Ammonia synthesis catalyst

By using composite oxides composed of Group II and Group I of specific properties to support metal particles such as cobalt to form high alkaline catalysts, the insufficient ammonia harvesting rate of ammonia synthesis catalysts in the prior art under low pressure conditions is solved. The problem is that efficient ammonia synthesis under mild conditions is achieved, reducing energy consumption.

CN115052838BActive Publication Date: 2024-11-12THE JAPAN SCI & TECH AGENCY
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202180010960.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-01-31
Filing Date
2021-01-29
Publication Date
2024-11-12
Estimated Expiration
2041-01-29

AI Technical Summary

Technical Problem

The existing ammonia synthesis catalysts have insufficient ammonia harvesting rate under low pressure conditions and need to be operated under high temperature and high pressure, resulting in high energy consumption. It is urgent to develop catalysts that can have high activity under mild conditions.

Method used

A composite oxide composed of Group II elements and Group I elements of specific properties is used as a support, and metal particles such as cobalt are supported by the stacking structure to form a high alkaline catalyst to improve ammonia synthesis activity.

Benefits of technology

A catalyst for efficient synthesis of ammonia under mild conditions is achieved, reducing energy consumption and improving ammonia synthesis activity, showing a higher ammonia harvest rate and lower operating temperature compared to conventional catalysts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115052838B_ABST
    Figure CN115052838B_ABST
Patent Text Reader

Abstract

The present invention provides a composite oxide formed of an oxide of a metal element L and an oxide of a metal element N, which is represented by the following general formula (1) and satisfies the following (a) to (d): n N 1-n (1) (a) the metal element L is (i) a Group I element, (ii) a Group II element, or (iii) a Group I element and a Group II element; (b) the metal element N is composed of Group I or Group II elements other than the metal element L; (c) n is 0.001 or more and 0.300 or less; (d) the oxide of the metal element L and the oxide of the metal element N do not form a solid solution, but the oxide particles of the metal element L are deposited on the surface of the oxide particles of the metal element N. In addition, the present invention provides a metal support in which at least one metal particle M selected from the group consisting of cobalt, iron, and nickel is supported on the composite oxide, and a catalyst for ammonia synthesis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a composite oxide that can be used to synthesize ammonia under mild conditions, a metal support and an ammonia synthesis catalyst using the composite oxide, and a method for producing the composite oxide, a method for producing the metal support, and a method for producing ammonia. Background Art

[0002] Ammonia is an important raw material in the modern chemical industry. More than 80% of the ammonia produced is used to make chemical fertilizers for crops. In addition, ammonia has also attracted attention as a carrier of energy and hydrogen. This is due to: (1) its high hydrogen content (17.6wt%), (2) its high energy density (12.8GJ / m 3 ), (3) No carbon dioxide is produced when decomposing to produce hydrogen. If ammonia can be efficiently produced from renewable energy sources such as solar and wind power, it will be possible to alleviate global issues related to energy and food crises.

[0003] The Haber-Bosch process, which is currently used to produce ammonia, consumes a large amount of energy, accounting for about 1-2% of the world's energy consumption. In this method, about 60% of the consumed energy is recovered, which can ensure the enthalpy of ammonia. However, most of the remaining energy is lost when producing hydrogen from natural gas, synthesizing ammonia, and separating gases. Since ammonia synthesis in the Haber-Bosch process is carried out at very high temperatures (>450°C) and pressures (>20MPa), it is urgent to reduce the large amount of energy used in this method. In order to suppress energy consumption on a global scale, a catalyst that can synthesize ammonia under milder conditions (lower temperature and pressure) than the iron-based catalyst used in the Haber-Bosch process is needed.

[0004] In recent years, a method for producing ammonia under low pressure conditions of about 1 MPa (10 atmospheres) has been known. The ruthenium catalyst used to produce ammonia is usually supported on a carrier. For example, Patent Document 1 discloses that if a rare earth oxide is used as a carrier for supporting ruthenium, the amount of ruthenium used can be reduced and the reaction temperature can be lowered. However, in the ammonia production method of Patent Document 1, when ammonia is produced under relatively low pressure conditions, the ammonia yield is insufficient. Therefore, the inventors have developed a method for reducing La reduced at 650°C. 0.5 Ce 0.5 O 1.75 A ruthenium catalyst used as a support was reported to exhibit excellent properties even under low pressure conditions (Non-Patent Document 4).

[0005] Furthermore, the present inventors have developed a binary composite oxide composed of two metal elements and a metal support (ammonia synthesis catalyst) in which a catalyst such as ruthenium is supported on the composite oxide (Patent Document 5, Patent Document 6). As an ammonia synthesis catalyst using a binary composite oxide (support) disclosed in this document, the following catalyst is disclosed.

[0006] Ru / Ce 0.85 La 0.15 O x _(500℃、600℃、650℃、700℃)reduction, Ru / Ce 0.67 La 0.33 O x _(500℃、600℃、650℃、700℃)reduction, Ru / Ce 0.33 La 0.67 O x _(500℃、600℃、650℃、700℃)reduction, Ru / Ce 0.15 La 0.85 O x _(500℃、600℃、650℃、700℃)reduction, Ru / Ce 0.5 La 0.5 O x _(500℃、650℃、800℃)reduction, Ru / Ce 0.5 Zr 0.5 O x _700℃ reduction, Ru / Ce 0.5 Pr 0.5 O x _(500℃、600℃、650℃、700℃、800℃)reduction, Ru / La 0.5 Pr 0.5 O x _(450℃, 500℃, 600℃, 650℃, 700℃) reduction, Ru / Ba 0.1 La 0.9 O x _(500℃, 700℃, 800℃, 900℃) reduction, Ru / Ba 0.1 Ce 0.9 O x _(500℃、700℃)reduction, Co / Ba 0.05 La 0.95 O x _(500℃、600℃、700℃、800℃)reduction, Co / Ba 0.01 La 0.99 O x _700℃ reduction, Co / Ba 0.03 La0.97 O x _700℃ reduction, Co / Ba 0.1 La 0.9 O x _Reduction at 700℃.

[0007] Furthermore, this document also describes 8.4wt%Ba / 4.5wt%Ru / MgO_(500°C, 700°C) reduction (Example 80, Example 81). These oxides are obtained by impregnating MgO as a carrier with a Ru solution and then firing it, and then using Ba(OH)2・8H2O to load Ba.

[0008] In addition to Patent Document 1 and Non-Patent Document 4, various patent documents disclose ammonia synthesis catalysts in which ruthenium is supported on various rare earth oxide supports. As representatives, Patent Documents 2 to 4 and Non-Patent Documents 1 to 3 can be cited. Patent Documents 2 and 4 disclose the selection of lanthanide oxides as supports, Patent Document 3 discloses the selection of praseodymium oxide as a support, and Non-Patent Document 1 discloses the selection of Ce oxide as a support. Non-Patent Document 2 discloses a Ru / CeO2-La2O3 catalyst manufactured by co-precipitating, drying, and activating hydroxides of Ru, Ce, and La.

[0009] In the prior art documents including Patent Documents 1, 2, 4 and Non-Patent Document 1, it is described that in the ruthenium catalyst used for synthesizing ammonia, Ru exists in the form of particles on the surface of its carrier. When it exists in the form of particles, there are reports that the average diameter is greater than 5nm (refer to Non-Patent Document 2), and there are reports that it is less than 2nm (Non-Patent Document 4). In addition, Patent Document 3 discloses that Ru has an eggshell structure.

[0010] On the other hand, regarding the carrier, non-patent document 3 discloses that when evaluating the ammonia synthesis activity of a Ru-loaded Y(La)-M-O (M is Ca, Sr, or Ba) catalyst, for the carrier oxide before loading Ru, it was found that when the sintering temperature of the carrier oxide was set to 450°C, the specific surface area of ​​the carrier oxide increased, and when the sintering temperature was increased to 650°C, the specific surface area of ​​the carrier decreased.

[0011] In addition, in view of the high price of Ru, a catalyst for ammonia synthesis in which a transition metal compound other than Ru is supported on a carrier, such as Co, has been proposed (for example, see Non-Patent Documents 5 and 6). However, although Non-Patent Document 6 discloses Co-BaO / C in which cobalt is supported on barium oxide, the ammonia synthesis activity is low. In addition, in Non-Patent Document 5, although calcium amide (Co / Ba-Ca(NH2)2) is used instead of oxide, the ammonia yield of the catalyst supported on Co at 1 MPa is not as good as that of the catalyst supported on Ru.

[0012] Prior art literature

[0013] Patent Literature

[0014] Patent Document 1: Japanese Patent Application Laid-Open No. 6-079177

[0015] Patent Document 2: Japanese Patent Application Publication No. 2013-111562

[0016] Patent Document 3: International Publication No. 2016 / 133213

[0017] Patent Document 4: Japanese Patent Application Publication No. 2017-018907

[0018] Patent Document 5: International Publication No. 2019 / 059190

[0019] Patent Document 6: International Publication No. 2019 / 216304

[0020] Non-patent literature

[0021] Non-patent literature 1: Y. Niwa and K. Aika, Chemistry Letters, (1996) 3-4

[0022] Non-patent document 2: X. Luo et al., Catalysis Letters 133, 382 (2009)

[0023] Non-patent document 3: AS Ivanova et al., Kinetics and Catalysis, Vol. 45, No. 4, 2004, pp. 541-546. Translated from Kinetikai Kataliz, Vol. 45, No. 4, 2004, pp. 574-579.

[0024] Non-patent document 4: Y. Ogura et al., "Efficient ammonia synthesis over a Ru / La 0, 5Ce0.5 O 1.75 Catalyst pre-reduced at high temperature”, Chemical Science, Vol. 9, pp. 2230-2237

[0025] Non-patent literature 5: M. Kitano et al., Angew. Chem. Int. Ed., 130 (2018) 2678

[0026] Non-patent document 6: W. Gao et al., ACS Catal., 7 (2017) 3654 Summary of the invention

[0027] Technical problem to be solved by the invention

[0028] Synthesis catalysts usually require high synthesis activity. For the catalysts currently being developed for ammonia synthesis, there is a continuous demand for high-activity catalysts that can achieve higher yields. Among binary catalysts, such as Co / BaLaO x Although such catalysts have sufficiently high ammonia synthesis activity, the activity needs to be further improved.

[0029] The present invention aims to provide a composite oxide such as BaLaO which can show a higher performance than conventional binary composite oxides containing rare earth elements when supporting cobalt. x A composite oxide having a higher ammonia synthesis activity. In addition, another object of the present invention is to provide a metal support and an ammonia synthesis catalyst showing such a high ammonia synthesis activity. Further, another object of the present invention is to provide a method for producing such a composite oxide and a metal support, and a method for producing ammonia.

[0030] Solutions to technical problems

[0031] The present inventors have found that, in order to solve the above-mentioned technical problems, a catalyst having high ammonia synthesis activity can be prepared by using two Group II elements having specific properties in combination as metal oxides constituting a composite oxide, thereby obtaining the following invention.

[0032] [1] A composite oxide comprising an oxide of a metal element L and an oxide of a metal element N, characterized in that it is represented by the following general formula (1) and satisfies the following (a) to (d):

[0033] L n N 1-n (1)

[0034] (a) The metal element L is an oxide of an element selected from any one of the following (i) to (iii):

[0035] (i) Group I elements,

[0036] (ii) Group II elements,

[0037] (iii) Group I elements and Group II elements;

[0038] (b) the metal element N consists of Group I or Group II elements other than the metal element L;

[0039] (c) said n is not less than 0.001 and not more than 0.300;

[0040] (d) The oxide of the metal element L and the oxide of the metal element N do not form a solid solution, but the oxide particles of the metal element L are deposited on the surfaces of the oxide particles of the metal element N.

[0041] [2] The composite oxide according to [1], wherein

[0042] (a) The metal element L represents the partial negative charge of oxygen in the state of oxide (-δ OA ) value is 0.56 or more and 0.70 or less, and is a metal element that is a strong alkaline element.

[0043] (b) The metal element N represents the partial negative charge of oxygen in the state of oxide (-δ OB A metal element that is a weakly alkaline element and has a ) value of 0.35 or more and 0.55 or less.

[0044] [3] The composite oxide according to [1] or [2], characterized in that it is a binary composite oxide consisting of metal element A included in metal element L and metal element B included in metal element N, wherein the general formula (1) is represented by the composition of the following general formula (2) and satisfies the following (a) to (d):

[0045] A n B 1-n (2)

[0046] (a) The metal element A represents the partial negative charge of oxygen in the state of oxide (-δ OA ) values ​​of 0.56 to 0.70, which are strong alkaline elements of Group 2;

[0047] (b) The metal element B represents the partial negative charge of oxygen in the state of oxide (-δ OB ) values ​​of 0.35 or more and 0.55 or less as weakly basic elements of Group 2;

[0048] (c) said n is not less than 0.001 and not more than 0.300;

[0049] (d) The oxide of the metal element A and the oxide of the metal element B do not form a solid solution, but the oxide particles of the metal element A are deposited on the surfaces of the oxide particles of the metal element B.

[0050] [4] A composite oxide comprising an oxide of a metal element L and an oxide of a metal element N, characterized in that it is represented by the following general formula (3) and satisfies the following (a) to (d):

[0051] L n N 1-n O x (3)

[0052] (a) The metal element L is an oxide of an element selected from any one of the following (i) to (iii):

[0053] (i) Group I elements,

[0054] (ii) Group II elements,

[0055] (iii) Group I and Group II elements,

[0056] (b) the metal element N is composed of a Group I element or a Group II element other than the metal element L;

[0057] (c) said n is not less than 0.001 and not more than 0.300;

[0058] (d) The oxide of the metal element L and the oxide of the metal element N do not form a solid solution, but the oxide particles of the metal element L are deposited on the surfaces of the oxide particles of the metal element N.

[0059] [5] The composite oxide according to [4], wherein

[0060] (a) The metal element L represents the partial negative charge of oxygen in the state of oxide (-δ OA ) value is 0.56 or more and 0.70 or less, and is a metal element that is a strong alkaline element.

[0061] (b) The metal element N represents the partial negative charge of oxygen in the state of oxide (-δ OB A metal element that is a weakly alkaline element and has a ) value of 0.35 or more and 0.55 or less.

[0062] [6] The composite oxide according to [4] or [5], characterized in that it is a binary composite oxide consisting of the metal element A included in the metal element L and the metal element B included in the metal element N, the general formula (3) is represented by the composition of the following general formula (4), and satisfies the following (a) to (d):

[0063] A n B 1-n O x (4)

[0064] (a) The metal element A represents the partial negative charge of oxygen in the state of oxide (-δ OA ) values ​​of 0.56 to 0.70, which are strong alkaline elements of Group II;

[0065] (b) The metal element B represents the partial negative charge of oxygen in the state of oxide (-δ OB ) values ​​of 0.35 or more and 0.55 or less as weakly basic elements of Group II;

[0066] (c) said n is not less than 0.001 and not more than 0.300;

[0067] (d) the oxide of the metal element A and the oxide of the metal element B do not form a solid solution, but the oxide particles of the metal element A are deposited on the surface of the oxide particles of the metal element B;

[0068] (e) The above x represents the number of oxygen atoms required for the composite oxide to maintain electrical neutrality.

[0069] [7] The composite oxide according to any one of [1] to [6], wherein the composite oxide is Ba n Mg 1- n O x , where 0.001≤n≤0.300.

[0070] [8] The composite oxide according to [7], characterized in that the composite oxide is Ba n Mg 1-n O x , where 0.01≤n≤0.10.

[0071] [9] The composite oxide according to [7] or [8], wherein the amount of carbonate contained in the composite oxide is 10 mol % or less compared to Ba.

[0072]

[10] A metal-supported material, characterized in that at least one metal particle M selected from the group consisting of cobalt, iron, and nickel is supported on the composite oxide according to any one of [1] to [9].

[0073] [10-1] A metal support, which is a composition formed by the metal particles M and the composite oxide described in any one of [1] to [3], and in which various elements can be confirmed as aggregates of particles, wherein a metal element L having a particle size of less than 10% of the particle size of the metal particles M can be observed to be distributed on the particles of the metal particles M, between the metal particles M and the metal oxide N, and on the metal oxide N.

[0074] [10-2] The metal-supported material according to [10-1], wherein it can be confirmed that the particles of the metal element L are uniformly distributed.

[0075] [10-3] The metal support as described in [10-1] or [10-2], wherein the particles of the metal element L are also distributed in the intermediate layer between the metal particles M and the metal element N.

[0076] [10-4] The metal support according to any one of [10-1] to [10-3], wherein the composite oxide is the composite oxide according to [6], the metal element A is selected from the metal element L, and the metal element B is selected from the metal element N.

[0077]

[11] The metal support according to

[10] , wherein the metal particles M are supported on the oxide of the metal element L deposited on the surface of the oxide of the metal element N, and the oxide particles of the metal element L are deposited on the surface of the metal particles M.

[0078]

[12] The metal support according to

[10] , wherein oxide particles of the metal element N are distributed between the oxide particles of the metal element L and the metal particles M.

[0079] [12-1] The metal support as described in

[11] or

[12] , wherein the composite oxide is the composite oxide as described in [6], the metal element A is selected from the metal element L, and the metal element B is selected from the metal element N.

[0080]

[13] The metal support as described in

[10] , characterized in that the metal particles M are cobalt particles.

[0081]

[14] A catalyst for ammonia synthesis, characterized in that the metal support described in

[10] is used.

[0082]

[15] A method for producing a metal support as described in

[10] , comprising the following steps (a) to (d):

[0083] (a) an impregnation step of impregnating an L precursor containing the metal element L with an N precursor containing the metal element N;

[0084] (b) a composite oxide calcining step of calcining the mixture at a temperature of 500° C. or higher to obtain a carrier composed of a composite oxide;

[0085] (c) a loading step of impregnating the composite oxide with a precursor of a compound containing the metal particles M to obtain an impregnated carrier; and

[0086] (d) a support calcining step of calcining the impregnated support at a temperature of 400° C. or higher.

[0087] [15-1] The method for producing a metal support as described in

[15] , wherein the metal element A is selected from the metal element L, and the metal element B is selected from the metal element N, and the method comprises the following steps (a) to (d):

[0088] (a) an impregnation step, wherein a B precursor containing the metal element B is impregnated with an A precursor solution containing the metal element A;

[0089] (b) a composite oxide calcining step of calcining the mixture at a temperature of 500° C. or higher to obtain a carrier composed of a composite oxide;

[0090] (c) a loading step of impregnating the composite oxide with a precursor solution of a compound containing the metal particles M to obtain an impregnated carrier; and

[0091] (d) a support calcining step of calcining the impregnated support at a temperature of 400° C. or higher.

[0092] [15-2] The method for producing a metal support as described in

[15] or [15-1], characterized in that the step (b) is performed in air.

[0093] [15-3] The method for producing a metal support as described in

[15] or [15-1], characterized in that the step (d) is performed in argon gas.

[0094]

[16] The method for producing a metal support as described in any one of

[15] to [15-3], characterized in that it also includes step (e):

[0095] (e) A reduction step of calcining the metal support obtained in the above (d) at 500° C. or higher in the presence of hydrogen.

[0096]

[17] A method for producing ammonia by bringing hydrogen and nitrogen into contact with a catalyst, wherein the catalyst is the ammonia synthesis catalyst as described in

[14] .

[0097] Effects of the Invention

[0098] According to the present invention, a composite oxide can be provided which, when supporting cobalt, is different from conventional binary composite oxides containing rare earths, such as Ru / BaLaO x In comparison, a higher ammonia synthesis activity can be shown. In addition, according to the present invention, a metal support and an ammonia synthesis catalyst showing such a high ammonia synthesis activity can be provided. Furthermore, according to the present invention, a method for producing such a composite oxide and a metal support, and a method for producing ammonia can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0099] Figure 1 The Co / Ba ratio in the embodiment is shown. 0.01 Mg 0.99 O x _A graph showing the ammonia synthesis activity of a 700°C reduced catalyst (a catalyst prepared by loading Co and then reducing it at 700°C).

[0100] Figure 2 The Co / BaMgO used in the example is shown x Co / BaMgO prepared by changing the amount of Ba added to the support in the catalyst x Graph showing the ammonia synthesis activity of the catalysts measured.

[0101] Figure 3 The Co / BaMgO used in the example is shown x BaMgO prepared by changing the amount of Ba added to the support in the catalyst x Graph showing the ammonia synthesis activity of the catalysts measured.

[0102] Figure 4 The Co / BaMgO used in the example is shown x Co / BaMgO prepared by changing the reduction temperature in the catalyst x Graph showing the ammonia synthesis activity of the catalysts measured.

[0103] Figure 5 The Co / BaMgO used in the example is shown x Co / BaMgO prepared by changing the reduction temperature in the catalyst x Graph showing the ammonia synthesis activity of the catalysts measured.

[0104] Figure 6The Co / BaMgO used in the example x Co / BaMgO prepared by changing the reduction temperature in the catalyst x XRD patterns of the catalysts.

[0105] Figure 7 The Co / BaMgO used in the example is shown x Co / BaMgO prepared by changing the Co loading in the catalyst x Graph showing the ammonia synthesis activity of the catalysts measured.

[0106] Figure 8 The Co / BaMgO used in the example is shown x Co / BaMgO prepared by changing the Co loading in the catalyst x Graph showing the ammonia synthesis activity of the catalysts measured.

[0107] Fig. 9 The Co / BaMgO x A graph showing the ammonia synthesis activity of the catalyst measured by varying the reaction pressure.

[0108] Fig.10 The Co / BaMgO x A graph showing the ammonia synthesis activity of the catalyst measured by varying the reaction pressure.

[0109] Fig.11 The Co / BaMgO x A graph showing the ammonia synthesis activity of the catalyst measured by varying the reaction pressure.

[0110] Fig.12 The Co / BaMgO used in the example is shown x Co / BaMgO prepared by changing the pretreatment conditions in the catalyst x Graph showing the ammonia synthesis activity of the catalysts measured.

[0111] Fig.13 The Co / BaMgO used in the example is shown x Co / BaMgO prepared by changing the Co precursor in the catalyst x Graph showing the ammonia synthesis activity of the catalysts measured.

[0112] Fig.14 The Co / BaMgO used in the example x Co / BaMgO prepared by changing the Co precursor in the catalyst x XRD patterns of the catalysts.

[0113] Fig.15The Co / BaMgO x A graph showing the ammonia synthesis activity measured by varying the SV of the catalyst.

[0114] Fig.16 The Co / BaMgO x A graph showing the ammonia synthesis activity measured by varying the SV of the catalyst.

[0115] Fig.17 The Co / BaMgO x This is a graph showing the ammonia synthesis activity of the catalyst measured at a low reaction temperature.

[0116] Fig.18 The Co / BaMgO x This is a graph showing the ammonia synthesis activity of the catalyst measured at a low reaction temperature.

[0117] Fig.19 The Ru / BaMgO of the embodiment is shown. x Graph of ammonia synthesis activity.

[0118] Fig. 20 The Fe / Ba ratio in the examples is shown. 0.01 Mg 0.99 O x _A graph showing the ammonia synthesis activity of a 700°C reduced catalyst (a catalyst prepared by loading Co and then reducing it at 700°C).

[0119] Fig.21 The Fe / BaMgO x Co / BaMgO prepared by changing the pretreatment conditions of the catalyst x Graph showing the measured ammonia synthesis activities of the catalysts.

[0120] Fig. 22 The Co / BaMgO of the embodiment is shown. x A graph showing the ammonia synthesis activity of a Co—Fe catalyst among catalysts.

[0121] Fig.23 The Co / BaMgO of Example 1 x H2-TPR measurement results of the catalyst.

[0122] Fig.24 The Co / MgO of Comparative Example 2 x H2-TPR measurement results of the catalyst.

[0123] Fig.25 The Co / BaMgO of Example 1 is shown in FIG. xThe element distribution diagram of the catalyst obtained by TEM is: Fig.25 (1) is the HAADF-STEM image, Fig.25 (2) is the element distribution diagram of Ba, Fig.25 (3) is the element distribution diagram of Mg, Fig.25 (4) is the element distribution diagram of Co, Fig.25 (5) is a diagram showing the superposition of the element distributions of Ba, Co, and Mg.

[0124] Fig.26 The Co / BaMgO x This is a graph showing the ammonia synthesis activity of catalysts obtained by replacing Ba in the catalyst with other Group II elements.

[0125] Fig. 27 This is a graph showing the ammonia synthesis activity measured by using a catalyst prepared using a Group I element instead of a Group II element.

[0126] Fig.28 This is a graph showing the ammonia synthesis activity of a catalyst obtained by using a carrier prepared by adding both a Group II element and a Group I element.

[0127] Fig.29 This is a graph showing the ammonia synthesis activity of a catalyst obtained by using a carrier prepared by adding both a Group II element and a Group I element.

[0128] Fig.30 This is a graph showing the ammonia synthesis activity of a catalyst obtained by using a carrier prepared by adding both a Group II element and a Group I element.

[0129] Fig.31 This is a graph showing the ammonia synthesis activity of a catalyst obtained by using a carrier prepared by adding both a Group II element and a Group I element.

[0130] Fig.32 This is a graph showing the ammonia synthesis activity of catalysts obtained using supports prepared using various transition metal elements.

[0131] Fig.33 This is a graph showing the ammonia synthesis activity of catalysts obtained using supports prepared using various transition metal elements.

[0132] Fig.34 The Co / BaMgO of Example 17 is shown x The element distribution diagram of the catalyst obtained by TEM is: Fig.34 (1) is the HAADF-STEM image, Fig.34 (2) is the element distribution diagram of Ba, Fig.34 (3) is the element distribution diagram of Mg, Fig.34 (4) is the element distribution diagram of Co, Fig.34 (5) is a superimposed diagram of the elemental diagrams of Ba, Co, and Mg.

[0133] Fig.35 This is a diagram for explaining the structural features of the metal supports of Examples 1 and 17.

[0134] Fig.36 These are the XANES spectra of the standardized catalyst and standard samples. DETAILED DESCRIPTION

[0135] <Compound oxide>

[0136] The composite oxide of the present invention is a composite oxide composed of an oxide of a metal element L and an oxide of a metal element N, characterized in that it is represented by the following general formula (1) and satisfies the following (a) to (d):

[0137] L n N 1-n (1)

[0138] The metal element L is an oxide of an element selected from any one of the following (i) to (iii):

[0139] (i) Group I elements,

[0140] (ii) Group II elements,

[0141] (iii) Group I elements and Group II elements.

[0142] It should be noted that in the present invention, the “metal element L” includes not only one element (a Group I element or a Group II element) but also two elements (a Group I element and a Group II element).

[0143] The Group I elements as the metal element L are metals called so-called alkali metals, and examples thereof include Li, Na, K, Rb, and Cs. In addition, the Group II elements are metals called alkaline earth metals, and examples thereof include Be, Mg, Ca, Sr, Ba, and Ra. In addition, there is a case where both Group I elements and Group II elements are used as the metal element L. The selection of these elements can be made based on consideration of alkalinity. Furthermore, the partial negative charge described below can also be calculated and used. When using Group I metals and Group II metals, the ratio thereof is preferably in the range of 0.1:1.9 to 1.9:0.1, more preferably in the range of 0.8:1.2 to 1.2:0.8, and particularly preferably 1:1. Based on the fact that the ammonia synthesis activity of the metal support described below is high, as the metal element L, it is preferred that it is a single Group II element, or a composite oxide of a Group I element and a Group II element.

[0144] The metal element N may be an oxide of an element of Group I or Group II other than the metal element L. The amount of the metal element L used is small relative to the metal element N. The metal element N is usually used in an amount of 0.001 or more and 0.300 or less relative to the total amount of the metal element of the metal element L, and is preferably used in an amount of 0.01 or more and 0.100 or less. The ratio of the metal element L affects the morphology during catalyst manufacture and also affects the activity of the catalyst. The oxide of the metal element L does not form a solid solution with the oxide of the metal element N, and the metal element L is observed on the metal element N. In this specification, this state is sometimes referred to as: the metal element L or the oxide of the metal element L is deposited on the metal element N or the oxide of the metal element N.

[0145] In the composite oxide used in the present invention, metal element A is selected from metal element L, and metal element B is selected from metal element L. In the case of a binary composite oxide, general formula (1) is represented by the following general formula (2).

[0146] A n B 1-n (2)

[0147] (a) The metal element A is an alkaline earth metal of Group II, and has a partial negative charge (-δ OA ) value is 0.56 to 0.70.

[0148] (b) The metal element B is an alkaline earth metal other than the metal element A, and represents a partial negative charge (-δ OB A Group II element which is a weakly basic element and has a ) value of 0.35 or more and 0.55 or less.

[0149] (c) The addition ratio of the metal element A relative to the whole is 0.001 or more and 0.300 or less. The form within this range has a positive influence on the catalyst activity.

[0150] (d) In addition, the state in which the oxide of the metal element A and the oxide of the metal element B do not form a solid solution, but the oxide particles of the metal element A are observed on the surface of the oxide particles of the metal element B is referred to as "deposition" in this specification.

[0151] As shown below, the composite oxide represented by the composition of the general formula (1) can be written as the formula (3) if described in other expressions. That is, the composite oxide used in the present invention is a composite oxide formed of an oxide of a metal element L and an oxide of a metal element N, characterized in that it is represented by the composition of the following general formula (3) and satisfies the following (a) to (d):

[0152] L n N 1-n O x (3)

[0153] (a) The metal element L is an oxide of an element selected from any one of the following (i) to (iii):

[0154] (i) Group I elements,

[0155] (ii) Group II elements,

[0156] (iii) Group I elements and Group II elements;

[0157] (b) Metal element N, consisting of Group I elements or Group II elements other than metal element L;

[0158] (c) said n is not less than 0.001 and not more than 0.300;

[0159] (d) the oxide of the metal element L and the oxide of the metal element N do not form a solid solution, but the oxide particles of the metal element L are deposited on the surface of the oxide particles of the metal element N;

[0160] (e) The above x represents the number of oxygen atoms required for the composite oxide to maintain electrical neutrality.

[0161] The composite oxide of the present invention is a binary composite oxide composed of a metal element A and a metal element B represented by the following general formula (4) when the general formula (2) is expressed in another way.

[0162] A n B 1-n O x (4)

[0163] (A, B, n, and x are as described in the above general formula (2).)

[0164] <Alkalinity>

[0165] The composite oxide used in the present invention does not form a solid solution between the oxide of the metal element L and the oxide of the metal element N. The metal element L is preferably an oxide with a partial negative charge (-δ OA) is 0.56 or more and 0.70 or less, and is a metal element that is a strong alkaline element, wherein the metal element N is preferably a partial negative charge (-δ OB A metal element that is a weakly alkaline element and has a value of 0.35 or more and 0.55 or less.

[0166] When the metal element A is selected from the metal element L, and the metal element B is selected from the metal element N, and a binary composite oxide is formed:

[0167] (a) The metal element A represents the partial negative charge of oxygen in the state of oxide (-δ OA ) value of 0.56 to 0.70, which is a Group II element that is a strong alkaline element,

[0168] (b) The metal element B represents the partial negative charge of oxygen in the state of oxide (-δ OB ) value of 0.35 or more and 0.55 or less, which is a weakly basic element of Group II,

[0169] (c) said n is not less than 0.001 and not more than 0.300,

[0170] (d) the oxide of the metal element A and the oxide of the metal element B do not form a solid solution, but the oxide particles of the metal element A are deposited on the surface of the oxide particles of the metal element B,

[0171] (e) The above x represents the number of oxygen atoms required for the composite oxide to maintain electrical neutrality.

[0172] Metal element A is the partial negative charge of oxygen in the oxide state (-δ O ) value is 0.56 or more and 0.70 or less. OA The value of is more preferably 0.60 or more, and most preferably 0.65 or more. Specifically, the metal element A can be selected from Ba (barium), Sr (strontium), and Ca (calcium).

[0173] Metal element B is the partial negative charge of oxygen in the oxide state (-δ O ) is a weakly alkaline element with a value of 0.35 or more and 0.55 or less. OB The value of is more preferably 0.40 or more. OB The value of is more preferably 0.50 or less, and most preferably 0.45 or less. Specifically, the metal element B can be selected from Mg (magnesium) and Be (beryllium).

[0174] -δ OA With -δ OBThe difference is preferably 0.10 to 0.40, more preferably 0.15 to 0.35, and most preferably 0.20 to 0.30.

[0175] In the present invention, the metal element A contained in the composite oxide is a strong basic element showing high basicity in the state of an oxide, and thus can improve the activity of the ammonia synthesis catalyst. The principle thereof will be briefly described below.

[0176] The metal element A is a strongly alkaline metal element. Electrons are generated from the base point of the composite oxide (support) of the element, and the electrons are supplied to the nitrogen molecules through the transition metal particles as a catalyst supported on the composite oxide, thereby weakening the nitrogen triple bond. The inventors call this stage the rate-determining stage of the ammonia synthesis reaction. It is believed that the energy of cutting the triple bond of the nitrogen molecule is reduced through the above-mentioned series of electron actions, thereby improving the ammonia synthesis activity of the metal support (catalyst).

[0177] The basicity (Lewis basicity) of metal oxides is related to the electron-donating ability. That is, it can be considered that the higher the electron-donating ability of a substance, the stronger the basicity. Basically, in oxides, oxygen acts as an electron donor, so the amount of charge carried by oxygen in the oxide, that is, the partial negative charge of oxygen, can be used as an indicator of basicity. In fact, it is shown in the non-patent literature (Sanderson, Inorganic Chemistry (Volume 1), Hirokawa Bookstore (1975), Table 12.7, page 276) that the value of the partial negative charge of oxygen is strongly correlated with the acidity and basicity shown by the oxide.

[0178] Here, regarding the oxides of individual metal elements, the partial negative charge of oxygen (-δ O ), the values ​​listed in Table 12.7 of the non-patent literature (Sanderson, Inorganic Chemistry (Volume 1), Hirokawa Shoten (1975), page 276) can be used. For oxides without listed values, the partial negative charge of oxygen can be calculated by the above calculation. The following table shows the partial negative charge of oxygen (-δ O ) value.

[0179]

Table 1

[0180]

[0181] On the other hand, for the calculation method of the partial negative charge of oxygen in the composite oxide as a whole, refer to the non-patent literature (Sanderson, Inorganic Chemistry (Volume 1), Hirokawa Bookstore (1975), page 122, Table 6.7, pages 126-128). First, find the composition ratio of each element in the composite oxide. For example, "Ce 0.5 La 0.5 O 1.75"La is 0.5, and this value is recorded as ni (i is the corresponding element). In addition, the electronegativity of each element is recorded as χi. Then, by (Π(χi ni ))^(1 / Σni) The geometric mean of the electronegativity of all atoms constituting the composite oxide is calculated. Next, in order to calculate the change in electronegativity of oxygen, the difference between the geometric mean and the electronegativity of oxygen (5.21) is calculated. Finally, the change in electronegativity of oxygen is divided by the change in electronegativity when one oxygen atom obtains one electron (-4.75). Through the above calculations, the partial negative charge of oxygen shown in the composite oxide can be calculated.

[0182] To summarize the above, the partial negative charge value of oxygen in the composite oxide is represented by the following formula (A) when the composition ratio of each element contained in the composite oxide is denoted by ni (i represents all elements in the composite oxide containing at least A, B, and O) and the electronegativity of each element is denoted by χi (i represents all elements in the composite oxide containing at least A, B, and O):

[0183] ((Π(χi ni ))^(1 / Σni)-5.21) / -4.75・・Formula (A).

[0184] When calculating the partial negative charge of oxygen in a composite oxide, among the elements forming the composite, (a) it can be obtained from the partial negative charge of oxygen in the state of an oxide, or (b) when the composition ratio of each element contained in the composite oxide is represented by ni (i represents all elements in the composite oxide containing A, B, and O) and the Sanderson electronegativity of each element is represented by χi (i represents all elements in the composite oxide containing A, B, and O), it can be obtained by the following formula (A):

[0185] ((Π(χi ni ))^(1 / Σni)-5.21) / -4.75・・Formula (A).

[0186] In the case where the composite oxide forms a uniform composite oxide, it is preferred to perform method (b). On the other hand, in the case where the composite oxide forms an inhomogeneous composite oxide, it is preferred to perform method (a), in which case the result of the element with the largest absolute value of the partial negative charge of oxygen of a single element can be used. In the composite oxide of the present invention, since the oxide of metal element A and the oxide of metal element B do not form a solid solution but form a phase separation, the value of the partial negative charge of oxygen of the composite oxide is preferably calculated by the above-mentioned method (a).

[0187] The value of the partial negative charge of oxygen in the composite oxide is preferably 0.35 or more, and more preferably 0.40 or more. When the value of the partial negative charge of oxygen in the composite oxide is 0.35 or more, the ammonia synthesis activity tends to be high.

[0188] <Removal of carbonates and hydroxides>

[0189] Metal elements L (alkali metals) and N (alkaline earth metals) are highly alkaline even in the form of oxides, and are easily reacted with carbon dioxide and water in the atmosphere to form metal carbonates and hydroxides. However, the metal carbonates and hydroxides reduce the alkalinity of the composite oxide and become the cause of the reduction in the ammonia synthesis activity of the catalyst. For example, Ba is easily formed into BaCO3 and Ba(OH)2 in the atmosphere, which reduces the ammonia synthesis activity. Therefore, the metal carbonates and hydroxides contained in the ammonia synthesis catalyst are as small as possible. In order to reduce the metal carbonates and hydroxides, it is preferred to perform a reduction treatment under the heating conditions described below, thereby decomposing the metal carbonates and hydroxides contained in the catalyst and preventing the alkalinity from decreasing. The amount of carbonate contained in the metal support is not particularly limited as long as it is within the range that does not hinder the ammonia synthesis activity, for example, it is 10 mol% or less, preferably 1 mol% or less, more preferably 0.1 mol% or less, and even more preferably 0.01 mol% or less compared to the metal element A.

[0190] As a method for quantifying the amount of carbonate present in the form of metal carbonate, there is a method in which a catalyst is heated under a hydrogen flow to hydrogenate the carbonate species to produce hydrocarbons such as methane, and the hydrocarbons are detected by a mass spectrometer or a hydrogen flame ionization detector (FID), a thermal conductivity detector (TCD), etc., and then converted.

[0191] Alternatively, infrared absorption spectroscopy, which is highly sensitive to metal carbonates, can be used. By irradiating the catalyst with infrared light and measuring the absorption intensity of the peak of the wave number characteristically absorbed by the carbonate, the amount of carbonate contained in the catalyst can be quantified. For example, the peak position that can be used for the quantification of Ba carbonate is at 3000 cm -1 Nearby, 2450cm -1 Nearby, 1750cm -1 Nearby, 1480cm -1 Nearby, 1060cm -1 Wait nearby.

[0192] The following table shows the melting points of oxides of Ba and Sr, which are elements of Group II and have relatively large partial negative charges on oxygen, and of Cs and K, which are alkali metals.

[0193]

Table 2

[0194]

[0195] Based on the H2-TPR measurement results described below, it is believed that the following reaction occurs.

[0196] BaCO3+4H2→BaO+CH4+2H2O (5)

[0197] In addition, although the melting point of the oxide of Ba is high, as mentioned above, when heat-treated under hydrogen atmosphere, a hydroxide with a lower melting point can be generated in the middle. Therefore, fluidity is obtained by the dissolution of the hydroxide. At this moment, it can be considered that: since Ba and the metallic element B both exist as strongly basic compounds, they repel each other, or due to interfacial tension or due to other certain reasons, so the result is that the compound of Ba flows on the metal particles, and the hydroxide of Ba is generated to be distributed on the surface of the metal particles in a particle-like state, and becomes an oxide after the reaction and loses fluidity and volume shrinks simultaneously, thereby directly being immobilized under this state with a gap, thus finding higher activity. In the present invention, the state of also having a particle-like existence on the metal surface is referred to as the state of "distribution", "pile-up".

[0198] As described above, since the basicity of the element itself is strong and it is easy to reduce carbonates that hinder the basicity, Ba is particularly preferred as the metal element A because it can enhance the ammonia synthesis activity.

[0199] The oxide of the metal element B is the main component of the composite oxide and exhibits weak alkalinity (including slight alkalinity in the following description). Ba is a binary composite oxide described in prior art documents. n La 1-n O x In the present invention, the partial negative charge value of the oxides of the two metal elements Ba and La is relatively high (Ba is 0.67, La is 0.56). In contrast, in the present invention, the partial negative charge value of the oxide of the metal element B is relatively low, being 0.35 or more and 0.55 or less.

[0200] <Accumulation>

[0201] In the present invention, the oxide of the metal element L and the oxide of the metal element N do not form a solid solution but form a phase separation, and the oxide of the metal element L is deposited on the surface of the oxide particles of the metal element N, and is deposited on the surface of the metal particles that support the oxide of the metal element L. Therefore, even if the basicity of the oxide of the metal element N is weak, as long as the basicity of the oxide of the metal element L is strong, the ammonia synthesis activity can be improved by the oxide of the metal element L. Therefore, even if the oxide ratio of the metal element N is lower than that of the prior art, a higher ammonia synthesis activity can be shown.

[0202] As the oxide of the metal element N, it is preferred that the specific surface area (SSA) is large. This is because when the specific surface area of ​​the oxide of the metal element N, which is the main component of the composite oxide, is large, fine nanoparticles such as Co can be firmly fixed, and the number of active sites of these nanoparticles increases, thereby improving the ammonia synthesis activity. Therefore, from the perspective of the size of the specific surface area, Mg (magnesium) is particularly preferred as the metal element N. Although the metal element N is the main component of the composite oxide, when it is used as a carrier for supporting transition metals to form a catalyst, the oxide of the metal element N plays a great role as a carrier.

[0203] Based on the above viewpoints, the composite oxides of formula (1) and formula (2) are preferably Ba n Mg 1-n O x (where 0.001≤n≤0.300).

[0204] Here, about Ba n Mg 1-n O x The composition ratio of Ba (i.e., the value of n) is preferably in the range of 0.01≤n≤0.10. As shown in the examples described below, when it is in the range of 0.01≤n≤0.10, the ammonia synthesis activity (yield, yield) tends to increase.

[0205] <Metal support>

[0206] The metal support of the present invention is a metal support in which particles of transition metals other than Group 4 are supported on the composite oxide of the present invention (hereinafter sometimes referred to as transition metal particles). As the transition metal, based on the viewpoint of high catalytic activity, it is preferred to select one or more from the group consisting of Ru, Fe, Co, Ni, Rh, Pd, Os, Ir, and Pt, and more preferably Ru, Co, or a mixture of Fe and Co. Among them, based on the height of ammonia synthesis activity when combined with the composite oxide of the present invention, Co is particularly preferred. The quantitative ratio of the transition metal to the composite oxide can be determined in consideration of the catalytic activity and the cost of the transition metal. For example, it is preferred that the ratio of the transition metal to the metal support as a whole is in the range of 0.1 to 50% by weight, and more preferably in the range of 5.0 to 30% by weight.

[0207] The transition metal M of the present invention does not form a solid solution with any of the oxides of the metal element L and the oxides of the metal element N. It is particularly preferred that the oxide particles of the metal element L are deposited and covered on the particles of the transition metal M, and further deposited on the surface of the oxide particles of the metal element N as the main component. That is, it is preferably in a so-called core / shell relationship with the transition metal M as the core and the metal element L as the shell. The entire transition metal M is covered with the oxide particles of the metal element L, and is supported on the oxide particles of the metal element N via the oxide of the metal element L. It can be considered that such a structure is that the metal L is supported on the metal N, and then the transition metal M is supported, which can be considered to be in order to allow the oxide of the metal L with fluidity to cover the transition metal M when performing a high-temperature reduction treatment. When the amount of metal L is too much compared to the amount of the metal element N as a carrier, or when it is too much compared to the amount of the transition metal, the layer will be too thick, so nitrogen and hydrogen cannot reach the transition metal surface as an active point, which is not preferred. Furthermore, when the firing is performed at a high temperature of 700° C. or higher or for a long time, the oxide particles of the metal L aggregate, and thus nitrogen and hydrogen cannot reach the transition metal surface serving as an active site, which is not preferable.

[0208] The composite oxide of the present invention is a mixed state of an oxide of a metal element L and an oxide of a metal element N. In particular, it is preferred that the laminated structure of the oxide particles of the metal element L is deposited on the surface of the oxide particles of the metal element N as the main component. It should be noted that it is most preferred that the two are in a so-called core / shell relationship. Furthermore, the metal element L may not exist inside the catalyst carrier, but it is preferred that the metal element L exists on the surface of the carrier.

[0209] In particular, the composite oxide of the present invention is a mixed state of an oxide of metal element A and an oxide of metal element B. In particular, it is preferred that the laminated structure of oxide particles of metal element A is deposited on the surface of oxide particles of metal element B as the main component. It should be noted that it is most preferred that the two are in a so-called core / shell relationship. Further, the metal element A may not exist inside the catalyst carrier, but it is preferred that the metal element A exists on the surface of the carrier.

[0210] Since the oxide of the metal element L and the oxide of the metal element N are not solid-dissolved but in a mixed state (phase separation), when used as a metal support (catalyst) described below, the transition metal particles are in direct contact with the oxide of the metal element L on the surface of the composite oxide. Since the oxide of the metal element L (such as Ba) is strongly basic, it is speculated that since the transition metal particles are in direct contact with these oxides, the number of active sites showing high activity increases, and the ammonia synthesis activity is improved. On the other hand, in the case of Co, the basicity of the cation is very important, and the larger the partial negative charge of oxygen in the oxide of the metal element A such as Ba, the higher the ammonia synthesis activity.

[0211] The particle size ratio A / M of the oxide particles of the metal element A to the metal particles M is usually 20% or less, preferably 10% or less, and more preferably 5% or less. In order to change the particle size, the ratio of the metal element A to the transition metal M can be adjusted. When the particle size ratio is too large or too small, it tends to be difficult to obtain the predicted catalyst activity.

[0212] In addition, the value of Co dispersion (D ads ), and the value of the Co dispersion predicted from the average particle size of Co particles obtained from TEM images (D TEM ), preferably satisfying 0<D ads / D TEM <1. The Co dispersion is expressed as the ratio of the number of Co atoms exposed on the surface of the metal support to the total number of Co atoms contained in the metal support. The Co dispersion can be determined from the amount of hydrogen adsorbed by the metal support supporting Co.

[0213] Specifically, assuming that one Co atom adsorbs one H atom, the ratio of the number of hydrogen atoms H corresponding to the number of Co atoms exposed on the surface of the metal support to the total number of Co atoms supported on the metal support (H / Co) is the Co dispersion. In the present invention, the Co dispersion based on the amount of hydrogen adsorption is denoted as D ads By comparing metal supports that carry the same amount (same number of atoms) of Co, it can be found that the higher the Co dispersion, the more catalyst active sites there are.

[0214] It is also known that if the shape of the Co particles is assumed to be a cube, the Co dispersion value can be geometrically calculated using the average particle diameter of Co (d, in nm) obtained by TEM observation (see the document "Dictionary of Catalysts"). This calculation method can be expressed by general formula (8). The average particle diameter of Co can be calculated by randomly extracting 100 to 150 Co particles from the TEM image, measuring the diameter of each particle, and calculating their average value. In the present invention, the value of the Co dispersion obtained based on general formula (4) is recorded as DTEM .

[0215] D TEM =0.732 / d (8)

[0216] Therefore, D ads / D TEM A value lower than 1 means that a portion of the Co particles, mainly the vicinity of the interface between the particles and the composite oxide (support) and the particle surface are covered with the oxide of the metal element B, thereby inhibiting the adsorption of H atoms to the Co particle surface.

[0217] TOF (catalyst rotation frequency) indicates the number of reactions that occur per unit time at one active point on the catalyst surface. In this application, it is expressed as the number of ammonia molecules generated per second at one surface Co atom that is an active point.

[0218] The average particle diameter of Co supported on the composite oxide is preferably 100 nm or less, more preferably 50 nm, and even more preferably 20 nm or less. The smaller the particle diameter of Co, the more active sites there are when used as an ammonia synthesis catalyst, which is advantageous. The lower limit of the average particle diameter of Co is not particularly limited, and may be, for example, 0.5 nm or more, or 1 nm or more.

[0219] The metal support of the present invention is fine particles with an average particle diameter of 100 nm or less of the supported metal cobalt, thereby showing a very high ammonia synthesis rate under mild ammonia synthesis conditions (300 to 500° C., 0.1 to 20 MPa).

[0220] It should be noted that in this specification, in order to make the description concise, "Ba loaded with Co" will be used. 0.01 Mg 0.99 O 1.00 "The metal support represented by "Co / Ba 0.01 Mg 0.99 O1", and the product after the metal support is reduced is recorded as "Co / Ba 0.01 Mg 0.99 O x The same notation is used for other supports. Here, x means that the molar ratio of oxygen during firing decreases from 1.00 to x as reduction occurs. When necessary, in this specification, when only ABO is used, x In the case of 1.00 B 1.00 O x Meaning.

[0221] In the general formula (2) representing the ratio of oxygen O in the composite oxide, x represents the number of oxygen atoms required for the composite oxide to maintain electrical neutrality. Although it depends on the types of elements A and B, x is usually in the range of 0.5<x≤2, and particularly in the range of 0.9<x≤1.

[0222] <Effect of reduction temperature on ammonia synthesis activity>

[0223] The catalyst of the present invention is activated by performing a hydrogen reduction pretreatment at a high temperature. This is because Co is reduced. In addition, at this time, a characteristic structure in which the oxide of the metal element A is deposited on the surface of the Co particles is found. Usually, if the reduction pretreatment is high temperature, the specific surface area decreases and the diameter of the metal particles increases with the sintering of the carrier, which can cause a decrease in the catalyst activity.

[0224] Figure 4 and Figure 5 It is shown that in the examples described below (Co / BaMgO x ), a graph of the ammonia synthesis activity of the catalyst produced by changing the reduction temperature. According to the graph, the ammonia synthesis activity increases with the increase of the reduction temperature, the ammonia synthesis rate increases when the reduction is performed at 700°C and 800°C, and the ammonia generation rate slightly decreases when the reduction is performed at 900°C compared to 800°C.

[0225] Figure 6 , showing the Co / BaMgO in the examples described below x XRD spectrum. According to this figure, before reduction, the peak from BaCO3 can be observed. If the reduction temperature is higher than 700°C, the peak of BaCO3 disappears, so it can be seen that BaCO3 is decomposed. In addition, it can be seen that if the reduction temperature is increased, the peak of Co becomes higher.

[0226] In addition, if Fig.12 As shown, the catalyst reduced at 500° C. for 72 hours showed performance comparable to that of the catalyst reduced at 700° C. for 1 hour. It can be seen that the catalyst of the present invention can obtain high activity for a long time if it is reduced at a low temperature, and can obtain high activity in a short time if it is reduced at a high temperature.

[0227] When the reduction temperature increases, TOF (catalyst rotation frequency) tends to increase.

[0228] That is, it can be considered that the reason why the ammonia generation rate decreases when the reduction temperature increases to greater than 800°C is that the sintering and enlargement of the carrier particles leads to a decrease in the specific surface area and the sintering of Co continues to progress, and the surface of the Co particles is excessively covered with the oxide of the metal element A, resulting in a decrease in the number of active points.

[0229] By using a metal support loaded with Co as a catalyst, nitrogen and hydrogen can be reacted to produce ammonia. The synthesis method of ammonia itself is not particularly limited. For example, ammonia can be produced by supplying a raw material gas composed of hydrogen and nitrogen into a reaction container filled with a catalyst. The reaction temperature is preferably 300 to 550°C, more preferably 300 to 500°C, and even more preferably 300 to 450°C.

[0230] The reaction pressure when ammonia synthesis is carried out using the catalyst of the present invention is preferably a low pressure of 0.1 to 20 MPa, more preferably 0.1 to 15 MPa, and even more preferably 0.1 to 10 MPa. Fig.10 and Fig.11 As shown, it can be seen that the activity of the catalyst loaded with Co is also increased under high-pressure reaction conditions compared with the catalyst loaded with Ru. This is because Co is less susceptible to hydrogen poisoning than Ru, so the activity is not easily reduced under high pressure. That is, in the case of Ru, the interaction between the hydrogen atoms adsorbed on the surface and Ru becomes stronger under high pressure, the detachment of hydrogen atoms is very difficult to occur, the active points on the Ru surface are blocked, and the ammonia synthesis reaction started by the nitrogen molecules being adsorbed on the active points is difficult to occur. Compared with Ru, the interaction between Co and hydrogen is weaker, so it is difficult to produce such a phenomenon, and it has the property that the ammonia synthesis activity is not easily reduced under high pressure. The ammonia synthesis reaction, generally according to thermodynamic equilibrium, has a tendency that the higher the pressure, the higher the ammonia yield. Therefore, by using the catalyst for ammonia synthesis of the present invention, it can be expected to obtain a further higher yield under high-pressure conditions of, for example, about 10 MPa. In addition, compared with Ru, Co has a crustal presence of more than 10,000 times that of Ru and exists in large quantities, so it has higher versatility and lower cost than Ru.

[0231] When a metal support carrying Co is used as a catalyst, it is preferred that the composite oxide serving as a support contains Ba from the viewpoint of catalyst activity. Based on this combination, sufficient ammonia synthesis activity can be exerted by using Co, which is cheaper than Ru. In addition, even when the reaction pressure is high, it is not as susceptible to hydrogen poisoning as the Ru catalyst. Therefore, the reaction pressure is most preferably 1 to 10 MPa.

[0232] <Method for producing composite oxide and metal-supported material>

[0233] Next, the production method of the composite oxide and the metal support of the present invention will be described. The composite oxide of the present invention can be produced by the following method.

[0234] (a) an impregnation step of impregnating an L precursor containing a metal element L with an N precursor containing the metal element N;

[0235] (b) a composite oxide calcining step of calcining the mixture at a temperature of 500° C. or higher to obtain a carrier composed of a composite oxide;

[0236] The metal support of the present invention can be further produced by using the following method on the composite oxide obtained by the above (a) and (b).

[0237] (c) a loading step of impregnating the composite oxide with a precursor of a compound containing the metal particles M to obtain an impregnated carrier;

[0238] (d) a support calcining step of calcining the impregnated support at a temperature of 400° C. or higher.

[0239] Step (a) is described below. Step (a) is a method for producing a composite oxide of the present invention. The composite oxide is a step of mixing and impregnating an L precursor containing a metal element L and an N precursor containing a metal element N to obtain a mixture (precursor of the composite oxide).

[0240] The precursor of the composite oxide can be prepared by various methods such as precipitation method, complex polymerization method, etc. For example, a neutralization precipitation method can be used in which a precipitant such as ammonia, sodium hydroxide, cesium hydroxide, etc. is reacted with nitrate, chloride, acetate, carbonate, sulfate of A or B to obtain a hydroxide.

[0241] The precursor of the composite oxide can also be obtained by preparing one or more products containing metal element L and metal element N separately and mixing them. In this way, the compound containing metal element L and the compound containing metal element N are mixed to obtain a mixture.

[0242] Next, step (b) is described. This step is a step of firing the mixture obtained in step (a). Thus, the generated mixture (composite oxide precursor) is converted into a composite oxide having a high specific surface area by firing.

[0243] The firing is preferably carried out at a low temperature of about 200 to 400° C. for about 1 to 10 hours, at an intermediate temperature of about 400 to 600° C. for about 1 to 10 hours, and at a high temperature of about 600 to 700° C. for about 1 to 10 hours. The firing temperature in the final step is most preferably 700° C. The firing can be carried out in an atmosphere containing oxygen such as air or a mixed gas of an inert gas and oxygen, and can be carried out at any oxygen concentration.

[0244] The following is an explanation of step (c). In step (c), the composite oxide obtained in step (b) is stirred with a solvent in which a transition metal particle supply source such as cobalt, iron, or nickel is dissolved, so that the transition metal particle supply source is impregnated in the composite oxide, and then the solvent is removed by heating and the transition metal particle supply source is decomposed after the removal, thereby obtaining a pre-reduction-treated supported material in which transition metal particles are supported in the form of fine particles on the composite oxide support.

[0245] As the transition metal particle supply source of cobalt (cobalt supply source), various compounds containing Co can be cited, for example, organic metal compounds such as cobalt (II) acetylacetonate can be cited. Among them, cobalt (II) acetylacetonate is particularly preferred due to its high ammonia synthesis activity. Other cobalt supply sources that can support cobalt on the composite oxide can also be used, such as cobalt nitrate, cobalt chloride, cobalt nitrosyl nitrate, etc.

[0246] When an organic metal compound such as cobalt (II) acetylacetonate is used as a cobalt supply source, it is advantageous to use an organic solvent as a solvent. Examples of organic solvents include tetrahydrofuran (THF), methanol, ethanol, hexane, toluene, and the like. These solvents, if they are general commercial products, can be used without special pretreatment, but are preferably used after purification, dehydration, etc. The solid content concentrations of the composite oxide and the cobalt supply source relative to 1 liter of solvent are generally preferably about 1 to 30 g / liter and 0.1 to 3 g / liter, respectively, and more preferably about 10 to 30 g / liter and 0.1 to 0.3 g / liter, respectively. Stirring can be performed at room temperature, and the stirring time is preferably 1 to 24 hours, and more preferably 6 to 12 hours. The removal of the solvent can be performed by heating using various methods, preferably in a reduced pressure, low temperature atmosphere, such as using an evaporator. The decomposition of the cobalt supply source is performed by heating in an inert atmosphere such as helium, argon or nitrogen atmosphere. It can also be implemented in an atmosphere containing hydrogen. The heating is performed at a temperature of about 200 to 600° C. for about 1 to 12 hours. A more preferred heating temperature is about 300 to 500° C., and a more preferred heating time is about 3 to 6 hours.

[0247] As a ruthenium supply source, various compounds containing Ru can be used. Preferably, organic metal compounds such as triruthenium dodecacarbonyl and ruthenium acetylacetonate can be used. Other ruthenium supply sources that can support ruthenium on a composite oxide, such as ruthenium chloride, ruthenium nitrate, etc., can also be used.

[0248] The following is an explanation of step (d). Next, the support (impregnated support) before reduction treatment thus obtained is subjected to reduction treatment. The purpose of the reduction treatment is to reduce the transition metal particles and to destroy the carbonate described below. The reduction temperature is 400°C to 800°C, preferably 600 to 700°C. When the reduction temperature is a high temperature exceeding 500°C, the reduction time is usually from 10 minutes to 40 hours, preferably about 30 minutes to 5 hours. When the reduction temperature is a low temperature, the reduction time is 48 hours to 120 hours, preferably 60 hours to 100 hours. The reduction treatment can be carried out in the presence of a reducing gas such as hydrogen.

[0249] It is known that in the case of containing strongly alkaline Ba, BaO reacts with carbon dioxide in the air and the like to easily form barium carbonate (Ba(CO3)) and barium hydroxide (Ba(OH)2)). If carbonates and hydroxides are formed in this way, the partial negative charge of oxygen in BaO is significantly reduced, and high alkalinity cannot be obtained. Therefore, in order to show high ammonia synthesis activity, it is necessary to destroy the carbonates and hydroxides by appropriate treatment. For example, as a method of destroying Ba carbonate to form BaO, heating treatment (reduction treatment) under hydrogen flow is effective. The reaction is represented by the following formula.

[0250] BaCO3+4H2→BaO+CH4+2H2O (5)

[0251] By heating the catalyst in a hydrogen atmosphere, hydrogen dissociation occurs on the surface of the supported metal species, generating hydrogen species with strong reducing power. Under the action of the hydrogen species, Ba carbonate is destroyed and converted into BaO.

[0252] As a method for destroying Ba carbonate, the catalyst may be kept at a temperature of 550°C or higher for about 1 hour under a hydrogen flow. A preferred condition is about 600°C to 800°C.

[0253] Ba carbonate can also be destroyed by keeping the catalyst warm for a long time at low temperature and under hydrogen flow. Preferred conditions are 500°C for about 48 hours, 450°C for about 72 hours, and 400°C for more than 120 hours.

[0254] By using such a method, the carbonate of Ba can be destroyed. In order to show the alkaline properties of Ba, it is preferred to reduce the proportion of Ba in the form of carbonate as much as possible. The proportion of Ba in the catalyst in the form of carbonate is preferably 10 mol% or less, more preferably 1 mol% or less, even more preferably 0.1 mol% or less, and particularly preferably 0.01 mol% or less, compared to the total amount of Ba contained in the catalyst.

[0255] The calcination temperature in step (d) is most preferably 700 to 800° C. If the calcination temperature in this step is too high, the support and active metal will be excessively sintered during the reduction treatment, and the particle diameter will increase, thereby reducing the number of active sites and lowering the catalyst performance.

[0256] On the other hand, if the calcination temperature in this step is too high, the specific surface area of ​​the carrier will decrease, so the dispersion state of the active metal will deteriorate and the particle diameter will increase, so the number of active sites will decrease and the catalyst performance will decrease.

[0257] As for the relationship between the firing temperature and the reduction temperature, as described above, from the viewpoint of ammonia synthesis activity, it is preferred to fire the support at a temperature equal to or higher than the reduction treatment temperature.

[0258] Fig.35 The above situation is explained. Fig.35 , for metal supported Co / BaMgO x The difference caused by the different manufacturing methods is explained. In the previous research of the inventor, a Ba / Ru / MgO was disclosed (refer to Examples 80 and 81 of WO2019 / 059190). If the manufacturing method at that time is implemented in this application, it will be as follows. That is, Co is supported on Ba to form Fig.35 (1) Further loading of barium to form Fig.35 (2) Then, if high-temperature reduction is carried out at, for example, 700°C, the product is Fig.35 (2) Structure. That is, although a structure is formed in which transition metal Co is deposited on MgO as a carrier and barium oxide is deposited on transition metal Co, according to the cross section Fig.35 (3) It can be seen that Co is in direct contact with MgO.

[0259] On the other hand, when a metal support is produced by the method of the present invention, it is as follows. That is, since BaO is supported on MgO and then Co is supported, Fig.35 (4), then Fig.35 (4) For example, when reduced at 700°C, Figure (5) is generated. This is because the Ba compound supported during the high-temperature reduction process gains fluidity and moves, thereby covering Co. Therefore, when observing the cross section, Fig.35 (6) It is known that MgO and Co are not in direct contact, and Co is arranged on MgO via the Ba compound. Since barium oxide covers Co at an appropriate density, nitrogen and hydrogen can reach Co, which is an active site.

[0260] The metal support of the present invention thus obtained is superior in ease of handling and stability during reaction compared to metal supports conventionally used for ammonia synthesis catalysts.

[0261] It should be noted that, when Ba and the like are contained in the composite oxide, even if the catalyst is in an oxidized state during manufacture, it is easy to absorb CO2 and form carbonates if exposed to the atmosphere. Therefore, after decomposing Ba carbonate by the above-mentioned reduction treatment, it is preferably treated in a manner that will not be exposed to CO2 until the catalyst is used, and it is preferably stored in a container filled with an inert gas, etc., for example. However, in the case where a part of the carrier is assumed to become carbonate, decomposition by hydrogenation can reduce carbonates and restore ammonia synthesis activity.

[0262] The metal support loaded in the synthesis reactor and used as a catalyst must be replaced periodically. Since it is assumed to be used for a long time, a metal support that is easy to handle and has excellent stability is required. The metal support of the present invention is advantageous in this respect.

[0263] Example

[0264] Next, the present invention is further described by way of examples. Of course, the present invention is not limited to these examples.

[0265] <Measurement of ammonia synthesis activity>

[0266] The ammonia synthesis activity of the metal support was measured using a fixed bed flow reactor. The metal support pretreated by the method described in the examples and comparative examples was allowed to cool to 300°C while Ar was flowing. Ar was supplied while the temperature of the metal support layer was maintained at 300°C, and the pressure was increased to 1.0 MPa or 3.0 MPa through the back pressure valve at the outlet of the reaction tube. Ar was stopped, and H2 and N2 were respectively supplied at 90 mL min while the pressure was maintained. -1 、30mLmin -1 (Space speed 72L h -1 g -1) flows and changes to a reaction atmosphere. According to the level of NH3 synthesis activity, 200 mL of 1-100 mM (1, 5, 10, 25, 100 mM) sulfuric acid aqueous solution is added to a three-necked flask connected to a conductivity meter, and the mixed gas containing hydrogen (purity of 99.995%, manufactured by Fukuoka Oxygen), nitrogen (purity of 99.995%, manufactured by Fukuoka Oxygen), and NH3 flowing out from the outlet of the reaction tube is bubbled in the sulfuric acid aqueous solution. In addition, a gas purifier (gas purification filter MC50-904F, manufactured by SAES) is used to remove impurities such as water and oxygen, so that the purity is 99.99999999 or more. At this time, the amount of ammonia generated in the outlet gas is quantified by measuring the change in conductivity caused by the reaction of NH3 and sulfuric acid. Next, the temperature of the metal support layer is raised to 350°C, 400°C or 450°C. After the temperature of the metal support layer was stabilized at 350° C., 400° C. or 450° C., the layer was left to stand for 10 minutes, and the amount of ammonia generated was quantified by the same method as above.

[0267] <Powder X-ray Diffraction>

[0268] The powder X-ray diffraction pattern of the metal support (catalyst) was measured using SmartLab x-ray diffractometer (Rigaku Corporation).

[0269] <Specific surface area (SSA) measurement>

[0270] The specific surface area of ​​the metal support was determined by the BET method using BEL-sorp mini (BEL, Japan) based on the amount of nitrogen adsorption at 77 K. Before the measurement, vacuum heating at 300° C. was performed for 2 hours as a pretreatment.

[0271] 1. Co / Ba 0.01 Mg 0.99 O x _700℃ reduction and Co / Ba 0.05 La 0.95 O x _Comparison of reduction at 700℃

[0272] (Example 1)

[0273] <Co / Ba 0.01 Mg 0.95 O x _700℃ reduction>

[0274] <Preparation of composite oxide>

[0275] Ba 0.01 Mg 0.99 O xThe composite oxide was synthesized as follows. Ba(OH)2 (Wako Pure Chemical Industries, Ltd.) was dissolved in purified water to obtain a Ba(OH)2 aqueous solution, and 200 mL of a precursor solution containing 0.000625 mol of Ba was prepared. 2.5 g of MgO (Ube Industries, Ltd.) was added thereto, and the mixture was stirred at 320 rpm using a magnetic stirrer, and the stirring was continued at room temperature for 1 hour. The suspension was evaporated to dryness using a rotary evaporator, and the obtained powder was dried overnight using a furnace set at 80°C. The dried precipitate was crushed in a mortar, and the obtained powder was heated at 700°C in an air atmosphere for 5 hours using an electric furnace, thereby obtaining Ba 0.01 Mg 0.99 O x .

[0276] <Carrying of Co>

[0277] By impregnation method, Co was incorporated into the carrier Ba 0.01 Mg 0.99 O x Loading on. A tetrahydrofuran (THF) (Wako Pure Chemical Industries) solution containing cobalt (II) acetylacetonate (Wako Pure Chemical Industries) as a Co precursor was prepared in a 200 mL eggplant-shaped bottle, 1 g of the carrier was added thereto, and the mixture was stirred at room temperature for more than 18 hours. It should be noted that the amounts of cobalt (II) acetylacetonate and the carrier used were appropriately adjusted so that the amount of Co contained in the catalyst after heating under the argon atmosphere described below was 20 wt %. The stirred suspension was dried under reduced pressure using a rotary evaporator at 35°C and 0.3 atm, and then dried in a furnace at 80°C for 18 hours. The obtained powder was heated in a tubular electric furnace at 80 mL min -1 The precursor was heated at 500°C for 5 hours under an argon flow to remove the acetylacetonate ligand in the precursor. 0.01 Mg 0.99 O x Metal carrier.

[0278] <Pretreatment before hydrogen reduction>

[0279] For the Co / Ba 0.01 Mg 0.99 O x, use the following method to carry out hydrogen reduction pretreatment (referred to as "pretreatment" for short). After the powder of the metal support is pressurized at 20 MPa for 5 minutes to make a disk, the disk is crushed with a mortar, and classified with a sieve to make pellets. The size of the pellets is adjusted to be 250-500 μm in diameter. Use 100 mg of pellets and fill them in a catalyst reaction tube made of Inconel (インコネル (trademark)) with a diameter of 7 mm, and fix the front and back of the catalyst layer with quartz wool. The reaction tube is set in a fixed bed flow reactor for measuring ammonia synthesis activity, and 60 mLmin is circulated in the reaction tube filled with pellets. -1 H2, heated at 700℃ for 1 hour, to obtain Co / Ba 0.01 Mg 0.99 O x _Reduction at 700℃.

[0280] (Comparative Example 1)

[0281] <Co / Ba 0.05 La 0.95 O x _700℃ reduction>

[0282] The Co / Ba of Example 101 of Patent Document 6 (International Publication No. 2019 / 216304) 0.05 La 0.95 O x _700℃ reduction is used as a comparative example. Co / Ba 0.05 La 0.95 O x _Reduction at 700℃.

[0283] The metal supports of Example 1 and Comparative Example 1 were subjected to ammonia synthesis at a reaction pressure of 1 MPa and various temperatures (300° C., 350° C., 400° C., and 450° C.), and the ammonia synthesis activity was measured by the above-mentioned method. The results are shown in the table below.

[0284]

Table 3

[0285]

[0286] In addition, the results Figure 1 The right side of the vertical axis of the figure represents the ammonia synthesis rate, the left side of the vertical axis represents the ammonia yield, and the horizontal axis represents the reaction temperature. According to the figure, at any reaction temperature, the metal support of Example 1 exceeds the metal support of Comparative Example 1 in terms of ammonia synthesis rate and yield. It can also be seen that the higher the reaction temperature of ammonia synthesis, the higher the ammonia synthesis activity (synthesis rate, yield).

[0287] 2. Discussion on the amount of Ba added (Examples 1 to 6, Comparative Example 2)

[0288] In Example 1, the ratio of the molar number of Ba to the total molar number of Ba and Mg was variously changed (0 mol% (Comparative Example 2), 0.5 mol% (Example 2), 1 mol% (Example 1), 2 mol% (Example 3), 3 mol% (Example 4), 5 mol% (Example 5), 10 mol% (Example 6)) to produce a metal support.

[0289] Ammonia synthesis was carried out on the metal supports of Examples 1 to 6 and Comparative Example 2 at a reaction pressure of 1 MPa and various temperatures (300° C., 350° C., 400° C., and 450° C.), and the ammonia synthesis activity was measured by the above method. The results are shown in the table below.

[0290]

Table 4

[0291]

[0292] In addition, the results Figure 2 and Figure 3 As shown in the figure, it can be seen that, although the ammonia synthesis activity increases with the increase in the amount of Ba added, the ammonia synthesis activity is the highest when the addition amount is 1 mol%, and when the addition amount increases to more than this amount, the ammonia synthesis activity gradually decreases. In addition, according to Figure 3 It is found that the amount of Ba added, which provides high ammonia synthesis activity, is in the range of 0.5 to 3 mol %.

[0293] 3. Discussion of reduction temperature (Examples 7 to 11)

[0294] In Example 1, the Co loading was set to 20 wt %, and the reduction temperature was changed to various levels (500° C. (Example 7), 650° C. (Example 8), 700° C. (Example 9), 800° C. (Example 10), and 900° C. (Example 11)) to produce a metal support.

[0295] The metal supports of Examples 7 to 11 were subjected to ammonia synthesis at a reaction pressure of 1 MPa and various temperatures (300° C., 350° C., 400° C., and 450° C.), and the ammonia synthesis activity was measured by the above-mentioned method. The results are shown in the table below.

[0296]

Table 5

[0297]

[0298] In addition, the results Figure 4 and Figure 5As shown in FIG. 1 , it can be seen that, although the ammonia synthesis activity is relatively low when the reduction temperature is 500° C., the ammonia synthesis activity increases at 650° C. or higher.

[0299] Figure 6 The XRD spectra of the metal supports in Example 7 (reduction temperature 500°C), Example 9 (reduction temperature 700°C), and Example 10 (reduction temperature 800°C) are shown. "Fresh" in the figure refers to the sample before the reduction treatment. As can be seen from the figure, the reduction treatment causes BaCO3 to decompose. When the reduction temperature is increased to about 700°C, the peak of BaCO3 cannot be observed, so it can be seen that BaCO3 is decomposed. In addition, it can be seen that when the reduction temperature is increased to 800°C, the peak of metal Co that has not been observed so far can be observed. It can be considered that the reason is that the peak of metal Co that has not been observed because the Co particles are highly dispersed can be observed when it is agglomerated into slightly dispersed Co particles under the action of high-temperature reduction treatment.

[0300] The following table shows various parameters of the metal supports of Example 7 (reduction temperature 500°C), Example 9 (reduction temperature 700°C), Example 10 (reduction temperature 800°C), and Comparative Example 2 (no Ba, reduction temperature 700°C) at a reaction temperature of 350°C. As can be seen from the table, although the specific surface area (SSA) decreases as the reduction temperature increases, the ammonia synthesis activity increases.

[0301]

Table 6

[0302]

[0303] 4. Discussion on Co loading (Example 12, Example 1, Example 15)

[0304] In Example 1, the supported amount of Co was variously changed (5 wt % (Example 12), 10 wt % (Example 13), 20 wt % (Example 1), 30 wt % (Example 15)) to produce a metal supported material.

[0305] Ammonia synthesis was carried out on the metal supports of Example 12, Example 1, and Example 15 at a reaction pressure of 1 MPa and various temperatures (300° C., 350° C., 400° C., and 450° C.), and the ammonia synthesis activity was measured by the above method. The results are shown in the table below.

[0306]

Table 7

[0307]

[0308] In addition, the results Figure 7 and Figure 8As shown in FIG. 1 , it can be seen that the ammonia synthesis activity increases as the Co loading increases, and the ammonia synthesis activity is substantially maximum at 20 wt %.

[0309] (Comparative Examples 1, 4, and 5)

[0310] As a comparative example, Co / Ba 0.05 La 0.95 O x (Comparative Example 1), Ru / CeO x , (Comparative Example 4), Cs + / Ru / MgO x (Comparative Example 5).

[0311] Ru / CeO x , (Comparative Example 4) was prepared by the following method. Ru was loaded on CeO2 by impregnation. Ru3(CO) 12 (Furuya Metal) tetrahydrofuran (THF) (Wako Pure Chemical Industries, Ltd.), 5 g of CeO2 (Daiichi Kizen Chemical Industry) was added thereto, and stirred at room temperature for more than 18 hours. It should be noted that the Ru3(CO) used was appropriately adjusted. 12 The amount of the catalyst and the carrier was adjusted so that the amount of Ru contained in the catalyst after heating in an argon atmosphere was 5 wt%. The stirred suspension was dried under reduced pressure using a rotary evaporator at 35°C and 0.3 atm, and then dried in a furnace at 80°C for 18 hours. The obtained powder was heated in a tubular electric furnace at 500°C and 80 mL min -1 The precursor was heated for 5 hours under a flow of argon gas to remove the carbonyl ligands in the precursor. Ru / CeO2 was obtained by the above operation. The reduction treatment was carried out at 400°C.

[0312] Cs + / Ru / MgO x (Comparative Example 5) was prepared by the method described in the non-patent literature (F. Rosowski, A. Hornung, O. Hinrichsen, D. Herein, M. Muhler and G. Ertl, Appl. Catal., A, 1997, 151, 443-460.). It should be noted that the Ru loading was set to 5 wt%, and the Cs / Ru ratio was set to 1 / 1 (mol / mol). The reduction treatment was performed at 500°C.

[0313] The metal supports of Comparative Examples 3 to 5 were subjected to ammonia synthesis at various temperatures (300°C, 350°C, 400°C, and 450°C) and pressures (0.1 MPa, 1.0 MPa, and 3.0 MPa), and the ammonia synthesis activity was measured by the above-mentioned method. The results are shown in the table below.

[0314]

Table 8

[0315]

[0316] In addition, the results Fig.10 (reaction temperature 350°C) and Fig.11 (reaction temperature 400°C) is shown in Example 3 (Co / Ba 0.01 Mg 0.99 O x ) are also shown in the figure. As can be seen from the figure, the metal supports of the examples have higher ammonia synthesis activity than the metal supports of the comparative examples 1, 4, and 5.

[0317] 6. Effect of pretreatment conditions (reduction conditions) (Example 1, Example 17, Comparative Example 6)

[0318] In Example 1, the temperature and time of the hydrogen reduction pretreatment were changed to 500°C and 72 hours to produce a metal support (Example 17). As a comparative example, 5wt%Ru / MgO (Comparative Example 6) was produced in the same manner as in Comparative Example 4 except that MgO (Ube Materials) was used as the support.

[0319] Ammonia synthesis was carried out on the metal supports of Example 1, Example 17 and Comparative Example 6 at a reaction pressure of 1 MPa and various temperatures (300°C, 350°C, 400°C, 450°C), and the ammonia synthesis activity was measured by the above method. The results are shown in the table below.

[0320]

Table 9

[0321]

[0322] In addition, the results Fig.12 As shown in FIG. 1 , it can be seen that even if the reduction condition is low pressure, the ammonia synthesis activity is improved by a long period of reduction.

[0323] 7. Effect of Co Precursor (Example 1, Example 18)

[0324] In Example 1, a metal support (Example 18) was prepared by the same method as in Example 1, except that Co(NO3)2·6H2O (Wako Pure Chemical Industries, Ltd.) was used instead of Co acetylacetone(II) (Co(acac)) as a Co precursor, purified water was used instead of THF, and air was used as the atmosphere during firing.

[0325] The metal supports of Example 1 and Example 18 were subjected to ammonia synthesis at a reaction pressure of 1 MPa and various temperatures (300° C., 350° C., 400° C., and 450° C.), and the ammonia synthesis activity was measured by the above-mentioned method. The results are shown in the table below.

[0326]

Table 10

[0327]

[0328] In addition, the results Fig.13 As shown in FIG. 1 , it can be seen that, regarding the Co precursor, Co(acac) can improve the ammonia synthesis activity more than Co nitrate.

[0329] Fig.14 The XRD of the metal supports of Example 1 (Co(acac)) and Example 17 (Co nitrate) are shown. As can be seen from the figure, the peak derived from metal Co cannot be observed in the metal support using Co(acac) as a precursor, but the peak derived from metal Co is observed in the metal support using nitric acid as a precursor. It can be inferred that the metal support using Co(acac) as a precursor has a higher dispersion of Co than the metal support using Co nitrate as a precursor, resulting in an increase in ammonia synthesis activity.

[0330] 8. SV Discussion (Example 1)

[0331] In Example 1, Co(NO3)2·6H2O (Wako Pure Chemical Industries, Ltd.) was used instead of Co acetylacetonate(II) (Co(acac)) as a Co precursor to prepare a metal support (Example 18).

[0332] Regarding the metal support of Example 1, the reaction pressure was 1 MPa and various temperatures (300°C, 350°C, 400°C, 450°C) and various SV (18 L / h -1 g -1 , 36L / h -1 g -1 , 72L / h -1 g -1 ) and the ammonia synthesis activity was measured by the above method. The results are shown in the following table.

[0333]

Table 11

[0334]

[0335] In addition, the results Fig.15 and Fig.16 As shown in the figure, it can be seen that as the value of SV increases, the ammonia synthesis rate increases ( Fig.15 ), but the ammonia yield is reduced ( Fig.16 ).

[0336] 9. Discussion of Carrier Characteristics (Example 1, Comparative Example 7, Comparative Example 1)

[0337] (5wt%Ru / Ba 0.1 La 0.45 Ce 0.45 O x : Comparative Example 7)

[0338] In Comparative Example 1, Ba was used instead of CeO2. 0.1 La 0.45 Ce 0.45 , and appropriately adjust the Ru content to make 5wt%Ru / Ba 0.1 La 0.45 Ce 0.45 O x(Comparative Example 7). It should be noted that the carrier was synthesized as follows using the reverse homogeneous precipitation method according to the method described in Example 6 of Patent Document 6 (International Publication No. 2019 / 216304). La(NO3)3・6H2O (Wako Pure Chemical Industries, Ltd.) was dissolved in purified water to form a La(NO3)3 aqueous solution. Ce(NO3)3・6H2O (Kanto Chemical Industries, Ltd.) was dissolved in purified water to form a Ce(NO3)3 aqueous solution. Ba(NO3)2・6H2O (Wako Pure Chemical Industries, Ltd.) was dissolved in purified water to form a Ba(NO3)2 aqueous solution. The La(NO3)3 aqueous solution and the Ce(NO3)3 aqueous solution were mixed, and the Ba(NO3)2 aqueous solution was mixed to prepare 250 mL of a carrier precursor solution containing a total of 0.0625 mol of La, Ce, and Ba. Add 250 mL of 28% NH3 aqueous solution (Wako Pure Chemical Industries, Ltd.) to a 1000 mL beaker, and while stirring at 320 rpm using a magnetic stirrer, add the above-mentioned carrier precursor solution all at once, and stir for 1 hour. Then let it stand for 12 hours, and separate the precipitate (1) by suction filtration. The separated filtrate is recovered in a 2 L beaker. Add 350 mL of ion exchange water to the separated precipitate (1), stir for 30 minutes and wash the precipitate, and separate the precipitate (1) by suction filtration. This washing operation is performed 3 times. All the ion exchange water used in the washing is recovered, and the filtrate and washing liquid are added to a 2 L beaker and mixed. The mixed solution is allowed to stand for 12 hours to produce a white precipitate (2), and the produced precipitate (2) is recovered by suction filtration. The precipitate (1) and the precipitate (2) are mixed, and dried at 80°C for 15 hours in a furnace. The dried precipitate is crushed in a mortar, and the obtained powder is heated at 700°C in an air atmosphere for 5 hours using an electric furnace, thereby obtaining Ba. 0.1 La 0.45 Ce 0.45 O x .

[0339] Ammonia synthesis was carried out on the metal supports of Example 1, Comparative Example 1 and Comparative Example 7 at a reaction pressure of 1 MPa and a reaction temperature of 350° C., and the ammonia synthesis activity was measured by the above-mentioned method. The results are shown in the following table.

[0340]

Table 12

[0341]

[0342] According to the table, the 20wt%Co / Ba 0.01 Mg 0.99 O x , the specific surface area (SSA) is large, which can be inferred to contribute to the increase of ammonia synthesis activity.

[0343] 10. Activity at low temperature (Example 1, Comparative Example 9, Comparative Example 10)

[0344] As a comparative example, Ru / Ba was produced using the method described in Example 6 of Patent Document 6 (International Publication No. 2019 / 216304). 0.1 La 0.45 Ce 0.45 O x (700°C, 1h, red) (Comparative Example 9).

[0345] In addition, the Ru / La 0.5 Ce 0.5 O x (650°C, 1h, red) (Comparative Example 10).

[0346] Regarding Example 1, ammonia synthesis was performed at various temperatures (150°C, 200°C, 250°C) and various pressures (0.1 MPa, 1.0 MPa, 3.0 MPa), and the ammonia synthesis activity was measured by the above method. In addition, regarding the metal supports of Comparative Examples 9 and 10, ammonia synthesis was performed at various temperatures (150°C, 200°C, 250°C) (pressure 1.0 MPa), and the ammonia synthesis activity was measured by the above method. The results are shown in the following table.

[0347]

Table 13

[0348]

[0349] In addition, the results Fig.17 , Fig.18 According to Fig.17 It can be seen that under low temperature conditions, the Co-supported catalyst shows higher activity than the Ru-supported catalyst. Fig.18 It can be seen that under low temperature conditions, the ammonia synthesis activity increases with increasing pressure.

[0350] 11. Discussion of Ru-supported catalysts (Example 21, Comparative Examples 11 to 14)

[0351] (Example 21)

[0352] <Ru / Ba 0.01 Mg 0.99 O x _700℃ reduction>

[0353] Except that in Example 1, Co(II) acetylacetonate was replaced by Ru3(CO) as the Ru precursor 12(Guwu Metal), the same operation as in Example 1 was carried out to obtain Ru / Ba 0.05 Mg 0.95 O x _Reduction at 700℃.

[0354] 11. Discussion of Fe-supported catalysts (Example 22, Comparative Example 15, Comparative Example 16)

[0355] (Example 22)

[0356] <Fe / Ba 0.01 Mg 0.99 O x _700℃ reduction>

[0357] The same operation as in Example 1 was carried out except that Co(II) acetylacetonate was replaced with Fe(III) acetylacetonate (Dojin Chemical Research Institute) as an Fe precursor to obtain Fe / Ba 0.01 Mg 0.99 O x _Reduction at 700℃.

[0358] (Comparative Example 15, Comparative Example 16)

[0359] As a comparative example, a 20 wt% Fe / Ba composite was prepared in the same manner as in Comparative Example 9 except that Ru was replaced with Fe and the amount of Ba was changed. 0.1 La 0.45 CeO x (700° C., 1 hour reduction) (Comparative Example 15) In addition, by the same method as in Comparative Example 6, 5 wt % Ru / MgO was prepared (Comparative Example 16).

[0360] The metal supports of Example 22, Comparative Example 15, and Comparative Example 16 were subjected to ammonia synthesis at a reaction pressure of 1 MPa and various temperatures (300° C., 350° C., 400° C., and 450° C.), and the ammonia synthesis activity was measured by the above method. The results are shown in the table below.

[0361]

Table 14

[0362]

[0363] In addition, the results Fig. 20 As shown in the figure, the metal support loaded with Fe is 5wt%Ru / MgO and 20wt%Fe / Ba 0.1 La 0.45 CeO x (700℃, 1 hour reduction) compared with the previous study, the ammonia synthesis activity is higher.

[0364] 12. Discussion of pretreatment conditions: Fe-supported catalyst (Example 23, Example 24, Comparative Example 16)

[0365] In Example 22, the pretreatment conditions were variously changed (H2+N2, 500°C, 72 hours of reduction (Example 23); H2 only, 700°C, 1 hour of reduction (Example 24)) to produce a metal support.

[0366] The metal supports of Example 23, Example 24, and Comparative Example 16 were subjected to ammonia synthesis at a reaction pressure of 1 MPa and various temperatures (300° C., 350° C., 400° C., and 450° C.), and the ammonia synthesis activity was measured by the above method. The results are shown in the table below.

[0367]

Table 15

[0368]

[0369] In addition, the results Fig.21 As shown in FIG. 1 , it can be seen that the ammonia synthesis activity is greatly improved depending on the pretreatment conditions.

[0370] 13. Discussion of Co-Fe Catalyst (Examples 25 to 27)

[0371] In Example 7 (20wt%Co / Ba 0.05 Mg 0.95 O x ), the Fe precursor of Example 22 was added to the Co precursor to adjust the mixing ratio, and a metal support was produced (Example 25).

[0372] Ammonia synthesis was carried out on the metal supports of Examples 7, 22 and 25 at various temperatures (300° C., 350° C., 400° C. and 450° C.), and the ammonia synthesis activity was measured by the above-mentioned method. The results are shown in the table below.

[0373]

Table 16

[0374]

[0375] In addition, the results Fig. 22 As shown in FIG. 1 , it can be seen that the ammonia synthesis activity of Co alone is higher than that of Fe alone and the Fe-Co mixed catalyst.

[0376] 14. H2-TPR measurement results (Example 1, Comparative Example 2)

[0377] For Example 1 (Co / Ba 0.05 Mg 0.95 O x_700℃ reduction), Comparative Example 2 (Co / MgO x ), and H2-TPR (H-Temperature Programmed Reduction: H-programmed temperature reduction) measurement. H2-TPR means that the temperature of the solid is continuously raised at a certain rate under the circulation of hydrogen (H2) diluted with an inert gas such as argon, the consumption rate of hydrogen and the generation rate of reaction products are measured, and a mass spectrometer is used as a detector. The results are Fig.23 , Fig.24 Shown in.

[0378] according to Fig.23 It can be seen that the Co / BaMgO of Example 1 x , absorbs hydrogen with a molecular weight of 2 at over 500°C and releases methane with a molecular weight of 16. It is also known that water with a molecular weight of 18 is released at over 600°C. Fig.24 It can be seen that the Co / MgO of Comparative Example 2 x , there is no such absorption and release. From these, it can be seen that in Example 1, the reduction reaction of the following formula (5) occurred with respect to Ba.

[0379] BaCO3+4H2→BaO+CH4+2H2O (5)

[0380] This result shows that although Co / BaMgO x The catalyst generates BaCO3 and Ba(OH)2 on the surface, but through heat treatment under hydrogen, H2 reacts with BaCO3 at more than 500°C to decompose into Ba(OH)2 and CH4, and Ba(OH)2 decomposes into BaO and H2O at more than 600°C. That is, it can be considered that the BaCO3 and Ba(OH)2 generated on the surface are converted into BaO by heat treatment under hydrogen, so the catalyst activity is improved.

[0381] Fig.25 , is an electron microscope photograph of the catalyst of Example 1. Fig.25 (1) is the HAADF-STEM image. Fig.25 (2)~ Fig.25 From the element distribution image of (5), we can get the following information. Fig.25 The whitest part in (1) is Co, and the next light gray part is the part where magnesium oxide exists. Fig.25(5) It can be seen that the particles of barium oxide are evenly distributed on Co / MgO in a smaller particle form than the particles of Co. The particle size of the barium oxide particles is at most about 10% of the particle size of the Co particles. The order of catalyst preparation is to support barium hydroxide on the magnesium oxide carrier, then support cobalt on the barium hydroxide, and then the barium oxide particles move to the cobalt particles under the catalyst manufacturing conditions. Before the cobalt is supported, the barium compound is evenly distributed on the surface of the magnesium oxide, so it can be considered that Ba also exists near the interface between magnesium oxide and cobalt. According to Fig.25 From the overlapped images of (5), it can be seen that there is a nanoscale core (Co particle) / shell (barium oxide) structure in which Ba covers the periphery of Co. It should be noted that in this catalyst, the surface cobalt atoms close to the barium oxide receive strong electrical supply, thus showing a high ammonia synthesis activity. This fact proves the above research.

[0382] Fig.34 , is an electron microscope photograph of the catalyst of Example 17. FIG. (1) is a HAADF-STEM image. Fig.34 (2) to (5) are element distribution images, and Fig.25 By comparison, the following results can be obtained. Fig.34 ) and 700℃, 1 hour reduction ( Fig.25 ), the reduction temperature is lower than that of the first embodiment, so although a nanoscale core (Co particle) / shell (barium oxide) structure can be observed, the particle diameter of barium oxide is small, and the mobility of barium oxide on the cobalt particles is also slightly low. However, corresponding to the long-term reduction treatment, the decomposition of barium carbonate and hydroxide proceeds more continuously than the case of 500°C, 1 hour reduction (Example 7). On the other hand, due to the low reduction temperature, the diameter of cobalt particles is small. In addition, corresponding to the long-term reduction treatment, the reduction degree of cobalt is higher than the case of 500°C, hour reduction (Example 7), and the number of surface cobalt atoms in a metallic state that contributes to ammonia synthesis increases. Therefore, the catalyst of Example 17 shows an ammonia synthesis activity comparable to that of the catalyst of Example 1.

[0383] As shown in Examples 33 and 34 described below, in the case of dual addition of Group I element + Group II element, it was found that the ammonia synthesis activity was further improved compared with Example 17. This is because the Group I element, which is a more alkaline element than the oxide of the Group II element, is introduced into the shell structure of barium oxide, and the surface cobalt atoms close to the shell receive very strong electrical supply.

[0384] 15. Ammonia synthesis activity of catalysts after Ba was replaced with other Group II elements (Sr, Ca) (Examples 26-27)

[0385] In Example 1, Sr(OH)2 and Ca(OH)2 were used instead of Ba(OH)2 to prepare 20wt%Co / Sr 0.01 Mg 0.99 O x (Example 26) and 20wt%Co / Ca 0.01 Mg 0.99 O x (Example 27). Ammonia synthesis was carried out on these metal supports at various temperatures (300°C, 350°C, 400°C, and 450°C), and the ammonia synthesis activity was measured by the above method. The ammonia synthesis conditions were as follows: the reaction pressure was set to 1.0 MPa, the reaction gas was H2 / N2=90 / 30 cc / min (total flow rate was 120 cc / min), and the catalyst amount was 0.1 g (SV=72 Lh -1 g -1 ). The results are shown in the following table.

[0386]

Table 17

[0387]

[0388] In addition, the results Fig.26 As shown in FIG. 1 , it can be seen that the Group II elements (Sr, Ca) other than Ba ​​are more active than MgO alone, and the effect of improving the ammonia synthesis activity by adding these elements can be confirmed.

[0389] 16. Addition of Group I elements in place of Group II elements (Examples 28 to 31)

[0390] In Example 1, KNO3, KOH, LiNO3, and LiOH were used instead of Ba(OH)2 as the raw material to produce composite oxides at various reduction temperatures. 0.03 Mg 0.97 O x (Example 28), 20wt%Co / K 0.03 Mg 0.97 O x (Example 29), 20wt%Co / Li 0.03 Mg 0.97 O x (Example 30), 20wt%Co / Li 0.03 Mg 0.97 O x (Example 31) Ammonia synthesis was carried out on these metal supports at various temperatures (300°C, 350°C, 400°C, and 450°C), and the ammonia synthesis activity was measured by the above-mentioned method. Fig. 27As shown in FIG. 1 , it can be seen that in the system where K is added using KOH, although some effect of improving ammonia activity is observed, the ammonia synthesis activity is not significantly improved like that of Group II elements.

[0391] 17. Double addition of Group I elements + Group II elements (Examples 32 to 34)

[0392] In Example 1, in addition to the raw material Ba(OH)2, CsOH, RbOH, and KOH were used to produce composite oxides, and pre-treated under the reduction conditions of 700°C for 1 hour to produce 20wt% Co / Cs 0.01 Ba 0.01 Mg 0.98 O x _700℃, 1h reduction (Example 32), 20wt%Co / Rb 0.01 Ba 0.01 Mg 0.98 O x _700℃, 1h reduction (Example 33), 20wt%Co / K 0.01 Ba 0.01 Mg 0.98 O x _700℃, 1h reduction (Example 34). Ammonia synthesis was carried out on these metal supports at various temperatures (300℃, 350℃, 400℃, 450℃), and the ammonia synthesis activity was measured by the above method. The results are shown in the following table.

[0393]

Table 18

[0394]

[0395] In addition, the results Fig.28 . As shown in the figure, when 1 mol% of the Group I element is added and the pretreatment conditions are fixed at 700°C and 1 hour, the activity of either of them is slightly lower than that of the case where no Group I element is added (Ba alone), but the ammonia synthesis activity of the same degree as that of the case where only Ba is added is obtained. Among them, since the ammonia synthesis activity of the case where only Ba is added is the highest, the improvement of the ammonia synthesis activity obtained by adding the Group I element (double addition) is not found.

[0396] 18. Double addition of Group I element + Group II element (Discussion of reduction conditions 1) (Examples 35-36)

[0397] In Example 30, the amount of KOH in the raw material was increased, the reduction conditions were changed, and 20 wt% Co / K 0.03 Ba 0.01 Mg 0.96 O x_500℃, 72h reduction (Example 35), 20wt%Co / K 0.03 Ba 0.01 Mg 0.96 O x _700℃, 1h reduction (Example 36). Ammonia synthesis was carried out on these metal supports at various temperatures (300℃, 350℃, 400℃, 450℃), and the ammonia synthesis activity was measured by the above method. The results are shown in the table below.

[0398]

Table 19

[0399]

[0400] In addition, the results Fig.29 As shown in FIG. 1 , it can be seen that in the case of 3 mol % K + 1 mol % Ba, even if the reduction is carried out at a low temperature for a long time, the effect of improving the ammonia synthesis activity is not observed.

[0401] 19. Double addition of Group I element + Group II element (Discussion of reduction conditions 2) (Example 37)

[0402] In Example 30, the amount of KOH in the raw material was not changed, but the reduction conditions were changed to produce 20 wt% Co / K 0.01 Ba 0.01 Mg 0.98 O x _500℃, 72h reduction (Example 37). Ammonia synthesis was carried out on these metal supports at various temperatures (300℃, 350℃, 400℃, 450℃), and the ammonia synthesis activity was measured by the above method. The results are shown in the table below.

[0403]

Table 20

[0404]

[0405] In addition, the results Fig.30 As shown in . According to the figure, in the case of 1 mol% K + 1 mol% Ba, the activity is improved if the reduction is carried out for a long time at a low temperature. It should be noted that in the figure, the influence of equilibrium appears near the reaction temperature of 450°C, and it can be inferred that either has the same degree of ammonia synthesis activity.

[0406] 20. Double addition of Group I element + Group II element (Discussion of reduction conditions 3) (Example 38)

[0407] In Example 29, the reduction conditions were changed to produce 20wt%Co / Rb 0.01 Ba 0.01 Mg 0.98 Ox _500℃, 72h reduction (Example 38). Ammonia synthesis was carried out on these metal supports at various temperatures (300℃, 350℃, 400℃, 450℃), and the ammonia synthesis activity was measured by the above method. The results are shown in the table below.

[0408]

Table 21

[0409]

[0410] In addition, the results Fig.31 As shown in . According to the figure, in the case of 1 mol% Rb + 1 mol% Ba, the activity is improved if the reduction is carried out for a long time at a low temperature. It should be noted that in the figure, the influence of equilibrium appears near the reaction temperature of 450°C, and it can be inferred that either has the same degree of ammonia synthesis activity.

[0411] 21. Ni instead of Co (Discussion of reaction pressure 1) (Example 39)

[0412] In Example 1, the same operation as in Example 1 was performed except that Co(II) acetylacetonate was replaced with nickel(II) acetylacetonate (Kishida Chemical) as a Ni precursor to obtain Ni / Ba 0.01 Mg 0.99 O x _700°C, 1 hour reduction (Example 35). The metal support (Example 39) and the metal supports of Examples 1 and 22 were subjected to ammonia synthesis at 1.0 MPa and various temperatures (300°C, 350°C, 400°C, 450°C), and the ammonia synthesis activity was measured by the above method. The results are shown in the following table.

[0413]

Table 22

[0414]

[0415] In addition, the results Fig.32 As shown in FIG. 1 , it can be seen that the Ni-supported catalyst has a higher ammonia synthesis activity at 450° C. than the Fe-supported catalyst.

[0416] 22. Ni instead of Co (Discussion of Reaction Pressure 2) (Example 40)

[0417] Ammonia synthesis was carried out on the metal supports of Example 1, Example 22 and Example 40 under the condition of 3.0 MPa, and the ammonia synthesis activity was measured by the above-mentioned method. The results are shown in the following table.

[0418]

Table 23

[0419]

[0420] In addition, the results Fig.33 As shown in the figure, the Ni-supported catalyst and the Fe-supported catalyst also showed quite high activity at 3 MPa. Among them, it can be observed that the Ni-supported catalyst was slightly affected by poisoning.

[0421] 23. Reduction degree of Co

[0422] In order to compare the effect of hydrogen reduction treatment on the reduction state of Co in the catalyst, the Co / BaMgO x The X-ray absorption near edge structure (XANES) spectrum of the CoK absorption end was measured.

[0423] The catalyst before reduction treatment and the standard sample as a comparison object were configured as follows for XANES spectrum measurement. The catalyst before reduction treatment and the standard sample were ground and mixed with boron nitride powder in the atmosphere, and the mixed powder was pressed into a disk with a diameter of 10 mm. At this time, the ratio of each catalyst and standard sample to boron nitride and the thickness of the disk were appropriately adjusted so that the concentration of Co in the measurement object was the most suitable for the absorbance of the X-ray transmitted during the spectrum measurement.

[0424] The catalyst after reduction treatment was configured with a sample for XANES spectrum measurement according to the following method. The catalyst was filled in a sample tube and connected to a fixed bed flow-type reactor, and heated at a predetermined temperature for 1 hour while circulating hydrogen gas, thereby performing reduction treatment. The catalyst after reduction treatment was placed to cool to room temperature while supplying an inert gas (Ar) to the sample tube. The sample tube of the reactor was equipped with cocks at the gas inlet and outlet sides, and the cocks were closed after being placed to cool, so that the catalyst could be kept from contacting the atmosphere even if it was taken out of the reactor. The catalyst reduced using the sample tube was transferred to a glove box filled with inert gas, and the reduced catalyst was ground and mixed with boron nitride powder in the glove box, and the mixed powder was pressed into a disk with a diameter of 10 mm. At this time, the ratio of each catalyst to boron nitride and the thickness of the disk were appropriately adjusted so that the concentration of Co in the measurement object was the most suitable for the absorbance of X-rays transmitted during spectrum measurement.

[0425] The formed disk was triple-sealed in an oxygen-blocking resin bag in a glove box, so that even if the resin bag was taken out of the glove box and exposed to the atmosphere, the spectrum could be measured without the catalyst being affected by reoxidation of oxygen.

[0426] The XANES spectra of each sample prepared for measurement were measured using BL01B1 of the large-scale radiation light facility (SPirng-8). The spectra measured using the transmission method using an ion chamber as a detector were analyzed using X-ray absorption spectrometry analysis software (Athena, Demeter 0.9.26).

[0427] Fig.36 In the figure, the XANES spectra of the standardized catalyst and the standard sample are shown. By comparing the spectral shapes of the unreduced catalyst and the standard sample, it is found that the energy position and shape of the XANES spectrum of the unreduced catalyst are very consistent with those of the oxide (II) (CoO) when Ba is contained and when it is not contained. Therefore, this indicates that Co exists in the form of CoO in the unreduced catalyst. In addition, by performing the reduction treatment, the shape of the XANES spectrum is close to the spectral shape of Co foil. This means that the Co in the catalyst changes to a metallic state by the reduction treatment.

[0428] Therefore, the standardized XANES spectra of each catalyst after reduction treatment were linearly combined and fitted based on the spectra of the standard sample metal Co foil and Co oxide (II) to find the ratio of metallic Co contained in the catalyst (reduction degree). x catalyst:

[0429] The Co reduction degree after reduction at 500℃ for 1 hour is 71%.

[0430] After reduction at 700°C for 1 hour (catalyst of Example 1), the degree of Co reduction was 93%.

[0431] It is clear that as the reduction treatment temperature increases, the ratio of Co oxides inactive in ammonia synthesis decreases, while the ratio of metallic Co active in ammonia synthesis increases.

Claims

1. A metal support, comprising metal particles M of a transition metal supported on a composite oxide formed of an oxide of a metal element L and an oxide of a metal element N, It is characterized in that The composite oxide is represented by the following general formula (1) and satisfies the following (a) to (d): L n N 1-n (1) (a) The metal element L is an oxide of an element selected from any one of the following (i) to (iii): (i) Group I elements, (ii) Group II elements, (iii) Group I elements and Group II elements; (b) the metal element N consists of Group I or Group II elements other than the metal element L; (c) n is greater than 0.001 and less than 0.300; (d) the oxide of the metal element L and the oxide of the metal element N do not form a solid solution, but the oxide particles of the metal element L are deposited on the surface of the oxide particles of the metal element N, and The transition metal is one or more selected from the group consisting of Ru, Fe, Co, Ni, Rh, Pd, Os, Ir, and Pt, The metal particles M are supported on the oxide of the metal element L deposited on the surface of the oxide of the metal element N, and the oxide particles of the metal element L are deposited on the surface of the metal particles M.

2. The metal support according to claim 1, It is characterized in that (a) the metal element represented by the metal element L is a strong alkaline element having a partial negative charge value of oxygen in an oxide state of not less than 0.56 and not more than 0.70, (b) The metal element represented by the metal element N is a weakly basic element in which the value of the partial negative charge of oxygen in the state of an oxide is 0.35 or more and 0.55 or less.

3. The metal support according to claim 1, It is characterized in that The composite oxide is a binary composite oxide composed of the metal element A included in the metal element L and the metal element B included in the metal element N. The general formula (1) is represented by the composition of the following general formula (2), and satisfies the following (a) to (d): A n B 1-n (2) (a) the metal element A is a Group II element which is a strong alkaline element and has a partial negative charge value of oxygen in an oxide state of not less than 0.56 and not more than 0.70; (b) the metal element B is a Group II element which is a weakly basic element and has a partial negative charge value of oxygen in an oxide state of not less than 0.35 and not more than 0.55; (c) n is greater than 0.001 and less than 0.300; and (d) The oxide of the metal element A and the oxide of the metal element B do not form a solid solution, but the oxide particles of the metal element A are deposited on the surfaces of the oxide particles of the metal element B.

4. A metal support, comprising metal particles M of a transition metal supported on a composite oxide formed of an oxide of a metal element L and an oxide of a metal element N, It is characterized in that The composite oxide is represented by the following general formula (3) and satisfies the following (a) to (d): L n N 1-n O x (3) (a) The metal element L is an oxide of an element selected from any one of the following (i) to (iii): (i) Group I elements, (ii) Group II elements, (iii) Group I elements and Group II elements; (b) the metal element N is composed of a Group I element or a Group II element other than the metal element L; (c) n is greater than 0.001 and less than 0.300; and (d) the oxide of the metal element L and the oxide of the metal element N do not form a solid solution, but the oxide particles of the metal element L are deposited on the surface of the oxide particles of the metal element N, and The transition metal is one or more selected from the group consisting of Ru, Fe, Co, Ni, Rh, Pd, Os, Ir, and Pt, The metal particles M are supported on the oxide of the metal element L deposited on the surface of the oxide of the metal element N, and the oxide particles of the metal element L are deposited on the surface of the metal particles M.

5. The metal support according to claim 4, It is characterized in that (a) the metal element L is a metal element which is a strong alkaline element and has a partial negative charge value of oxygen in an oxide state of not less than 0.56 and not more than 0.70, (b) The metal element N is a metal element that is a weakly basic element and in which the value of the partial negative charge of oxygen in the state of an oxide is 0.35 or more and 0.55 or less.

6. The metal support according to claim 4, It is characterized in that The composite oxide is a binary composite oxide composed of the metal element A included in the metal element L and the metal element B included in the metal element N. The general formula (3) is represented by the composition of the following general formula (4), and satisfies the following (a) to (d): A n B 1-n O x (4) (a) the metal element A is a Group II element which is a strong alkaline element and has a partial negative charge value of oxygen in an oxide state of 0.56 or more and 0.70 or less; (b) the metal element B is a Group II element which is a weakly basic element and has a negative partial charge value of oxygen in an oxide state of 0.35 or more and 0.55 or less; (c) said n is not less than 0.001 and not more than 0.300; (d) the oxide of the metal element A and the oxide of the metal element B do not form a solid solution, but the oxide particles of the metal element A are deposited on the surface of the oxide particles of the metal element B; and (e) The above x represents the number of oxygen atoms required for the composite oxide to maintain electrical neutrality.

7. The metal support according to claim 1 or 4, in, The composite oxide is Ba n Mg 1-n O x , where 0.001≤n≤0.

300.

8. The metal support according to claim 7, in, The composite oxide is Ba n Mg 1-n O x , where 0.01≤n≤0.

10.

9. The metal support according to claim 7, in, The amount of carbonate contained in the composite oxide is 10 mol % or less based on Ba.

10. The metal support according to claim 1, It is characterized in that The metal particles M are at least one selected from the group consisting of cobalt, iron, nickel, and ruthenium.

11. The metal support according to claim 1, It is characterized in that The metal element L is distributed on the metal particles M, between the metal particles M and the metal oxide N, and on the metal oxide N.

12. The metal support according to claim 10, It is characterized in that The metal particles M are cobalt particles.

13. A catalyst for ammonia synthesis, It is characterized in that The metal support according to claim 1 is used.

14. A method for manufacturing a metal support as claimed in claim 1, It is characterized in that The method comprises the following steps (a) to (e): (a) an impregnation step of impregnating an L precursor containing the metal element L on an N precursor containing the metal element N to obtain a mixture; (b) a composite oxide calcining step of calcining the mixture at a temperature of 500° C. or higher to obtain a carrier composed of a composite oxide; (c) a loading step of impregnating the composite oxide with a precursor of a compound containing the metal particles M to obtain an impregnated carrier; (d) a support firing step of firing the impregnated support at a temperature of 400° C. or higher; and (e) A reduction step of calcining the metal support obtained in the above (d) at 500° C. or higher in the presence of hydrogen.

15. A method for producing ammonia, comprising bringing hydrogen and nitrogen into contact with a catalyst. It is characterized in that The catalyst is the catalyst for ammonia synthesis according to claim 13.

Citation Information

Patent Citations

  • Ammonia synthesis catalyst and method for producing same

    WO2016133213A1

  • Composite oxide, metal-supporting material and ammonia synthesis catalyst

    WO2019059190A1

  • Biomorphic-composite-oxide loaded ruthenium catalyst for ammonia synthesis and preparation method thereof

    CN104289217A

  • Supported-metal article, supported metal catalyst, and ammonia synthesizing method in which said catalyst is used

    CN108348902A

  • Transition-metal-supporting intermetallic compound, supported metallic catalyst, and ammonia producing method

    CN108472632A