Method for manufacturing semiconductor device
By using multiple masks on the semiconductor substrate for conductivity-type impurity ion implantation, the base layer and contact layer of a multi-layer structure are formed, and the problems of large number of masks and fluctuations in the distribution of impurity layers are solved, and the performance of the semiconductor device is improved. Reliability reduces manufacturing costs.
Patent Information
- Application Number
- CN202210268777.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-03-25
- Filing Date
- 2022-03-18
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-03-18
AI Technical Summary
When manufacturing trench gate type IGBT and other semiconductor devices, there are problems such as large number of masks and fluctuations in the distribution of impurity layers, resulting in high manufacturing costs and unstable performance.
By using a plurality of masks on the main surface of the semiconductor substrate for conductivity-type impurity ion implantation, a base layer and a contact layer of a multi-layer structure are formed, thereby reducing the number of masks and stabilizing the distribution of impurity layers, and reducing manufacturing costs.
The number of masks required to form impurity layers is effectively reduced, the fluctuations in the distribution of impurity layers are reduced, the performance and reliability of semiconductor devices are improved, and the manufacturing cost is reduced.
Smart Images

Figure CN115132575B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a semiconductor device. Background Art
[0002] From the perspective of energy saving, IGBTs and diodes are used in power modules for variable speed control of three-phase motors in general-purpose inverters and AC servo mechanisms. In order to reduce inverter losses, IGBTs and diodes are required to have low switching losses and low on-voltage.
[0003] As a device with low switching loss, there is a trench gate IGBT. The N-channel trench gate IGBT has three impurity layers, namely a P-type base layer, an N-type emitter layer, and a P-type contact layer. Since each of these three impurity layers is formed using a different mask, there is a problem of high manufacturing cost. This problem is not limited to the trench gate IGBT, but also occurs in other semiconductor devices having a trench MOS gate structure.
[0004] To address this problem, Patent Document 1 proposes a method of forming an N-type emitter layer by using oblique implantation after forming a trench gate to allow N-type impurity ions to enter a P-type contact layer (paragraph 0064).
[0005] Patent Document 1: Japanese Patent Application Publication No. 2016-046445
[0006] According to the manufacturing method proposed in Patent Document 1, since the impurity layer is formed by using tilted implantation after forming the trench gate, there is a problem that the distribution of the impurity layer fluctuates due to the influence of the step on the surface of the semiconductor substrate. Summary of the invention
[0007] The present invention is proposed to solve the above-mentioned problems, and its object is to reduce the number of masks used to form an impurity layer and reduce the fluctuation of the distribution of the impurity layer in a semiconductor device having a trench-type MOS gate structure.
[0008] In a first method for manufacturing a semiconductor device of the present invention, the semiconductor device is divided into an active region, a boundary region surrounding the active region, and an edge region surrounding the boundary region when viewed from above, and the method for manufacturing a semiconductor device comprises the following steps: step (a), forming a first mask on a first main surface of a semiconductor substrate having a drift layer of a first conductive type; step (b), injecting second conductive type impurity ions into the first main surface of the semiconductor substrate by using the first mask, thereby forming a second conductive type base layer on the first main surface side of at least a portion of the drift layer in the active region; step (c), injecting the first conductive type impurity ions into the first main surface of the semiconductor substrate by using the first mask, thereby forming a second conductive type base layer on the first main surface side of at least a portion of the drift layer in the active region; and step (c), injecting the first conductive type impurity ions into the semiconductor substrate by using the first mask. The first main surface of the conductor substrate is injected to form an impurity layer of the first conductivity type on the first main surface side of the base layer; step (d), after steps (b) and (c), a trench is formed from the first main surface of the semiconductor substrate to the drift layer; step (e), a gate electrode is buried in the interior of the trench through an insulating film; step (f), a second mask having a pattern different from the first mask is formed on the first main surface of the semiconductor substrate; and step (g), by using the second mask, second conductivity type impurity ions having a higher dose than the first conductivity type impurity ions injected in step (c) are injected into the first main surface of the semiconductor substrate, thereby converting a portion of the impurity layer into a first contact layer of the second conductivity type.
[0009] In the manufacturing method of the second semiconductor device of the present invention, the semiconductor device is divided into an active area, a boundary area surrounding the active area, and an edge area surrounding the boundary area when viewed from above, and the manufacturing method of the semiconductor device has the following steps: step (a), forming a first mask on the first main surface of a semiconductor substrate having a drift layer of the first conductive type; step (b), using the first mask to inject second conductive type impurity ions into the first main surface of the semiconductor substrate, thereby forming a second conductive type base layer on the first main surface side of the drift layer at the active area; step (c), using the first mask to inject the second conductive type impurity ions into the semiconductor base; and step (d), injecting the second conductive type impurity ions into the first main surface of the semiconductor substrate. The first main surface of the semiconductor substrate is injected into the first main surface of the base layer, thereby forming a contact layer of the second conductivity type on the first main surface side of the base layer; a step (d), after the steps (b) and (c), forming a trench reaching the drift layer from the first main surface of the semiconductor substrate; a step (e), burying the gate electrode in the interior of the trench via an insulating film; a step (f), forming a second mask having a pattern different from the first mask on the first main surface of the semiconductor substrate; and a step (g), by using the second mask, injecting first conductivity type impurity ions having a higher dose than the second conductivity type impurity ions injected in the step (c) into the first main surface of the semiconductor substrate, thereby converting a portion of the contact layer into an impurity layer of the first conductivity type.
[0010] Effects of the Invention
[0011] According to the method for manufacturing a semiconductor device of the present invention, for a semiconductor device having a trench-type MOS gate structure, the number of masks for forming an impurity layer can be reduced, and the variation in the distribution of the impurity layer can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 It is a top view of the IGBT according to the first embodiment.
[0013] Figure 2 yes Figure 1 An enlarged top view of the IGBT of the first embodiment at a region P.
[0014] Figure 3 is along Figure 2 A cross-sectional view of the IGBT according to the first embodiment taken along line AA.
[0015] Figure 4 is along Figure 2 FIG. 2 is a cross-sectional view of the IGBT according to the first embodiment taken along line BB.
[0016] Figure 5 This is a flowchart showing the manufacturing process of the IGBT according to the first embodiment.
[0017] Figure 6 It is a plan view showing the manufacturing process of the IGBT according to the first embodiment.
[0018] Figure 7 It is a plan view showing the manufacturing process of the IGBT according to the first embodiment.
[0019] Figure 8 It is a plan view showing the manufacturing process of the IGBT according to the first embodiment.
[0020] Fig. 9 It is a cross-sectional view of an IGBT of a comparative example.
[0021] Fig.10 is along Figure 2 BB line is a cross-sectional view of an IGBT according to a modified example of the first embodiment.
[0022] Fig.11 is with Figure 4 This is a cross-sectional view of an IGBT according to the corresponding second embodiment.
[0023] Fig.12 This is a cross-sectional view of an IGBT showing a problem when the first contact layer is shallower than the emitter layer.
[0024] Fig.13 is with Figure 2 This is an enlarged plan view of the IGBT according to the corresponding third embodiment.
[0025] Fig.14is along Fig.13 A cross-sectional view of the IGBT according to Embodiment 3 along the C-C line.
[0026] Fig.15 is corresponding to Figure 2 An enlarged top view of the IGBT according to Embodiment 4.
[0027] Fig.16 is along Fig.14 A cross-sectional view of the IGBT according to Embodiment 4 along the B-B line.
[0028] Fig.17 is a flowchart showing the manufacturing process of the IGBT according to Embodiment 4.
[0029] Fig.18 is a top view showing the manufacturing process of the IGBT according to Embodiment 4.
[0030] Fig.19 is a top view showing the manufacturing process of the IGBT according to Embodiment 4.
[0031] Fig. 20 is a top view showing the manufacturing process of the IGBT according to Embodiment 4. Detailed Embodiment
[0032] Next, each embodiment will be described with reference to the attached Figure 1 drawings. Since the drawings are only schematically shown, the dimensional and positional relationships of the structures shown in different drawings are not necessarily accurate and can be appropriately changed. In each drawing, the same reference numerals are assigned to the same structural elements, and their names and functions are the same. Therefore, the detailed description of them is sometimes omitted.
[0033] In the following description, the first conductivity type is set to n-type and the second conductivity type is set to p-type for description. n + type means that the concentration of n-type impurities is higher than that of n-type, and p + type means that the concentration of p-type impurities is higher than that of p-type.
[0034] In addition, in the following description, terms such as "upper", "lower", "side", "bottom", "front", or "back" indicating specific positions and directions are sometimes used. However, these terms are only used for convenience in understanding the content of the embodiments and do not limit the direction during actual implementation.
[0035] <A. Embodiment 1>
[0036] <A-1. Structure>
[0037] Figure 1 is a top view of the semiconductor device, i.e., the IGBT 101, according to Embodiment 1. Figure 2 The IGBT 101 Figure 1 The area P is shown in an enlarged top view. Figure 3 is along Figure 2 FIG. 2 is a cross-sectional view of the IGBT 101 taken along line AA. Figure 4 is along Figure 2 FIG. 1 is a cross-sectional view of the IGBT 101 taken along line BB.
[0038] First, the planar structure of IGBT 101 is described. Figure 1 As shown, the IGBT 101 has an active region 10, a boundary region 50, and an edge region 30. That is, the IGBT 101 is divided into the active region 10, the boundary region 50, and the edge region 30 when viewed from above. The boundary region 50 surrounds the active region 10 when viewed from above. The edge region 30 surrounds the boundary region 50 when viewed from above. When viewed from above, a pad region 40 including a pad 41 may also be provided between the boundary region 50 and the edge region 30.
[0039] Next, refer to Figure 4 , a cross-sectional structure of the IGBT 101 common to the active region 10, the boundary region 50, and the edge region 30 is described. The IGBT 101 has a semiconductor substrate 8. The semiconductor substrate 8 has a first main surface S1 and a second main surface S2 opposite to the first main surface S1. The semiconductor substrate 8 is configured to have an n-type drift layer 1, an n-type buffer layer 3, and a p-type collector layer 16.
[0040] The buffer layer 3 is formed on the second main surface S2 side of the drift layer 1. The collector layer 16 is formed on the second main surface S2 side of the buffer layer 3. The lower surface of the collector layer 16 constitutes the second main surface S2. A collector electrode 7 is provided on the second main surface S2 of the semiconductor substrate 8.
[0041] Next, refer to Figures 2 to 4 , the cross-sectional structure of the IGBT 101 unique to the active region 10 is described. The active region 10 includes an n-type carrier storage layer 2, a p-type base layer 15, an n-type emitter layer 13, a p-type first contact layer 14a, an active trench gate 11, an interlayer insulating film 4, and an emitter electrode 6.
[0042] The carrier storage layer 2 is formed on the first main surface S1 side of the drift layer 1. The base layer 15 is formed on the first main surface S1 side of the carrier storage layer 2. The emitter layer 13 and the first contact layer 14a are formed on the first main surface S1 side of the base layer 15. The upper surfaces of the emitter layer 13 and the first contact layer 14a constitute the first main surface S1. The emitter layer 13 is an impurity layer, and is a source layer when the semiconductor device is a MOSFET.
[0043] like Figure 2 and Figure 3 As shown, a trench 11c is formed in the active region 10, which penetrates the emitter layer 13 or the first contact layer 14a, the base layer 15 and the carrier accumulation layer 2 from the first main surface S1 to reach the drift layer 1. A gate insulating film 11b is formed on the inner wall of the trench 11c, and a gate electrode 11a is buried in the trench 11c via the gate insulating film 11b. The gate electrode 11a and the gate insulating film 11b are collectively referred to as an active trench gate 11. In addition, a dummy trench gate 12 composed of a dummy trench electrode 12a and a dummy trench insulating film 12b may be formed in the active region 10. That is, a trench 12c is formed in the active region 10, which penetrates the emitter layer 13 or the first contact layer 14a, the base layer 15 and the carrier accumulation layer 2 from the first main surface S1 to reach the drift layer 1. Furthermore, a dummy trench insulating film 12 b is formed on the inner wall of the trench 12 c , and further, a dummy trench electrode 12 a is buried in the trench 12 c via the dummy trench insulating film 12 b .
[0044] like Figure 3 and Figure 4 As shown, a barrier metal 5 may be provided between the emitter electrode 6 and the interlayer insulating film 4, the emitter layer 13, the first contact layer 14a, the second contact layer 14b and the well layer 31. The emitter electrode 6 is made of a metal such as Al or AlSi. The barrier metal 5 is made of a metal such as Ti, TiN or TiSi, and may also include a plug made of W or the like.
[0045] like Figure 3 As shown, the emitter electrode 6 is formed on the upper portion of the gate electrode 11a via the interlayer insulating film 4. The emitter layer 13 and the first contact layer 14a are connected to the emitter electrode 6 via a contact hole.
[0046] Next, refer to Figure 2 and Figure 4 , the cross-sectional structure of the IGBT 101 unique to the edge region 30 and the boundary region 50 is described. In the edge region 30 and the boundary region 50, a p-type well layer 31 is formed on the first main surface S1 side of the drift layer 1. In the boundary region 50, a p-type second contact layer 14b is formed on the first main surface S1 side of the well layer 31. The second contact layer 14b is continuous with the first contact layer 14a of the active region 10. In the edge region 30, the upper surface of the well layer 31 constitutes the first main surface S1, and in the boundary region 50, the upper surface of the second contact layer 14b constitutes the first main surface S1.
[0047] The n-type impurity concentration of the second contact layer 14b is the same as the n-type impurity concentration of the drift layer 1. On the other hand, the n-type impurity concentration of the first contact layer 14a is greater than or equal to the n-type impurity concentration of the drift layer 1. Moreover, the net impurity concentration of the first contact layer 14a is lower than the net impurity concentration of the second contact layer 14b. The net impurity concentration means, in an n-type region, the concentration obtained by subtracting the p-type impurity concentration from the n-type impurity concentration of the region, and in a p-type region, the concentration obtained by subtracting the n-type impurity concentration from the p-type impurity concentration of the region.
[0048] <A-2. Manufacturing process>
[0049] Figure 5 is a flowchart showing the manufacturing method of the IGBT 101 of Embodiment 1. Figures 6 to 8 is a top view showing the state during the manufacturing of the IGBT 101. Next, with reference to Figures 5 to 8 the manufacturing method of the IGBT 101 will be described. In addition, the manufacturing method of the IGBT 101 described below is also applicable to the IGBT 103 of Embodiment 2 described later.
[0050] First, in step S101, an n-type semiconductor substrate is prepared. This semiconductor substrate has a first main surface S1 and a second main surface S2, and Figure 3 and Figure 4 is equivalent to the semiconductor substrate 8 shown, but at this stage only includes the drift layer 1, and does not yet include the carrier accumulation layer 2, the buffer layer 3, the collector layer 16, the base layer 15, the first contact layer 14a, and the emitter layer 13.
[0051] Next, in step S102, a p-type well layer 31 is formed on the first main surface S1 side of the outer peripheral portion of the semiconductor substrate. When viewed from above, the region of the semiconductor substrate where the well layer 31 is formed is the edge region 30 and the boundary region 50, and the region where the well layer 31 is not formed is the active region 10.
[0052] After that, in step S103, a first mask is formed on the first main surface S1 of the semiconductor substrate. The first mask covers the edge region 30 and the boundary region 50 and has openings in the entire active region 10.
[0053] Next, in step S104, n-type impurity ions are implanted into the active region 10 using the first mask to form the carrier accumulation layer 2. Next, in step S105, p-type impurity ions are implanted into the active region 10 using the first mask to form the base layer 15 on the carrier accumulation layer 2. Next, in step S106, n-type impurity ions are implanted into the active region 10 using the first mask to form the emitter layer 13 on the base layer 15. Thus, Figure 6In addition, as for each ion implantation in steps S104 to S106 , in addition to the active region 10 , the ion implantation can also be performed on the boundary region 50 .
[0054] Next, in step S107, an active trench gate 11 and a dummy trench gate 12 are formed in the boundary region 50 and the active region 10, and a Figure 7 The planar structure shown.
[0055] Then, in step S108, Figure 8 As shown, a second mask 61 is formed. The second mask 61 has a pattern different from that of the first mask, and has openings in the boundary region 50 and a part of the active region 10 .
[0056] Next, in step S109, p-type impurity ions are injected into a portion of the active region 10 and the boundary region 50 using the second mask 61. Here, the amount of ion injection per unit area is referred to as a dose. The dose of p-type impurity ions in this step is greater than the dose of n-type impurity ions injected in step S106 to form the emitter layer 13. Therefore, the conductivity type of the region in the emitter layer 13 into which the p-type impurity ions are injected in this step is changed to p-type, and becomes the first contact layer 14a. The region in the emitter layer 13 covered by the second mask 61 and into which the p-type impurity ions are not injected in this step remains in its original state as the emitter layer 13. In this way, Figure 2 The planar structure shown.
[0057] As described above, after the emitter layer 13 is formed using the first mask for forming the carrier storage layer 2 and the base layer 15 , the mask for forming the emitter layer 13 can be reduced by converting a portion of the emitter layer 13 into the first contact layer 14 a .
[0058] In addition, in step S109, the second contact layer 14b is formed on the first main surface S1 side of the well layer 31 by injecting p-type impurity ions into the boundary region 50. Since the second contact layer 14b is formed by injecting p-type impurity ions into the p-type well layer 31, the net impurity concentration is higher than that of the first contact layer 14a. By forming the second contact layer 14b in the boundary region 50, the formation of the emitter layer 13 in the edge region 30 due to manufacturing fluctuations is suppressed, and the breakdown tolerance is improved. In addition, in this step, ion implantation may not be performed in the boundary region 50.
[0059] Next, in step S110 , the interlayer insulating film 4 is formed on the first main surface S1 of the semiconductor substrate, and further, a contact hole is formed.
[0060] Thereafter, in step S111, the barrier metal 5 and the emitter electrode 6 are formed. In addition, the structures on the second main surface S2 side of the semiconductor substrate, that is, the buffer layer 3, the collector layer 16, and the collector electrode 7, are appropriately formed.
[0061] Ion implantation is performed in steps S104 - S106 and step S109. The activation annealing for activating the implanted ions can be performed each time after each ion implantation process, or can be concentrated after all ion implantation processes are completed. In addition, in step S107, the active trench gate 11 and the dummy trench gate 12 are formed, but the heat treatment when forming the gate insulating film 11b and the dummy trench insulating film 12b can also be used as the activation annealing for the ions implanted before that. In this case, the manufacturing cost can be reduced.
[0062] The formation of the first mask and the ion implantation using the first mask described in steps S103 to S106 can also be performed before the formation of the well layer 31 described in step S102. In addition, the formation of the second mask 61 and the ion implantation using the second mask 61 described in steps S108 and S109 can also be performed before the formation of the active trench gate 11 and the dummy trench gate 12 described in step S107. The active trench gate 11 and the dummy trench gate 12 are collectively referred to as the trench gate.
[0063] By forming the trench gate in step S107, a step is generated on the first main surface S1 of the semiconductor substrate 8. However, according to the above manufacturing method, in steps S104 - S106 before forming the trench gate, ion implantation is performed on the flat first main surface S1 of the semiconductor substrate 8, and the base layer 15, the carrier accumulation layer 2, and the emitter layer 13 can be formed. Therefore, the fluctuation of the impurity distribution due to the step on the surface of the semiconductor substrate 8 is suppressed.
[0064] In the above manufacturing method, the base layer 15 and the emitter layer 13 are formed by ion implantation using the same first mask. Therefore, the heat treatment performed after each ion implantation is the same. Therefore, if the diffusion coefficient of the p-type impurity constituting the base layer 15 in the semiconductor substrate 8 is smaller than the diffusion coefficient of the n-type impurity constituting the emitter layer 13 in the semiconductor substrate 8, then as Fig. 9 shown, the entire base layer 15 becomes the emitter layer 13, and the IGBT operation does not occur. Therefore, the diffusion coefficient of the p-type impurity constituting the base layer 15 in the semiconductor substrate 8 must be larger than the diffusion coefficient of the n-type impurity constituting the emitter layer 13 in the semiconductor substrate 8.
[0065] <A-3. Modification Example>
[0066] Fig.10 is along Figure 2Cross-sectional view of the IGBT 101A which is a modification of Embodiment 1 of the B-B line. The other cross-sectional structure and planar structure of the IGBT 101A are the same as those of the IGBT 101 in Embodiment 1. For the IGBT 101A, the first contact layer 14a is formed not only in the active region 10 but also in a part of the boundary region 50. Such a structure is achieved by making the opening of the first mask used for ion implantation when forming the carrier accumulation layer 2, the base layer 15, and the emitter layer 13 include not only the whole of the active region 10 but also a part of the boundary region 50. That is, as Fig.10 shown, the end EC of the region where n-type impurity ions constituting the carrier accumulation layer 2 are implanted and the end EB of the region where p-type impurity ions constituting the base layer 15 are implanted are both located in the boundary region 50 and overlap with the well layer 31. As described above, by overlapping the well layer 31 with the base layer 15, the breakdown voltage reduction due to the separation of the well layer 31 and the base layer 15 caused by manufacturing variations is suppressed.
[0067] <A-4. Effect>
[0068] The manufacturing method of the semiconductor device of Embodiment 1 has the following steps: Step (a), forming a first mask on the first main surface S1 of the semiconductor substrate 8 having the drift layer 1 of the first conductivity type; Step (b), by using the first mask, implanting second conductivity type impurity ions into the first main surface S1 of the semiconductor substrate 8, thereby forming a second conductivity type base layer 15 on the first main surface S1 side of at least a part of the drift layer 1 in the active region; Step (c), by using the first mask, implanting first conductivity type impurity ions into the first main surface S1 of the semiconductor substrate 8, thereby forming a first conductivity type impurity layer on the first main surface S1 side of the base layer 15; Step (d), after Steps (b) and (c), forming a trench 11c reaching the drift layer 1 from the first main surface S1 of the semiconductor substrate 8; Step (e), burying a gate electrode 11a in the trench 11c隔着栅极绝缘膜11b; Step (f), forming a second mask having a pattern different from that of the first mask on the first main surface S1 of the semiconductor substrate 8; and Step (g), by using the second mask, implanting second conductivity type impurity ions having a higher dose ratio than the first conductivity type impurity ions implanted in Step (c) into the first main surface S1 of the semiconductor substrate 8, thereby converting a part of the impurity layer into a second conductivity type first contact layer 14a. Thereby, the mask for forming the emitter layer 13 can be reduced. In addition, since ion implantation is performed on the flat first main surface S1 of the semiconductor substrate 8 before forming the trench gate to form the base layer 15, the carrier accumulation layer 2, and the emitter layer 13, the fluctuation of the impurity distribution caused by the step on the surface of the semiconductor substrate 8 is suppressed.
[0069] The manufacturing method of the semiconductor device of Embodiment 1 has: Step (h) of forming a well layer 31 of the second conductivity type in the boundary region 50 and the edge region 30 on the semiconductor substrate 8. Step (g) may also be a step of forming a second contact layer 14b of the second conductivity type on the first main surface S1 side of the well layer 31 in the boundary region 50 while converting a part of the impurity layer into the first contact layer 14a. Moreover, the net impurity concentration of the second contact layer 14b is higher than that of the first contact layer 14a. By forming the second contact layer 14b in the boundary region 50, the formation of the emitter layer 13 in the edge region 30 due to manufacturing fluctuations is suppressed, and the breakdown tolerance is improved.
[0070] <B. Embodiment 2>
[0071] <B-1. Structure>
[0072] Fig.11 is a cross-sectional view of the IGBT 102 of Embodiment 2 along the B-B line Figure 2 The other cross-sectional structure and planar structure of the IGBT 102 are the same as those of the IGBT 101 of Embodiment 1.
[0073] For the IGBT 102, the width Wi of the boundary region 50 is larger than the depth De of the emitter layer 13. In addition, for the IGBT 102, the depth Dh of the first contact layer 14a and the second contact layer 14b is deeper than the depth De of the emitter layer 13.
[0074] <B-2. Effect>
[0075] For the IGBT 102 of Embodiment 2, the width Wi of the boundary region 50 is larger than the depth De of the emitter layer 13. Therefore, even if the n-type impurity ions implanted to form the emitter layer 13 diffuse laterally in the semiconductor substrate 8, they will not reach the edge region 30. As a result, the formation of a parasitic emitter layer on the surface of the edge region 30 is suppressed, and the breakdown tolerance of the IGBT 102 is improved.
[0076] In addition, for the IGBT 102 of Embodiment 2, the depth Dh of the first contact layer 14a is larger than the depth De of the emitter layer 13. As in <a-2>As described above, the first contact layer 14a is formed by implanting p-type impurity ions into the emitter layer 13 to change the conductivity type from n-type to p-type. Therefore, if the depth Dh of the first contact layer 14a and the second contact layer 14b is shallower than the depth De of the emitter layer 13, as Fig.12 shown, the emitter layer 13 remains on the second main surface S2 side of the first contact layer 14a, becoming an n-type parasitic emitter layer 17. In the IGBT 102, with the above structure, the formation of the parasitic emitter layer 17 is suppressed, and the breakdown voltage is increased.
[0077] <C. Embodiment 3>
[0078] <C-1. Structure>
[0079] Fig.13 is Figure 1 an enlarged plan view of the IGBT 102 of Embodiment 2 at the region P. Fig.14 is a cross-sectional view of the IGBT 103 along the Fig.13 C-C line. As Fig.13 and Fig.14 shown, the IGBT 103 has a p-type third contact layer 14c sandwiched by the first contact layer 14a on both sides in the active region 10, and is otherwise the same as the IGBT 101.
[0080] The third contact layer 14c does not contain n-type impurities with a concentration greater than or equal to the n-type impurity concentration of the drift layer 1. The net impurity concentration of the third contact layer 14c is higher than the net impurity concentration of the first contact layer 14a. In Fig.14 , the base layer 15 and the carrier accumulation layer 2 directly below the third contact layer 14c are locally shallowed, but may be formed uniformly in the same manner as the IGBT 101 of Embodiment 1.
[0081] The base layer 15 and the carrier accumulation layer 2 directly below the third contact layer 14c are formed by the lateral diffusion of the base layer 15 and the carrier accumulation layer 2 directly below the adjacent first contact layer 14a. Therefore, the depth of the base layer 15 and the carrier accumulation layer 2 directly below the third contact layer 14c can be controlled by the diffusion depth of the base layer 15 and the carrier accumulation layer 2 and the interval of the trench gate, etc.
[0082] <C-2. Manufacturing Process>
[0083] Since the manufacturing process of the IGBT 103 of Embodiment 3 is the same as that in <a-2>The manufacturing process of the IGBT 101 according to the first embodiment described in the foregoing is basically the same, and therefore only the differences will be mainly described below.
[0084] After forming the well layer 31 in the edge region 30 and the boundary region 50 of the semiconductor substrate 8, a first mask is formed on the first main surface S1 of the semiconductor substrate 8. In the first and second embodiments, the first mask has an opening in the entire active region 10. In contrast, in the third embodiment, the first mask covers the formation region of the third contact layer 14c in the active region 10 and has an opening in other regions.
[0085] Next, n-type impurity ions are injected using the first mask to form the carrier accumulation layer 2. Next, p-type impurity ions are injected using the first mask to form the base layer 15 on the carrier accumulation layer 2. Next, n-type impurity ions are injected using the first mask to form the emitter layer 13 on the base layer 15. As described above, since the first mask covers the formation region of the third contact layer 14c, in these ion injection steps, ions are not directly injected into the formation region of the third contact layer 14c and directly below it. However, the injected ions diffuse in the lateral direction of the semiconductor substrate 8, thereby also forming the carrier accumulation layer 2 and the base layer 15 in the formation region of the third contact layer 14c and directly below it. However, with respect to the emitter layer 13, the diffusion depth of the n-type impurity ions is adjusted so that the emitter layer 13 is not formed in the formation region of the third contact layer 14c.
[0086] Next, the first mask is removed and a second mask is formed on the first main surface S1 of the semiconductor substrate 8. The second mask has a pattern different from that of the first mask and has openings in the entire boundary region 50 and a portion of the active region 10. In particular, the openings of the second mask are provided in the region of the active region 10 covered by the first mask.
[0087] Next, p-type impurity ions are implanted using the second mask to form the first contact layer 14a, the second contact layer 14b, and the third contact layer 14c. Specifically, p-type impurity ions are implanted into the region of the active region 10 located at the opening of the first mask and where the emitter layer 13 is formed, to form the first contact layer 14a. In addition, p-type impurity ions are implanted into the well layer 31 of the boundary region 50 to form the second contact layer 14b. In addition, p-type impurity ions are implanted into the region of the active region 10 covered by the first mask and where the emitter layer 13 is not formed, to form the third contact layer 14c. In this way, the first contact layer 14a, the second contact layer 14b, and the third contact layer 14c having different net impurity concentrations are formed through one ion implantation process. The net impurity concentration becomes higher in the order of the second contact layer 14b, the third contact layer 14c, and the first contact layer 14a.
[0088] <C-3. Effect>
[0089] According to the manufacturing method of the IGBT 103 of Embodiment 3, while transforming a part of the impurity layer, i.e., the emitter layer 13, into the first contact layer 14a, a third contact layer 14c of the second conductivity type is formed in the drift layer 1 in contact with the first main surface S1 of the semiconductor substrate 8 in the active region 10. The third contact layer 14c does not contain a first conductivity type impurity having a concentration higher than the first conductivity type impurity concentration of the drift layer 1, and the net impurity concentration of the third contact layer 14c is higher than the net impurity concentration of the first contact layer 14a. The third contact layer 14c has a higher ability to discharge holes when the IGBT 103 is turned off compared to the first contact layer 14a, so the breakdown withstand voltage of the IGBT 103 is improved.
[0090] <D. Embodiment 4>
[0091] <D-1. Structure>
[0092] Fig.15 Yes Figure 1 An enlarged top view of the IGBT 104 of Embodiment 4 at the region P. Fig.16 Is along Fig.15 Cross-sectional view of the IGBT 104 taken along the line B-B. Hereinafter, with reference to Fig.15 And Fig.16 The structure of the IGBT 104 will be described.
[0093] Compared with the IGBT 101, the IGBT 104 has a first well layer 31a, a second well layer 31b, and a third well layer 31c instead of the well layer 31, and has a p-type contact layer 14 instead of the first contact layer 14a and the second contact layer 14b. The first well layer 31a, the second well layer 31b, the third well layer 31c, and the contact layer 14 are all p-type.
[0094] In the active region 10, the contact layer 14 is formed on the first main surface S1 side of the base layer 15.
[0095] In the edge region 30 and the boundary region 50, the first well layer 31a is formed on the first main surface S1 side of the drift layer 1.
[0096] In the boundary region 50, the second well layer 31b is formed on the first main surface S1 side of the first well layer 31a. The third well layer 31c is formed between the second well layer 31b and the first well layer 31a. The contact layer 14 is formed on the first main surface S1 side of the second well layer 31b. The contact layer 14 in the active region 10 and the contact layer 14 in the boundary region 50 are continuous. The net concentration of the second well layer 31b is higher than that of the first well layer 31a. The net concentration of the third well layer 31c is lower than that of the first well layer 31a.
[0097] The emitter layer 13 contains impurities of a second conductivity type with a higher concentration than that of the base layer 15. The net impurity concentration of the emitter layer 13 is lower than the net impurity concentration of the contact layer 14.
[0098] <D-2. Manufacturing Process>
[0099] Fig.17 It is a flowchart showing the manufacturing method of the IGBT 104 according to Embodiment 4. Figures 18 to 20 It is a top view showing the state during the manufacturing of the IGBT 104. Next, with reference to Figures 17 to 20 the manufacturing method of the IGBT 104 will be described.
[0100] First, in step S201, an n-type semiconductor substrate is prepared. This semiconductor substrate has a first main surface S1 and a second main surface S2, corresponding to Fig.16 the semiconductor substrate 8 shown, but at this stage it only contains the drift layer 1 and does not yet contain the carrier accumulation layer 2, the buffer layer 3, the collector layer 16, the base layer 15, the contact layer 14, and the emitter layer 13.
[0101] Next, in step S202, a p-type first well layer 31a is formed on the first main surface S1 side of the outer peripheral portion of the semiconductor substrate. When viewed from above, the region of the semiconductor substrate where the first well layer 31a is formed is the edge region 30 and the boundary region 50, and the region where the first well layer 31a is not formed is the active region 10.
[0102] After that, in step S203, a first mask is formed on the first main surface S1 of the semiconductor substrate. The first mask covers the edge region 30 and has openings in the entire active region 10 and the boundary region 50.
[0103] Next, in step S204, n-type impurity ions are implanted into the active region 10 and the boundary region 50 using the first mask, and a carrier accumulation layer 2 is formed in the active region 10, and a third well layer 31c is formed in the boundary region 50.
[0104] After that, in step S205, p-type impurity ions are implanted into the active region 10 and the boundary region 50 using the first mask, and a base layer 15 is formed on the carrier accumulation layer 2 in the active region 10, and a second well layer 31b is formed on the third well layer 31c in the boundary region 50.
[0105] Next, in step S206, p-type impurity ions are implanted into the active region 10 and the boundary region 50 using the first mask, and a contact layer 14 is formed on the base layer 15 in the active region 10 and on the second well layer 31b in the boundary region 50. Thus, the Fig.18 plane structure shown is obtained.
[0106] Next, in step S207, an active trench gate 11 and a dummy trench gate 12 are formed in the boundary region 50 and the active region 10, and a Fig.19 The structure shown.
[0107] Then, in step S208, Fig. 20 As shown, a second mask 62 is formed. The second mask 62 has a pattern different from that of the first mask and has an opening in a part of the active region 10 .
[0108] Next, in step S209, n-type impurity ions are injected into a portion of the active region 10 using the second mask 62. The dose of n-type impurity ions in this step is greater than the dose of p-type impurity ions injected in step S206 to form the contact layer 14. Therefore, the conductivity type of the region in the contact layer 14 into which n-type impurity ions are injected in this step is changed to n-type, and becomes the emitter layer 13. The region in the contact layer 14 covered by the second mask 62 and into which n-type impurity ions are not injected in this step remains as the contact layer 14. In this way, Fig.15 The planar structure shown.
[0109] As described above, after the contact layer 14 is formed using the first mask for forming the carrier storage layer 2 and the base layer 15 , a portion of the contact layer 14 is converted into the emitter layer 13 , thereby reducing the number of masks for forming the contact layer 14 .
[0110] Next, in step S210 , the interlayer insulating film 4 is formed, and further, contact holes are formed.
[0111] Thereafter, in step S211, the barrier metal 5 and the emitter electrode 6 are formed. In addition, the structures on the second main surface S2 side of the semiconductor substrate, that is, the buffer layer 3, the collector layer 16, and the collector electrode 7 are formed as appropriate.
[0112] Ion implantation is performed in steps S204-S106 and step S209. Activation annealing for activating the implanted ions can be performed after each ion implantation process, or can be performed collectively after all ion implantation processes are completed. In addition, in step S207, the active trench gate 11 and the dummy trench gate 12 are formed, but the heat treatment when forming the gate insulating film 11b and the dummy trench insulating film 12b can also be used as the activation annealing of the previously implanted ions. In this case, the manufacturing cost can be reduced.
[0113] The formation of the first mask and the ion implantation using the first mask, which are described in steps S203 to S206, may also be performed before the formation of the well layer 31 described in step S202. In addition, the formation of the second mask 61 and the ion implantation using the second mask 61, which are described in steps S208 and S209, may also be performed before the formation of the active trench gate 11 and the dummy trench gate 12 described in step S207.
[0114] By forming the trench gate in step S207, a step is generated on the first main surface S1 of the semiconductor substrate 8. However, according to the above manufacturing method, in steps S204 - S206 before forming the trench gate, the first main surface S1 of the semiconductor substrate 8 is ion-implanted, and the base layer 15, the carrier accumulation layer 2, and the contact layer 14 can be formed. Therefore, the fluctuation of the impurity distribution due to the step on the surface of the semiconductor substrate 8 is suppressed.
[0115] <D-3. Effect>
[0116] The manufacturing method of the semiconductor device according to Embodiment 4 has the following steps: step (a), forming a first mask on the first main surface S1 of the semiconductor substrate 8 having the drift layer 1 of the first conductivity type; step (b), injecting second conductivity type impurity ions into the first main surface S1 of the semiconductor substrate 8 by using the first mask, thereby forming a second conductivity type base layer 15 on the first main surface S1 side of the drift layer in the active region (10); step (c), injecting second conductivity type impurity ions into the first main surface S1 of the semiconductor substrate 8 by using the first mask, thereby forming a second conductivity type contact layer 14 on the first main surface S1 side of the base layer 15; step (d), after steps (b) and (c), forming a trench 11c reaching the drift layer 1 from the first main surface S1 of the semiconductor substrate 8; step (e), burying a gate electrode 11a in the trench 11c隔着栅极绝缘膜11b; step (f), forming a second mask 62 having a pattern different from that of the first mask on the first main surface S1 of the semiconductor substrate 8; and step (g), injecting first conductivity type impurity ions having a dose ratio higher than that of the second conductivity type impurity ions injected in step (c) into the first main surface S1 of the semiconductor substrate 8 by using the second mask 62, thereby converting a part of the contact layer 14 into a first conductivity type impurity layer. Therefore, the mask of the contact layer can be reduced.
[0117] In addition, the method for manufacturing a semiconductor device according to the fourth embodiment includes: step (h) of forming a first well layer 31a of the second conductivity type on the semiconductor substrate 8 in the boundary region 50 and the edge region 30, and step (b) may be a step of forming a second well layer 31b of the second conductivity type on the first main surface S1 side of the first well layer 31a in the boundary region 50 while forming the base layer 15. The net impurity concentration of the second well layer 31b is higher than that of the first well layer 31a. In this case, by forming the second well layer 31b in the boundary region 50, the hole discharge capability at the time of cutoff can be improved, thereby improving the breakdown tolerance.
[0118] Furthermore, the various embodiments may be freely combined, and the various embodiments may be appropriately modified or omitted.
[0119] Description of the label
[0120] 1 drift layer, 2 carrier accumulation layer, 3 buffer layer, 4 interlayer insulating film, 5 barrier metal, 6 emitter electrode, 7 collector electrode, 8 semiconductor substrate, 10 active region, 11 active trench gate, 11a gate electrode, 11b gate insulating film, 11c, 12c trenches, 12 dummy trench gate, 12a dummy trench electrode, 13 emitter layer, 14 contact layer, 14a first contact layer, 14b second contact layer, 14c third contact layer, 15 base layer, 16 collector layer, 17 parasitic emitter layer, 30 edge region, 31 well layer, 31a first well layer, 31b second well layer, 31c third well layer, 40 pad region, 41 pad, 50 boundary region, 61, 62 second mask.
Claims
1. A method for manufacturing a semiconductor device, wherein the semiconductor device is divided into an active area, a boundary area surrounding the active area, and an edge area surrounding the boundary area when viewed from above, The method for manufacturing a semiconductor device comprises the following steps: Step (a), forming a first mask on a first main surface of a semiconductor substrate having a drift layer of a first conductivity type; Step (b), implanting second conductivity type impurity ions into the first main surface of the semiconductor substrate using the first mask, thereby forming a second conductivity type base layer on the first main surface side of at least a portion of the drift layer in the active region; (c) forming a first conductivity type impurity layer on the first main surface side of the base layer by implanting first conductivity type impurity ions into the first main surface of the semiconductor substrate using the first mask; Step (d), after the steps (b) and (c), forming a trench extending from the first main surface of the semiconductor substrate to the drift layer; Step (e), burying a gate electrode in the interior of the trench via an insulating film; Step (f), forming a second mask having a pattern different from that of the first mask on the first main surface of the semiconductor substrate; as well as Step (g), by using the second mask to inject second conductive type impurity ions with a higher dose than the first conductive type impurity ions injected in the step (c) into the first main surface of the semiconductor substrate, thereby converting a portion of the impurity layer into a first contact layer of the second conductive type.
2. The method for manufacturing a semiconductor device according to claim 1, wherein: The method further comprises: a step (h) of forming a well layer of a second conductivity type in the semiconductor substrate in the boundary region and the edge region. The step (g) is a step of converting a portion of the impurity layer into the first contact layer and forming a second contact layer of the second conductivity type on the first main surface side of the well layer in the boundary region. The second contact layer has a higher net impurity concentration than the first contact layer.
3. The method for manufacturing a semiconductor device according to claim 1, wherein: The diffusion coefficient of the second conductive type impurity ions implanted in the step (b) in the semiconductor substrate is greater than the diffusion coefficient of the first conductive type impurity ions implanted in the step (c) in the semiconductor substrate.
4. The method for manufacturing a semiconductor device according to any one of claims 1 to 3, wherein: The width of the boundary region is greater than the depth of the impurity layer.
5. The method for manufacturing a semiconductor device according to any one of claims 1 to 4, wherein: The depth of the first contact layer is greater than the depth of the impurity layer.
6. The method for manufacturing a semiconductor device according to any one of claims 1 to 5, wherein: The step (g) is a step of converting a portion of the impurity layer into the first contact layer and forming a third contact layer of the second conductivity type in the drift layer in contact with the first main surface of the semiconductor substrate in the active region. the third contact layer does not contain the first conductivity type impurity having a concentration higher than the first conductivity type impurity concentration of the drift layer, The net impurity concentration of the third contact layer is higher than the net impurity concentration of the first contact layer.
7. A method for manufacturing a semiconductor device, wherein the semiconductor device is divided into an active area, a boundary area surrounding the active area, and an edge area surrounding the boundary area when viewed from above, The method for manufacturing a semiconductor device comprises the following steps: Step (a), forming a first mask on a first main surface of a semiconductor substrate having a drift layer of a first conductivity type; Step (b) of forming a second conductivity type base layer on the first main surface side of the drift layer in the active region by implanting second conductivity type impurity ions into the first main surface of the semiconductor substrate using the first mask; Step (c) of forming a second conductivity type contact layer on the first main surface side of the base layer by injecting second conductivity type impurity ions into the first main surface of the semiconductor substrate using the first mask; Step (d), after the steps (b) and (c), forming a trench extending from the first main surface of the semiconductor substrate to the drift layer; Step (e), burying a gate electrode in the interior of the trench via an insulating film; Step (f), forming a second mask having a pattern different from that of the first mask on the first main surface of the semiconductor substrate; as well as Step (g), by using the second mask to inject the first conductive type impurity ions with a higher dose than the second conductive type impurity ions injected in the step (c) into the first main surface of the semiconductor substrate, thereby converting a portion of the contact layer into an impurity layer of the first conductive type.
8. The method for manufacturing a semiconductor device according to claim 7, wherein: The method further comprises: a step (h) of forming a first well layer of a second conductivity type in the semiconductor substrate in the boundary region and the edge region; The step (b) is a step of forming a second well layer of the second conductivity type on the first main surface side of the first well layer in the boundary region simultaneously with the formation of the base layer. The net impurity concentration of the second well layer is higher than that of the first well layer.