A method for cleaning and regenerating quartz parts for semiconductor dry etching equipment
Through processes such as organic solvents, acid solutions and ultrasonic cleaning, the problem of difficult regeneration of quartz components in semiconductor etching equipment has been successfully solved, and efficient cleaning and regeneration of quartz components has been achieved, extending the life of the components and reducing production costs.
Patent Information
- Application Number
- CN202211082883.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-06
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-09-06
AI Technical Summary
Medium and large-size quartz parts are difficult to effectively clean and regenerate after use in semiconductor etching equipment, resulting in high scrap processing costs and affecting production efficiency and cost control.
Using seven steps, including organic solvents, high-concentration nitric acid fluoric acid aqueous solution, ammonia hydrogen peroxide aqueous solution, hydrochloric acid solution, low-concentration nitric acid fluoric acid aqueous solution, ultrasonic cleaning and dust-free oven drying, the sediment on the surface of quartz parts is gradually removed and corrosion-breaking. quartz grains realize cleaning and regeneration of components.
Through this method, the surface of the quartz component becomes neat and pollution-free, and the quartz grains are dense and full, which extends the service life of the component, reduces production costs, and meets the requirements of regeneration.
Smart Images

Figure CN115591850B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of semiconductor equipment parts regeneration, and in particular to a cleaning and regeneration method for a quartz part used in semiconductor etching equipment. Background Art
[0002] In recent years, with the increasing demand for chip products in various industries and changes in the international situation, semiconductors and related industries have developed rapidly in China, including photolithography equipment, etching equipment, production processes, raw materials, etc.
[0003] In plasma etching equipment, high-purity quartz parts are widely used, such as quartz rings, quartz tubes, quartz windows, etc. Quartz material has many advantages: for example, high temperature resistance, good thermal stability, can be used for a long time at 1150℃; corrosion resistance, except for hydrofluoric acid, it hardly reacts chemically with other acids, and also has excellent chemical stability at high temperature; good light transmittance, visible light transmittance is above 93%, and in the ultraviolet spectrum region, the transmittance can reach more than 80%; good electrical insulation performance, has good insulation performance at both room temperature and high temperature. At present, the production process of high-purity quartz products is relatively mature, and some small-sized quartz rings and other parts are relatively low in price and can be scrapped after multiple uses, but some medium and large-sized quartz windows and other parts are expensive, and the cost of scrapping is relatively high. Therefore, without affecting the quality of the product, we try to clean and repair the relevant equipment parts after use to extend their service life and reduce production costs. Summary of the invention
[0004] The present invention is carried out to solve the above technical problems, and its purpose is to provide a method for cleaning and regenerating quartz parts for semiconductor dry etching equipment. The cleaning and regeneration of quartz parts is achieved based on seven steps: organic solvent treatment, high-concentration nitric acid and hydrofluoric acid aqueous solution treatment, ammonia and hydrogen peroxide aqueous solution treatment, hydrochloric acid solution treatment, low-concentration nitric acid and hydrofluoric acid aqueous solution treatment, ultrasonic cleaning, and dust-free oven drying. The surface of the treated quartz parts is clean and pollution-free, and the quartz grains are dense and full, meeting the requirements of regeneration. The specific scheme adopted by the present invention is as follows:
[0005] (1) Soaking in organic solvents
[0006] The parts to be cleaned are immersed in an organic solvent for 15 to 20 minutes, and then rinsed with pure water for 1 to 2 minutes to remove oil stains and pollutants on the surface of the quartz window, and to loosen and soften silicon, nitrogen and other deposits; wherein the organic solvent is selected from any one of ethanol, isopropanol and acetone.
[0007] (2) Soaking in high concentration mixed acid solution
[0008] The component treated in step (1) is immersed in a hydrochloric acid and hydrofluoric acid aqueous solution for 30-60 minutes, the optimal solution temperature being 20-35° C., and then washed with pure water to remove most of the surface deposits and react with the quartz grains broken in the etching process; in the mixed acid solution, the volume percentages of the hydrochloric acid and hydrofluoric acid aqueous solutions are: 10%-12% hydrochloric acid, 40%-50% hydrofluoric acid, and the balance is pure water.
[0009] The concentration of the hydrochloric acid solution is 37%, the concentration of the fluoric acid solution is 49%, the pure water is deionized water with a resistivity greater than 16 MΩ, and the pure water rinsing time is 1-2 minutes.
[0010] (3) Immersion in oxidant solution
[0011] After the treatment in step (2), the quartz component is immersed in a 20-35°C ammonia hydrogen peroxide solution for 30-60 minutes to soften and remove the surface sediment, and the residual liquid and residue are rinsed with pure water. The volume percentages of the ammonia hydrogen peroxide solution are: 20%-25% ammonia, 40%-50% hydrogen peroxide, and the remainder is pure water. The concentration of ammonia is 25%, the concentration of hydrogen peroxide is 30%, and the pure water is deionized water with a resistivity greater than 16MΩ. The pure water rinsing time is 1-2 minutes.
[0012] (4) Soak in sulfuric acid solution,
[0013] The quartz component treated in step (3) is immersed in a sulfuric acid solution with a volume percentage of 25%-35% for 30-60 minutes to further remove the surface deposits; the sulfuric acid concentration is 50%, the pure water is deionized water with a resistivity greater than 16MΩ, and the pure water rinsing time is 1-2 minutes.
[0014] (5) Soaking in low concentration mixed acid solution
[0015] The quartz component treated in step (4) is immersed in a low concentration hydrochloric acid and hydrofluoric acid aqueous solution at 20-35° C. for 25-30 minutes to further remove the surface deposits.
[0016] In the low-concentration hydrochloric acid and hydrofluoric acid aqueous solution, the volume percentages of the hydrochloric acid and hydrofluoric acid aqueous solutions are: 4%-5% hydrochloric acid, 2%-3% hydrofluoric acid, and the remainder is pure water; the concentration of the hydrochloric acid solution is 37%, the concentration of the hydrofluoric acid solution is 49%, the pure water is deionized water with a resistivity greater than 16MΩ, and the pure water rinsing time is 1-2 minutes.
[0017] (6) Ultrasonic cleaning
[0018] The quartz parts after step (5) are placed in an ultrasonic cleaning tank for cleaning, with a pure water overflow rate greater than 360 L / h, a pure water resistivity greater than 16 MΩ, and an ultrasonic intensity of 6-10 w / in 2, ultrasonic cleaning time is 30-40 minutes, pure water rinsing time is 1-2 minutes, to remove particles on the surface and in the pores of quartz parts;
[0019] (7) Dust-free drying
[0020] Use a dust-free oven to dry the quartz parts to remove moisture from the surface and make them completely dry. During the drying process, the constant temperature drying temperature is 145-155℃, the constant temperature drying time is 2 hours, and the parts are taken out after cooling to room temperature.
[0021] Through the above treatment method, the silicon, nitrogen and other deposits and related pollutants on the surface of the quartz parts can be removed quickly and efficiently, and the corroded and broken quartz grains can be reacted away to expose dense and smooth quartz grains, thereby achieving the purpose of cleaning and regeneration.
[0022] The beneficial effects of the present invention are as follows:
[0023] The method provided by the present invention uses seven processes in sequence, namely, organic solvent treatment, high-concentration mixed acid solution treatment, oxidant solution treatment, sulfuric acid solution treatment, low-concentration mixed acid solution treatment, ultrasonic cleaning, and dust-free oven drying, to remove the sediment on the surface of the quartz component and the corroded and broken quartz grains. The surface of the treated quartz component is clean and pollution-free, and the quartz grains are dense and full, meeting the requirements of regeneration. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a schematic diagram of the cleaning and regeneration process of the present invention;
[0025] Figure 2 This is a 1000x magnified image of the quartz component surface before cleaning;
[0026] Figure 3 This is a 1000x magnified image of the surface of the quartz component after cleaning. DETAILED DESCRIPTION
[0027] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments. It should be understood by those skilled in the art that the following specific description is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.
[0028] See also Figure 1 The cleaning and regeneration method of the quartz component of the semiconductor etching equipment parts in this embodiment comprises the following steps:
[0029] (1) Soaking in organic solvents
[0030] The samples were immersed in an organic solvent for 15 minutes, the organic solvent was isopropyl alcohol, and the pure water rinsing time was 2 minutes.
[0031] (2) High concentration mixed acid solution treatment
[0032] The quartz parts are immersed in a high concentration hydrochloric acid and hydrofluoric acid aqueous solution for 30 minutes at a solution temperature of 25°C. The volume percentages of the nitric acid and hydrofluoric acid aqueous solution are: 10% hydrochloric acid, 45% hydrofluoric acid, and 45% pure water; the hydrochloric acid concentration is 37%, the hydrofluoric acid concentration is 49%, the pure water is deionized water with a resistivity greater than 16MΩ, and the pure water rinsing time is 2 minutes.
[0033] (3) Oxidant solution treatment;
[0034] Immerse the quartz parts in an ammonia-hydrogen peroxide solution for 30 minutes at a solution temperature of 25°C. The volume percentages of the ammonia-hydrogen peroxide solution are: 20% ammonia, 40% hydrogen peroxide, and 40% pure water; the ammonia concentration is 25%, the hydrogen peroxide concentration is 30%, the pure water is deionized water with a resistivity greater than 16MΩ, and the pure water rinsing time is 2 minutes.
[0035] (4) Sulfuric acid solution treatment;
[0036] The quartz parts are immersed in a sulfuric acid solution for 30 minutes at a solution temperature of 25°C. The volume percentages of the sulfuric acid aqueous solution are: 25% sulfuric acid and 75% pure water. The sulfuric acid concentration is 50%, the pure water is deionized water with a resistivity greater than 16MΩ, and the pure water rinsing time is 2 minutes.
[0037] (5) Low concentration mixed acid solution treatment;
[0038] The quartz parts are immersed in a low-concentration hydrochloric acid and hydrofluoric acid aqueous solution for 30 minutes. The solution temperature is 25°C. The volume percentages of the nitric acid and hydrofluoric acid aqueous solution are: 5% hydrochloric acid, 2% hydrofluoric acid, and 93% pure water; the hydrochloric acid concentration is 37%, the hydrofluoric acid concentration is 49%, the pure water is deionized water with a resistivity greater than 16MΩ, and the pure water rinsing time is 2 minutes.
[0039] (6) Ultrasonic cleaning;
[0040] Place the quartz parts in an ultrasonic cleaning tank for cleaning, with a pure water overflow greater than 360L / h, a pure water resistivity greater than 16MΩ, an ultrasonic intensity of 10w / in2, a cleaning time of 30 minutes, and a pure water rinse time of 2 minutes.
[0041] (7) Dust-free oven drying;
[0042] Place the quartz parts in a dust-free oven and dry them at a constant temperature of 150°C for 2 hours. Take out the parts after cooling to room temperature.
[0043] Figure 2 , Figure 3The following are 1000 times magnified microscope images of the quartz component surface before and after cleaning. By comparison, it can be found that the component surface is clean and pollution-free after cleaning, and the quartz grains are dense and full, achieving the purpose of cleaning and regeneration.
[0044] The preferred embodiments of the present invention have been specifically described above, but the present invention is not limited to the embodiments. Those skilled in the art may make various equivalent modifications or substitutions without violating the spirit of the present invention. These equivalent modifications or substitutions are all included in the scope defined by the claims of this application.
Claims
1. A method for cleaning and regenerating quartz parts for semiconductor dry etching equipment, It is characterized in that The steps include: (1) Soaking in organic solvents Soak the parts to be cleaned in an organic solvent for 15 to 20 minutes, and then rinse with pure water to remove oil stains and pollutants on the surface of the quartz window, and loosen and soften silicon and nitrogen deposits; (2) Soaking in high concentration mixed acid solution The component treated in step (1) is immersed in a hydrochloric acid and hydrofluoric acid aqueous solution for 30-60 minutes, the optimal temperature of the solution being 20-35° C., and then washed with pure water to remove most of the surface deposits and react with the quartz grains broken in the etching process; the volume percentages of the hydrochloric acid and hydrofluoric acid aqueous solutions in the mixed acid solution are: 10%-12% hydrochloric acid, 40%-50% hydrofluoric acid, and the balance is pure water; (3) Immersion in oxidant solution Soak the quartz component after the treatment in step (2) in an ammonia-hydrogen peroxide solution at 20-35° C. for 30-60 minutes to soften and remove surface deposits, wherein the volume percentages of the ammonia-hydrogen peroxide solution are: 20%-25% ammonia, 40%-50% hydrogen peroxide, and the remainder is pure water; (4) Soaking in sulfuric acid solution Soak the quartz component after treatment in step (3) in a 25% to 35% by volume sulfuric acid solution for 30 to 60 minutes to further remove surface deposits; (5) Soaking in low concentration mixed acid solution The quartz window treated in step (4) is immersed in a low-concentration hydrochloric acid and fluoric acid aqueous solution at 20-35° C. for 25-30 minutes to further remove the surface sediment; in the low-concentration hydrochloric acid and fluoric acid aqueous solution, the volume percentages of nitric acid and fluoric acid aqueous solution are: 4%-5% hydrochloric acid, 2%-3% fluoric acid, and the balance is pure water; (6) Ultrasonic cleaning Place the quartz parts after step (5) in an ultrasonic cleaning tank for cleaning at an ultrasonic intensity of 6-10w / in 2 , remove particles on the surface and in the pores of quartz parts; (7) Dust-free drying Use a dust-free oven to dry the quartz parts to remove moisture from the surface and keep them in a completely dry state.
2. The method for cleaning and regenerating a quartz component for semiconductor dry etching equipment according to claim 1, characterized in that: in, In step (1), the organic solvent is selected from any one of ethanol, isopropanol and acetone, and the pure water rinsing time is 1-2 minutes.
3. The method for cleaning and regenerating a quartz component for semiconductor dry etching equipment according to claim 1, characterized in that: in, In step (2), the concentration of hydrochloric acid is 37%, the concentration of hydrofluoric acid solution is 49%, the pure water is deionized water with a resistivity greater than 16 MΩ, and the pure water rinsing time is 1-2 minutes.
4. The method for cleaning and regenerating a quartz component for semiconductor dry etching equipment according to claim 3, characterized in that: in, In step (3), the concentration of ammonia water is 25%, the concentration of hydrogen peroxide is 30%, the pure water is deionized water with a resistivity greater than 16 MΩ, and the pure water rinsing time is 1-2 minutes.
5. The method for cleaning and regenerating a quartz component for semiconductor dry etching equipment according to claim 1, characterized in that: in, In step (4), the concentration of sulfuric acid is 50%, the pure water is deionized water with a resistivity greater than 16 MΩ, and the pure water rinsing time is 1-2 minutes.
6. The method for cleaning and regenerating a quartz component for semiconductor dry etching equipment according to claim 3, characterized in that: in, In step (5), the concentration of hydrochloric acid is 37%, the concentration of fluoric acid solution is 49%, the pure water is deionized water with a resistivity greater than 16 MΩ, and the pure water rinsing time is 1-2 minutes.
7. The method for cleaning and regenerating a quartz component for semiconductor dry etching equipment according to claim 6, characterized in that: in, In step (6), during ultrasonic cleaning, the pure water overflow rate is greater than 360 L / h, the pure water resistivity is greater than 16 MΩ, the ultrasonic cleaning time is 30-40 minutes, and the pure water rinsing time is 1-2 minutes.
8. The method for cleaning and regenerating a quartz component for semiconductor dry etching equipment according to claim 1, characterized in that: in, In step (7), the constant temperature drying temperature is 150° C., the constant temperature drying time is 2 hours, and the parts are taken out after cooling to room temperature.
Citation Information
Cited By
A method for regenerating and repairing a quartz boat for semiconductor wafer processing
CN122938093A