Alumina powder, resin composition and heat dissipation component
Through a specific combination of alumina particles and flame melting technology, the problem of thickening of alumina particles when filled in resin is solved, and the preparation of high thermal conductivity resin compositions and heat dissipation components is achieved.
Patent Information
- Application Number
- CN202180017944.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-03-31
- Filing Date
- 2021-03-24
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-03-24
AI Technical Summary
In the prior art, the high specific surface area and poor shape of alumina particles lead to thickening when filled in resin, making it difficult to realize heat dissipation components with high thermal conductivity.
Using a specific combination of first alumina particles, second alumina particles and third alumina particles, the average particle size and sphericity are determined through laser diffraction scattering particle size distribution measurement and microscopy, combined with flame melting device manufacturing, to control the α crystal phase content, forming an alumina powder that can be filled with resin at a high proportion.
It is possible to suppress the viscosity increase in the resin, improve the thermal conductivity, and prepare a resin composition and heat dissipation component with high thermal conductivity.
Smart Images

Figure CN115210183B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to aluminum oxide powder, a resin composition and a heat dissipation component. Background Art
[0002] In recent years, electrical devices have been miniaturized and have become more advanced in performance. As the size and performance of electrical devices have increased, the density of electronic components included in the electrical devices has increased, and the need to effectively release heat generated by the electronic components has increased.
[0003] In addition, in power device applications such as electric vehicles that can suppress environmental loads, high voltages are sometimes applied to electronic components or large currents flow through them. In this case, high heat is generated, and in order to cope with the high heat generated, it is necessary to release the heat more effectively than before. As a technology for responding to such requirements, for example, a resin composition comprising three types of alumina fillers is disclosed in Patent Document 1. In addition, alumina compounding particles comprising spherical alumina particles and non-spherical alumina particles and a resin composition comprising the particles are disclosed in Patent Document 2.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2009-164093
[0007] Patent Document 2: Japanese Patent Application Publication No. 2009-274929 Summary of the invention
[0008] However, in Patent Documents 1 and 2, there is a problem that the resin becomes thicker when filled with alumina particles, and it is difficult to fill the resin with a large amount of alumina particles because the alumina particles have a high specific surface area and poor shape. Therefore, the moldability is poor, and it is difficult to obtain a heat dissipation component with high thermal conductivity.
[0009] The present invention has been made in view of the above problems, and an object of the present invention is to provide an alumina powder capable of suppressing viscosity increase when filled with a resin and achieving high thermal conductivity of a resin composition containing the resin, as well as a resin composition and a heat dissipation component containing the alumina powder.
[0010] The inventors of the present invention have conducted repeated and in-depth studies to achieve the above-mentioned purpose, and as a result, have found that an alumina powder comprising specific first alumina particles, specific second alumina particles, and specific third alumina particles can suppress the increase in viscosity when filled into a resin, and that by including the alumina powder, a resin composition and a heat dissipation component capable of achieving high thermal conductivity can be obtained, thereby completing the present invention.
[0011] That is, the present invention is as follows.
[0012] [1] An alumina powder comprising first alumina particles having an average particle size of 0.1 μm or more and less than 1 μm, second alumina particles having an average particle size of 1 μm or more and less than 10 μm, and third alumina particles having an average particle size of 10 μm to 100 μm, wherein each of the above average particle sizes is a particle size measured by a laser diffraction scattering particle size distribution measuring machine, the first alumina particles having a projected area circle equivalent diameter of 0.1 μm to 1 μm by a microscope have an average sphericity of 0.80 to 0.98, and the specific surface area of the first alumina particles is 1.9 m 2 / g~20.0m 2 / g, and the content of the α crystal phase is 80 mass % or more.
[0013] [2] The alumina powder according to [1], wherein the content of the α crystal phase in the alumina powder is 60% by mass or more.
[0014] [3] A resin composition comprising a resin and the alumina powder according to [1] or [2].
[0015] [4] The resin composition according to [3], wherein the resin comprises at least one selected from silicone resin, epoxy resin, polyurethane resin and acrylic resin.
[0016] [5] A heat dissipation component comprising the alumina powder described in [1] or [2] or the resin composition described in [3] or [4].
[0017] According to the present invention, it is possible to provide an alumina powder capable of suppressing an increase in viscosity when filled into a resin and achieving high thermal conductivity of a resin composition containing the resin, as well as a resin composition and a heat dissipating component containing the alumina powder. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a schematic diagram showing a flame melting device used when producing the second alumina particles and the third alumina particles according to the present embodiment. DETAILED DESCRIPTION
[0019] Hereinafter, a mode for carrying out the present invention (hereinafter referred to as "this embodiment") will be described in detail. It should be noted that the following this embodiment is an example for explaining the present invention, and the present invention is not limited to this embodiment.
[0020] The alumina powder of the present embodiment includes specific first alumina particles, specific second alumina particles, and specific third alumina particles.
[0021] [Alumina powder]
[0022] (First Alumina Particles and Method for Producing the Same)
[0023] The average particle size of the first alumina particles of this embodiment is 0.1 μm or more and less than 1 μm. By using the first alumina particles, the resin composition can be filled with alumina particles at a high ratio. The first alumina particles preferably have an average particle size of 0.2 μm to 0.9 μm, more preferably 0.3 μm to 0.8 μm.
[0024] In addition, in this embodiment, the average particle size is measured by a laser diffraction scattering particle size distribution analyzer. The specific measurement method is described in the Examples.
[0025] The average sphericity of the first alumina particles of the present embodiment is 0.80 to 0.98. If the alumina powder contains first alumina particles having an average sphericity of 0.80 or more, it is not easy to thicken when the alumina powder is filled in the resin. If the alumina powder contains first alumina particles having an average sphericity of 0.98 or less, the contact between the first alumina particles and other alumina particles becomes more sufficient, and the contact area becomes larger, resulting in a resin composition and a heat dissipation component with higher thermal conductivity. The average sphericity is determined by the following microscopic method. That is, an image of the particles taken by a scanning electron microscope, a transmission electron microscope, etc. is taken into an image analysis device, and the projected area (A) and the circumference (PM) of the particles are measured from the photograph. If the area of a perfect circle having the same circumference as the circumference (PM) is set to (B), the sphericity of the particle is A / B. Therefore, if a perfect circle having the same circumference as the circumference (PM) of the sample is assumed, then since PM = 2πr, B = πr 2 , so B = π × (PM / 2π) 2 , the sphericity of each particle is sphericity = A / B = A×4π / (PM) 2 . As described above, the sphericity of 200 arbitrary particles whose projected area circle equivalent diameter is within the specified range is calculated, and the summed average value is taken as the average sphericity. It should be noted that the specific measurement method is as described in the examples. In addition, the projected area circle equivalent diameter refers to the diameter of a perfect circle having the same projected area as the projected area (A) of the particle. When calculating the average sphericity of the first alumina particles, the above-mentioned "specified range" is 0.1μm to 1μm.
[0026] From the viewpoint of obtaining a resin composition and a heat dissipating material having a low contact resistance at the interface with the resin and being less likely to cause an increase in viscosity, the specific surface area of the first alumina particles is 1.9 m 2 / g~20.0m 2 / g, preferably 2.0m 2 / g~6.0m 2 In addition, in this embodiment, the specific surface area is measured by the BET flow method, and the specific measurement method is described in the examples.
[0027] From the viewpoint of obtaining a resin composition and a heat dissipation material having a higher thermal conductivity, the content of the α-crystalline phase in the first alumina particle is 80% by mass or more, preferably 85% by mass or more. From the viewpoint of more effectively improving thermal conductivity, the content of the α-crystalline phase in the first alumina particle is preferably higher than the content of the α-crystalline phase in the third alumina particle described later. The upper limit is, for example, 100% by mass. It should be noted that in the present embodiment, the content of the α-crystalline phase is measured by a calibration line method using an X-ray diffraction device. The specific measurement method is described in the examples.
[0028] According to the alumina powder of this embodiment, when the alumina powder is filled in the resin, the viscosity increase can be suppressed, and the resin composition and the heat dissipation component containing the alumina powder can achieve high thermal conductivity. The present inventors have not yet clarified the reason, but speculated as follows. However, the reason is not limited to this.
[0029] In a resin composition and a heat dissipation component comprising alumina particles and a resin, heat is transmitted through the alumina particles in the resin. Therefore, it is preferred to make the resin contain particles with a large average particle size such as the second alumina particles and the third alumina particles, so that the path of heat transfer becomes larger. However, since the average particle size of the second alumina particles and the third alumina particles is large, gaps are easily generated between the particles, and it is necessary to fill them with resin. Therefore, if these alumina particles are filled into the resin at a high ratio, the viscosity will increase. Therefore, it is difficult to fill these alumina particles into the resin at a high ratio. If the filling rate of the particles is low, the gaps between the particles will further increase, and the heat path between the particles will be hindered, so it is difficult to achieve high thermal conductivity. On the other hand, the first alumina particles have a high average sphericity, a small average particle size compared to the second alumina particles and the third alumina particles, and a low specific surface area compared to alumina particles with the same average particle size, so the contact resistance at the interface between the alumina particles and the resin can be reduced. Furthermore, the first alumina particles have a high thermal conductivity because the α crystallization rate of the particles themselves is as high as 80% by mass or more. However, since the average particle size of the first alumina particles is small, the heat path is also small, and the first alumina particles alone cannot effectively conduct heat. Therefore, it is difficult to achieve high thermal conductivity using only the first alumina particles. Therefore, in the alumina powder of this embodiment, by combining the first alumina particles with a small average particle size with the second alumina particles and the third alumina particles, the first alumina particles can be filled in the gaps between the second alumina particles and the third alumina particles. Since the contact resistance of the interface between the alumina particles and the resin of the first alumina particles is low, and the average sphericity is high, the gaps between the particles of the second alumina particles and the third alumina particles are filled in by virtue of fluidity, so the alumina powder containing these particles can be filled into the resin at a high ratio. Moreover, since the first alumina particles have a high thermal conductivity, a heat path is easily formed at the interface between the first alumina particles and the second alumina particles and the third alumina particles, and high thermal conductivity can be achieved. Furthermore, the first alumina particles are fluidly filled in the gaps between the second alumina particles and the third alumina particles, and after filling, each particle is in a state that is not easy to agglomerate with each other, so it is also difficult to cause viscosity to rise.
[0030] The first alumina particles of the present embodiment can be manufactured according to the methods described in Japanese Patent Application Laid-Open No. 6-191835, Japanese Patent Application Laid-Open No. 7-187663, and Japanese Patent Application Laid-Open No. 8-290914, for example. In addition, two or more alumina particles can be mixed to form the first alumina particles. In the case of mixing, since the average particle size, average sphericity, specific surface area, and content of the α-crystalline phase are substantially additive, these average particle size, average sphericity, specific surface area, and content of the α-crystalline phase can be appropriately adjusted to become target values.
[0031] (Second Alumina Particles and Method for Producing the Same)
[0032] The average particle size of the second alumina particles of this embodiment is greater than 1 μm and less than 10 μm. The second alumina particles are combined to improve the fluidity of the alumina particles in the resin. If only the first alumina particles and the third alumina particles are used, and the alumina particles are filled into the resin to a degree that can achieve high thermal conductivity of the resin composition, there is a tendency for the filling rate of the alumina particles to become too high, and it is difficult to obtain fluidity, and it is difficult to suppress the increase in viscosity when the alumina powder is filled into the resin. The second alumina particles preferably have an average particle size of 2 μm to 9 μm, and more preferably 3 μm to 8 μm.
[0033] In the second alumina particles of the present embodiment, except that the "prescribed range" exceeds 1 μm and is 10 μm or less, the average sphericity of the second alumina particles whose projected area circle equivalent diameter is within the prescribed range obtained in the same manner as above is preferably 0.80 to 0.98, and more preferably 0.85 to 0.97. If the alumina powder contains second alumina particles having an average sphericity of 0.80 or more, the fluidity of the alumina particles in the resin tends to be further improved. If the alumina powder contains second alumina particles having an average sphericity of 0.98 or less, the fluidity of the alumina particles in the resin can be prevented from being excessively increased and the excessive decrease in viscosity when the alumina powder is filled in the resin tends to be suppressed.
[0034] The second alumina particles of the present embodiment can be obtained as follows. Figure 1 The flame melting device is briefly described. The raw material is sprayed into the flame from the raw material powder supply pipe 5, and the raw material is melted in the melting furnace 1. Dry ice is continuously supplied to the melting furnace 1 from the cooling medium supply port 6 to perform a quenching treatment. The cooling effect produced by the quenching treatment is confirmed by measuring the temperature in the melting furnace 1 before and after the dry ice is supplied. The temperature is measured using an R thermocouple 9, which is usually inserted into the furnace wall from a height of 100 cm from the furnace top of the melting furnace 1. The obtained spheroidized product is transported to the bag filter 7 together with the exhaust gas through the blower 8 for capture. The formation of the flame is carried out by spraying fuel gases such as hydrogen, natural gas, acetylene, propane and butane from the fuel gas supply pipe 4 and combustion-supporting gases such as air and oxygen from the combustion-supporting gas supply pipe 3 from the burner 2 arranged in the melting furnace 1. As a carrier gas for supplying raw material powder, air, nitrogen, oxygen and carbon dioxide can be used. Below, the method for producing the second alumina particles of this embodiment is described in detail.
[0035] As the raw material used when obtaining the second alumina particles, for example, aluminum hydroxide powder or its slurry and alumina powder or its slurry can be cited, but among them, since it usually has an α crystal phase as the main crystal phase, it is preferable to use alumina powder or its slurry. It should be noted that the particle size of the obtained alumina particles can be adjusted according to the particle size of the particles used in the raw material. Specifically, if the particle size of the particles used in the raw material is increased, the particle size of the alumina particles will also become larger, and if the particle size of the particles used in the raw material is reduced, the particle size of the alumina particles will also become smaller.
[0036] In the present embodiment, when alumina powder is used as the raw material of the second alumina particles, the slurry concentration of the alumina powder may preferably be 10% to 70% by mass. By having a slurry concentration of 10% by mass or more, productivity is further improved, and by being 70% by mass or less, there is a tendency to suppress the increase in slurry viscosity, and to facilitate transportation and spraying. As a solvent for dispersing alumina powder in the slurry, water is preferred from the viewpoints of dispersibility, safety, and economy. However, if the alumina powder as a raw material can be dispersed, it may also be a flammable liquid such as alcohol and a mixed liquid such as water-alcohol. For the preparation of the slurry, it is sufficient to put a specified amount of solvent and raw material powder into a container for preparation and mix them with a stirrer until they are fully dispersed, and no special preparation method is required.
[0037] In order to spheroidize the aluminum oxide powder, a thermal spraying method is generally used. According to the thermal spraying method, it has the advantage of being easy to spheroidize. It should be noted that the aluminum oxide powder can also be dispersed in a solvent to form a slurry state and supplied to the flame in a fine mist spray. As a spraying method, a spray nozzle used in a spray dryer can be used, but it is preferred to use a feed pipe with a strong dispersing function. For the spraying of a wet slurry using a solvent, a two-fluid nozzle is preferred.
[0038] In addition, instead of the above-mentioned wet slurry, a dry feeding method in which the aluminum oxide powder is dispersed in a gas such as oxygen and air may be used. In this case, it is important to fully disperse by a feeding method having a strong dispersing function, for example, preferably using a feeding pipe portion formed in the shape of an ejector nozzle and performing dispersion by a ring nozzle method utilizing shear force generated by a high-speed air flow.
[0039] In order to form a flame, a fuel gas such as hydrogen, natural gas, acetylene, propane and butane and a combustion-supporting gas such as air and oxygen can be sprayed and burned from a nozzle. The flame temperature is preferably maintained at 2050°C to 2300°C. If the flame temperature is higher than 2300°C, it is difficult to obtain a quenching effect. In addition, if the flame temperature is lower than 2050°C, it is difficult to achieve a high sphericity. The flame temperature can be controlled by, for example, changing the flow rate of the fuel gas, thereby making it possible to produce alumina powders of different sphericity. If the temperature is high, the sphericity is high, and if the time is long, the sphericity becomes higher.
[0040] The alumina powder sprayed into the flame is subjected to high-temperature heat treatment to spheroidize the alumina powder. At this time, the content of the α crystal phase can be adjusted by a rapid cooling treatment using dry ice. Specifically, if the amount of dry ice introduced into the furnace as a rapid cooling condition is increased, the content of the α crystal phase tends to decrease.
[0041] The heat-treated powder is sucked into the blower together with the exhaust gas, and is captured by the collector of the cyclone separator or bag filter. The capture temperature at this time is preferably above 500°C. By setting the capture temperature above 500°C, it is possible to suppress the Na component gasified by thermal spraying from adhering to the captured powder and precipitating, and as a result, it is easy to remove Na, so it is preferred. However, based on the material of the collector, the upper limit is preferably around 1100°C. In addition, by setting the capture temperature above 500°C, it is possible to suppress the mixing of other cationic impurities and anionic impurities in large quantities, so that the neutrality of the alumina powder is more sufficient.
[0042] In addition, it is preferred that ionic impurities such as cations and anions be removed from the obtained alumina powder using ion exchange water or the like.
[0043] (Third Alumina Particles and Method for Producing the Same)
[0044] The average particle size of the third alumina particles of this embodiment is 10 μm to 100 μm. The third alumina particles contribute most to thermal conductivity in the alumina powder of this embodiment and are blended for resin filling. From the viewpoint of high thermal conductivity and resin filling, the third alumina particles preferably have an average particle size of 15 μm to 90 μm, and more preferably 20 μm to 80 μm.
[0045] In the third alumina particles of the present embodiment, the average sphericity of the third alumina particles whose projected area circle equivalent diameter is within the specified range, which is obtained in the same manner as above, except that the "predetermined range" is greater than 10 μm and less than 100 μm, is preferably 0.80 to 0.98, and more preferably 0.85 to 0.97. If the alumina powder contains third alumina particles having an average sphericity of 0.80 or more, there is a tendency to further improve the resin filling property. If the alumina powder contains third alumina particles having an average sphericity of 0.98 or less, there is a tendency to suppress excessive viscosity reduction during resin filling.
[0046] The third alumina particles of the present embodiment can be obtained, for example, by the same production method as the second alumina particles described above.
[0047] (Contents of the First Alumina Particles, the Second Alumina Particles, and the Third Alumina Particles)
[0048] In the present embodiment, from the viewpoint of further improving the fluidity during resin filling, the content of the first alumina particles is preferably 2.0 to 20.0 parts by mass, more preferably 4.0 to 18.0 parts by mass, and further preferably 5.0 to 16.0 parts by mass. In addition, the content of the second alumina particles is preferably 3.0 to 50.0 parts by mass, more preferably 5.0 to 45.0 parts by mass, and further preferably 10.0 to 40.0 parts by mass. Furthermore, the content of the third alumina particles is preferably 30.0 to 95.0 parts by mass, more preferably 35.0 to 90.0 parts by mass, and further preferably 40.0 to 85.0 parts by mass. It should be noted that the total of the first alumina particles, the second alumina particles, and the third alumina particles is set to 100 parts by mass.
[0049] By including the first alumina particles, the second alumina particles, and the third alumina particles in the above-mentioned content, these alumina particles can be closely arranged in the form of filling the gaps in the resin, so that the alumina powder can be filled into the resin at a high ratio. Therefore, the alumina particles can contact each other at multiple points and surfaces, and a heat path can be easily formed, and high thermal conductivity can be achieved. In addition, since these alumina particles can be closely arranged in the form of filling the gaps in the resin, the alumina powder has good fluidity in the resin. As a result, the viscosity increase when the alumina powder is filled in the resin can be suppressed.
[0050] In the present embodiment, the content of each aluminum oxide particle is measured by, for example, classifying an aluminum oxide powder into each aluminum oxide particle by the method described in Examples.
[0051] (Average sphericity of alumina powder)
[0052] In the alumina powder of this embodiment, since the fluidity when filled into the resin is further improved, the average sphericity of the alumina particles whose projected area circle equivalent diameter is within the prescribed range, which is obtained in the same manner as above, is preferably 0.80 or more, except that the "prescribed range" is 0.1 μm to 10 μm. In addition, since it is possible to suppress excessive increase in fluidity when filled into the resin, the upper limit is preferably 0.98 or less.
[0053] Since the fluidity when filled in the resin is further improved, the average sphericity of the alumina particles whose projected area circle equivalent diameter is within the prescribed range, which is obtained in the same manner as above, is preferably 0.80 or more, except when the "prescribed range" is greater than 10 μm and less than 100 μm. In addition, since excessive increase in fluidity can be suppressed when filled in the resin, the upper limit is preferably 0.98 or less.
[0054] (Content ratio of α crystal phase in alumina powder)
[0055] From the viewpoint of being able to obtain a resin composition and a heat dissipation material having a higher thermal conductivity, the content of the α crystal phase in the alumina powder of this embodiment is preferably 60% by mass or more. The upper limit is, for example, 100% by mass. The content of the α crystal phase is measured by X-ray diffraction. The specific measurement method is described in the examples.
[0056] (Total content of first alumina particles, second alumina particles, and third alumina particles in alumina powder)
[0057] In the present embodiment, the total content of the first alumina particles, the second alumina particles, and the third alumina particles in the alumina powder is preferably 85 mass % to 100 mass %. The content of components other than the first alumina particles, the second alumina particles, and the third alumina particles is usually 15 mass % or less, preferably 10 mass % or less, and more preferably 7 mass % or less. As components other than the first alumina particles, the second alumina particles, and the third alumina particles, there can be cited alumina particles having an average particle size of less than 0.1 μm, alumina particles having an average particle size of more than 100 μm, fillers other than alumina particles, additives other than fillers, and impurities.
[0058] (Method for producing alumina powder)
[0059] The method for producing alumina powder of the present embodiment preferably comprises mixing 2.0 to 20.0 mass % of first alumina particles, 3.0 to 50.0 mass % of second alumina particles, and 30.0 to 95.0 mass % of third alumina particles. The mixing method may be a known method and is not particularly limited.
[0060] [Resin composition and method for producing the same]
[0061] The resin composition of the present embodiment contains at least a resin and the alumina powder of the present embodiment. The resin composition of the present embodiment can have high thermal conductivity while suppressing thickening by containing the alumina powder.
[0062] (resin)
[0063] As the resin, various polymer compounds such as thermoplastic resins and oligomers thereof, and elastomers can be used, for example, epoxy resins, phenolic resins, melamine resins, urea resins, unsaturated polyesters, polyurethane resins, acrylic resins, and fluororesins can be used; polyamides such as polyimide, polyamide-imide, and polyether-imide; polyesters such as polybutylene terephthalate and polyethylene terephthalate; polyphenylene sulfide, aromatic polyester, polysulfone, liquid crystal polymer, polyether sulfone, polycarbonate, maleimide-modified resin, ABS (acrylonitrile butadiene styrene) resin, AAS (acrylonitrile acrylic rubber styrene) resin, AES (acrylonitrile ethylene propylene diene rubber styrene) resin, EVA (ethylene vinyl acetate copolymer) resin, and silicone resin can be used. These resins can be used alone or in combination of two or more.
[0064] Among these resins, from the viewpoint of heat resistance temperature, strength and hardness after curing, epoxy resin, phenolic resin, polyurethane resin, acrylic resin, fluororesin, polyimide, polyphenylene sulfide, polycarbonate, ABS resin and silicone resin are preferred, silicone resin, epoxy resin, polyurethane resin and acrylic resin are more preferred, and silicone resin is further preferred.
[0065] As the silicone resin, it is preferable to use a rubber or gel obtained from a one-component or two-component addition reaction type liquid silicone having an organic group such as a methyl group or a phenyl group. Examples of such rubber or gel include "YE5822A Liquid / YE5822B Liquid" manufactured by Momentive Performance Materials Japan Co., Ltd. and "SE1885A Liquid / SE1885B Liquid" manufactured by Toray-Dow Corning Co., Ltd.
[0066] (Content of alumina powder and resin)
[0067] In the resin composition of the present embodiment, from the viewpoint of expressing the characteristics of the filled filler, the content of the alumina powder of the present embodiment is preferably 65% to 95% by mass relative to the total amount of the resin composition. The alumina powder of the present embodiment is not easy to thicken even if filled in the resin, so even if it is included in the resin composition within the above range, the thickening of the resin composition can be suppressed. In addition, if the content of the alumina powder is less than 65% by mass, it tends to be difficult to obtain a resin composition and a heat dissipation component that can achieve good high thermal conductivity, and if it exceeds 95% by mass, the resin component that binds the alumina powder becomes less, so it is not easy to be used in heat dissipation components.
[0068] In the resin composition of the present embodiment, from the viewpoint of expressing the characteristics of the filled filler, the content of the resin of the present embodiment is preferably 5% by mass to 35% by mass based on the total amount of the resin composition.
[0069] (Other ingredients)
[0070] The resin composition of the present embodiment may contain, in addition to the alumina powder and the resin of the present embodiment, inorganic fillers such as fused silica, crystalline silica, zircon, calcium silicate, calcium carbonate, silicon carbide, aluminum nitride, boron nitride, beryllium oxide, and zirconium oxide as needed, nitrogen-containing compounds such as melamine and benzoguanamine, and Flame retardant compounds such as oxazine ring compounds and phosphate compounds of phosphorus compounds, aromatic condensed phosphate esters, and halogen-containing condensed phosphate esters; additives, etc. As additives, reaction retardants such as dimethyl maleate, curing agents, curing accelerators, flame retardant aids, flame retardants, colorants, tackifiers, ultraviolet absorbers, antioxidants, fluorescent whitening agents, photosensitizers, thickeners, lubricants, defoamers, surface adjusters, brighteners and polymerization inhibitors can be cited. These ingredients can be used alone or in combination of two or more. In the resin composition of this embodiment, the content of other ingredients is usually 0.1% by mass to 30% by mass.
[0071] (Method for producing resin composition)
[0072] The method for producing the resin composition of the present embodiment can include, for example, a method of fully stirring a resin, an alumina powder, and other components as required. The resin composition of the present embodiment can be produced, for example, by mixing a predetermined amount of each component by a mixer and a Henschel mixer, kneading by a heating roll, a kneader, a single-shaft or double-shaft extruder, cooling, and then pulverizing.
[0073] [Heat dissipation components]
[0074] The heat dissipation component of the present embodiment includes the alumina powder or resin composition of the present embodiment. The heat dissipation component of the present embodiment can achieve high thermal conductivity, that is, can have high heat dissipation by using the above-mentioned alumina powder or resin composition. From the viewpoint of being able to achieve higher thermal conductivity, the content of alumina powder in the heat dissipation component of the present embodiment is preferably 30 volume % to 85 volume %. As heat dissipation components, for example, heat sinks, heat dissipation grease, heat dissipation gaskets, semiconductor sealing materials, and heat dissipation coatings (heat dissipation coating agents) can be cited.
[0075] Example
[0076] The present invention will be described in detail below with reference to Examples and Comparative Examples, but the present invention is not limited to these Examples at all.
[0077] [Method for classifying individual alumina particles from alumina powder]
[0078] The first aluminum oxide particles, the second aluminum oxide particles, and the third aluminum oxide particles are obtained by classifying aluminum oxide powder by the following method.
[0079] First, 4 L of ion exchange water and 1 kg of alumina powder were placed in a polypropylene handle beaker (5 L) manufactured by SANPLATEC, and mixed at 600 rpm for 10 minutes using a Three-One Motor BL3000 (trade name) manufactured by Shinto Scientific. Then, the agitator was stopped and allowed to stand for 6 hours, and then 15 cm of slurry was extracted from the water surface of the polycontainer using a volumetric liquid feed roller pump RP-1000 (trade name, tube diameter 4.8 mmφ) manufactured by Tokyo Rikaki Co., Ltd. The extracted slurry was transferred to a SUS bucket, and then dried at 120° C. for 72 hours using a dryer CLEAN OVEN DE-61 (trade name) manufactured by Yamato Scientific Co., Ltd., thereby taking out alumina particles, which were used as first alumina particles. Then, 3.5 L of ion exchange water was added to the original slurry, and mixed at 600 rpm for 10 minutes. Then, the stirrer was stopped and the mixture was allowed to stand for 15 minutes. Then, 15 cm of the slurry was extracted from the water surface of the polymerization container in the same manner as before, and dried at 120° C. for 72 hours to remove alumina particles, which were used as second alumina particles. In addition, the residue of the slurry was also dried in the same manner to remove alumina particles, which were used as third alumina particles. In these operations, the liquid temperature was adjusted to 20° C. from mixing with the stirrer to extraction of the slurry.
[0080] In the following evaluation, when an alumina powder including first alumina particles, second alumina particles, and third alumina particles was used, evaluation of each particle was performed by classification using this method.
[0081] [Evaluation Method]
[0082] (1) Average particle size and particle size distribution of alumina particles
[0083] The average particle size and particle size distribution of alumina particles were measured using a laser diffraction scattering particle size distribution measuring machine LS-230 (trade name) manufactured by Beckman Coulter, Inc. During the measurement, 0.04 g of each alumina particle obtained in the embodiment and comparative example to be measured was added to a mixed solution of 0.5 mL of ethanol as a solvent and 5 mL of ion exchange water, pretreated for 2 minutes, and dispersed for 30 seconds using an ultrasonic generator UD-200 (equipped with an ultra-micro chip TP-030) (trade name) manufactured by TOMY SEIKO Co., Ltd. to obtain a slurry. Using this slurry, the particle size distribution was measured at a pump speed of 60 rpm. In the analysis of the particle size distribution, the refractive indices of water and alumina particles were 1.333 and 1.768, respectively. The analysis of the particle size distribution was performed by volume fraction-cumulative. In the measured mass-based particle size distribution, the particles with a cumulative mass of 50% were taken as the average particle size (μm).
[0084] (2) Average sphericity
[0085] As shown in the above-mentioned microscopy method, the particle image taken by a scanning electron microscope (SEM) (JSM-6301F model (trade name) manufactured by JEOL Ltd.) is taken into an image analysis device ("MacView" (trade name) manufactured by Mountech), and the projection area (A) and the circumference (PM) of 200 alumina particles (the projection area circle equivalent diameter based on the microscopy method is 0.1 μm to 100 μm) obtained in the examples and comparative examples are arbitrarily measured from the photograph. The sphericity of each particle and its ratio are calculated using these values, and the summed average of the sphericity of each particle is taken as the average sphericity. By this method, the average sphericity of the first alumina particles having a projection area circle equivalent diameter of 0.1 μm to 1 μm, the second alumina particles having a projection area circle equivalent diameter of more than 1 μm and less than 10 μm, and the third alumina particles having a projection area circle equivalent diameter of more than 10 μm and less than 100 μm are measured. In addition, the average sphericity of aluminum oxide particles with a projected area circle equivalent diameter of 0.1 μm to 10 μm and the average sphericity of aluminum oxide particles with a projected area circle equivalent diameter exceeding 10 μm and 100 μm or less are also determined by measuring using the same method as above and then analyzing according to the particle size.
[0086] (3) Specific surface area
[0087] The specific surface area is a value based on the BET method. The specific surface area (m2) was determined by using a specific surface area measuring machine "Macsorb HMmodel-1208 (trade name)" manufactured by Mountech Co., Ltd. and using 1.0 g of each sample of the alumina particles obtained in the Examples and Comparative Examples. 2 / g). It should be noted that, before the measurement, each of the aluminum oxide particles obtained in the examples and comparative examples was heated in a nitrogen atmosphere at 300°C for 18 minutes as a pretreatment. In addition, in the BET measurement, a mixed gas of 30% nitrogen and 70% helium was used as the adsorption gas, and the flow rate was adjusted so that the indication value of the main flow meter became 25 ml / min.
[0088] (4) Content of α-crystal phase in first alumina particles and content of α-crystal phase in alumina powder
[0089] The content rate of the α crystal phase in the alumina particles and the content rate of the α crystal phase in the alumina powder were measured by the following method.
[0090] Using NIST-676a (α-alumina) and θ·δ·γ-alumina as intensity standard materials for X-ray diffraction (XRD), each alumina was weighed so as to have a total of 2 g, and then mixed with a pestle for 15 minutes to prepare a sample for making a calibration line. Then, for each sample, a sealed tube-type X-ray diffractometer (D8 ADVANCE (trade name) manufactured by Bruker) was used to calculate the integrated intensity (Cps×deg) under the following measurement conditions to make a calibration line. It should be noted that three diffraction peaks in α-alumina (2θ=25.6°(012), 35.2°(104) and 2θ=43.4°(113)) were used in the determination of the content of the α crystal phase.
[0091] (Measurement conditions)
[0092] θ·θ scanning, tube voltage: 40kV, tube current: 40mA, X-ray source: CuKα Slit: DS, 0.5°, Light slit: 2.5deg.
[0093] Next, using each aluminum oxide particle obtained in the examples and comparative examples, the diffraction peak area (Y) from the (113) plane of the α-crystalline phase of aluminum oxide was measured, and the content (mass %) of the α-crystalline phase was calculated using the above-mentioned calibration line. It should be noted that the measurement uses the diffraction peak detected at 2θ=10° to 70°. In addition, using each aluminum oxide powder obtained in the examples and comparative examples, the diffraction peak area (Y) from the (113) plane of the α-crystalline phase of aluminum oxide was measured, and the content (mass %) of the α-crystalline phase was calculated using the above-mentioned calibration line. It should be noted that the measurement uses the diffraction peak detected at 2θ=10° to 70°.
[0094] (5) Viscosity
[0095] The aluminum oxide powders obtained in the examples and comparative examples were added to the silicone rubber A liquid (vinyl-containing polymethylsiloxane, Momentive Performance Materials Japan Co., Ltd. YE5822A liquid (trade name)) after being placed for 1 day (aluminum oxide powder filling rate: 87.9 mass%), mixed using a stirrer (Tokyo Rikaki Co., Ltd. NZ-1100 (trade name)), and vacuum degassed to obtain a composition. For the obtained composition, the viscosity (Pa·s) was measured using a B-type viscometer (Toki Industry Co., Ltd. TVB-10 (trade name)). The viscosity measurement was performed using a No7 spindle with a rotation speed of 20 rpm at room temperature of 20°C.
[0096] (6) Thermal conductivity
[0097] Into silicone rubber liquid A (vinyl-containing polymethylsiloxane, YE5822A liquid (trade name) manufactured by Momentive Performance Materials Japan) were added the respective alumina powders obtained in the examples and comparative examples, a reaction retarder (dimethyl maleate, manufactured by Kanto Chemical Co., Ltd.) and silicone rubber liquid B (YE5822B liquid (trade name) manufactured by Momentive Performance Materials Japan, containing a crosslinking agent, etc.), stirred, and then degassed to obtain a slurry sample. It should be noted that their mixing ratio was calculated as follows: relative to 100 parts by mass of a silicone rubber mixed liquid obtained by mixing 10 parts by volume of silicone rubber liquid A with 1 part by volume of silicone rubber liquid B, 0.01 parts by mass of a reaction retarder was added to obtain a liquid, and the alumina powders obtained in the examples and comparative examples with the maximum filling amount that can be heat-molded were added to the above liquid; the ratios are shown in Table 1.
[0098]
[0099] Then, the obtained slurry sample was poured into a mold with a depression of 28 mm in diameter and 3 mm in thickness, and after degassing, it was heated and molded at 150°C for 20 minutes. The obtained molded product was sandwiched between a 15 mm × 15 mm copper heater housing and a copper plate, and set with a tightening torque of 5 kgf·cm. Then, 15 W of power was applied to the copper heater housing and maintained for 4 minutes, and the temperature difference between the copper heater housing and the copper plate was measured, and the thermal resistance was calculated by the following formula.
[0100] Thermal resistance (℃ / W) = Temperature difference between copper heater housing and copper plate (℃) / Heater power (W)
[0101] Next, use the thermal resistance (℃ / W), thermal conductivity area [area of the copper heater housing] (m 2 ) and the thickness (m) of the molded body when the tightening torque is 5 kgf·cm, and the thermal conductivity is calculated by the following formula. That is, the thermal conductivity is the value when each alumina powder obtained in the embodiment and the comparative example is filled with the maximum filling amount that can be heat-molded. It should be noted that as a thermal conductivity measuring device, ARC-TC-1 model (trade name) manufactured by AGNE was used.
[0102] Thermal conductivity (W / m·K) = molded body thickness (m) / {thermal resistance (℃ / W) × thermal conductivity area (m 2 )}
[0103] 〔Alumina particles〕
[0104] (1) First Alumina Particles
[0105] As a raw material of the first alumina particles, the following alumina particles were used: The average sphericity is a value of particles having a projected area circle equivalent diameter of 0.1 μm to 1 μm.
[0106] (1-1) Advanced Alumina AA-03 manufactured by Sumitomo Chemical Co., Ltd. (trade name, average particle size: 0.3 μm, average sphericity: 0.83, specific surface area: 5.2 m 2 / g, content of α crystal phase: 99 mass %)
[0107] (1-2) Advanced Alumina AA-05 manufactured by Sumitomo Chemical Co., Ltd. (trade name, average particle size: 0.5 μm, average sphericity: 0.86, specific surface area: 3.0 m 2 / g, content of α crystal phase: 99 mass %)
[0108] (1-3) Advanced Alumina AA-07 manufactured by Sumitomo Chemical Co., Ltd. (trade name, average particle size: 0.7 μm, average sphericity: 0.87, specific surface area: 2.2 m 2 / g, content of α crystal phase: 99 mass %)
[0109] (1-4) Advanced Alumina AA-1.5 manufactured by Sumitomo Chemical Co., Ltd. (trade name, average particle size: 1.5 μm, average sphericity: 0.85, specific surface area: 1.0 m 2 / g, content of α crystal phase: 99 mass %)
[0110] (1-5) Advanced Alumina AA-3 manufactured by Sumitomo Chemical Co., Ltd. (trade name, average particle size: 3.0 μm, average sphericity: 0.84, specific surface area: 0.5 m 2 / g, content of α crystal phase: 99 mass %)
[0111] (1-6) Alumina particles A (average particle size: 0.05 μm, average sphericity: 0.94, specific surface area: 40.1 m 2 / g, content of α crystal phase: 1 mass %)
[0112] (1-7) Alumina particles B (average particle size: 0.1 μm, average sphericity: 0.91, specific surface area: 19.7 m 2 / g, content of α crystal phase: 81 mass %)
[0113] (1-8) Alumina particles C (average particle size: 0.3 μm, average sphericity: 0.92, specific surface area: 10.0 m 2 / g, content of α crystal phase: 1 mass %)
[0114] (1-9) Alumina particles D (average particle size: 0.5 μm, average sphericity: 0.98, specific surface area: 6.0 m 2 / g, content of α crystal phase: 1 mass %)
[0115] (1-10) Alumina particles E (average particle size: 0.5 μm, average sphericity: 0.99, specific surface area: 5.8 m 2 / g, content of α crystal phase: 97 mass %)
[0116] (1-11) Alumina particles F (average particle size: 0.7 μm, average sphericity: 0.92, specific surface area: 2.8 m 2 / g, content of α crystal phase: 93 mass %)
[0117] (1-12) Alumina particles G (average particle size: 0.5 μm, average sphericity: 0.76, specific surface area: 6.0 m 2 / g, content of α crystal phase: 97 mass %)
[0118] In addition, alumina particles A to F are suitably produced by the method described in International Publication No. 2008 / 053536, etc. Alumina particles G are produced by the method described below.
[0119] The first alumina particles are prepared by appropriately mixing the above-mentioned alumina particles and adjusting the average particle size, sphericity, etc. to be within the ranges shown in Tables 2 and 3.
[0120] (2) Alumina particles G, second alumina particles, and third alumina particles
[0121] As a raw material, alumina LS-21 (trade name, average particle size: 55 μm) manufactured by Nippon Light Metal Co., Ltd. was melted in an arc furnace, cooled and pulverized to prepare fused alumina pulverized material. The pulverization was performed using a ball mill, and alumina balls were used as pulverizing media.
[0122] Alumina particles G, alumina raw material 1 (average particle size: 2 μm), alumina raw material 2 (average particle size: 5 μm), alumina raw material 3 (average particle size: 10 μm), alumina raw material 4 (average particle size: 20 μm), alumina raw material 5 (average particle size: 50 μm) and alumina raw material 6 (average particle size: 80 μm) are prepared from the obtained alumina crushed material by classification treatment.
[0123] The obtained alumina raw materials 1 to 6 are appropriately used as alumina raw materials for producing the second alumina particles or the third alumina particles.
[0124] [Example 1]
[0125] As the first alumina particles, 80 parts by mass of (1-1) alumina particles (Advanced Alumina AA-03 (trade name) manufactured by Sumitomo Chemical Co., Ltd.) and 20 parts by mass of (1-8) alumina particles C were mixed using a high-power rubber mixer EL-1 (trade name) manufactured by Nipponeirich Co., Ltd. to produce the alumina particles.
[0126] The second alumina particles are prepared by the following method. Figure 1 The manufacturing apparatus shown in the figure makes the alumina raw material 1 and oxygen (gas flow rate: 50Nm 3 / hour) are supplied from the spray nozzle to the flame, and fuel gas (LP gas, gas flow rate: 10Nm 3 During the flame melting treatment, dry ice was appropriately supplied into the furnace for cooling in order to control the content of the α crystal phase of the alumina powder.
[0127] In addition, the third alumina particles were produced by the following method. Figure 1 The manufacturing apparatus shown in the figure makes the alumina raw material 4 and oxygen (gas flow rate: 75Nm 3 / hour) are supplied from the spray nozzle to the flame, and fuel gas (LP gas, gas flow rate: 15Nm 3 During the flame melting treatment, dry ice was appropriately supplied into the furnace for cooling in order to control the content of the α crystal phase of the alumina powder.
[0128] The physical properties of the obtained first alumina particles, second alumina particles, and third alumina particles were evaluated. The results are shown in Table 2.
[0129] Then, 3.0 parts by mass of the obtained first alumina particles, 37.0 parts by mass of the second alumina particles, and 60.0 parts by mass of the third alumina particles were mixed using a high-power rubber mixer EL-1 (trade name) manufactured by NIPPON EIRICH CO., LTD. to produce an alumina powder 1 .
[0130] Table 2 shows the evaluation results using the obtained alumina powder 1.
[0131] [Examples 2 to 12]
[0132] As first alumina particles, first alumina particles having the physical properties shown in Table 2 were produced in the same manner as in Example 1.
[0133] In addition, except that the types of alumina raw materials (raw materials 1 to 6), the flow rates of oxygen and fuel gas were changed according to Table 2, the same procedure as in Example 1 was carried out to obtain second alumina particles having the properties shown in Table 2.
[0134] Furthermore, except that the types of alumina raw materials (raw materials 1 to 6), the flow rates of oxygen and fuel gas were changed according to Table 2, the same procedure as in Example 1 was carried out to obtain third alumina particles having the properties shown in Table 2.
[0135] The first alumina particles, second alumina particles, and third alumina particles thus obtained were mixed in the amounts shown in Table 2 using a high-power rubber mixer EL-1 (trade name) manufactured by NIPPON EIRICH CO., LTD. to produce alumina powders 2 to 12, respectively.
[0136] The evaluation results using the alumina powders 2 to 12 are shown in Table 2 together with the physical properties of the first alumina particles, the second alumina particles, and the third alumina particles obtained.
[0137] [Comparative Example 1]
[0138] As the first alumina particles, 15 parts by mass of (1-6) alumina particles A and 85 parts by mass of (1-7) alumina particles B were mixed using a high-power rubber mixer EL-1 (trade name) manufactured by NIPPON EIRICH CO., LTD. to produce the alumina particles.
[0139] The second alumina particles are prepared by the following method. Figure 1 The manufacturing apparatus shown in the figure makes the alumina raw material 1 and oxygen (gas flow rate: 15Nm 3 / hour) are supplied from the spray nozzle to the flame, and fuel gas (LP gas, gas flow rate: 3Nm 3 During the flame melting treatment, dry ice was appropriately supplied into the furnace for cooling in order to control the content of the α crystal phase of the alumina powder.
[0140] In addition, the third alumina particles were produced by the following method. Figure 1 The manufacturing apparatus shown in the figure makes the alumina raw material 3 and oxygen (gas flow rate: 15Nm 3 / hour) are supplied from the spray nozzle to the flame, and fuel gas (LP gas, gas flow rate: 3Nm 3 During the flame melting treatment, dry ice was appropriately supplied into the furnace for cooling in order to control the content of the α crystal phase of the alumina powder.
[0141] The physical properties of the obtained first alumina particles, second alumina particles, and third alumina particles were evaluated. The results are shown in Table 3.
[0142] Then, 5.3 parts by mass of the obtained first alumina particles, 47.0 parts by mass of the second alumina particles, and 47.7 parts by mass of the third alumina particles were mixed using a high-power rubber mixer EL-1 (trade name) manufactured by NIPPON EIRICH CO., LTD. to produce alumina powder a.
[0143] Table 3 shows the evaluation results using the obtained alumina powder a.
[0144] [Comparative Examples 2 to 11]
[0145] As first alumina particles, first alumina particles having the physical properties shown in Table 3 were produced in the same manner as in Example 1.
[0146] In addition, except that the types of alumina raw materials (raw materials 1 to 6), the flow rates of oxygen and fuel gas were changed according to Table 3, the same procedure as in Example 1 was carried out to obtain second alumina particles having the properties shown in Table 3.
[0147] Furthermore, except that the types of alumina raw materials (raw materials 1 to 6), the flow rates of oxygen and fuel gas were changed according to Table 3, the same procedure as in Example 1 was carried out to obtain third alumina particles having the properties shown in Table 3.
[0148] The first alumina particles, second alumina particles, and third alumina particles thus obtained were mixed in the amounts shown in Table 3 using a high-power rubber mixer EL-1 (trade name) manufactured by NIPPON EIRICH CO., LTD. to produce alumina powders b to k, respectively.
[0149] The evaluation results using the alumina powders b to k are shown in Table 3 together with the physical properties of the first alumina particles, the second alumina particles, and the third alumina particles obtained.
[0150]
[0151]
[0152] In Tables 2 and 3, the average sphericity of alumina particles with a projected area circle equivalent diameter of 0.1 μm to 10 μm is 0.99 for Example 6 and 0.79 for Example 7, and the range of 0.80 to 0.98 for the other particles. In addition, the average sphericity of alumina particles with a projected area circle equivalent diameter exceeding 10 μm and 100 μm or less is 0.99 for Example 10 and 0.79 for Example 11, and the range of 0.80 to 0.98 for the other particles.
[0153] It should be noted that when the first alumina particles are not included, the thermal conductivity is reduced. When the second alumina particles are not included, the fluidity is poor, so it cannot be formed and the thermal conductivity cannot be measured. When the third alumina particles are not included, the fluidity is poor, but it can be formed. However, the thermal conductivity is low.
[0154] This application is based on Japanese patent application (Japanese Patent Application No. 2020-063554) filed on March 31, 2020, the contents of which are incorporated herein by reference.
[0155] Industrial Applicability
[0156] The alumina powder of the present embodiment and the resin composition using the alumina powder can be used in various applications and are suitable for heat dissipation parts such as heat sinks, heat dissipation grease, heat dissipation gaskets, semiconductor sealing materials, and heat dissipation paints (heat dissipation coating agents).
[0157] Explanation of symbols
[0158] 1…melting furnace, 2…burner, 3…fuel gas supply pipe, 4…combustion-supporting gas supply pipe, 5…raw material powder supply pipe, 6…cooling medium supply port, 7…bag filter, 8…blower, 9…R thermocouple.
Claims
1. An aluminum oxide powder comprising: first alumina particles having an average particle size of 0.1 μm or more and less than 1 μm, second alumina particles having an average particle size of 1 μm or more and less than 10 μm, and The third aluminum oxide particles have an average particle size of 10 μm to 100 μm, Each of the above average particle sizes is a particle size measured by a laser diffraction scattering particle size distribution measuring machine. The average sphericity of the first aluminum oxide particles having a projection area circle equivalent diameter of 0.1 μm to 1 μm measured by a microscope is 0.80 to 0.98, The specific surface area of the first alumina particles is 1.9 m 2 / g~20.0m 2 / g, and the content of the α crystal phase is 80 mass % or more.
2. The aluminum oxide powder according to claim 1, wherein The content of the α crystal phase in the alumina powder is 60 mass % or more.
3. A resin composition comprising a resin and the alumina powder according to claim 1 or 2.
4. The resin composition according to claim 3, wherein The resin includes at least one selected from silicone resin, epoxy resin, polyurethane resin and acrylic resin. 5 . A heat dissipation component, comprising the alumina powder according to claim 1 or 2 or the resin composition according to claim 3 or 4.