fibrillation using an alkaline aqueous solution. However, the polymerization degree of the regenerated cellulose fiber is specified to be 300 or more, and since the treatment method is a treatment in an alkaline aqueous solution, the regenerated cellulose fiber is structurally easy to fibrillate only in an alkaline aqueous solution, and is therefore difficult to fibrillate in weakly alkaline water washing, and the shedding of fibrils caused by water washing is not mentioned.
[0006] The following Patent Document 3 does not describe the polymerization degree of regenerated cellulose fibers, but discloses a method using an acid aqueous solution or an oxidant aqueous solution. The conditions of the treatment method described in Patent Document 3 are compared with the conditions disclosed in this specification. In order to suppress the reduction in strength, the fiber is treated for a long time in a high-concentration acid solution at a high temperature under normal pressure, but there is no description of the strength reduction rate caused by this treatment method. Furthermore, there is a description that the strength is reduced if the treatment is performed under high pressure, which is completely inconsistent with the processing conditions disclosed in this specification.
[0007] In the following Patent Document 4, although there is no description of the polymerization degree of the regenerated cellulose fiber, a method using an acid aqueous solution is disclosed. In Patent Document 4, a treatment using an acid aqueous solution for 30 to 80 minutes for the purpose of reducing strength and a high-speed tumbling treatment in a dry state are described in order to remove long fibrils. However, the fabric containing Lyocell disclosed in Patent Document 4 removes the long fibrils that provide the "hairy effect" as the characteristic surface feeling disclosed in this specification to the fabric surface, and the short fibrils existing on the fabric surface are different from the fibrillated regenerated cellulose fibers disclosed in this specification because Patent Document 4 describes a "clean" surface finishing characterized by substantially no "hairy effect". In addition, Patent Document 4 does not describe the strength reduction rate of the fabric caused by the aforementioned treatment method for removing long fibrils, and further, does not mention the shedding of fibrils caused by water washing.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Laid-Open No. 08-113846
[0011] Patent Document 2: Japanese Patent Application Laid-Open No. 06-166956
[0012] Patent Document 3: Japanese Patent Application Laid-Open No. 11-315474
[0013] Patent Document 4: UK Patent No. 2399094A Summary of the invention
[0014] Problem that the invention aims to solve
[0015] In view of the above prior art, the object of the present invention is to provide a high-quality fibrillated regenerated cellulose fiber having a characteristic surface feel, softness and a resilient feel, which is fibrillated by friction / kneading in a wet state and has excellent persistence of surface feel and feel after washing with water, and a cloth made using the fiber.
[0016] Solutions for solving problems
[0017] The present inventors conducted in-depth research to solve the above-mentioned problems, and found that, compared with modification in a way that the appeared fibrils do not fall off, modification in a way that the fibrils will reappear during washing even if they fall off is effective. Based on the above-mentioned discovery, in-depth research and repeated experiments were conducted on the method of modifying the fiber in a way that the fibrils will reappear during washing even if they fall off. As a result, it was unexpectedly found that if the degree of polymerization of the regenerated cellulose fiber is controlled to 100 to 250, the fibrils will easily appear only by the weak rubbing effect of washing, and the hand feel shows a light, soft and resilient feel, thereby completing the present invention.
[0018] That is, the present invention is as follows.
[0019] [1] A surface-fibrillated regenerated cellulose fiber having a degree of polymerization of 100 to 250 and a tensile strength when dried exceeding 1.0 cN / dtex and not more than 3.0 cN / dtex.
[0020] [2] The regenerated cellulose fiber according to [1], wherein the regenerated cellulose fiber is an organic solvent-grown cellulose fiber.
[0021] [3] A fabric comprising the regenerated cellulose fiber according to [1] or [2] as a constituent fiber.
[0022] [4] A method for producing the regenerated cellulose fiber described in [1] or [2] or the fabric described in [3], comprising the step of modifying the regenerated cellulose fiber in the form of a thread or a fabric in an acid solution at a temperature of 110°C to 150°C for 10 minutes to 30 minutes and a pH of 2.6 to 3.4.
[0023] Effects of the Invention
[0024] The fibrillated regenerated cellulose fiber of the present invention has a characteristic surface feel, softness and a resilient feel, and is a high-quality fiber that is fibrillated by rubbing / kneading the cloth in a wet state and has excellent durability of the surface feel and feel after washing. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1This is a photograph showing the surface of a woven fabric in a fibrillated state of regenerated cellulose fibers constituting the yarn.
[0026] Figure 2 This is a photograph showing an enlarged state of fibrillation of regenerated cellulose fibers. DETAILED DESCRIPTION
[0027] Hereinafter, embodiments of the present invention will be described in detail.
[0028] One embodiment of the present invention is a surface fibrillated regenerated cellulose fiber having a degree of polymerization of 100 to 250 and a tensile strength when dried exceeding 1.0 cN / dtex and not more than 3.0 cN / dtex.
[0029] The regenerated cellulose fiber refers to a regenerated cellulose fiber obtained by dissolving and spinning a cellulose raw material, such as cuprammonium rayon and organic solvent-based cellulose fiber, and cuprammonium rayon and organic solvent-based cellulose fiber are preferred, and organic solvent-based cellulose fiber is more preferred.
[0030] The yarn form of the regenerated cellulose fiber can be any of short fibers and long fibers, preferably multifilaments of long fibers. There is no particular restriction on the single fiber fineness, and it can be preferably 0.5 to 5.0 dtex. There is no particular restriction on the total fineness, and it is preferably 22 to 330 dtex. There is no particular restriction on the count, but it is preferably 5 to 100 cotton counts. There is no particular restriction on the cross-sectional shape of the single fiber. There is no particular restriction on the twist, and it can be untwisted, false twisted, or twisted. There is no particular restriction on the number of twists, and it can be preferably an additional twist of less than 2000 times. From the perspective of feel, it is preferably untwisted.
[0031] Since this embodiment is not affected by other raw materials, there is no particular limitation on compounding with other raw materials. However, as a processing method, high pressure treatment is performed, so acrylic acid, diacetate, and wool are not preferred as compounding objects, i.e., other raw materials, because they are likely to cause strength reduction, hardening of the feel, and devitrification.
[0032] There is no particular restriction on the ratio of the regenerated cellulose fiber used in the fabrics including woven fabrics and nonwoven fabrics, but in order to exert the desired effect well, it is preferably 10% by weight or more of the total weight of the fabric, more preferably 20% by weight or more, and further preferably 30% by weight or more. If the ratio is less than 10% by weight, although fibrillation is found, it is difficult to obtain softness and rebound feeling. In addition, as a composite method of the silk, it can be any one of twisting, interlacing, taslan, covering, cotton blending, drawing, and worsted twisting.
[0033] The degree of polymerization of the fibrillated regenerated cellulose fiber of the present embodiment is 100 to 250, preferably 150 to 250, and more preferably 200 to 250. If the degree of polymerization is less than 100, the tensile strength at break when dried is less than 1.0 cN / dtex, and the necessary silk properties for post-processing until forming a cloth and use as a clothing product cannot be achieved. On the other hand, if the degree of polymerization is higher than 250, the reappearance of the original fibers achieved by washing with water cannot be obtained, so it is not preferred. The degree of polymerization refers to the value obtained by measuring the viscosity method using a cuprammonia solution.
[0034] The fabric can be any one of woven fabric, warp knitted fabric, circular knitted fabric, horizontal knitted fabric, and nonwoven fabric, preferably woven fabric, warp knitted fabric, circular knitted fabric, horizontal knitted fabric, and more preferably woven fabric and circular knitted fabric. There is no particular restriction on the organization and density of the fabric. As a composite method when composited with other raw materials, it can be any one of interweaving, cross knitting, using composite yarn, and inserting weft yarn in warp knitting.
[0035] In the present embodiment, there is no particular restriction on the method of modifying the degree of polymerization of the fibrillated regenerated cellulose fibers to 100 to 250. However, by treating the regenerated cellulose fibers having a degree of polymerization of 250 or more and a tensile strength of 2.0 cN / dtex or more when dried in an acid solution, the degree of polymerization is adjusted to 100 to 250, and the tensile strength when dried is adjusted to more than 1.0 cN / dtex and less than 3.0 cN / dtex. The modification is excellent in terms of easy adjustment of the fiber properties and the degree of polymerization, and is therefore particularly preferably used. There is no particular restriction on the type of acid used, and it can be any one of citric acid, malic acid, acetic acid, formic acid, sulfuric acid, nitric acid, hydrochloric acid, oxalic acid, etc., preferably an acid with low corrosiveness to metals, more preferably formic acid, citric acid, and malic acid. For the treatment temperature, in order to modify to the target degree of polymerization and the target tensile strength, it is preferably 110°C to 150°C, more preferably 120°C to 150°C, and further preferably 130°C to 140°C. When it is lower than 110°C, a long treatment time is required for the modification, and even if the modification reaches the target degree of polymerization and tensile strength, the modification will be significantly reduced, so it is not preferred. In addition, when the treatment is carried out for a short time at a temperature lower than 110°C, the pH needs to be lowered. When the treatment is carried out for a short time at a low pH, a local decrease in the degree of polymerization and a decrease in strength will occur, making it difficult to modify uniformly. In addition, a deviation in the quality of each modification treatment will occur, so it is not preferred. On the other hand, when it is above 150°C, it is difficult to manage the temperature and difficult to modify uniformly, so it is not preferred. The treatment pH and treatment time need to be adjusted according to the regenerated cellulose fiber used. The treatment pH is preferably 2.6 to 3.4, more preferably 2.8 to 3.2, and the treatment time is preferably 10 minutes to 30 minutes, more preferably 12 minutes to 28 minutes, and further preferably 15 minutes to 25 minutes. For example, when formic acid is used to treat regenerated cellulose fibers with a polymerization degree of about 450 to 600 and a tensile strength of 2.0 cN / dtex or more when dried, the polymerization degree can be modified to 100 to 250 and the tensile strength when dried can be maintained at more than 1.0 cN / dtex and less than 3.0 cN / dtex in an acid bath with a 76% formic acid concentration of 1.0 g / L and a pH of 2.8 at 130°C for 20 minutes. In order to reduce the polymerization degree to the target polymerization degree in a short time and to modify the tensile strength when dried to more than 1.0 cN / dtex and less than 3.0 cN / dtex, it is necessary to use a low concentration of acid for a short time modification treatment, and for this purpose, a high temperature and high pressure treatment of more than 110°C is required.
[0036] The form of the modified treatment is not particularly limited, but preferably the form of a thread strip or a cloth, and more preferably the form of a cloth. The equipment used for the processing is not particularly limited in the form of a thread strip or a cloth, but preferably a package dyeing machine or a hank dyeing machine is used for the thread strip form, and preferably a liquid flow dyeing machine, an air flow dyeing machine, a beam dyeing machine, a jigger dyeing machine, a paddle dyeing machine, a drum dyeing machine, a washer dyeing machine, a capstan rope dyeing machine, and more preferably a liquid flow dyeing machine or an air flow dyeing machine is used for the cloth form.
[0037] In order to produce fibrils after the modification treatment, fibrillation treatment in water is required, so it is necessary to carry out fibrillation treatment simultaneously with the modification treatment, or to carry out fibrillation treatment after the modification treatment. As the form of fibrillation treatment, there is no particular restriction, but it is preferably a cloth form. There is no particular restriction on the equipment used during processing, but it is preferably a liquid flow dyeing machine, an air flow dyeing machine, a paddle dyeing machine, a drum dyeing machine, a washer dyeing machine, a capstan rope dyeing machine, and more preferably a liquid flow dyeing machine and an air flow dyeing machine. As the fibrillation treatment in water, there is no particular restriction, for example, it is preferably a fibrillation treatment in which the equipment is a liquid flow dyeing machine, an air flow dyeing machine or a capstan rope dyeing machine, the temperature is 10 to 130°C, the speed of the cloth is 100m / min or more, and the treatment time is more than 20 minutes, or the equipment is a paddle dyeing machine, a drum dyeing machine or a washer dyeing machine, the temperature is 10 to 130°C, and the treatment time is more than 20 minutes. In addition, after the fibrils appear, it is necessary that the fibrils will not be removed. Therefore, it is preferred that after the fibrils appear, no treatment for providing the feel in a dry state is performed, or when a treatment for providing the feel in a dry state is performed, the treatment for providing the feel is performed under the conditions of, for example, using an air flow dyeing machine or an air drum dryer as equipment, a fabric speed of less than 800 m / min, a treatment time of less than 60 minutes, or using an intermittent drum dryer as equipment, a treatment time of less than 60 minutes.
[0038] The tensile strength of the regenerated cellulose fiber of the present embodiment when dried exceeds 1.0 cN / dtex and is 3.0 cN / dtex or less, preferably 1.3 cN / dtex or more and 2.5 cN / dtex or less, and more preferably 1.5 cN / dtex or more and 2.0 cN / dtex or less. If the tensile strength when dried is 1.0 cN / dtex or less, it is damaged in various processes until the fabric is manufactured, making it difficult to obtain a practical fabric and impairing the sense of rebound, while if it exceeds 3.0 cN / dtex, the softness is impaired.
[0039] The term "fibrillated" in the fibrillated regenerated cellulose fiber of the present embodiment means a state in which a fibril aggregate mainly composed of cellulose microfibrils constituting the surface of the regenerated cellulose fiber is split in the fiber axis direction. Figure 1The photograph is a photo of the surface of a fabric showing a fibrillated state of regenerated cellulose fibers constituting the yarn. Reference numeral 1 indicates a state in which a fibril assembly mainly composed of cellulose microfibrils is split in the fiber axis direction (fibrillated state). Figure 2 In the photograph showing the enlarged state of the fibrillated regenerated cellulose fiber, reference numeral 2 denotes cellulose microfibril.
[0040] Example
[0041] The present invention will be described in detail below with reference to Examples, but the present invention is not limited to these Examples. It should be noted that various performance evaluations of each yarn or fabric in the Examples were performed by the following methods.
[0042] (1) Determination of degree of polymerization
[0043] The viscosity of the solution formed by dissolving cellulose fibers in a cuprammonia solution is based on the following formula:
[0044] ηsp / c=KmM
[0045] {where ηsp: specific viscosity, c: cellulose concentration (basic molecular mole / 100 ml), Km: constant (5×10 -4 The viscosity method is carried out by determining the viscosity by using the Standinger viscosity regulation shown in (a) and (b) where M is the molecular weight of cellulose.
[0046] Several cellulose fiber samples with different polymerization degrees are dissolved in a copper ammonia solution in a molecularly dispersed state, and their polymerization degrees are measured using a Nakano viscometer based on the above formula. Then, the viscosity of the cellulose samples when dissolved in a copper ammonia solution of a certain concentration is measured using a TAPPI viscometer, and the relationship between the viscosity and the polymerization degree is calculated in advance. The viscosity is actually measured using a TAPPI viscometer when the cellulose samples are dissolved in the above copper ammonia solution of a certain concentration, and the polymerization degree is calculated from the relationship table between the viscosity and the polymerization degree calculated in advance.
[0047] The method for measuring the viscosity using a TAPPI type viscosity tube is as follows. Place the sample in a constant temperature and humidity chamber at a temperature of 20°C and a humidity of 65% for more than 24 hours to balance the moisture content. Weigh and collect 0.1g of the sample. Add a wedge and a sample to the TAPPI type viscosity tube, then suck the copper ammonia solution (composition: ammonia: 205g / L, copper (I) hydroxide: 11.0g / L, sucrose: 10g / L) into the viscosity tube and cover it with a stopper. Install the viscosity tube on a rotating device and rotate it at a speed of 3RPM for 30 minutes to dissolve the sample. Remove the viscosity tube from the rotating device and immerse it in a constant temperature water bath at 20°C for 5 minutes. Remove the stopper at the bottom of the viscosity tube and insert the viscosity tube into the jacket installed in the constant temperature water bath. Open the valve of the stopper on the top of the viscosity tube and measure the time it takes for the solution to flow between the markings A and B on the viscometer. Use the following calculation formula:
[0048] V=d / C(tK / t)
[0049] {Wherein, V: absolute viscosity (cP), d: specific gravity of the solution (g / cm 3 ), C: TAPPI viscometer constant, t: flow time between the marking lines A and B (seconds), and K: TAPPI viscometer flow energy constant} to obtain the absolute viscosity (V). Next, the obtained absolute viscosity value is compared with the above-mentioned viscosity and polymerization degree relationship table to obtain the polymerization degree.
[0050] (2) Tensile strength test method when dry
[0051] The sample was placed in a constant temperature and humidity chamber at 20°C and 65% humidity for more than 24 hours to allow the moisture content to balance. The sample was stretched using a TENSILON universal material testing machine RTC series (manufactured by A&D Company, Limited) with a sample length (filament length) of 200 mm and a tensile speed of 200 mm / min to measure the strength at break.
[0052] (3) Washing test method
[0053] Implemented according to JIS L0217-103 method. Add 2g of detergent for dissolving clothes to 1L of water with a liquid temperature of 40℃, and use it as the washing liquid. Put the sample silk and load cloth into the washing liquid at a bath ratio of 1:30 and start operation. After washing for 5 minutes, dehydrate, then rinse with normal temperature water at the same bath ratio for 2 minutes and dehydrate, rinse with normal temperature water at the same bath ratio for 2 minutes and dehydrate again, and then end one washing. Drying method: Drum drying at 80℃ for 20 minutes.
[0054] (4) Fibrillation degree
[0055] The sample was mounted on a microscope VHX-6000 (manufactured by KEYENCE CORPORATION), and the lens VH-Z20 (manufactured by KEYENCE CORPORATION) was set at a magnification of 200 times. The sample was illuminated with light parallel to the fibrils to form white dots while adjusting the brightness and sensitivity conditions. The ratio of the area of the white dots to the photographed area was then calculated, and the degree of fibrillation was evaluated based on the following three-level evaluation criteria.
[0056] ○ (fibrillation): The area ratio of white spots is 10% or more
[0057] △ (Insufficient fibrillation): The area ratio of white spots is 5% or more and less than 10%
[0058] × (no fibrillation): The ratio of the area of white spots is less than 5%
[0059] (5) Change in fibrillation degree due to washing
[0060] The samples before and after washing were mounted on a microscope VHX-6000 (manufactured by KEYENCE CORPORATION), and the samples were photographed while adjusting the brightness and sensitivity conditions, while irradiating the sample with light that made the fibrils appear as white dots. Then, the ratio of the area of the white dots to the photographed area was calculated for the samples before and after washing, using the following calculation formula:
[0061] X=AW-BW
[0062] {Wherein, X: change in fibrillation degree due to washing (%), AW: ratio of the area of white spots in the sample after washing (%), and BW: ratio of the area of white spots in the sample before washing (%)} The rate of change in fibrillation degree is calculated, and the degree of change in fibrillation degree is evaluated based on the following 3-level evaluation criteria.
[0063] ○ (No change in fibrillation): Change is -10% or more and less than +10%
[0064] × (fibrillation changes): the change is less than -10% or more than +10%
[0065] (6) Feel
[0066] The sample before washing was evaluated for feel by a sensory test of feel by repeated grasping operation based on the following 3-level evaluation criteria, and the sample after washing was evaluated for the case where the evaluation result of the sample before washing was 0 or △:
[0067] ○: Excellent softness and rebound feeling
[0068] △: Slightly insufficient softness or rebound feeling
[0069] ×: Poor softness or rebound feeling
[0070] [Example 1]
[0071] Prepare copper ammonium rayon 84dtex / 45 filaments with a degree of polymerization of 580 and a tensile strength of 2.3cN / dtex when dried. The raw silk is subjected to a modification treatment at 130°C for 20 minutes using a bobbin dyeing machine using 76% formic acid at 1.0g / L, and the degree of polymerization is set to 200 to obtain modified copper ammonium rayon. The modified copper ammonium rayon obtained is used as the warp and weft to weave a 2 / 1 twill fabric with a warp density of 144 strands / 2.54cm and a weft density of 100 strands / 2.54cm. The obtained grey cloth is subjected to a scouring, relaxation and fibrillation treatment at 80°C for 20 minutes using a liquid flow dyeing machine with a nonionic surfactant of 1g / L, and then the copper ammonium rayon is dyed again using a liquid flow dyeing machine at a dyeing temperature of 60°C for 60 minutes, and then soaped at 80°C for 10 minutes. After dyeing and drying, the fabric was impregnated with an aqueous solution containing 1% by weight of a silicone softener, squeezed to 80% wet pick-up at a squeeze ratio of 80%, dried at 150°C for 1 minute, subjected to a treatment for providing a hand feel by passing through an air roller at 80°C for 30 minutes and a speed of 700 m / min, and finally set at 130°C for 1 minute to obtain a dyed fabric having a warp density of 153 yarns / 2.54 cm and a weft density of 104 yarns / 2.54 cm. The degree of polymerization of the cuprammonium rayon 84 dtex / 45 filaments of the warp yarns taken out from the fabric was 200.
[0072] [Example 2]
[0073] The warp and weft yarns were made of 84dtex / 45 filaments of copper ammonium rayon with a polymerization degree of 580 and a tensile strength of 2.3cN / dtex when dried, and a 2 / 1 twill fabric with a warp density of 144 yarns / 2.54cm and a weft density of 100 yarns / 2.54cm was woven. The resulting grey fabric was subjected to a modification treatment and fibrillation treatment at 130°C for 20 minutes using a liquid jet dyeing machine using 76% formic acid at 1.0g / L, and after the polymerization degree was set to 200, the copper ammonium rayon was dyed again at a dyeing temperature of 60°C for 60 minutes using a liquid jet dyeing machine, and then soaped at 80°C for 10 minutes. After dyeing and drying, the fabric was impregnated with an aqueous solution containing 1 wt% of a silicone softener, squeezed at a squeeze ratio of 80%, dried at 150°C for 1 minute, and subjected to a treatment for providing a hand feel by passing through an air roller at 80°C for 30 minutes at a speed of 700 m / min. The fabric was finally set at 130°C for 1 minute to obtain a dyed fabric having a warp density of 153 yarns / 2.54 cm and a weft density of 104 yarns / 2.54 cm. The degree of polymerization of the cuprammonium rayon 84 dtex / 45 filaments of the warp yarns taken out from the fabric was 200.
[0074] [Example 3]
[0075] Prepare 89dtex / 30 filaments of organic solvent-based cellulose fiber with a degree of polymerization of 490 and a tensile strength of 3.5cN / dtex when dried. The raw silk is subjected to a modification treatment at 130°C for 20 minutes using a bobbin dyeing machine using 76% formic acid at 1.0g / L, and the degree of polymerization is set to 220 to obtain modified organic solvent-based cellulose fiber. The obtained modified organic solvent-based cellulose fiber is used as the warp and weft to weave a plain fabric consisting of a warp density of 105 strands / 2.54cm and a weft density of 89 strands / 2.54cm. The obtained grey cloth is subjected to a scouring, relaxation and fibrillation treatment at 80°C for 20 minutes using a liquid flow dyeing machine with a nonionic surfactant of 1g / L, and then the organic solvent-based cellulose fiber is dyed again at a dyeing temperature of 60°C for 60 minutes using a liquid flow dyeing machine, and then soaped at 80°C for 10 minutes. After dyeing and drying, the fabric was impregnated with an aqueous solution containing 1% by weight of a silicone softener, squeezed at a squeeze ratio of 80%, dried at 150°C for 1 minute, and subjected to a treatment for providing a hand feel by passing through an air roller at 80°C for 30 minutes and a speed of 700 m / min. The fabric was finally set at 130°C for 1 minute to obtain a dyed fabric having a warp density of 109 strands / 2.54 cm and a weft density of 92 strands / 2.54 cm. The degree of polymerization of the organic solvent-processed cellulose fiber 89 dtex / 30 filaments of the warp yarn taken out from the fabric was 220.
[0076] [Example 4]
[0077] The warp and weft yarns were 89 dtex / 30 filaments of organic solvent-processed cellulose fibers with a polymerization degree of 490 and a tensile strength of 3.5 cN / dtex when dried, and a plain weave fabric consisting of a warp density of 105 yarns / 2.54 cm and a weft density of 89 yarns / 2.54 cm was woven. The resulting grey fabric was subjected to a modification treatment and fibrillation treatment at 130°C for 20 minutes using a liquid jet dyeing machine using 76% formic acid at 1.0 g / L, and after the polymerization degree was set to 220, the organic solvent-processed cellulose fibers were dyed again at a dyeing temperature of 60°C for 60 minutes using a liquid jet dyeing machine, and then soaped at 80°C for 10 minutes. After dyeing and drying, the fabric was impregnated with an aqueous solution containing 1% by weight of a silicone softener, squeezed at a squeeze ratio of 80%, dried at 150°C for 1 minute, and subjected to a treatment for providing a hand feel by passing through an air roller at 80°C for 30 minutes and a speed of 700 m / min. The fabric was finally set at 130°C for 1 minute to obtain a dyed fabric having a warp density of 109 strands / 2.54 cm and a weft density of 92 strands / 2.54 cm. The degree of polymerization of the organic solvent-processed cellulose fiber 89 dtex / 30 filaments of the warp yarn taken out from the fabric was 220.
[0078] [Comparative Example 1]
[0079] The warp and weft yarns were made of 84dtex / 45 copper ammonium rayon filaments with a polymerization degree of 580 and a tensile strength of 2.3 cN / dtex when dried, and a 2 / 1 twill fabric consisting of a warp density of 144 strands / 2.54 cm and a weft density of 100 strands / 2.54 cm was woven. The resulting grey cloth was not subjected to modification and fibrillation treatment, but dyeing and finishing were performed in the same manner as in Example 2 to obtain a dyed fabric with a warp density of 153 strands / 2.54 cm and a weft density of 104 strands / 2.54 cm. The polymerization degree of the 84dtex / 45 copper ammonium rayon filaments of the warp yarn taken out from the fabric was 580.
[0080] [Comparative Example 2]
[0081] The warp and weft yarns were 89 dtex / 30 cellulose fibers of organic solvent process with a polymerization degree of 490 and a tensile strength of 3.5 cN / dtex when dried, and a plain weave fabric consisting of a warp density of 109 yarns / 2.54 cm and a weft density of 92 yarns / 2.54 cm was woven. The obtained grey cloth was not subjected to modification and fibrillation treatment, but dyeing and finishing were performed in the same manner as in Example 4 to obtain a dyed fabric with a warp density of 109 yarns / 2.54 cm and a weft density of 92 yarns / 2.54 cm. The degree of polymerization of the 89 dtex / 30 cellulose fibers of organic solvent process taken out from the fabric was 490.
[0082] [Comparative Example 3]
[0083] The warp and weft yarns were made of 84dtex / 45 filaments of cuprammonium rayon with a polymerization degree of 580 and a tensile strength of 2.3cN / dtex when dried, and a 2 / 1 twill fabric with a warp density of 144 yarns / 2.54cm and a weft density of 100 yarns / 2.54cm was woven. The obtained grey fabric was subjected to fibrillation treatment at 80°C for 120 minutes using a liquid jet dyeing machine with 40g / L of sodium hydroxide, and then dyed with cuprammonium rayon at a dyeing temperature of 60°C for 60 minutes using a liquid jet dyeing machine, and then soaped at 80°C for 10 minutes. After dyeing and drying, the fabric was impregnated with an aqueous solution containing 1 wt% of a silicone softener, squeezed at a squeeze ratio of 80%, dried at 150°C for 1 minute, and subjected to a treatment for providing a hand feel by passing through an air roller at 80°C for 30 minutes and a speed of 700 m / min. The fabric was finally set at 130°C for 1 minute to obtain a dyed fabric having a warp density of 153 yarns / 2.54 cm and a weft density of 104 yarns / 2.54 cm. The degree of polymerization of the cuprammonium rayon 84 dtex / 45 filaments of the warp yarns taken out from the fabric was 440.
[0084] [Comparative Example 4]
[0085] The warp and weft yarns were made of 84dtex / 45 filaments of cuprammonium rayon with a polymerization degree of 580 and a tensile strength of 2.3cN / dtex when dried, and a 2 / 1 twill fabric with a warp density of 144 yarns / 2.54cm and a weft density of 100 yarns / 2.54cm was woven. The obtained grey fabric was subjected to fibrillation treatment at 100°C for 60 minutes with 50g / L of 75% phosphoric acid using a jet dyeing machine, and then dyed with cuprammonium rayon at a dyeing temperature of 60°C for 60 minutes using a jet dyeing machine, and then soaped at 80°C for 10 minutes. After dyeing and drying, the fabric was impregnated with an aqueous solution containing 1 wt% of a silicone softener, squeezed at a squeeze ratio of 80%, dried at 150°C for 1 minute, and subjected to a treatment for providing a hand feel by passing through an air roller at 80°C for 30 minutes at a speed of 700 m / min. The fabric was finally set at 130°C for 1 minute to obtain a dyed fabric having a warp density of 153 yarns / 2.54 cm and a weft density of 104 yarns / 2.54 cm. The degree of polymerization of the cuprammonium rayon 84 dtex / 45 filaments of the warp yarns taken out from the fabric was 400.
[0086] [Comparative Example 5]
[0087] The warp and weft yarns were made of 84 dtex / 45 filaments of cuprammonium rayon with a polymerization degree of 580 and a tensile strength of 2.3 cN / dtex when dried, and a 2 / 1 twill fabric with a warp density of 144 yarns / 2.54 cm and a weft density of 100 yarns / 2.54 cm was woven. The obtained grey fabric was subjected to fibrillation treatment at 100° C. for 60 minutes using a jet dyeing machine with 30 g / L of a 35% hydrogen peroxide aqueous solution, and then dyed with cuprammonium rayon at a dyeing temperature of 60° C. for 60 minutes using a jet dyeing machine, and then soaped at 80° C. for 10 minutes. After dyeing and drying, the fabric was impregnated with an aqueous solution containing 1 wt% of a silicone softener, squeezed at a squeeze ratio of 80%, dried at 150°C for 1 minute, and subjected to a treatment for providing a hand feel by passing through an air roller at 80°C for 30 minutes at a speed of 700 m / min. The fabric was finally set at 130°C for 1 minute to obtain a dyed fabric having a warp density of 153 yarns / 2.54 cm and a weft density of 104 yarns / 2.54 cm. The degree of polymerization of the cuprammonium rayon 84 dtex / 45 filaments of the warp yarns taken out from the fabric was 180.
[0088] [Comparative Example 6]
[0089] The warp and weft yarns were made of 84dtex / 45 filaments of cuprammonium rayon with a polymerization degree of 580 and a tensile strength of 2.3cN / dtex when dried, and a 2 / 1 twill fabric with a warp density of 144 yarns / 2.54cm and a weft density of 100 yarns / 2.54cm was woven. The obtained grey fabric was subjected to fibrillation treatment at 130°C for 45 minutes using an air flow dyeing machine with 6.4g / L acetic acid, and then dyed with cuprammonium rayon again at a dyeing temperature of 60°C for 360 minutes using an air flow dyeing machine, and then soaped at 80°C for 10 minutes. After dyeing and drying, the fabric was impregnated with an aqueous solution containing 1 wt% of a silicone softener, squeezed at a squeeze ratio of 80%, dried at 150°C for 1 minute, and subjected to a treatment to provide a feel by passing through an air roller at 100°C for 30 minutes and a speed of 900 m / min. The fabric was finally set at 130°C for 1 minute to obtain a dyed fabric having a warp density of 153 yarns / 2.54 cm and a weft density of 104 yarns / 2.54 cm. The degree of polymerization of the cuprammonium rayon 84 dtex / 45 filaments of the warp yarn taken out from the fabric was 190.
[0090] For the fabrics obtained in Examples 1 to 4 and Comparative Examples 1 to 6, the degree of fibrillation, the amount of change in the fibrillation degree due to washing, and the hand feeling were evaluated for the sample fabrics that were repeatedly washed 10 times using the aforementioned washing test method and the sample fabrics that were not washed. In addition, the copper ammonium rayon 84 dtex / 45 filaments and organic solvent-processed cellulose fiber 89 dtex / 30 filaments that were subjected to modification and fibrillation treatment were taken out from the fabric samples of Examples 1 to 4, and the copper ammonium rayon 84 dtex / 45 filaments and organic solvent-processed cellulose fiber 89 dtex / 30 filaments that were not subjected to modification or subjected to different fibrillation treatments were taken out from the fabric samples of Comparative Examples 1 to 6, and the tensile strength of the warp yarns when dried was measured. The raw materials, modification treatment, and fibrillation treatment of the sample yarns used in Examples 1 to 4 and Comparative Examples 1 to 6 are summarized in Table 1 below, and the evaluation results are shown in Table 2 below.
[0091] [Table 1]
[0092]
[0093] [Table 2]
[0094]
[0095] It can be seen that the fabrics using modified cellulose fibers of Examples 1 to 4 have no change in the original fiber feel due to washing, have a good hand feel of softness and a sense of resilience, and have a tensile strength exceeding 1.0 cN / dtex. That is, Examples 1 to 4 have a characteristic surface feel, softness, and a sense of resilience after washing, and are excellent in the durability of the surface feel and hand feel after washing.
[0096] In contrast, it can be seen that the tensile strength of the fabrics of Comparative Examples 1 to 6 is less than 1.0 cN / dtex, or the fibrils are removed before washing, or the degree of polymerization exceeds 250 and the fibrils fall off after washing, or the fibrillation degree changes. That is, for Comparative Examples 1 to 6, the surface feel and hand feel change greatly due to washing, or the strength as a fabric cannot be maintained, holes are formed due to wear during wearing or washing, or the fibrils are removed before washing, and therefore they are not suitable as fiber products with fibrils that require a good hand feel.
[0097] Industrial Applicability
[0098] The present invention can provide a high-quality regenerated cellulose fiber having a characteristic surface feel, softness, and a resilient feel, which can be easily fibrillated by friction / rubbing the cloth in a wet state, and has excellent persistence of surface feel and feel after water washing, and a fabric using the fiber, so the present invention has industrial applicability.
[0099] Description of Reference Numerals
[0100] 1. The state in which the fibril aggregate, which is mainly composed of cellulose microfibrils, is split in the fiber axis direction (fibrillated state)
[0101] 2 Cellulose microfibrils
Claims
1. A surface fibrillated regenerated cellulose fiber having a degree of polymerization of 100 to 250 and a tensile strength when dried exceeding 1.0 cN / dtex and not more than 3.0 cN / dtex.
2. The regenerated cellulose fiber according to claim 1, wherein The degree of polymerization is 150-250.
3. The regenerated cellulose fiber according to claim 1 or 2, wherein The degree of polymerization is 200-250.
4. The regenerated cellulose fiber according to claim 1, wherein The tensile strength during drying is 1.3 cN / dtex or more and 2.5 cN / dtex or less.
5. The regenerated cellulose fiber according to claim 1 or 4, wherein The tensile strength during drying is 1.5 cN / dtex or more and 2.0 cN / dtex or less.
6. The regenerated cellulose fiber according to claim 1, wherein The regenerated cellulose fiber is cuprammonium rayon and / or organic solvent-processed cellulose fiber.
7. The regenerated cellulose fiber according to claim 6, wherein The regenerated cellulose fiber is an organic solvent-processed cellulose fiber. 8 . A cloth comprising the regenerated cellulose fiber according to claim 1 as a constituent fiber.
9. The fabric according to claim 8, wherein The regenerated cellulose fiber accounts for more than 10% by weight of the total weight of the fabric.
10. The fabric according to claim 8, wherein The regenerated cellulose fiber accounts for more than 20% by weight of the total weight of the fabric.
11. The fabric according to claim 8, wherein The regenerated cellulose fiber accounts for more than 30% by weight of the total weight of the fabric.
12. A method for producing the regenerated cellulose fiber according to any one of claims 1 to 7 or the fabric according to any one of claims 8 to 11, comprising the step of modifying the regenerated cellulose fiber in the form of a thread or a fabric in an acid solution at a temperature of 110° C. to 150° C. for 10 minutes to 30 minutes and a pH of 2.6 to 3.
4.
13. The manufacturing method according to claim 12, wherein: The acid used in the acid solution is any one of formic acid, citric acid and malic acid.
14. The manufacturing method according to claim 12, wherein: The temperature is 120°C to 150°C.
15. The manufacturing method according to claim 12, wherein: The temperature is 130°C to 140°C.
16. The manufacturing method according to claim 12, wherein: The pH is 2.8 to 3.
2.
17. The manufacturing method according to claim 12, wherein: The time is 12 minutes to 28 minutes.
18. The manufacturing method according to claim 12, wherein: The time is 15 to 25 minutes.